Use of organosilicon surfactant, method for improving sensitivity of electron beam photoresist, electron beam photoresist and preparation and use thereof
By adding silicone surfactant containing alkylene oxide and dimethylsiloxane structures to the electron beam photoresist, the problem of low sensitivity of electron beam photoresist in the prior art is solved, and a higher sensitivity is achieved lithographic pattern resolution and sensitivity.
Patent Information
- Application Number
- CN202110982032.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-08-25
AI Technical Summary
The existing electron beam photoresist has low sensitivity and is difficult to meet the high requirements of nanoscale lithography technology.
Add silicone surfactant containing alkylene oxide and dimethylsiloxane structures to the electron beam photoresist to improve its sensitivity.
By adding silicone surfactant, the sensitivity of the electron beam photoresist is significantly improved, and the sensitivity can be adjusted within a suitable range, the exposure energy can be reduced, and the resolution of the photolithographic pattern can be improved.
Smart Images

Figure CN113671796B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electron beam photoresists, and in particular to the use of an organosilicon surfactant, a method for improving the sensitivity of electron beam photoresists, electron beam photoresists, and preparation and use thereof. Background Art
[0002] Electron-beam Lithography (EBL), as the next generation of lithography technology, is considered to be one of the most promising lithography technologies below the 22-nanometer node due to its high resolution and stable performance. The progress of lithography technology is often inseparable from the development of lithography materials. In recent years, electron beam, as a nanoscale lithography technology, has put forward higher requirements for lithography materials. Electron beam photoresist is a type of lithography material coated on the surface of the substrate to achieve pattern transfer through electron beam exposure. Electron beam photoresist can be divided into positive photoresist and negative photoresist according to whether cross-linking or chemical bond breaking occurs before and after polymer irradiation.
[0003] After the photoresist is exposed to electron beam, its polymer chemical bonds break, and the broken polymer fragments are easily soluble in the developer, which is a positive photoresist. On the contrary, after exposure, the photoresist is cross-linked and polymerized from small molecules to large molecules, and the exposed photoresist is difficult to dissolve in the developer, which is a negative photoresist. Polymethyl methacrylate (PMMA) is the earliest and most common positive electron beam photoresist. PMMA can be used to prepare graphics with very high resolution, and its maximum size can even be less than 10nm, but it has the problem of low sensitivity.
[0004] Therefore, there is an urgent need for an electron beam photoresist with high sensitivity in this field. Summary of the invention
[0005] The purpose of the present invention is to provide an application of an organosilicon surfactant and a method for improving the sensitivity of an electron beam photoresist in order to overcome the defects of the above-mentioned prior art.
[0006] The purpose of this application is also to provide a highly sensitive electron beam photoresist and a preparation method and a use method thereof.
[0007] In order to achieve the purpose of the present invention, this application provides the following technical solutions.
[0008] In a first aspect, the present application provides a use of an organosilicon surfactant for improving the sensitivity of an electron beam photoresist.
[0009] In a preferred embodiment of the first aspect, at least one of the following technical features is also included:
[0010] 1a) The organosilicon surfactant includes a surfactant containing an alkylene oxide group and a dimethylsiloxane group structure;
[0011] 1b) the electron beam photoresist comprises polymethyl methacrylate, a solvent and the organosilicon surfactant;
[0012] 1c) The organic silicon surfactant accounts for 0.1% to 3% of the mass of the polymer resin in the electron beam photoresist.
[0013] In a preferred embodiment of the first aspect, at least one of the following technical features is also included:
[0014] 2a) The surfactant containing an alkylene oxide group and a dimethylsiloxane group structure has a structure as shown in Formula I:
[0015]
[0016] Wherein, R is hydrogen or alkyl; x is an integer of 1 to 20; m is an integer of 2 to 100; n is an integer of 2 to 100; preferably, R is a C1 to C5 alkyl;
[0017] 2b) In the surfactant containing epoxyalkylene and dimethylsiloxane structures, the mass fraction of epoxyalkylene and dimethylsiloxane groups is 15% to 85%;
[0018] 2c) In the organosilicon surfactant, the mass fraction of the surfactant containing epoxyalkyl group and dimethylsiloxane group structure is 30% to 100%;
[0019] 2d) The mass percentages of the components of the electron beam photoresist are as follows:
[0020] Polymethyl methacrylate 2-15%;
[0021] Solvent 84.85~97.998%;
[0022] Silicone surfactant 0.002~0.15%;
[0023] 2e) The weight average molecular weight of the polymethyl methacrylate is in the range of 30,000 to 1,000,000;
[0024] 2f) The molecular weight distribution of the polymethyl methacrylate is less than 3;
[0025] 2g) the solvent is selected from at least one of anisole, toluene, xylene, trimethylbenzene, chlorobenzene, dichlorobenzene, propylene glycol monoacetate, propylene glycol monoethyl ether, propylene glycol methyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol methyl ethyl ether, butyl acetate, neopentyl acetate, ethyl lactate, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, diacetone alcohol, gamma-butyrolactone and ethyl lactate;
[0026] 2h) The electron beam photoresist further comprises an auxiliary agent, wherein the auxiliary agent is selected from at least one of a photoacid generator, a viscosity controller, a stabilizer and a leveling agent; preferably, the mass percentage of each component of the electron beam photoresist is as follows:
[0027] Polymethyl methacrylate 2-15%;
[0028] Solvent 84.7~97.996%;
[0029] Silicone surfactant 0.002~0.15%;
[0030] Additives: 0.002~0.15%.
[0031] In a second aspect, the present application provides a method for improving the sensitivity of electron beam photoresist, the method comprising: adding an organic silicon surfactant when preparing the electron beam photoresist.
[0032] In a preferred embodiment of the second aspect, at least one of the following technical features is also included:
[0033] 3a) The organosilicon surfactant includes a surfactant containing an alkylene oxide group and a dimethylsiloxane group structure;
[0034] 3b) the electron beam photoresist comprises polymethyl methacrylate, a solvent and the organosilicon surfactant;
[0035] 3c) The organic silicon surfactant accounts for 0.1% to 3% of the mass of the polymer resin in the electron beam photoresist.
[0036] In a preferred embodiment of the second aspect, at least one of the following technical features is also included:
[0037] 4a) The surfactant containing an alkylene oxide group and a dimethylsiloxane group structure has a structure as shown in Formula I:
[0038]
[0039] Wherein, R is hydrogen or alkyl; x is an integer of 1 to 20; m is an integer of 2 to 100; n is an integer of 2 to 100; preferably, R is a C1 to C5 alkyl;
[0040] 4b) In the surfactant containing epoxyalkylene and dimethylsiloxane structures, the mass fraction of epoxyalkylene and dimethylsiloxane groups is 15% to 85%;
[0041] 4c) In the organosilicon surfactant, the mass fraction of the surfactant containing epoxyalkyl group and dimethylsiloxane group structure is 30% to 100%;
[0042] 4d) The mass percentages of the components of the electron beam photoresist are as follows:
[0043] Polymethyl methacrylate 2-15%;
[0044] Solvent 84.85~97.998%;
[0045] Silicone surfactant 0.002~0.15%;
[0046] 4e) The weight average molecular weight of the polymethyl methacrylate is in the range of 30,000 to 1,000,000;
[0047] 4f) the molecular weight distribution of the polymethyl methacrylate is less than 3;
[0048] 4g) the solvent is selected from at least one of anisole, toluene, xylene, trimethylbenzene, chlorobenzene, dichlorobenzene, propylene glycol monoacetate, propylene glycol monoethyl ether, propylene glycol methyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol methyl ethyl ether, butyl acetate, neopentyl acetate, ethyl lactate, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, diacetone alcohol, gamma-butyrolactone and ethyl lactate;
[0049] 4h) The electron beam photoresist further comprises an auxiliary agent, wherein the auxiliary agent is selected from at least one of a photoacid generator, a viscosity controller, a stabilizer and a leveling agent; preferably, the mass percentage of each component of the electron beam photoresist is as follows:
[0050] Polymethyl methacrylate 2-15%;
[0051] Solvent 84.7~97.996%;
[0052] Silicone surfactant 0.002~0.15%;
[0053] Additives: 0.002~0.15%.
[0054] In a third aspect, the present application also provides an electron beam photoresist, wherein the electron beam photoresist comprises the following components in percentage by mass:
[0055] Polymethyl methacrylate 2-15%;
[0056] Solvent 84.85~97.998%;
[0057] Silicone surfactant 0.002~0.15%.
[0058] In a preferred embodiment of the third aspect, at least one of the following technical features is also included:
[0059] 5a) The organosilicon surfactant includes a surfactant containing an alkylene oxide group and a dimethylsiloxane group structure;
[0060] Preferably, the surfactant containing an alkylene oxide group and a dimethylsiloxane group structure has a structure as shown in Formula I:
[0061]
[0062] Wherein, R is hydrogen or alkyl; x is an integer of 1 to 20; m is an integer of 2 to 100; n is an integer of 2 to 100; preferably, R is a C1 to C5 alkyl;
[0063] Preferably, in the surfactant containing epoxyalkylene groups and dimethylsiloxane groups, the mass fraction of epoxyalkylene groups and dimethylsiloxane groups is 15% to 85%;
[0064] Preferably, in the organosilicon surfactant, the mass fraction of the surfactant containing epoxyalkyl group and dimethylsiloxane group structure is 30% to 100%;
[0065] 5b) The mass percentages of the components of the electron beam photoresist are as follows:
[0066] Polymethyl methacrylate 2-15%;
[0067] Solvent 84.85~97.998%;
[0068] Silicone surfactant 0.002~0.15%;
[0069] 5c) The weight average molecular weight of the polymethyl methacrylate is in the range of 30,000 to 1,000,000;
[0070] 5d) the molecular weight distribution of the polymethyl methacrylate is less than 3;
[0071] 5e) the solvent is selected from at least one of anisole, toluene, xylene, trimethylbenzene, chlorobenzene, dichlorobenzene, propylene glycol monoacetate, propylene glycol monoethyl ether, propylene glycol methyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol methyl ethyl ether, butyl acetate, neopentyl acetate, ethyl lactate, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, diacetone alcohol, gamma-butyrolactone and ethyl lactate;
[0072] 5f) The electron beam photoresist further comprises an auxiliary agent, wherein the auxiliary agent is selected from at least one of a photoacid generator, a viscosity controller, a stabilizer and a leveling agent; preferably, the mass percentages of the components of the electron beam photoresist are as follows:
[0073] Polymethyl methacrylate 2-15%;
[0074] Solvent 84.7~97.996%;
[0075] Silicone surfactant 0.002~0.15%;
[0076] Additives 0.002~0.15%;
[0077] 5g) The organic silicon surfactant is 0.1% to 3% of the mass of the polymer resin in the electron beam photoresist.
[0078] In a fourth aspect, the present application also provides a method for preparing the electron beam photoresist as described above, wherein the polymethyl methacrylate, a solvent and an organosilicon surfactant are mixed to obtain the electron beam photoresist.
[0079] In a fifth aspect, the present invention further provides a method for using the electron beam photoresist as described above, the method comprising the following steps:
[0080] The electron beam photoresist is coated on a silicon wafer, and subjected to pre-baking, exposure and development in sequence to obtain a photolithography pattern; preferably, at least one of the following technical features is also included:
[0081] 6a) The pre-baking temperature is 100-200°C;
[0082] 6b) Pre-baking time is 60 to 180 seconds;
[0083] 6c) Exposure energy is 0.1~20C / m 2 ;
[0084] 6d) the developer comprises at least one selected from methyl isobutyl ketone and isopropyl alcohol; preferably, the developer contains water;
[0085] 6e) The developing time is 30 to 90 seconds.
[0086] Compared with the prior art, the present invention has the following beneficial effects:
[0087] The invention proposes that an organic silicon surfactant is used to improve the sensitivity of electron beam photoresist, and the electron beam photoresist has better sensitivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0088] Figure 1 This is the photolithography pattern obtained by the electron beam photoresist in Example 1.
[0089] Figure 2 This is the photolithography pattern obtained by the electron beam photoresist of Example 2.
[0090] Figure 3 This is the photolithography pattern obtained by the electron beam photoresist of Example 3. DETAILED DESCRIPTION
[0091] Unless otherwise indicated, implied from the context, or customary in the prior art, all parts and percentages in this application are based on weight, and the test and characterization methods used are all current as of the filing date of this application. Where applicable, the contents of any patent, patent application or publication referred to in this application are fully incorporated herein by reference, and their equivalent patent families are also incorporated by reference, especially the definitions of synthesis techniques, product and processing designs, polymers, comonomers, initiators or catalysts disclosed in these documents in the art. If the definition of a specific term disclosed in the prior art is inconsistent with any definition provided in this application, the definition of the term provided in this application shall prevail.
[0092] Numerical ranges in this application are approximate values, so unless otherwise specified, they may include values outside the range. Numerical ranges include all values from the lower limit to the upper limit increased by 1 unit, provided that there is an interval of at least 2 units between any lower value and any higher value. For example, if the recorded component, physical or other properties (such as molecular weight, melt index, etc.) are 100 to 1000, it means that all single values are clearly listed, such as 100, 101, 102, etc., and all sub-ranges, such as 100 to 166, 155 to 170, 198 to 200, etc. For a range comprising a value less than 1 or comprising a fraction greater than 1 (such as 1.1, 1.5, etc.), 1 unit is appropriately regarded as 0.0001, 0.001, 0.01 or 0.1. For ranges containing single digit numbers less than 10 (e.g., 1 to 5), 1 unit is generally considered to be 0.1. These are only specific examples of what is intended, and all possible combinations of numerical values between the lowest and highest values recited are considered to be expressly stated in this application. The numerical ranges within this application provide, among other things, calcium-containing filler content, stirring temperature, and various features and properties of these components.
[0093] When used with respect to chemical compounds, unless expressly specified otherwise, the singular includes all isomeric forms and vice versa (e.g., "hexane" includes all isomers of hexane, individually or collectively). In addition, nouns using "a," "an," or "the" also include their plural forms unless expressly specified otherwise.
[0094] The terms "comprising", "including", "having" and their derivatives do not exclude the presence of any other components, steps or processes, and are irrelevant to whether these other components, steps or processes are disclosed in this application. To eliminate any doubt, unless explicitly stated, all compositions using the terms "comprising", "including", or "having" in this application may include any additional additives, adjuvants or compounds. On the contrary, except for those necessary for operating performance, the term "essentially consisting of..." excludes any other components, steps or processes from the scope of any description of the term below. The term "consisting of..." does not include any components, steps or processes that are not specifically described or listed. Unless explicitly stated, the term "or" refers to the listed individual members or any combination thereof.
[0095] A first aspect of the present invention provides a use of an organosilicon surfactant for improving the sensitivity of electron beam photoresist.
[0096] Preferably, it also includes at least one of the following technical features:
[0097] 1a) The organosilicon surfactant includes a surfactant containing an alkylene oxide group and a dimethylsiloxane group structure;
[0098] 1b) the electron beam photoresist comprises polymethyl methacrylate, a solvent and the organosilicon surfactant;
[0099] 1c) The organic silicon surfactant is 0.1% to 3% by mass of the polymer resin in the electron beam photoresist, such as 0.1% to 0.2%, 0.2% to 0.4%, 0.4% to 0.6% or 0.6% to 3%.
[0100] The organosilicon surfactant improves the stretchability of the polymethyl methacrylate chain in the film, increases the free volume, is beneficial to the diffusion of electrons and interacts with the main chain or side chain of the polymethyl methacrylate, thereby improving the sensitivity.
[0101] More preferably, it also includes at least one of the following technical features:
[0102] 1a1) In feature 1a), in the surfactant containing an alkylene oxide and a dimethylsiloxane structure, the mass percentage of the alkylene oxide and the dimethylsiloxane group is 15% to 85%;
[0103] 1a2) In feature 1a), the surfactant containing an alkylene oxide group and a dimethylsiloxane group structure has a structure as shown in Formula I:
[0104]
[0105] Wherein, R is hydrogen or an alkyl group; x is an integer of 1 to 20; m is an integer of 2 to 100; and n is an integer of 2 to 100. More preferably, R is a C1 to C5 alkyl group.
[0106] The surfactant containing an alkylene oxide group and a dimethylsiloxane group structure may be BYK306 (BYK Chemical), BYK307 (BYK Chemical), SH7PA (Toray Dow Corning), SH21PA (Toray Dow Corning), SH28PA (Toray Dow Corning), SH30PA (Toray Dow Corning), Troysol S366 (Troy Chemicals), etc.
[0107] 1a3) In feature 1a), in the silicone surfactant, the mass percentage of the surfactant containing epoxyalkylene and dimethylsiloxane structures is 30% to 100%;
[0108] Preferably, the mass percentages of the components of the electron beam photoresist are as follows:
[0109] Polymethyl methacrylate 2-15%, such as 2-5%, 5-6% or 6-15%;
[0110] Solvent 84.85-97.998%, such as 84.85-94%, 94-94.7% or 94.7-97.998%;
[0111] The organic silicon surfactant is 0.002-0.15%, such as 0.002-0.012%, 0.012-0.024%, 0.024-0.036% or 0.036-0.15%.
[0112] Preferably, the weight average molecular weight of the polymethyl methacrylate is in the range of 30,000 to 1,000,000.
[0113] Preferably, the molecular weight distribution of the polymethyl methacrylate is less than 3.
[0114] Preferably, the solvent is selected from at least one of anisole, toluene, xylene, trimethylbenzene, chlorobenzene, dichlorobenzene, propylene glycol monoacetate, propylene glycol monoethyl ether, propylene glycol methyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol methyl ethyl ether, butyl acetate, neopentyl acetate, ethyl lactate, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, diacetone alcohol, γ-butyrolactone and ethyl lactate.
[0115] Preferably, the electron beam photoresist further comprises an auxiliary agent, and the auxiliary agent is selected from at least one of a photoacid generator, a viscosity control agent, a stabilizer and a leveling agent. More preferably, the photoacid generator is selected from N-hydroxynaphthalene imide trifluoromethanesulfonic acid, (4,8-dihydroxy-1-naphthyl) dimethylsulfonium trifluoromethanesulfonate, (4,7-dihydroxy-1-naphthyl) dimethylsulfonium trifluoromethanesulfonate, (4-methoxynaphthyl) diphenylsulfonium trifluoromethanesulfonate, (4-phenylthiophenyl) diphenylsulfonium trifluoromethanesulfonate, 2-(benzo[d][1,3]dioxolan-5-yl)-4,6-bis(trichloromethyl)-1,3,5-triazine, At least one of 2-(2,4-dimethoxyphenyl)-4,6-bis(trichloromethyl)-1,3,5-triazine and 2-[4-(4-methoxyphenyl)phenyl]-4,6-bis(trichloromethyl)-1,3,5-triazine, the viscosity control agent is selected from butanol, chloroform, ethanol, water, acetonitrile, hexane and isopropanol, the stabilizer is selected from at least one of p-benzoquinone, methyl hydroquinone, p-hydroxyanisole, 2-tert-butylhydroquinone and 2,5-di-tert-butylhydroquinone. The leveling agent is selected from one or more of acrylic leveling agents and fluorine-containing leveling agents, such as BYK350, BYK352, MEGAFACE F-563 (purchased from DIC Corporation), MEGAFACE F-470, etc.
[0116] Further more preferably, the mass percentage of each component of the electron beam photoresist is as follows:
[0117] Polymethyl methacrylate 2-15%;
[0118] Solvent 84.7~97.996%;
[0119] Silicone surfactant 0.002~0.15%;
[0120] Additives: 0.002~0.15%.
[0121] The second aspect of the present invention provides a method for improving the sensitivity of electron beam photoresist. When preparing the electron beam photoresist, an organic silicon surfactant is added.
[0122] Preferably, it also includes at least one of the following technical features:
[0123] 2a) The organosilicon surfactant includes a surfactant containing an alkylene oxide group and a dimethylsiloxane group structure;
[0124] 2b) the electron beam photoresist comprises polymethyl methacrylate, a solvent and the organosilicon surfactant;
[0125] 2c) The organic silicon surfactant accounts for 0.1% to 3% of the mass of the polymer resin in the electron beam photoresist.
[0126] More preferably, it also includes at least one of the following technical features:
[0127] 2a1) In feature 2a), in the surfactant containing an alkylene oxide and a dimethylsiloxane structure, the mass percentage of the alkylene oxide and the dimethylsiloxane group is 15% to 85%;
[0128] 2a2) In feature 2a), the surfactant containing an alkylene oxide group and a dimethylsiloxane group structure has a structure as shown in Formula I:
[0129]
[0130] Wherein, R is hydrogen or an alkyl group; x is an integer of 1 to 20; m is an integer of 2 to 100; and n is an integer of 2 to 100.
[0131] The surfactant containing an alkylene oxide group and a dimethylsiloxane group structure may be BYK306 (BYK Chemical), BYK307 (BYK Chemical), SH7PA (Toray Dow Corning), SH21PA (Toray Dow Corning), SH28PA (Toray Dow Corning), SH30PA (Toray Dow Corning), Troysol S366 (Troy Chemicals), etc.
[0132] 2a3) In feature 2a), in the silicone surfactant, the mass percentage of the surfactant containing epoxyalkylene and dimethylsiloxane structures is 30% to 100%.
[0133] 2b1) In feature 2b), the mass percentages of the components of the electron beam photoresist are as follows:
[0134] Polymethyl methacrylate 2-15%;
[0135] Solvent 84.85~97.998%;
[0136] Silicone surfactant 0.002~0.15%.
[0137] 2b2) In feature 2b), the weight average molecular weight of the polymethyl methacrylate is in the range of 30,000 to 1,000,000.
[0138] 2b3) In feature 2b), the molecular weight distribution of the polymethyl methacrylate is <3.
[0139] 2b4) In feature 2b), the solvent is selected from at least one of anisole, toluene, xylene, trimethylbenzene, chlorobenzene, dichlorobenzene, propylene glycol monoacetate, propylene glycol monoethyl ether, propylene glycol methyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol methyl ethyl ether, butyl acetate, neopentyl acetate, ethyl lactate, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, diacetone alcohol, γ-butyrolactone and ethyl lactate.
[0140] 2b5) In feature 2b), the electron beam photoresist further comprises an auxiliary agent, wherein the auxiliary agent is selected from at least one of a photoacid generator, a viscosity controller, a stabilizer and a leveling agent.
[0141] More preferably, in feature 2a2), R is a C1-C5 alkyl group.
[0142] Further more preferably, in feature 2b5), the mass percentages of the components of the electron beam photoresist are as follows:
[0143] Polymethyl methacrylate 2-15%;
[0144] Solvent 84.7~97.996%;
[0145] Silicone surfactant 0.002~0.15%;
[0146] Additives: 0.002~0.15%.
[0147] The third aspect of the present invention provides an electron beam photoresist, comprising the following components in percentage by mass:
[0148] Polymethyl methacrylate 2-15%;
[0149] Solvent 84.85~97.998%;
[0150] Silicone surfactant 0.002~0.15%.
[0151] Preferably, it also includes at least one of the following technical features:
[0152] 3a) The weight average molecular weight of the polymethyl methacrylate is in the range of 30,000 to 1,000,000.
[0153] 3b) The molecular weight distribution of the polymethyl methacrylate is less than 3.
[0154] 3c) the solvent is selected from at least one of anisole, toluene, xylene, trimethylolbenzene, chlorobenzene, dichlorobenzene, propylene glycol monoacetate, propylene glycol monoethyl ether, propylene glycol methyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol methyl ethyl ether, butyl acetate, neopentyl acetate, ethyl lactate, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, diacetone alcohol, gamma-butyrolactone and ethyl lactate.
[0155] 3d) The organosilicon surfactant includes a surfactant containing an alkylene oxide group and a dimethylsiloxane group structure.
[0156] 3e) The electron beam photoresist further comprises an auxiliary agent, wherein the auxiliary agent is selected from at least one of a photoacid generator, a viscosity controller, a stabilizer and a leveling agent; preferably, the mass percentage of each component of the electron beam photoresist is as follows:
[0157] Polymethyl methacrylate 2-15%;
[0158] Solvent 84.7~97.996%;
[0159] Silicone surfactant 0.002~0.15%;
[0160] Additives: 0.002~0.15%.
[0161] 3f) The organic silicon surfactant accounts for 0.1% to 3% of the mass of the polymer resin in the electron beam photoresist.
[0162] More preferably, in feature 3d), in the surfactant containing an alkylene oxide and a dimethylsiloxane structure, the mass percentage of the alkylene oxide and the dimethylsiloxane group is 15% to 85%.
[0163] More preferably, in feature 3d), the surfactant containing an alkylene oxide group and a dimethylsiloxane group structure contains a structure as shown in Formula I:
[0164]
[0165] Wherein, R is hydrogen or an alkyl group; x is an integer of 1 to 20; m is an integer of 2 to 100; and n is an integer of 2 to 100.
[0166] The surfactant containing an alkylene oxide group and a dimethylsiloxane group structure may be BYK306 (BYK Chemical), BYK307 (BYK Chemical), SH7PA (Toray Dow Corning), SH21PA (Toray Dow Corning), SH28PA (Toray Dow Corning), SH30PA (Toray Dow Corning), Troysol S366 (Troy Chemicals), etc.
[0167] More preferably, in feature 3d), in the silicone surfactant, the mass percentage of the surfactant containing epoxyalkylene group and dimethylsiloxane group structure is 30% to 100%;
[0168] A fourth aspect of the present invention provides a method for preparing the electron beam photoresist, comprising the following steps: mixing the components of the electron beam photoresist to obtain the electron beam photoresist.
[0169] The fifth aspect of the present invention provides a method for using the electron beam photoresist, comprising the following steps: coating the electron beam photoresist on a silicon wafer, and sequentially performing pre-baking, exposure and development to obtain a photolithography pattern.
[0170] Preferably, it also includes at least one of the following technical features:
[0171] 4a) The pre-baking temperature is 100-200°C.
[0172] 4b) The pre-baking time is 60 to 180 seconds.
[0173] 4c) Exposure energy is 0.1~20C / m 2 , such as 0.1~6C / m 2 , 6~7C / m 2 ,7~13C / m 2 , 13~16C / m 2 or 16~20C / m 2 .
[0174] 4d) The developer comprises at least one selected from methyl isobutyl ketone and isopropyl alcohol and optionally water.
[0175] 4e) The developing time is 30 to 90 seconds.
[0176] Example
[0177] The embodiments of the present invention will be described in detail below. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.
[0178] Example 1
[0179] An organic silicon surfactant is used for improving the sensitivity of electron beam photoresist. The organic silicon surfactant is BYK307, and the added amount is 0.2% of the mass of polymer resin (ie polymethyl methacrylate) in the electron beam photoresist.
[0180] The electron beam photoresist comprises the following components in percentage by mass: 6% of polymethyl methacrylate; 93.988% of anisole; and 0.012% of an organic silicon surfactant SH21PA, wherein the polymethyl methacrylate is polymerized with methyl methacrylate as a monomer, has a weight average molecular weight range of 500K, and a molecular weight distribution of 2.1.
[0181] The method for preparing the electron beam photoresist comprises the following steps: mixing the components of the electron beam photoresist and stirring them to achieve complete dissolution to obtain the electron beam photoresist.
[0182] The method for using the electron beam photoresist specifically comprises the following steps: spin coating the electron beam photoresist on a 4-inch silicon wafer, wherein the coating thickness of the electron beam photoresist is 1500A; pre-baking at 180°C for 120s; exposing in an electron beam lithography machine, wherein the electron beam lithography voltage is 100KeV and the current is 500pA; developing in a developer, wherein the developer is isopropanol and water in a mass ratio of 2:1, and the developing time is 60s, to obtain a photolithography pattern under the condition of a designed line width of 50nm, as shown in FIG. Figure 1 , energy 16C / m 2 , isolated opening 50nm.
[0183] Example 2
[0184] An organic silicon surfactant is used for improving the sensitivity of electron beam photoresist. The organic silicon surfactant is SH30PA, and the added amount is 0.4% of the mass of the polymer resin in the electron beam photoresist.
[0185] The electron beam photoresist comprises the following components in percentage by mass: 6% of polymethyl methacrylate; 93.976% of anisole; and 0.024% of an organic silicon surfactant SH21PA, wherein the polymethyl methacrylate is polymerized with methyl methacrylate as a monomer, has a weight average molecular weight range of 500K, and a molecular weight distribution of 2.1.
[0186] The method for preparing the electron beam photoresist comprises the following steps: mixing the components of the electron beam photoresist and stirring them to achieve complete dissolution to obtain the electron beam photoresist.
[0187] The method for using the electron beam photoresist specifically comprises the following steps: spin coating the electron beam photoresist on a 4-inch silicon wafer, wherein the coating thickness of the electron beam photoresist is 1500A; pre-baking at 180°C for 120s; exposing in an electron beam lithography machine, wherein the electron beam lithography voltage is 100KeV and the current is 500pA; developing in a developer, wherein the developer is isopropanol and water in a mass ratio of 2:1, and the developing time is 60s, to obtain a photolithography pattern under the condition of a designed line width of 50nm, as shown in FIG. Figure 2 , energy 13C / m 2 , the pattern shows an isolated opening of 57nm.
[0188] Example 3
[0189] An organic silicon surfactant is used for improving the sensitivity of electron beam photoresist. The organic silicon surfactant is SH21PA, and the added amount is 0.6% of the mass of the polymer resin in the electron beam photoresist.
[0190] The electron beam photoresist comprises the following components in percentage by mass: 6% polymethyl methacrylate; 93.964% anisole; and 0.036% organic silicon surfactant, wherein the polymethyl methacrylate is polymerized with methyl methacrylate as a monomer, has a weight average molecular weight range of 500K, and a molecular weight distribution of 2.1.
[0191] The method for preparing the electron beam photoresist comprises the following steps: mixing the components of the electron beam photoresist and stirring them to achieve complete dissolution to obtain the electron beam photoresist.
[0192] The method for using the electron beam photoresist specifically comprises the following steps: spin coating the electron beam photoresist on a 4-inch silicon wafer, wherein the coating thickness of the electron beam photoresist is 1500A; pre-baking at 180°C for 120s; exposing in an electron beam lithography machine, wherein the electron beam lithography voltage is 100KeV and the current is 500pA; developing in a developer, wherein the developer is isopropanol and water in a mass ratio of 2:1, and the developing time is 60s, to obtain a photolithography pattern under the condition of a designed line width of 50nm, as shown in FIG. Figure 3 , energy 7C / m 2 , the pattern shows an isolated opening of 57nm.
[0193] Example 4
[0194] An organic silicon surfactant is used to improve the sensitivity of electron beam photoresist. The organic silicon surfactant is SH21PA, and the added amount is 0.1% of the mass of polymer resin (ie polymethyl methacrylate) in the electron beam photoresist.
[0195] The electron beam photoresist comprises the following components in percentage by mass: 2% polymethyl methacrylate; 97.996% anisole; 0.002% organic silicon surfactant SH21PA; 0.002% stabilizer methyl hydroquinone, wherein the polymethyl methacrylate is polymerized with methyl methacrylate as a monomer, has a weight average molecular weight range of 500K, and a molecular weight distribution of 2.1.
[0196] The method for preparing the electron beam photoresist comprises the following steps: mixing the components of the electron beam photoresist and stirring them to achieve complete dissolution to obtain the electron beam photoresist.
[0197] The method for using the electron beam photoresist specifically comprises the following steps: spin coating the electron beam photoresist on a 4-inch silicon wafer, wherein the coating thickness of the electron beam photoresist is 1500A; pre-baking at 180°C for 120s; exposing in an electron beam lithography machine, wherein the electron beam lithography voltage is 100KeV and the current is 500pA; developing in a developer, wherein the developer is isopropanol and water in a mass ratio of 2:1, and the developing time is 60s, and a photolithography pattern under the condition of a designed line width of 50nm is obtained, and the energy is 20C / m 2 , isolated opening 52nm.
[0198] Example 5
[0199] An organic silicon surfactant is used to improve the sensitivity of electron beam photoresist. The organic silicon surfactant is SH21PA, and the added amount is 3% of the mass of polymer resin (ie polymethyl methacrylate) in the electron beam photoresist.
[0200] The electron beam photoresist comprises the following components in percentage by mass: 5% polymethyl methacrylate; 94.7% anisole; 0.15% organic silicon surfactant SH21PA; 0.15% viscosity control agent isopropyl alcohol; wherein the polymethyl methacrylate is polymerized with methyl methacrylate as a monomer, has a weight average molecular weight range of 500K, and a molecular weight distribution of 2.1.
[0201] The method for preparing the electron beam photoresist comprises the following steps: mixing the components of the electron beam photoresist and stirring them to achieve complete dissolution to obtain the electron beam photoresist.
[0202] The method for using the electron beam photoresist specifically comprises the following steps: spin coating the electron beam photoresist on a 4-inch silicon wafer, wherein the coating thickness of the electron beam photoresist is 1500A; pre-baking at 180°C for 120s; exposing in an electron beam lithography machine, wherein the electron beam lithography voltage is 100KeV and the current is 500pA; developing in a developer, wherein the developer is isopropanol and water in a mass ratio of 2:1, and the developing time is 60s, and a photolithography pattern under the condition of a designed line width of 50nm is obtained, and the energy is 6C / m 2, isolated opening 54nm.
[0203] It can be seen that the present application can effectively improve the sensitivity of the electron beam photoresist by adding an organosilicon surfactant to the electron beam photoresist. Moreover, within a suitable range, the energy will gradually decrease with the addition of the organosilicon surfactant, so the sensitivity can be improved by adjusting the amount of the organosilicon surfactant, and the organosilicon surfactant plays a role in adjusting the sensitivity.
[0204] The above description of the embodiments is to facilitate those of ordinary skill in the art to understand and apply the present application. It is obvious that those familiar with the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without having to pay creative labor. Therefore, the present application is not limited to the embodiments herein, and improvements and modifications made by those skilled in the art based on the contents disclosed in the present application without departing from the scope and spirit of the present application are within the scope of the present application.
Claims
1. An electron beam photoresist, characterized in that The electron beam photoresist comprises the following components in percentage by mass: Polymethyl methacrylate 2-15%; Solvent 84.85~97.998%; Silicone surfactant 0.002~0.15%; The organosilicon surfactant is SH21PA.
2. The electron beam photoresist according to claim 1, characterized in that It also includes at least one of the following technical features: 2a) The weight average molecular weight of the polymethyl methacrylate is in the range of 30,000 to 1,000,000; 2b) the molecular weight distribution of the polymethyl methacrylate is less than 3; 2c) the solvent is selected from at least one of anisole, toluene, xylene, trimethylbenzene, chlorobenzene, dichlorobenzene, propylene glycol monoacetate, propylene glycol methyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, diethylene glycol methyl ether, diethylene glycol ethyl ether, diethylene glycol methyl ethyl ether, butyl acetate, neopentyl acetate, methyl ethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, diacetone alcohol, gamma-butyrolactone and ethyl lactate; 2d) The electron beam photoresist further comprises an auxiliary agent, wherein the auxiliary agent is selected from at least one of a photoacid generator, a viscosity controller and a stabilizer.
3. The electron beam photoresist according to claim 1, characterized in that The mass percentages of the components of the electron beam photoresist are as follows: Polymethyl methacrylate 2-15%; Solvent 84.85~97.996%; Silicone surfactant 0.002~0.15%; Additives: 0.002~0.15%.
4. A method for preparing an electron beam photoresist as claimed in any one of claims 1 to 3, characterized in that: The electron beam photoresist is obtained by mixing the polymethyl methacrylate, the solvent and the organosilicon surfactant.
5. A method for using the electron beam photoresist according to any one of claims 1 to 3, characterized in that: The method of use comprises the following steps: The electron beam photoresist is spin-coated on a silicon wafer, and is subjected to pre-baking, exposure and development in sequence to obtain a photolithography pattern.
6. The method for using the electron beam photoresist as claimed in claim 5, characterized in that: It also includes at least one of the following technical features: 6a) The pre-baking temperature is 100-200°C; 6b) Pre-baking time is 60 to 180 seconds; 6c) Exposure energy is 0.1~20C / m 2 ; 6d) the developer comprises at least one selected from methyl isobutyl ketone and isopropyl alcohol; 6e) The developing time is 30 to 90 seconds.
7. The method for using the electron beam photoresist as claimed in claim 6, characterized in that: The invention comprises the following technical features: the developer contains water.