A thermal aging test platform and test method for aviation motor winding insulation

By designing a multi-temperature and multi-parameter thermal aging test platform for aviation motor winding insulation, using high-temperature aging oven groups and twisted wire pairs combined with megohmmeters and LCR precision instruments, the method's lack of adaptability in the research on thermal aging of low-voltage aviation motor winding insulation was solved. problem, achieving fast, comprehensive and accurate insulation status assessment.

CN113671298BActive Publication Date: 2024-10-22CHONGQING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111113010.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-09-23
Publication Date
2024-10-22
Estimated Expiration
2041-09-23

AI Technical Summary

Technical Problem

The existing technology has insufficient method adaptability in the study of thermal aging characteristics of low-voltage aircraft motor winding insulation, which results in difficult, high-cost and inaccurate test operations. A single parameter cannot fully reflect the winding insulation state.

Method used

Design a multi-temperature multi-parameter aviation motor winding insulation thermal aging test platform, including a high-temperature aging oven group and twisted wire pairs, combined with a megohmmeter and LCR precision instrument, to simulate the aviation motor winding inter-turn insulation, and accelerate thermal aging through periodicity and Insulation parameter measurement enables characteristic analysis of multiple insulation characterization parameters.

Benefits of technology

It achieves a rapid, comprehensive and accurate assessment of the thermal aging characteristics of the aviation motor winding insulation, reduces the test cost and time, and improves the accuracy and feasibility of the assessment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113671298B_ABST
    Figure CN113671298B_ABST
Patent Text Reader

Abstract

The present invention discloses a thermal aging test platform and test method for insulation of aviation motor windings. The test platform includes a high-temperature aging oven group and a twisted wire pair. The high-temperature aging oven group includes multiple high-temperature aging ovens. The high-temperature aging oven has a multi-layer test bench. The twisted wire pair is placed on the test bench. It also includes a megohmmeter and an LCR precision meter. The test method includes S1: making and drying a twisted wire pair sample; S2: placing the twisted wire pair sample into the high-temperature aging oven group, performing periodic accelerated thermal aging and insulation parameter measurement; S3: after the insulation parameter measurement, performing insulation failure judgment on the twisted wire pair sample. If it fails, the aging ends, otherwise the aging continues until the insulation fails; S4: averaging the insulation parameter measurement values ​​of the same group of samples at the same temperature point, and analyzing to obtain the thermal aging characteristic curves of the winding insulation at different temperatures. The test platform and method of the present invention can obtain the thermal aging characteristics of the insulation of aviation motor windings in a relatively short time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of aviation electrification, and in particular relates to a multi-temperature and multi-parameter aviation motor winding insulation thermal aging test platform and test method. Background Art

[0002] Aviation electromechanical transmission devices use a large number of low-voltage motors with insulation type I structure (rated voltage less than 700V), and the safe operation of these motors will be directly related to the safety, reliability and stability of aircraft operation. In motors, the number of winding insulation failures accounts for more than 40% of the total number of failures. For low-voltage motors in aviation applications, due to the requirements of high power density, their rated working current is large and the heat generation is serious; when the aircraft is cruising normally, the motor needs to run at full heat load for a long time, and due to the space limitations of the aircraft, the heat dissipation of the motor winding is difficult, resulting in a higher operating temperature of the aircraft motor winding than that of ordinary motors, resulting in thermal aging becoming the main cause of its insulation degradation. Therefore, it is of great significance to evaluate the insulation status of aviation motor winding insulation by the thermal aging characteristics.

[0003] However, the current research on the thermal aging of motor winding insulation is more focused on the electrical aging characteristics of large generators in power systems or high-voltage variable-frequency traction motors in the field of rail transportation. Therefore, there is a lack of method adaptability in the study of the thermal aging characteristics of low-voltage motors. For low-voltage aviation motors, it is usually required to be able to operate without failure for more than 20,000 hours at normal operating temperatures. Therefore, it takes a long time to study its thermal aging characteristics under conventional working conditions. In addition, in the aging characteristic test, if the actual application motor is directly used for testing, the test operation is difficult, the cost is high, the actual application is difficult, and the feasibility is low. In addition, a single insulation state parameter can only reflect the local defects of the winding insulation, so when a single parameter is used to evaluate the winding insulation state, there will be a big difference from the actual situation. Therefore, a test platform and test method that can quickly, comprehensively and accurately reflect the thermal aging characteristics of aviation motor winding insulation are needed. Summary of the invention

[0004] In view of this, one of the purposes of the present invention is to provide a test platform that is more time efficient and can more comprehensively and accurately simulate the characteristic analysis of aviation motor winding insulation under thermal stress.

[0005] After research, the above-mentioned purpose of the present invention adopts the following technical scheme:

[0006] A thermal aging test platform for insulation of aircraft motor windings includes a high-temperature aging oven group and a twisted wire pair. The high-temperature aging oven group includes multiple high-temperature aging ovens, and the twisted wire pair is located in each of the high-temperature aging ovens. It also includes a megohmmeter for measuring the insulation resistance of the twisted wire pair, and an LCR precision meter for measuring the dielectric loss tangent and insulation capacitance of the twisted wire pair. The high-temperature aging oven is used to provide multiple test temperatures, the twisted wire pair simulates the inter-turn insulation of the aircraft motor winding, and the megohmmeter and the LCR precision meter are used to detect multiple test parameters.

[0007] Furthermore, the high-temperature aging oven is provided with a multi-layer test bench, and the twisted wire pair is placed on the test bench.

[0008] Furthermore, the high temperature aging oven group consists of three high temperature aging ovens with a temperature control accuracy of within ±3°C and a temperature control range of 0-800°C.

[0009] Preferably, the temperature control accuracy of the high-temperature aging oven is within ±1°C, the temperature control range is 0-500°C, the megohmmeter is a digital megohmmeter with multiple voltage levels and a measurement range of 1000GΩ; the LCR precision meter can achieve a measurement frequency range of 20Hz-5MHz.

[0010] Furthermore, the twisted wire pair is made of m (m≥1) thermal grade aviation motor winding wire, the bending part of the electrode end of the twisted wire pair is 20-50mm long, the end of the electrode end is 10-30mm long and is bare copper, the parallel part of the twisted wire pair is 50-150mm long, and the bending part at the end of the twisted wire pair is 10-30mm long; the bare copper part of the electrode end is used as an electrode for measuring insulation state parameters.

[0011] A second object of the present invention is to provide a fast, comprehensive and accurate accelerated test method for testing the thermal aging characteristics of aviation motor winding insulation.

[0012] After research, the above-mentioned purpose of the present invention adopts the following technical scheme:

[0013] This test method includes the following steps:

[0014] S1: Prepare and dry the twisted wire pair specimens;

[0015] S2: Place the twisted wire pair samples in an aging chamber for periodic accelerated thermal aging and insulation parameter measurement;

[0016] S3: After the insulation parameters are measured, the insulation failure of the winding is judged. If it fails, the aging process ends; otherwise, the aging process continues until the insulation fails.

[0017] S4: Take the average of the insulation parameter measurement values ​​of the same group of samples at the same temperature point, and analyze to obtain the thermal aging characteristic curve of winding insulation at different temperatures.

[0018] Further, the specific process in step S1 is as follows: according to the aforementioned twisted wire pair parameters, 3-6N (N≥5) twisted wire pair samples are prepared using the m-type winding wires required for the thermal aging test, and the prepared samples are placed in an oven and dried at 50-150° C. for 2-5 hours. In addition, during the production process, the twisted wire parts are twisted as evenly as possible, and bending and folding at the ends of the twisted wire pairs are avoided as much as possible to avoid mechanical damage to the insulating material.

[0019] Furthermore, the specific process in step S2 is as follows: select 3-6 temperature points within 250°C higher than the thermal grade temperature of the winding wire, and place N samples of each type of twisted wire pair on the test bench in the high-temperature aging oven at each temperature point, and perform accelerated thermal aging for a fixed period (5-500h) at the same time at three aging temperatures.

[0020] Furthermore, after each aging cycle, the metal oxide layer at the electrode portion of the twisted wire pair sample is first removed, and then the dielectric loss tangent tanδ, insulation capacitance IC, and insulation resistance IR are measured in turn.

[0021] Furthermore, the specific process of tanδ measurement in step S2 is as follows: select n (n≥2) frequency points in the range of 1kHz-5MHz to measure tanδ j The average value is taken as the dielectric loss characterization value of the sample, that is, the tanδ of the sample can be calculated as follows:

[0022]

[0023] Furthermore, the specific process of IC measurement in step S2 is as follows: n (n≥2) frequency points in the range of 1kHz-5MHz are selected to measure IC j The average value is taken as the insulation capacitance value of the sample, and the calculation formula is as follows:

[0024]

[0025] Furthermore, the specific process of IR measurement in step S2 is as follows: the measured value of the megohmmeter when pressurized for 1 minute is selected as the insulation resistance of the twisted wire pair. When measuring, first use the low voltage gear for measurement, and if the measurement exceeds the range, gradually increase to a higher voltage gear.

[0026] IR=IR 1min (3)

[0027] Furthermore, the specific process in step S3 is as follows: after each aging cycle is completed and the insulation parameters are measured, a DC or AC withstand voltage test with an effective voltage value of 0.5-10 kV is performed on the twisted wire pair for 0.5-1 min. If the twisted wire pair fails the withstand voltage test, the insulation fails and the aging is completed; otherwise, the insulation does not fail and the thermal aging test is continued until the insulation fails.

[0028] Furthermore, the specific process in step S4 is as follows: first, the mean values ​​of tanδ, IC, and IR of N samples of the same thermal grade at the same aging temperature are calculated according to formula (4) (where P represents tanδ, IC, IR, θ represents temperature, and j represents the sample number), and the variation curves of tanδ, IC, and IR with aging time are obtained by fitting with the matlab data fitting tool.

[0029]

[0030] The beneficial effects of the present invention are:

[0031] The present invention provides a test platform and a test method for simulating the inter-turn insulation of aviation motor windings with twisted wire pairs, and capable of simultaneously realizing characteristic analysis of multiple insulation characterization parameters of aviation motor winding insulations of multiple thermal grades under different thermal stresses. The test platform and a test method can more quickly, accurately and comprehensively analyze and study the thermal aging characteristics of motor winding insulation, so that the insulation state evaluation of aviation motor winding insulation under thermal stress can be realized in an economical, time-efficient and more accurate manner, and the test platform and a test method have practical feasibility and wide popularization. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 It is a schematic diagram of a multi-temperature and multi-parameter aviation motor winding insulation thermal aging test oven group and a twisted wire pair of the present invention;

[0033] Figure 2 This is a physical picture of a twisted wire pair sample of the present invention;

[0034] Figure 3 It is a flow chart of the test method for thermal aging characteristics of aviation motor winding insulation of the present invention. DETAILED DESCRIPTION

[0035] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Embodiment 1: As attached Figure 1As shown, this embodiment provides a thermal aging test platform for multi-temperature and multi-parameter measurement of aviation motor winding insulation, including a high-temperature aging oven group 1 for providing a heat source; a twisted wire pair sample 2 for simulating the inter-turn insulation of the aviation motor winding, a megohmmeter for insulation resistance measurement, and an LCR precision meter for measuring dielectric loss tangent and insulation capacitance.

[0037] In this embodiment, the high temperature aging oven group is composed of 3 high-precision high temperature aging ovens with a temperature control accuracy of ±3°C and a temperature control range of 0-800°C; each high temperature aging oven is provided with a vertical multi-layer test bench, and the twisted wire pair sample is placed on the test bench. The megohmmeter is a digital megohmmeter with multiple voltage levels and a measurement range of up to 1000GΩ; the LCR precision meter can achieve a measurement frequency range of 20Hz-1MHz.

[0038] The temperature control accuracy of the high temperature aging oven can be selected but not limited to ±1°C, ±2°C or ±3°C. As an implementation in this embodiment, the temperature control accuracy of the high temperature aging oven is ±1°C, and the temperature control range is set to 50-500°C.

[0039] In this embodiment, correspondingly, the twisted wire pair samples are made of aviation motor winding wires of three types of thermal grades, namely QZY-2 / 180, QXY-2 / 200, and QY-2 / 220, and 30 samples of each type of thermal grade twisted wire pair are produced.

[0040] The length of the bent portion of the electrode end of the finished twisted wire pair is 20-50mm, which can be selected but not limited to 20mm, 25mm, 30mm, 35mm, 40mm, 45mm or 50mm. In this embodiment, the length of the electrode end of the twisted wire pair is 35mm. As the end portion of the electrode segment, the surface insulation layer needs to be stripped to expose the bare copper as the electrode for measuring the insulation state parameter. The length of the bare copper part is 10-30mm, which can be selected but not limited to 10mm, 15mm, 20mm, 25mm or 30mm. In this embodiment, the length of the bare copper is 15mm. The length of the parallel part of the twisted wire pair is 50-150mm, which can be selected but not limited to 50mm, 60mm, 70mm, 80mm, 90mm, 100mm, 110mm, 120mm, 130mm, 140mm or 150mm. In this embodiment, the length of the parallel part is 80mm. The length of the bent portion of the end of the twisted wire pair (the other end opposite to the electrode end) is 10-30 mm, which can be selected but not limited to 10 mm, 15 mm, 20 mm, 25 mm or 30 mm. In this embodiment, the length of the bent portion of the end of the twisted wire pair is 10 mm. Figure 2 shown.

[0041] See attached Figure 3This embodiment also provides a test method for performing a thermal aging characteristic test of aviation motor winding insulation using the above-mentioned thermal aging test platform, comprising the following steps:

[0042] S1: Prepare and dry the twisted wire pair specimens;

[0043] S2: Place the twisted wire pair samples on various test benches in a high-temperature aging oven to perform periodic accelerated thermal aging and insulation parameter measurements;

[0044] S3: After measuring the insulation parameters, the insulation failure of the winding is judged. If it fails, the aging process ends; otherwise, the aging process continues until the insulation fails.

[0045] S4: Take the average of the insulation parameter measurement values ​​of the same group of samples at the same temperature point, and analyze to obtain the thermal aging characteristic curve of winding insulation at different temperatures.

[0046] In this embodiment, the specific process of step S1 is as follows: according to the above-mentioned twisted wire pair parameters, 30 twisted wire pair samples are made, and the made samples are placed in an oven and dried at 100° C. for 2 hours. During the production process, the twisted wire parts are twisted as evenly as possible, and bending and folding at the ends of the twisted wire pairs are avoided as much as possible to avoid mechanical damage to the insulating material.

[0047] In addition, the drying temperature of the twisted wire pair may be selected but not limited to 80°C, 90°C, 110°C, 120°C, 130°C, 140°C or 150°C, and the drying time may be selected but not limited to 3h, 4h or 5h.

[0048] In this embodiment, the specific process in step S2 is as follows: the aging temperature of the high temperature aging oven group is selected as 240℃, 260℃, 280℃, 300℃, 320℃, and 340℃. Among them, 240℃, 260℃, and 280℃ are used as the first group for aging test; after the first group of aging is completed, 300℃, 320℃, and 340℃ are used as the second group for aging test. During the test, 5 samples of twisted wire pairs of 3 types of temperature grades are placed in each of the three high temperature aging ovens, and accelerated thermal aging tests with an aging cycle of 10 hours are carried out at the same time at the three aging temperatures. The aging cycle can also be selected but not limited to 5h, 50h, 100h, 150h, 200h, 250h, 300h, 350h, 400h, 450h or 500h.

[0049] In this embodiment, after every 10-hour aging cycle in step S2, the metal oxide layer at the electrode portion of the twisted wire pair sample is first removed, and then the dielectric loss tangent tanδ, insulation capacitance IC, and insulation resistance IR are measured in sequence.

[0050] In this embodiment, the specific process of tanδ measurement in step S2 is as follows: 10 logarithmically spaced frequency points between 100kHz and 1MHz are selected to measure tanδ j The value is taken as the single sample tanδ measurement value, that is, the sample tanδ can be calculated as follows:

[0051]

[0052] In this embodiment, the specific process of IC measurement in step S2 is as follows: 10 logarithmically spaced frequency points between 100kHz and 1MHz are selected to measure IC j The value is taken as the IC measurement value of a single sample and is calculated as follows:

[0053]

[0054] In this embodiment, the specific process of IR measurement in step S2 is as follows: the measured value of the megohmmeter under pressure for 1 minute is selected as the insulation resistance of the twisted wire pair. When measuring, first use the low voltage gear for measurement, and if the measurement exceeds the range, gradually increase to a higher voltage gear.

[0055] IR=IR 1min (3)

[0056] In this embodiment, the specific process in step S3 is as follows: after each aging cycle is completed and the insulation parameters are measured, a 5000V DC withstand voltage test is performed on the twisted wire pair for 1 minute. If the twisted wire pair fails the withstand voltage test, the insulation fails and the aging is completed. Otherwise, the insulation does not fail, and the thermal aging test is continued until the insulation fails.

[0057] In this embodiment, the specific process in step S4 is as follows: first, the average values ​​of tanδ, IC, and IR of 5 samples of the same thermal grade at the same aging temperature are calculated according to formula (4) (where P represents tanδ, IC, IR, θ represents temperature, and j represents the sample number), and the variation curves of tanδ, IC, and IR with aging time are obtained by fitting with the matlab data fitting tool.

[0058]

[0059] The present embodiment provides a test platform and test method for simulating the inter-turn insulation of aviation motor windings with twisted wire pairs, and capable of simultaneously realizing characteristic analysis of multiple insulation characterization parameters of aviation motor winding insulation of multiple thermal grades under different thermal stresses. The test platform and test method can more quickly, accurately and comprehensively analyze and study the thermal aging characteristics of motor winding insulation, so that the insulation status evaluation of aviation motor winding insulation under thermal stress can be realized in an economical, time-efficient and more accurate manner, and the test platform and test method have practical feasibility and wide applicability.

Claims

1. A method for thermal aging test of aviation motor winding insulation, characterized in that: The invention comprises an aviation motor winding insulation thermal aging test platform, the test platform comprises a high-temperature aging oven group and a twisted wire pair, the high-temperature aging oven group comprises a plurality of high-temperature aging ovens, the high-temperature aging oven has a multi-layer test bench, the twisted wire pair is placed on the test bench, and also comprises a megohmmeter for measuring the insulation resistance of the twisted wire pair, and an LCR precision meter for measuring the dielectric loss tangent and insulation capacitance of the twisted wire pair; The test method comprises the following steps: S1: Prepare and dry the twisted wire pair specimens; The twisted wire pair is made of M-class thermal grade aviation motor winding wire, m≥1, the bending part of the electrode end of the twisted wire pair is 20-50mm long, the end of the electrode end is 10-30mm long and is bare copper, the parallel part of the twisted wire pair is 50-150mm long, and the bending part of the end of the twisted wire pair is 10-30mm long; the bare copper part of the electrode end is used as an electrode for measuring insulation state parameters; S2: placing the twisted wire pair sample into the high temperature aging oven group to perform periodic accelerated thermal aging and insulation parameter measurement; The number of samples of each type of thermal grade twisted wire pair in S1 is ≥3N, N ≥5, and the prepared samples are placed in an oven and dried at 50-150°C for 2-5 hours; In S2, 3-6 temperature points within 250°C higher than the thermal grade temperature of the winding wire are selected, and N samples of each type of thermal grade twisted wire pair are placed in a high-temperature aging oven at 3 different temperature points at the same time, and accelerated thermal aging is performed for a fixed period of 5-500h. After each aging cycle, the dielectric loss tangent tanδ, insulation capacitance IC, and insulation resistance IR are measured in turn; S3: After the insulation parameters are measured, the insulation failure of the stranded wire pair sample is judged. If it fails, the aging is terminated, otherwise, the aging is continued until the insulation fails; S4: Take the average of the insulation parameter measurement values ​​of the same group of samples at the same temperature point, and analyze to obtain the thermal aging characteristic curve of winding insulation at different temperatures.

2. The aviation motor winding insulation thermal aging test method according to claim 1, characterized in that: The tanδ measurement method in S2 is: select n frequency points in the range of 1kHz-5 MHz, n≥2, and measure tanδ j The average value is taken as the dielectric loss characterization value of the sample, that is, the tanδ of the sample can be calculated as follows: The IC measurement method in S2 is: select n (n≥2) frequency points in the range of 1kHz-5 MHz to measure IC j The average value is taken as the insulation capacitance value of the sample, and the calculation formula is as follows: The IR measurement method in S2 is: select the measured value of the megohmmeter when it is pressurized for 1 minute as the insulation resistance of the twisted wire pair. When measuring, first use the low voltage gear to measure. If the measurement exceeds the range, gradually increase to a higher voltage gear. The calculation formula is: IR = IR 1min .

3. The method for thermal aging test of aviation motor winding insulation according to claim 1, characterized in that: In S3, after each aging cycle is completed and the insulation parameters are measured, a DC or AC withstand voltage test with an effective voltage of 0.5-10kV is performed on the twisted pair for 0.5-1min. If the twisted pair passes the withstand voltage test, the insulation has not failed and the thermal aging test continues. Otherwise, the insulation fails and the aging test ends.

4. The method for thermal aging test of aviation motor winding insulation according to claim 1, characterized in that: In S4, firstly, the average values ​​of tanδ, IC, and IR of N twisted wire pairs of samples with the same thermal grade at the same aging temperature are calculated, and the variation curves of the winding insulation parameters with the aging time at different temperatures are obtained by data fitting.