A method for improving thermal shock reliability of DCB copper-clad ceramic substrate
By increasing the film design spacing, increasing the etching line speed, and optimizing the etching factor in the preparation of DCB copper-clad ceramic substrates, the problem of insufficient reliability of existing DCB products in hot and cold shock tests has been solved, and its performance in harsh environments has been significantly improved. Lower performance and expanded application scenarios.
Patent Information
- Application Number
- CN202110948243.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-08-18
AI Technical Summary
Existing DCB copper-clad ceramic substrates show low reliability in hot and cold shock tests, limiting their application scenarios. Due to restrictions in ceramic suppliers, DCB manufacturers have difficulty improving performance by changing ceramic manufacturers and must rely on process improvements. .
In the preparation process of DCB copper-clad ceramic substrates, increase the film design spacing and increase the etching line speed. Specific measures include increasing the film design spacing to 0.43mm and etching line speed to 0.8250m/min, and adjusting the etching factor to 2 to 3 , make sure the bottom spacing is 0.5±0.1mm.
By optimizing the process and reducing the etching factor, the thermal shock reliability of DCB products has been significantly improved, the service life of the products in harsh environments has been extended, and customers' trust in the products has been enhanced.
Smart Images

Figure CN113686718B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of DCB substrate preparation, and in particular to a method for improving the thermal shock reliability performance of a DCB copper-clad ceramic substrate. Background Art
[0002] When evaluating DCB copper-clad ceramic substrates, there is a performance indicator: thermal temperature cycle, which can also be called thermal shock performance. The general test conditions in the industry are: thermal shock conditions: -55℃~+150℃, 1cycle 15min conversion time <6min. Depending on the different ceramic combinations, the relevant indicators are also different. At present, the industry's 0.30mm Cu / 0.38mmAl 2 O 3 / 0.30mm Cu, without dimple is 45cycle; 0.30mm Cu / 0.635mm Al 2 O 3 / 0.30mm Cu, without dimple is 60cycle; 0.30mm Cu / 0.635mm AlN / 0.30mm Cu, without dimple is 35cycle.
[0003] For DCB products that are used in increasingly harsh environments, the stronger their ability to withstand thermal shocks means that their applications will be more extensive. At present, the industry's approach to improving thermal shock resistance is to select ceramics from different manufacturers. Due to different ceramic formulas and sintering processes, the performance of different manufacturers will be different. However, due to customer restrictions, there will be restrictions on ceramic suppliers, which limits the selection of ceramic manufacturers. DCB manufacturers can only improve their own processes to improve thermal shock reliability. Summary of the invention
[0004] In order to overcome the above technical defects, the purpose of the present invention is to provide a method for improving the thermal shock reliability of DCB copper-clad ceramic substrates. During the preparation process of DCB copper-clad ceramic substrates, the film design spacing is increased in the exposure process, and the corrosion line speed is increased in the etching process.
[0005] Furthermore, the film design spacing was increased to 0.43 mm and the etching line speed was increased to 0.8250 m / min.
[0006] Furthermore, the copper thickness of the pattern surface of the DCB copper-clad ceramic substrate is 0.3±0.02 mm, the top spacing is 0.7 mm, the bottom spacing should meet 0.5±0.1 mm, and the etching factor is 2-3.
[0007] Furthermore, the bottom spacing is 0.426 mm and the etching factor is 2.19.
[0008] Compared with the prior art, the above technical solution has the following beneficial effects:
[0009] The present application improves the preparation process of DCB copper-clad ceramic substrates, for example, by increasing the DCB film design spacing and improving the etching line speed, thereby reducing the etching factor of DCB products, and ultimately improving the thermal shock reliability of DCB products such as semiconductor refrigerators, LEDs, and power semiconductors, and improving customers' increasingly stringent requirements for product usage and usage environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 It is a schematic diagram for explaining the parameters in the calculation formula of the etching factor F;
[0011] Figure 2 This is an ultrasonic scanning photo of the DCB copper-clad ceramic substrate after the hot and cold cycle test;
[0012] Figure 3 A is a photo of the bottom spacing of the DCB copper-clad ceramic substrate in a comparative example after the thermal shock reliability test; B is a photo of the top spacing of the DCB copper-clad ceramic substrate in the comparative example after the thermal shock reliability test;
[0013] Figure 4 A is a bottom spacing photo of a DCB copper-clad ceramic substrate after a thermal shock reliability test in one embodiment of the present application; B is a top spacing photo of a DCB copper-clad ceramic substrate after a thermal shock reliability test in one embodiment of the present application;
[0014] Figure 5A-5E This is a comparison chart of the results of thermal shock reliability tests on DCB copper-clad ceramic substrates etched using etching processes with a large etching factor and a small etching factor. DETAILED DESCRIPTION
[0015] The advantages of the present invention are further described below in conjunction with the accompanying drawings and specific embodiments. Those skilled in the art should understand that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0016] like Figure 1 As shown, the calculation formula of the etching factor F is: F=t / A=2×copper thickness / (top spacing-bottom spacing).
[0017] Currently, the internal control requirement of enterprises is F>2.
[0018] 1. Comparative Example
[0019] In the prior art, the basic process of DCB copper-clad ceramic substrate is: raw material cleaning - oxidation - sintering - pre-treatment - film lamination - exposure (film) - development - etching (corrosion) - post-treatment - cutting - inspection - packaging.
[0020] The specific steps and parameters of raw material cleaning, oxidation, sintering, pre-treatment, film lamination, development, post-treatment, cutting, inspection and packaging can be carried out by using common technical means in the art.
[0021] For the design film spacing, it is generally 0.34mm in the prior art; for the etching line speed, it is generally 0.7316m / min in the prior art;
[0022] The copper thickness of the product graphic surface is 0.3±0.02mm, the top spacing is 0.648mm, the bottom spacing is 0.470mm, and the size spacing (bottom) is required to be 0.5±0.1mm;
[0023] The actual measured etching factor F=0.3*2 / (0.648-0.470)=3.37.
[0024] Considering that the company's internal control F>2, combined with copper thickness and etching line speed, the actual etching factor in the existing technology is generally 3 to 5.
[0025] 2. Embodiment
[0026] In the process of preparing the DCB copper-clad ceramic substrate, the present application adopts an optimized exposure and etching process, which is as follows:
[0027] Step 1: In the exposure process, the film pitch is designed to be increased to 0.43mm;
[0028] Step 2: In the etching process, the etching line speed is increased to 0.8250 m / min;
[0029] Note: The specific steps and parameters of other processes (such as raw material cleaning, oxidation, sintering, pre-treatment, film lamination, development, post-treatment, cutting, inspection and packaging) are consistent with the above comparative examples.
[0030] Among them, the copper thickness of the product graphic surface is 0.3±0.02mm, the top spacing is 0.7mm, the bottom spacing is 0.426mm, and the bottom spacing meets 0.5±0.1mm;
[0031] The actual measured etching factor is reduced by 0.3*2 / (0.7-0.426)=2.19.
[0032] Preferably, the etching factor in the present application is 2-3.
[0033] 3. Effect example test hot and cold shock reliability performance
[0034] 1. Test instrument: high and low temperature cycle test chamber.
[0035] 2. Test purpose: to test the parameters and performance of the products and materials in the above embodiments and comparative examples after being subjected to high temperature, low temperature, or constant temperature environment changes.
[0036] 3. Thermal shock reliability test environment: Among them, the temperature thermal shock condition: -55℃~+150℃, 1 cycle 15min conversion time <6min. Judgment standard: If the edge of the DCB copper-clad ceramic substrate is less than 2mm, the ceramic crack and copper peeling (such as Figure 2 As shown in the figure, if the porcelain cracks and copper loss in the inner box appear white after ultrasonic scanning, it is considered to be failed.
[0037] 4. Test results: See the size test results Figure 3 , Figure 4 , the bottom spacing before improvement is 0.470mm (i.e. Figure 3 A), the size spacing (bottom) is required to be 0.5±0.1mm, and the bottom spacing after optimization is 0.426mm (i.e. Figure 4 A) in the bottom spacing should meet 0.5±0.1mm. Figure 5A-5E It can be seen that after the hot and cold cycle test, the effect of the DCB copper clad ceramic substrate with 60 times after improvement (after the etching factor becomes smaller) is equivalent to the DCB copper clad ceramic substrate with 45 times before improvement (the etching factor is large). Therefore, the hot and cold cycle test of the DCB copper clad ceramic substrate after the etching factor becomes smaller is increased by 15 times, an increase of 33%.
[0038] It should be noted that the embodiments of the present invention have better practicability and do not impose any form of limitation on the present invention. Any technician familiar with the field may use the technical content disclosed above to change or modify it into an equivalent effective embodiment. However, any modification or equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A method for improving the thermal shock reliability of a DCB copper-clad ceramic substrate, characterized in that: In the preparation process of DCB copper-clad ceramic substrate, the film design spacing is increased to 0.43mm in the exposure process, and the etching line speed is increased to 0.8250m / min in the etching process. The copper thickness of the pattern surface of the DCB copper-clad ceramic substrate is 0.3±0.02 mm, the top spacing is 0.7 mm, the bottom spacing should meet 0.5±0.1 mm, and the etching factor is 2-3.
2. The method for improving the thermal shock reliability of a DCB copper-clad ceramic substrate according to claim 1, characterized in that: The bottom spacing is 0.426 mm and the etching factor is 2.19.