A method for measuring the integral casting thickness of the permanent layer of the ladle wall
By measuring the core mold spacing and permanent layer thickness before and after the overall casting of the permanent layer of the ladle wall, the problems of uneven casting thickness and repair difficulty are solved, and uniform casting and precise quantity repair of the permanent layer of the ladle wall are achieved, reducing the risk of steel leakage.
Patent Information
- Application Number
- CN202010423756.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-05-19
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-05-19
AI Technical Summary
When the permanent layer of the ladle wall is poured, the casting thickness is uneven due to the wear of the rubber pad at the bottom of the core mold and the deformation of the ladle, resulting in steel leakage accidents, and it is difficult to determine the repair thickness when the core mold spacing cannot be adjusted.
Before and after the ladle wall permanent layer is poured, the core mold spacing and permanent layer thickness are measured by opening holes at multiple measurement points, and the data is measured and recorded using steel needles to adjust the core mold position and determine the repair thickness.
The uniform casting of the permanent layer thickness of the ladle wall and the precise quantification of the later repair thickness are achieved, reducing the risk of steel leakage and improving the service life of the ladle.
Smart Images

Figure CN113686223B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an integral casting process of a permanent layer refractory material of a ladle wall, in particular to a method for measuring the integral casting thickness of a permanent layer of a ladle wall. Background Art
[0002] Ladle is a container for carrying molten steel and refining outside the furnace. It is an indispensable tool for transportation, refining outside the furnace and pouring molten steel in the process of connecting the converter to the continuous casting steelmaking production. The refractory materials of the ladle lining are usually divided into a working layer and a permanent layer; among them, the permanent layer, as an important component of the ladle lining, is the last barrier for the safe operation of the ladle and a reliable guarantee for maximizing the value of the working layer. Furthermore, the permanent layer of the ladle wall mainly plays a role of insulation and insurance; insulation effect: the key is the ladle wall. Since the molten steel stays in the ladle for a long time, the permanent layer has good insulation performance, which can reduce the heat loss of the molten steel, reduce the temperature of the steel structure shell of the ladle, and extend its service life; insurance effect: when the working layer is infiltrated with steel or even the melting loss is zero, the permanent layer can at least block the smelting of one furnace of molten steel without leaking steel through the ladle.
[0003] At present, the permanent layer of the ladle wall is mainly cast as a whole, and the implementation of the integral casting is inseparable from the core mold and the placement of the core mold. During the integral casting, the alignment and placement of the core mold is adjusted by the support cylinder and the centering cylinder. However, in actual application, due to the uneven wear of the rubber pad at the bottom of the core mold or the deformation of the ladle body due to long-term use, it is easy to cause a large error in the spacing between the upper and lower ends of the ladle wall and the core mold during the integral casting of the ladle wall. If the upper end spacing error is large, the operator can see it and correct it in time, but because the core mold is as high as 5 meters, the lower end spacing cannot be determined, resulting in uneven casting thickness. If the thickness of the permanent layer of the ladle wall is uneven, the inner lining castable will be washed and melted by the molten steel during the turnover of the ladle on the line. In the later stage of the use of the ladle wall, the refractory material is at risk of being penetrated by the molten steel. There have been several ladle wall leakage accidents in the integral casting ladles of major domestic steel mills, including ladle wall leakage accidents caused by uneven ladle casting thickness. In addition, when the ladle body is severely deformed in the later stage of furnace service, the core mold spacing cannot be adjusted in place no matter what. At this time, it is difficult to determine the exact spacing value of the substandard part, and it is also impossible to determine the repair thickness. Summary of the invention
[0004] In view of the shortcomings of the prior art mentioned above, the purpose of the present invention is to provide a method for measuring the overall casting thickness of the permanent layer of the ladle wall, so as to quantify the thickness of the permanent layer of the ladle wall, and at the same time provide strong data support for the uniformity of the overall casting thickness of the permanent layer of the ladle wall and the subsequent determination of the repair thickness.
[0005] To achieve the above object, the present invention provides a method for measuring the integral casting thickness of the permanent layer of the ladle wall, the measuring method comprising the following steps in sequence:
[0006] S1. Before the permanent layer of the ladle wall is poured as a whole, a core mold is placed on the inner periphery of the ladle body;
[0007] S2. Select at least two layers of measuring positions at different heights on the ladle body, each layer of measuring positions having a plurality of measuring points distributed along the circumference of the ladle body; open a hole at each measuring point, so as to form a measuring hole that penetrates the ladle body radially along the ladle body at each measuring point;
[0008] S3, measuring and recording the core mold spacing L1 between the ladle body and the core mold at each measuring point, and adjusting the position of the core mold according to the core mold spacing L1;
[0009] S4, injecting the material of the permanent layer of the ladle wall between the ladle body and the core mold to perform the pouring operation of the permanent layer of the ladle wall;
[0010] S5. After the permanent layer of the ladle wall is poured, the thickness L2 of the permanent layer is measured and recorded at each measuring point.
[0011] Furthermore, in step S3 or step S5, a steel needle is used to measure the core mold spacing L1 or the permanent layer thickness L2, and the steel needle has an abutting end abutting the core mold and a hand-held part located outside the ladle body; when measuring the core mold spacing L1 or the permanent layer thickness L2, the steel needle is inserted into the measuring hole, and the abutting end of the steel needle is abutted against the core mold, and then the depth H of the steel needle inserted into the ladle body is obtained.
[0012] Furthermore, a scale is provided on the surface of the steel needle, and the zero scale position on the scale is located at the abutment end; when measuring the core mold spacing L1 or the permanent layer thickness L2, the steel needle is inserted into the measuring hole, and the abutment end of the steel needle is abutted against the core mold, and then the scale on the surface of the steel needle is read to directly obtain the depth H of the steel needle inserted into the ladle body.
[0013] Furthermore, the measuring positions have two layers, one of which has a height of 500 mm and the other has a height of 1500 mm.
[0014] Furthermore, the number of measurement points in each layer of measurement position is 8.
[0015] Furthermore, the diameter of the measuring hole is 10 mm.
[0016] Furthermore, a layer of insulation bricks is fixedly provided on the inner circumferential surface of the ladle body.
[0017] Furthermore, the thermal insulation bricks are lightweight thermal insulation bricks.
[0018] As described above, the method for measuring the integral casting thickness of the permanent layer of the ladle wall according to the present invention has the following beneficial effects:
[0019] In the present application, the core mold spacing L1 between the ladle body and the core mold can be obtained before the overall pouring of the permanent layer refractory material of the ladle wall, and the permanent layer thickness L2 can be obtained after the overall pouring of the permanent layer refractory material of the ladle wall. The core mold spacing L1 is used to provide data support for adjusting the core mold position before pouring, which is beneficial to the uniform thickness of the permanent layer of the ladle wall after the overall pouring; the permanent layer thickness L2 is used to provide data support for determining the repair thickness later. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Schematic diagram of the relationship between the ladle body and the core mold before pouring.
[0021] Figure 2 This is a schematic diagram of measuring the core mold distance L1 before pouring.
[0022] Figure 3 This is a schematic diagram of measuring the permanent layer thickness L2 after pouring.
[0023] Component number description
[0024] 10 Ladle body
[0025] 11 Measuring hole
[0026] 20 core mold
[0027] 30 Insulation Brick
[0028] 40 Steel Needle
[0029] 41 Butt end
[0030] 42 Handheld DETAILED DESCRIPTION
[0031] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification.
[0032] It should be noted that the structures, proportions, sizes, etc. drawn in the drawings of this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions for the implementation of the present invention, so they have no substantial technical significance. Any modification of the structure, change of the proportional relationship or adjustment of the size should still fall within the scope of the technical content disclosed by the present invention without affecting the effects and purposes that can be achieved by the present invention. At the same time, the terms such as "upper", "lower", "left", "right", "middle" and "one" quoted in this specification are only for the convenience of description, and are not used to limit the scope of the implementation of the present invention. The change or adjustment of their relative relationship should also be regarded as the scope of the implementation of the present invention without substantially changing the technical content.
[0033] The present application relates to the field of refractory material construction technology in molten steel metallurgical steel containers, specifically to a process for integrally pouring a permanent layer of refractory materials on a ladle wall, and in particular to a method for measuring the integral pouring thickness of the permanent layer of the ladle wall. The measuring method is used to measure the core mold spacing L1 between the ladle body 10 and the core mold 20 before the integral pouring of the permanent layer of refractory materials on the ladle wall, and the measuring method is used to measure the permanent layer thickness L2 after the integral pouring of the permanent layer of refractory materials on the ladle wall.
[0034] The following provides a preferred embodiment of a method for measuring the integral casting thickness of a permanent layer of a ladle wall involved in the present application.
[0035] The method for measuring the integral casting thickness of the permanent layer of the ladle wall involved in the present application comprises the following steps in sequence:
[0036] S1. Before the permanent layer of the ladle wall is poured as a whole, Figure 1 and Figure 2 As shown, a core mold 20 is placed on the inner periphery of the ladle body 10, and a layer of insulation bricks 30 is fixed on the inner periphery of the ladle body 10. The insulation bricks 30 are preferably lightweight insulation bricks.
[0037] S2, such as Figure 1 As shown, two layers of measuring positions with different heights are selected on the ladle body 10, one of which has a height of 500 mm and the other has a height of 1500 mm. Each layer of measuring positions has 8 measuring points distributed along the circumference of the ladle body 10. A hole is opened at each measuring point, and the diameter of the hole is 10 mm, so that a measuring hole 11 is formed at each measuring point that penetrates the ladle body 10 radially along the ladle body 10, and the diameter of the measuring hole 11 is 10 mm. In addition, when drilling, use an electric drill to clean the slag in the hole, and conduct the measuring hole 11 to improve the measurement accuracy of the subsequent core mold spacing L1 and the permanent layer thickness L2.
[0038] S3, such as Figure 2As shown, the core mold spacing L1 between the ladle body 10 and the core mold 20 is measured and recorded at each measuring point. The specific data of the core mold spacing L1 at 16 measuring points evenly distributed at different heights provide strong data support for adjusting the position of the core mold 20 before pouring, and intuitively show the core mold spacing L1 between the ladle body 10 and the core mold 20. The staff adjusts the position of the core mold 20 according to the core mold spacing L1, and more accurately controls the orientation and position of the core mold 20, so that the thickness of the permanent layer of the ladle wall is uniform after the entire casting.
[0039] S4, injecting the material of the permanent layer of the ladle wall between the ladle body 10 and the core mold 20, and performing the pouring operation of the permanent layer of the ladle wall.
[0040] S5. After the permanent layer of the ladle wall is poured, Figure 3 As shown, the permanent layer thickness L2 is measured and recorded at each measuring point. The permanent layer thickness L2 is used to provide data support for determining the repair thickness later, so that the overall casting thickness of different parts of the permanent layer of the ladle wall can be quantitatively described, guiding the subsequent repair and thickening of the permanent layer of the ladle wall to ensure the safety of the ladle in online use.
[0041] Therefore, the present application can obtain the core mold spacing L1 between the ladle body 10 and the core mold 20 before the overall pouring of the permanent layer refractory material of the ladle wall, and can obtain the permanent layer thickness L2 after the overall pouring of the permanent layer refractory material of the ladle wall, so that the core mold spacing L1 before pouring and the permanent layer thickness L2 after pouring can be quantitatively described. The core mold spacing L1 is used to provide data support for adjusting the position of the core mold 20 before pouring, which is beneficial to the uniform thickness of the permanent layer of the ladle wall after the overall pouring; the permanent layer thickness L2 is used to provide data support for determining the repair thickness later.
[0042] Furthermore, in the above step S3 or step S5, the method for measuring the core mold spacing L1 or the permanent layer thickness L2 is: using a steel needle 40 to measure the core mold spacing L1 or the permanent layer thickness L2, such as Figure 2 or Figure 3 As shown, the steel needle 40 has an abutting end 41 abutting against the core mold 20, and a hand-held portion 42 located outside the ladle body 10. When measuring the core mold spacing L1, as shown in FIG. Figure 2 As shown, the steel needle 40 is inserted into the measuring hole 11, and the abutting end 41 of the steel needle 40 is abutted against the core mold 20, and then the depth H of the steel needle 40 inserted into the ladle body 10 is obtained, and the core mold spacing L1 = the insertion depth H of the steel needle 40-the thickness W1 of the ladle body 10-the thickness W2 of the insulation brick 30. When measuring the permanent layer thickness L2, as Figure 3As shown, after pouring the refractory material between the ladle body 10 and the core mold 20, when the refractory material has not cooled and is still soft, insert the steel needle 40 into the measuring hole 11, and make the abutting end 41 of the steel needle 40 abut against the core mold 20, and then obtain the depth H of the steel needle 40 inserted into the ladle body 10, then the permanent layer thickness L2 = the insertion depth H of the steel needle 40 - the thickness W1 of the ladle body 10 - the thickness W2 of the insulation brick 30. Therefore, the present application calculates the core mold spacing L1 and the permanent layer thickness L2 respectively by directly measuring the depth H of the steel needle 40 inserted into the ladle body 10 before and after pouring. The thickness W1 of the ladle body 10 and the thickness W2 of the insulation brick 30 are known parameters; in this embodiment, the thickness W1 of the ladle body 10 is 32 mm, and the thickness W2 of the insulation brick 30 is 18 mm, so the length of the steel needle 40 should be greater than 50 mm. In addition, the depth H of the steel needle 40 inserted into the ladle body 10 also refers to: when the abutting end 41 of the inner end of the steel needle 40 abuts against the core mold 20, the distance between the abutting end 41 of the inner end of the steel needle 40 and the outer periphery of the ladle body 10.
[0043] Preferably, the surface of the steel needle 40 is provided with a scale, and the zero scale position on the scale is located at the abutment end 41; when measuring the core mold spacing L1 or the permanent layer thickness L2, the steel needle 40 is inserted into the measuring hole 11, and the abutment end 41 of the steel needle 40 is abutted against the core mold 20, and then the scale on the surface of the steel needle 40 is read to directly obtain the depth H of the steel needle 40 inserted into the ladle body 10, which is convenient and intuitive to operate. Alternatively, if the surface of the steel needle 40 is not provided with a scale, the depth H of the steel needle 40 inserted into the ladle body 10 can be measured in combination with a tape measure.
[0044] When measuring the core mold spacing L1 and the permanent layer thickness L2 before and after pouring, the core mold spacing L1 and the permanent layer thickness L2 can be first recorded on the ladle body 10 next to each measuring hole 11 during the measurement process. After the measurement is completed, all data are recorded uniformly to improve the measurement efficiency.
[0045] In summary, after the core mold 20 is placed before pouring, the present application can obtain accurate data of the core mold spacing L1 by measuring the core mold spacing L1 at multiple measuring points at different heights, which can accurately guide the core mold 20 to adjust the placement position. After pouring, by measuring the permanent layer thickness L2 at multiple measuring points at different heights, accurate data of the permanent layer thickness L2 can be obtained. The permanent layer thickness L2 is also the actual thickness of the permanent layer, which is convenient for subsequent targeted repairs. Furthermore, since the core mold 20 will be displaced to a certain extent due to vibration and other reasons during the pouring process, the permanent layer thickness L2 obtained after pouring is not necessarily equal to the core mold spacing L1 obtained before pouring.
[0046] Therefore, the present invention effectively overcomes various shortcomings in the prior art and has high industrial utilization value.
[0047] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for measuring the integral casting thickness of the permanent layer of the ladle wall, characterized in that: The measuring method comprises the following steps in sequence: S1. Before the permanent layer of the ladle wall is integrally poured, a core mold (20) is placed on the inner periphery of the ladle body (10); S2. Selecting at least two layers of measuring positions at different heights on the ladle body (10), each layer of measuring positions having a plurality of measuring points distributed along the circumference of the ladle body (10); opening a hole at each measuring point, thereby forming a measuring hole (11) penetrating the ladle body (10) radially along the ladle body (10) at each measuring point; S3, measuring and recording the core mold spacing L1 between the ladle body (10) and the core mold (20) at each measuring point, obtaining data of the core mold spacing L1 by measuring the core mold spacing L1 at multiple measuring points at different heights, and adjusting the position of the core mold (20) according to the data of the core mold spacing L1; S4, injecting the material of the permanent layer of the ladle wall into between the ladle body (10) and the core mold (20), and performing a pouring operation of the permanent layer of the ladle wall; S5. After the permanent layer of the ladle wall is poured, the permanent layer thickness L2 is measured and recorded at each measuring point. The data of the permanent layer thickness L2 is obtained by measuring the permanent layer thickness L2 at multiple measuring points at different heights. In step S3 or step S5, a steel needle (40) is used to measure the core mold spacing L1 or the permanent layer thickness L2. The steel needle (40) has an abutting end (41) abutting against the core mold (20) and a hand-held portion (42) located outside the ladle body (10). The surface of the steel needle (40) is provided with a scale, and the zero scale position on the scale is located at the abutting end (41). When measuring the core mold spacing L1 or the permanent layer thickness L2, the steel needle (40) is inserted into the measuring hole (11), and the abutting end (41) of the steel needle (40) is abutted against the core mold (20). Then, the scale on the surface of the steel needle (40) is read to directly obtain the depth H of the steel needle (40) inserted into the ladle body (10).
2. The measuring method according to claim 1, characterized in that: The measuring positions have two layers, wherein the height of one layer of measuring positions is 500 mm, and the height of the other layer of measuring positions is 1500 mm.
3. The measuring method according to claim 1, characterized in that: The number of measurement points in each layer measurement position is 8.
4. The measuring method according to claim 1, characterized in that: The diameter of the measuring hole (11) is 10 mm.
5. The measuring method according to claim 1, characterized in that: A layer of insulation bricks (30) is fixedly arranged on the inner peripheral surface of the ladle body (10).
6. The measuring method according to claim 5, characterized in that: The thermal insulation brick (30) is a lightweight thermal insulation brick.