Gold-containing catalyst, preparation method and use

By adding additives such as inorganic oxide to the catalyst to form an inorganic oxide layer, the problems of low stability of the gold-containing catalyst and nanotube formation are solved, and the stability of the catalyst and the conversion rate of vinyl chloride monomer are improved.

CN113692316BActive Publication Date: 2024-11-26JOHNSON MATTHEY DAVY TECHNOLOGIES LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080028998.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-06-20
Filing Date
2020-06-19
Publication Date
2024-11-26
Estimated Expiration
2040-06-19

AI Technical Summary

Technical Problem

The existing gold-containing catalysts have problems of low stability and fast inactivation in the manufacturing of vinyl chloride monomers (VCMs), especially because the formation of gold nanoparticles leads to the formation of carbon nanotubes, resulting in catalyst powdering and gold loss.

Method used

By adding inorganic oxides, hydroxides, oxygen-containing salts or oxygen-containing acids to the catalyst as additives, an inorganic oxide layer surrounding gold particles is formed, thereby inhibiting the formation of gold nanoparticles and the deactivation of the catalyst.

Benefits of technology

The stability and activity of the gold-containing catalyst is significantly improved, the formation of nanotubes is reduced, the service life of the catalyst is extended, and the conversion rate of vinyl chloride monomers is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113692316B_ABST
    Figure CN113692316B_ABST
Patent Text Reader

Abstract

The present invention relates to the improvement of known gold-containing catalysts. In particular, the present invention relates to improving the stability of gold-containing catalysts and / or inhibiting the deactivation of gold-containing catalysts by adding inorganic oxides, hydroxides, oxygen-containing salts or oxygen-containing acids. The present invention also discloses a method for preparing the catalyst most suitably by an impregnation method. Such catalysts can be used to prepare vinyl chloride monomer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to providing improved gold-containing catalysts and methods for preparing the same. In particular, but not exclusively, the present invention relates to improving the stability of gold-containing catalysts and / or inhibiting their deactivation by adding additives selected from inorganic oxides, hydroxides, oxygen-containing salts or oxygen-containing acids, methods for preparing the same, and use thereof in the manufacture of vinyl chloride monomer (VCM). Background Art

[0002] A known commercial process for making vinyl chloride monomer (VCM) mixes ethylene, hydrogen chloride (HCl), and oxygen in the presence of cupric chloride to form ethylene dichloride, which decomposes at high temperatures to form VCM and HCl. In an alternative commercial process, carbide gas (acetylene) from carbide is reacted with HCl over a mercury-based catalyst. This method is preferred in the case of obtaining cheap carbide gas via carbide from abundant coal resources. The mercury catalyst used in this method (typically 8%-10% mercuric chloride supported on activated carbon) is highly toxic. Such toxicity forms problems caused by handling during the manufacture of the catalyst, as well as during the loading of the catalyst and the removal of the catalyst after the production campaign. The production campaign typically has a duration of six months. Deactivation of the mercury catalyst and loss of HgCl during use due to sublimation or volatilization from the reactor 2 Significant problems can result. The carbide process using mercury-based catalysts requires lower capital investment than the ethylene process. It would be a significant advantage if a non-volatile and less toxic catalyst could replace the mercury catalyst in an existing plant design without requiring significant changes to the plant.

[0003] WO2013 / 008004 (the teachings of which are incorporated herein in their entirety) describes a catalyst with improved toxicity compared to an early VCM catalyst, which can be used in a catalytic process for producing VCM from carbide gas. However, commercial access to such catalysts is hampered by the cost of gold required to make the active catalyst. When a relatively low level of gold content (to avoid high production costs) is employed, the stability of the catalyst is adversely affected, and the catalytic activity is reduced. In addition, it has been found that when such gold-containing catalysts are manufactured, gold nanoparticles are typically formed, which in turn can result in the formation of carbon nanotubes during use of the catalyst, which subsequently result in catalyst pulverization, thereby resulting in the loss of gold and the deactivation of the catalyst. Therefore, it is desirable to provide a gold-containing catalyst having a relatively low level of expensive gold active material, but which does not exhibit an undesirable reduction in catalyst stability, activity or selectivity, and preferably, wherein the formation of gold nanoparticles is reduced or eliminated to avoid the formation of carbon nanotubes in use.

[0004] Preferred embodiments of the present invention attempt to overcome one or more of the above-mentioned disadvantages of the prior art. In particular, preferred embodiments of the present invention attempt to provide improved gold-containing catalysts by adding inorganic oxides, hydroxides, oxygen-containing salts or oxygen-containing acids, and methods of making such improved catalysts and their use in chemical processes for making vinyl chloride monomer (VCM) from acetylene are described herein. Summary of the invention

[0005] According to a first aspect of the present invention, there is provided a catalyst comprising the following substances on a carrier:

[0006] Gold complexes with sulfur-containing ligands; and

[0007] The additive is selected from: inorganic oxides, hydroxides, oxygen-containing salts or oxygen-containing acids.

[0008] According to a second aspect of the present invention, there is provided a method for preparing the catalyst, wherein:

[0009] i) providing a gold solution,

[0010] ii) providing a solution of a sulfur-containing ligand,

[0011] iii) providing a solution of the additive or a precursor thereof,

[0012] iv) mixing the gold solution with the sulfur-containing ligand solution to provide a gold complex impregnation solution, and

[0013] vi) impregnating a catalyst support with the gold complex impregnation solution and then drying the impregnated support, then impregnating with the solution from (iii) and then drying the impregnated support, or

[0014] v-ii) impregnating the catalyst support with the solution from step (iii) and then drying the impregnated support, and then impregnating with the gold complex impregnation solution and then drying the impregnated support.

[0015] According to a third aspect of the present invention, there is provided an alternative method for producing the catalyst, characterized in that:

[0016] i) providing an impregnation solution, the impregnation solution comprising a gold complex and an additive or a precursor thereof;

[0017] ii) impregnating a catalyst support with the solution from step (i) to produce an impregnated support, and then drying the impregnated support.

[0018] According to a fourth aspect of the present invention, there is provided a process for the hydrochlorination of an alkyne, the process comprising reacting the alkyne with HCl in the presence of a catalyst according to the first aspect of the present invention.

[0019] Unless otherwise indicated, all % herein relate to percentages by weight of the total catalyst. DETAILED DESCRIPTION

[0020] catalyst

[0021] In the catalyst of the present invention, the active catalytic material comprises gold (Au) in a positive oxidation state, preferably Au 3+ and Au 1+ , but some of the gold present may be in the form of metallic gold (Au 0 In some embodiments of the present invention, the catalyst may be considered to comprise gold particles having a core comprising metallic gold and a core comprising a higher oxidation state gold species (including Au 3+ The shell need not be complete, but preferably all or substantially all of the exposed surface of the particle has a gold species in a surface higher oxidation state; for example, if the metallic gold is partially surrounded by a support, the "shell" may extend only over the exposed particle surface. Au 3+ is not necessarily the only higher oxidation state gold species present in the shell, and for example Au 1+ It may also be present. For example, in prior art catalysts, such higher oxidation state species may be stabilized by halides. It has been widely proposed in the prior art that gold species in higher oxidation states are active species for catalyzing the reaction of acetylene with HCl. It is believed that in the catalysts of the present invention, gold is stabilized in a higher oxidation state by complexing with sulfur-containing ligands. The core of the particle typically comprises metallic gold (Au 0 ), but alternative gold species may also be present in the core.

[0022] As used herein, the term "additive" means an inorganic oxide, hydroxide, oxy-salt or oxy-acid. Herein, "inorganic" means not containing carbon. As used herein, the term "additive precursor" means a material that can be converted into an inorganic oxide, hydroxide, oxy-salt or oxy-acid, typically after hydrolysis and / or drying. The additive precursor may or may not contain carbon.

[0023] As will be further described below, the method of the present invention prepares the catalyst by impregnating the catalyst support with an additive or an additive precursor. Without wishing to be bound by theory, it is believed that the additive or additive precursor forms at least a partial layer around the gold particles. After hydrolysis and / or drying, the result is typically an inorganic oxide layer around the gold complex particles, but the layer may comprise one or more of an inorganic oxide, a hydroxide, an oxygen-containing salt or an oxygen-containing acid, depending on the preparation method. It is believed that the presence of this layer prevents the gold particles from being deactivated.

[0024] Suitably, the catalyst comprises between 10% and 0.01% additive, preferably between 10% and 0.1% additive, preferably between 5% and 0.1%, more preferably between 3% and 0.5% additive. Low levels of additive are preferred to avoid that the level of additive has an adverse effect on the activity of the catalyst, however sufficient additive must be present to achieve an increase in catalyst stability, and levels of additive between 5% and 0.1% have been found to achieve the best balance of these two requirements, but different amounts of additive may be preferred depending on the salt or acid selected and the various operating parameters of any process in which the catalyst is used. The additive may comprise a mixture of one or more of an inorganic oxide, hydroxide, oxygen-containing salt or oxygen-containing acid.

[0025] As used herein, an oxygen-containing salt is a salt comprising the formula [M x O y ] z- Salts of anions where M is an element other than carbon or oxygen. Examples include metasilicates [SiO 3 ] 2- 、Orthosilicate [SiO 4 ] 4- , tetraborate [B 4 O 7 ] 2- and phosphate [PO 4 ] 3-。 Oxygen acids are the corresponding protonated forms, such as [PO 4 ] 3- and H 3 PO 4 , which in some cases can depolymerize, for example [B 4 O 7 ] 2- and B(OH) 3 Preferred elements M include Zr, Ce, La, Y, Ti, Bi, Zn, Al, V, Cr, Mn, Mo, W, Re, B, N, Si, P, S, Ge, As, Se, Sn, Sb, Te, Cl, Br and I. More preferred elements M include Zr, Ce, La, B, Si, P and S.

[0026] In a preferred embodiment, the additive is:

[0027] (i) oxides or hydroxides of metals, metalloids or non-metal elements; or

[0028] (ii) Oxygen-containing salts or acids of metalloids or non-metallic elements.

[0029] Herein, the metalloid element is one selected from B, Si, Ge, As, Sb and Te; preferred metalloids are B and Si, especially Si. Preferred non-metals are S and P, especially P.

[0030] In a preferred embodiment, the additive is an oxide, hydroxide, oxysalt or oxyacid of boron, silicon, sulfur or phosphorus, more preferably an oxide, hydroxide, oxysalt or oxyacid of boron, silicon or phosphorus, more preferably an oxide, hydroxide, oxysalt or oxyacid of boron or silicon. The typical content of boron, silicon, sulfur or phosphorus will be 0.01 wt %-10 wt %, such as 0.1 wt %-10 wt %, such as 0.5 wt %-10 wt % or 0.5 wt %-5 wt %, based on the total weight of the catalyst. The content of these elements can be measured by techniques known to those skilled in the art, such as inductively coupled plasma (ICP) techniques, including ICP-MS, ICP-AES and ICP-OES.

[0031] In a preferred embodiment, the additive is an oxide, hydroxide, oxygen-containing salt or oxygen-containing acid of silicon. The catalyst may include one or more silicon materials, such as silicon dioxide, silicate, metasilicate, etc. Based on the gross weight of the catalyst, a typical silicon content will be 0.01 wt %-10 wt %, such as 0.1 wt %-10 wt %, such as 0.5 wt %-10 wt % or 0.5 wt %-5 wt %. The content of silicon can be measured by techniques known to those skilled in the art, such as inductively coupled plasma (ICP) technology, including ICP-MS, ICP-AES and ICP-OES.

[0032] Advantageously, the additive should be a stable, relatively low or non-reducing / oxidizing oxide, hydroxide, oxygen-containing salt or oxygen-containing acid of a metal or non-metal element. In some embodiments, the additive or additive precursor is an alkali metal salt, an alkaline earth metal salt or a rare earth metal salt. Preferred counterions include ammonium or alkali metals, for example: ammonium silicate, ammonium borate, ammonium sulfate, ammonium phosphate, sodium silicate, sodium borate, sodium sulfate or sodium phosphate.

[0033] Particularly suitable inorganic oxygen acids are boric acid, phosphoric acid, silicic acid or sulfuric acid. Boric acid (B(OH) 3 ) is a particularly preferred boron-containing oxygen acid.

[0034] More particularly, the following additives have been found to be particularly useful: sodium metasilicate pentahydrate, sodium tetraborate, boric acid, and trisodium orthophosphate. In particular, the additive is preferably a sodium silicate salt, and most preferably sodium metasilicate pentahydrate.

[0035] In some embodiments, the additive may be a product derived from an additive precursor which, upon being deposited on the catalyst support, is converted (usually by thermal or chemical degradation, and, where appropriate, hydrolysis) to form a non-reducible inorganic oxide; preferred inorganic oxides that may be formed in this manner include SiO 2 、Al 2 O 3 、TiO 2 、ZrO 2 ,La 2 O 3 、CeO 2 , their suboxides or mixtures thereof. The additive precursor may be inorganic or organic. Suitable inorganic and organic precursors will be understood by the skilled person and will include alkoxides of the above elements, such as tetraethyl orthosilicate (TEOS), isopropoxy titanium, etc. Alternative precursors include metal salts, such as metal chlorides or metal nitrates, which are converted into the corresponding hydroxides and oxides by hydrolysis.

[0036] Typically, the catalyst contains less than 1% gold. Preferably, the catalyst contains less than 0.5% gold. Preferably, the catalyst contains less than 0.1% gold. More preferably, the catalyst contains no more than 0.075% gold, and most preferably, the catalyst contains no more than 0.05% gold. For some uses, the catalyst may contain no more than 0.025% gold, but without losing commercially acceptable catalyst activity. A gold content of less than 0.1% by weight of the catalyst can be considered a catalyst with a low gold content and is atypical. Since the cost of manufacturing the catalyst is correspondingly reduced, it is attractive to use lower levels of gold, because gold will generally be the most expensive component in the catalyst. However, to date, the ability to utilize these relatively low levels of gold (especially no more than 0.05%) has been limited, due to the loss of stability of the catalyst product resulting in unacceptably low catalyst activity levels, which are observed as unacceptably low product conversion levels. The incorporation of additives into the catalyst overcomes the disadvantages associated with the use of relatively low levels of gold (no more than 0.05%). Surprisingly, it has been found that the addition of additives to the gold-containing catalysts of the invention is advantageous.

[0037] In addition or alternatively, even in low gold-containing catalysts with relatively high levels of gold content (i.e., more than 0.05%), improvements in catalyst properties are observed. More specifically, nanotube formation has been advantageously suppressed. Therefore, the addition of additives to gold-containing catalysts containing relatively high levels of gold (i.e., more than 0.05%) has a surprisingly beneficial effect. Nanotube formation leads to catalyst deactivation, and therefore it has been found that the addition of additives inhibits the deactivation of gold-containing catalysts. The catalyst deactivation process via nanotube formation occurs largely due to the reduction of oxidized gold in the catalyst and the growth of gold particles, thereby forming relatively large (>200nm) gold nanoparticles. It is also believed that the nanoparticles can also serve as cores for the formation of carbon nanotubes. The formation of nanotubes is manifested as a yellow powdery deposit on the catalyst pellets, resulting in dust formation and loss of gold contained in the powder, thereby causing catalyst deactivation.

[0038] Without being bound by theory, a thin film of the additive or additive precursor may form around the gold particles, inhibiting sintering and nanotube nucleation. The additive precursor may undergo hydrolysis or partial hydrolysis to form its corresponding non-reducible oxide or suboxide around the gold particles; this may prevent migration and sintering of the gold particles of the catalyst when / during use, or act as a barrier between the carbon support and the metal particles.

[0039] In view of the above paragraphs, the skilled person will appreciate that the beneficial effects of including additives in gold-containing catalysts according to the present invention are twofold: first, improving the stability of low gold-containing catalysts (up to 0.05%) and eliminating activity losses, and second, inhibiting the deactivation of the gold-containing catalyst, generally by limiting the formation of nanotubes on the catalyst surface.

[0040] Any known catalyst support may be used to prepare the catalyst of the present invention. Typical metal oxide supports such as alumina, silica, zeolite, silica-alumina, titania or zirconia and composites thereof may be used.

[0041] Most preferably, the catalyst support is made of carbon, including carbon supports derived from natural sources (peat, wood, coal graphite, etc. or combinations thereof) or synthetic carbon. The carbon is preferably activated carbon, such as activated carbon activated by steam, acid or other chemical means. Preferred carbon supports include high surface area activated carbon, preferably having greater than 800 m 2 / g surface area, such as 1300m 2 / g of carbon extrudate. Carbon extrudates are commercially available in "high purity" or "ultra-high purity" grades, and such grades are typically acid washed to remove impurities. Combinations of metal oxides and carbon can also be used as catalyst supports.

[0042] The catalyst carrier can take the form of powder, microparticles or particles formed in various shapes ("shaped units"). Preferred shaped units include spheres, tablets, cylinders, multi-leaf cylinders, rings, miniliths, etc., or bulk catalyst units such as monoliths. Alternatively, the catalyst in powder form may be included in a coating formulation and applied to a reactor wall or a shaped substrate such as a monolith. A preferred form of the catalyst carrier includes a plurality of shaped units in the form of a cylinder, a sphere or a leafed cylinder, each cylinder, a sphere or a leafed cylinder having a diameter of 0.1 mm-10 mm, or more preferably having a diameter in the range of 1 mm-3 mm. In the case of a cross-sectional shape with an uneven diameter, such as a leafed cylinder, the diameter is an average diameter. Such catalyst carrier shapes are commercially available and can be made by extrusion, tableting or other methods.

[0043] Sulfur can be present in the catalyst in the form of a sulfur compound containing sulfur in a reduced or oxidized state or in a combination of reduced and oxidized states, for example, in the form of a thiosulfate ion. More specifically, sulfur is present in a sulfur-containing compound that is a ligand that can form a complex with a gold substance or complex with a gold substance. More preferably, the sulfur-containing ligand can stabilize the gold in the positive oxidation state form. Suitable sulfur-containing ligands are oxidizing ligands containing sulfur in a positive oxidation state, especially oxygen-donating ligands, or sulfur-donating ligands. Preferred sulfur-containing compounds include sulfates, sulfonates, thiosulfates, thiocyanates, thioureas, mercaptans, and thionyl chloride. Preferred thioureas include thioureas themselves or substituted thioureas. Preferred mercaptans include thiopropionic acid and thiomalic acid.

[0044] In a preferred embodiment, the sulfur-containing compound is a part that can form a complex with the gold material through a sulfur atom or a complex with the gold material through a sulfur atom. In this embodiment, the part comprises one or more sulfur atoms, at least one of which is a sulfur-donating atom. Preferred sulfur-donating ligands include thiosulfate, thiocyanate, thiourea, mercaptan and thionyl chloride. Preferred thiourea includes thiourea itself or substituted thiourea. Preferred mercaptan includes thiopropionic acid and thiomalic acid.

[0045] The amount of sulfur in the fresh catalyst is preferably in the range of about 0.005 wt % to 15 wt %, more preferably 0.03 wt % to 7 wt %, especially up to about 5 wt % of the dry catalyst. In one embodiment of the invention, wherein the gold complex is a gold-thiosulfate complex, the molar ratio of S to Au in the complex is preferably in the range of about 3:1 to about 8:1. In such embodiments comprising the preferred amount of gold, the amount of sulfur in the catalyst may be in the range of 0.03 wt % to 1.50 wt %. Some sulfur derived from sources other than the S-containing complex may also be present in the catalyst, for example incorporated into the support material.

[0046] The catalyst may additionally comprise a metal other than gold or any metal forming a carrier compound. Known promoters used with gold catalysts for hydrochlorination include compounds of cobalt, copper or lanthanum, and such metals may be present in the catalyst of the present invention or in the catalyst used in the method of the present invention. Group 1 and Group 2 metals may also be advantageously incorporated into the catalyst of the present invention. Therefore, in addition to gold, the catalyst may also comprise a metal or a compound of a metal selected from cobalt, copper, lanthanum, cerium, lithium, sodium, potassium, rubidium, cesium, magnesium, calcium, strontium and barium. The additional metal may exist as a promoter, or may have another function in the catalyst or its preparation. For example, it is believed that some metals such as calcium inhibit the formation of carbon deposits on the catalyst, and therefore may be used to help maintain the activity of the catalyst over a period of time. Therefore, even if there is a metal that does not increase the activity of the catalyst in the short term, it may still be considered a promoter if it has a tendency to reduce catalyst deactivation during its use in the reaction or has another beneficial effect on the actual use of the catalyst.

[0047] Catalyst manufacturing

[0048] According to a second aspect of the present invention, there is provided a method for manufacturing the catalyst according to the first aspect of the present invention, wherein:

[0049] i) providing a gold solution,

[0050] ii) providing a solution of a sulfur-containing ligand,

[0051] iii) providing a solution of the additive or a precursor thereof,

[0052] iv) mixing the gold solution with the sulfur-containing ligand solution to provide a gold complex impregnation solution, and

[0053] vi) impregnating a catalyst support with the gold complex impregnation solution and then drying the impregnated support, then impregnating with the solution from (iii) and then drying the impregnated support, or

[0054] v-ii) impregnating the catalyst support with the solution from step (iii) and then drying the impregnated support, and then impregnating with the gold complex impregnation solution and then drying the impregnated support.

[0055] It is generally preferred to carry out the impregnation sequence shown in vi).

[0056] According to a third aspect of the present invention, there is provided an alternative method for producing the catalyst according to the first aspect of the present invention, wherein:

[0057] i) providing an impregnation solution, the impregnation solution comprising a gold complex and an additive or a precursor thereof;

[0058] ii) impregnating a catalyst support with the solution from step (i) to produce an impregnated support, and then drying the impregnated support.

[0059] This alternative process is preferred because it requires only one impregnation and drying step, thereby providing a simpler and less costly route to catalyst preparation.

[0060] In a preferred embodiment according to the third aspect of the present invention,

[0061] i) providing a gold solution,

[0062] ii) providing a solution of a sulfur-containing ligand,

[0063] iii) before step iv), adding an additive or a precursor thereof to the gold solution or the sulfur-containing ligand solution,

[0064] iv) mixing the gold solution with the sulfur-containing ligand solution to provide an impregnation solution, wherein the gold solution or the sulfur-containing ligand solution further comprises the additive or a precursor thereof,

[0065] v) impregnating a catalyst support with the impregnation solution and then drying the impregnated support.

[0066] As provided by the method according to the third aspect of the invention, an additive or an additive precursor may be added to the gold solution or the sulfur-containing ligand solution. Preferably, the additive or additive precursor is added to the sulfur-containing ligand solution where it will precipitate gold out of solution if added to the gold-containing solution, and alternatively, the additive or additive precursor is added to the gold-containing solution where it may cause an adverse reaction with the ligand if introduced into the ligand-containing solution.

[0067] In some embodiments, it is preferred that the pH of the gold solution (before the formation of the gold complex) is neither too acidic nor too basic. Under strongly acidic conditions, some sulfur-containing ligands are unstable, which is not conducive to the formation of the gold complex and leads to undesirable impurities in the impregnation solution. For example, thiosulfate is known to form tetrathiosulfonate ions ([S 4 O 6 ] 2- ). Under strong alkaline conditions, the gold solution may form colloids, which is also not conducive to the formation of gold complexes. The preferred pH range of the gold solution is pH 5-8, preferably pH 5.5-7.5. In a preferred embodiment, HAuCl is adjusted by using a base such as NaOH or KOH 4 to prepare a gold solution.

[0068] According to an additional and alternative embodiment of the present invention, a method for making the catalyst is provided, wherein the step of impregnating the catalyst support with the additive is achieved by providing an additive precursor and converting the precursor into an inorganic oxide, hydroxide, oxygen-containing salt or oxygen-containing acid to cause the catalyst support to be impregnated with the desired additive, which can then be dried as desired. In this case, the catalyst support can be impregnated with the additive precursor, and then the precursor is preferably converted into the additive by thermal degradation or chemical degradation. This will result in the catalyst support being impregnated with the selected additive.

[0069] In the method according to the second aspect of the present invention, involving the sequential impregnation of a gold complex and subsequently an additive precursor, it is sometimes preferred that a strongly alkaline solution of the gold complex is used for the first impregnation step if the additive precursor is resistant to hydrolysis under neutral or moderately alkaline conditions. In this embodiment, the pH of the impregnation solution containing the gold complex is preferably pH 9 or higher, preferably pH 10 or higher, more preferably pH 11 or higher. Once the gold complex has been formed, the appropriate pH can be achieved by adding a base such as NaOH or KOH. Without being bound by any theory, it is believed that the alkaline solution of the gold complex used to impregnate the catalyst support alkalizes the support, thereby pre-conditioning the support to hydrolyze the additive precursor in a subsequent impregnation step. This is particularly preferred when it is necessary to hydrolyze the precursor to form the corresponding oxide, for example in the case where the inorganic precursor is a metal nitrate or metal chloride.

[0070] The catalyst can be prepared using a variety of catalyst preparation techniques generally known in the art, such as impregnation, preferably using an initial impregnation method, or by a deposition-precipitation method. In the method for manufacturing the catalyst according to the present invention, the catalyst is preferably prepared by impregnating the carrier with a solution of a complex of gold and a sulfur-containing ligand (for forming a gold complex) and a combination of an additive or an additive precursor. The preferred gold complex is soluble in readily available solvents, which is almost harmless to the environment. The preferred solvent is an organic solvent, water or a mixture thereof. The solvent is preferably water. The preferred impregnation solution includes an aqueous solution of gold sulfate, sulfonate, thiosulfate, thiocyanate, thiourea, thionyl chloride, thiopropionic acid and thiomalic acid.

[0071] In a preferred embodiment, the process of the invention comprises impregnating a particulate carbon support with an aqueous solution comprising a complex comprising a compound of gold and a compound comprising thiosulfate ions and an additive or an additive precursor, and then, if necessary, separating excess solution and then drying the impregnated material.

[0072] Preferably, the impregnation is carried out by an initial impregnation method or a "pore filling" scheme, wherein the amount of solution used is calculated to just fill the pores of the support. Suitably, the gold compound and the compound containing thiosulfate ions together form a gold-thiosulfate complex, and the additive has a stabilizing effect on the gold-containing complex formed. Typically, the volume of the impregnation solution used is 100% ± up to about 20% of the measured (or calculated) pore volume of the support using the initial impregnation method of impregnation. The support is usually mixed with the impregnation solution by rolling, or the impregnation solution can be added to a stirred bed of the support, such as dropwise or by spraying, over a period of time. Alternatively, an excess volume of the impregnation solution can be used to impregnate the catalyst support with an impregnation solution containing the gold complex and the additive or additive precursor, so that the gold and / or sulfur compound is deposited on the catalyst support by absorption or by ion exchange reaction. Technicians in the field of catalyst manufacturing are familiar with such methods of preparing catalysts by impregnating support materials with solutions of active metal compounds.

[0073] The amounts of gold, sulfur and additive or additive precursor in the impregnation solution are calculated to provide the desired amounts of gold, sulfur and additive in the finished catalyst.

[0074] The impregnation solution comprising the gold complex may comprise an additional metal compound, for example a compound comprising a metal selected from the group consisting of cobalt, copper, lanthanum, cerium, lithium, sodium, potassium, rubidium, cesium, magnesium, calcium, strontium and barium. If present, the additional metal may alternatively be added to the catalyst in a separate step, for example by impregnating the gold-containing catalyst particles with a solution of the compound of the additional metal, or by impregnating the support material with such a solution prior to adding the gold-containing complex solution to the catalyst.

[0075] In an alternative but less preferred method of manufacture, the catalyst may be prepared by known solid state methods, for example, by mixing dry support, gold, ligand, and additive or additive precursor components. In this case, the gold-ligand complex may be preformed in an initial step. Ball milling is a particularly suitable solid state process, however, a more uniform application of the active components to the catalyst support may be achieved via the support impregnation methods disclosed herein.

[0076] As mentioned above, the catalyst support is preferably carbon, and this may be subjected to an acid wash, preferably using hydrochloric acid, nitric acid, phosphoric acid or sulfuric acid, which may preferably be carried out before impregnation with an impregnation solution comprising the gold complex. This may be done, for example, by dispersing the carbon in hydrochloric acid, optionally heating, possibly to boiling, draining, washing with distilled or deionized water and drying in air. As an alternative to using an acid wash procedure in catalyst preparation, when it is desired to use the carbon support in acid washed form, the pretreated or acid washed support may be obtained as a commercial material from the manufacturer of the carbon support.

[0077] Optionally, the catalyst may require an activation step prior to use in a chemical process. In this case, it may be more correct to refer to the dried, impregnated catalyst support as a catalyst precursor, but for simplicity, such materials are referred to herein as catalysts, regardless of whether they require activation (or pre-activation) to obtain their full catalytic activity.

[0078] Uses of Catalysts

[0079] It is envisioned that the catalyst of the present invention will be useful in any chemical process in which a gold-containing catalyst is known to have utility. However, a preferred chemical process of the present invention includes a method for making vinyl chloride (also known as vinyl chloride monomer or VCM) by hydrochlorination of acetylene, the method comprising reacting acetylene with hydrogen chloride (HCl) in the presence of a catalyst, the catalyst comprising a complex of gold and a sulfur-containing ligand on a support and an additive. Preferably, the catalyst is a catalyst according to the present invention and / or a catalyst prepared using the method of the present invention. The method is carried out at an elevated temperature, typically between about 100°C and 250°C, more preferably <200°C. Preferably, HCl and acetylene are premixed, and also preferably preheated to the reaction temperature. Typically, HCl is present in an amount in excess of that required for the stoichiometric reaction. The catalyst may be present in a reactor in the form of a fixed bed of catalyst particles, the catalyst particles being arranged so that the feed gas passes through or through the catalyst bed. Alternative reactor arrangements may be used, including fluidized beds or other moving bed arrangements. Alternatively, the catalyst may be provided in the form of a monolith or coated on the wall of the reaction vessel. If necessary, the catalyst bed may have means for regulating the temperature to avoid overheating due to the exothermic reaction, or to increase the temperature. It may be preferred to treat the catalyst with HCl before use in the process. The treatment is generally carried out by flowing HCl over the catalyst at a temperature of at least 50°C, more particularly >100°C, for a period of at least one hour. The pretreatment can be carried out in the reactor by operating with a flow of HCl in the absence of acetylene at a suitable temperature.

[0080] It should be understood that features described with respect to one aspect of the present invention may also apply to another aspect of the present invention. For example, features described with respect to the catalyst of the present invention may also apply to the catalyst prepared by the manufacturing method of the present invention, and vice versa.

[0081] The present invention will now be further described in the following examples with reference to the accompanying drawings, in which:

[0082] Figure 1 SEM image of the fresh, untreated catalyst surface containing 0.1% gold.

[0083] Figure 2SEM image of the surface of a fresh catalyst containing 0.1% gold treated with 1% boric acid.

[0084] Figure 3 SEM images of nanotube formation on the surface of a used untreated catalyst containing 0.1% gold.

[0085] Figure 4 is a SEM image of a used 1% boric acid treated 0.1% gold containing catalyst with no carbon nanotube formation.

[0086] Figure 5 Shown are the relative conversions to VCM obtained for the untreated 0.1% and 0.05% gold containing catalysts relative to the 0.05% gold containing catalyst treated with the addition of sodium silicate.

[0087] Figure 6 The significant increase in VCM conversion obtained with a catalyst containing 0.05% gold with the addition of silicate relative to a gold-containing catalyst in the absence of such silicate is shown.

[0088] Example

[0089] Embodiment 1 (comparison): A 0.1% gold thiosulfate catalyst was prepared according to the prior art.

[0090] 0.142 g of HAuCl containing 41% Au 4 The solution was diluted in 24 mL of water. Separately, 0.186 g of anhydrous sodium thiosulfate was dissolved in 24 mL of water. The gold-containing solution was then added to the thiosulfate solution under stirring to obtain a light yellow mixed solution of the prepared gold complex. 4.8 ml of this gold complex solution was then added to 5.8 g of commercially available activated carbon pellets under stirring. The carbon absorbed all the liquid in about 5 minutes. After leaving the product to dry in air for about an hour, the material was then heated at 120 ℃ The catalyst was dried overnight at 4 °C to obtain a catalyst containing approximately 0.1% Au. Figure 1 is a SEM image of this freshly prepared untreated catalyst.

[0091] Embodiment 2: Testing of carbon nanotube formation.

[0092] 5 g of the catalyst prepared as described in Example 1 was loaded into a stainless steel tube of 2 cm in diameter and the resulting bed was supported at either end by quartz wool packings. The tube was then placed in a tube furnace. ℃ At a temperature of 2 H 2A mixture of (molar ratio of 1.2:1) was passed over the catalyst at a flow rate of 240 ml / min. The initial conversion to VCM was about 90%, which dropped to 65% after 48 hours. After 48 hours, the catalyst was purged with nitrogen, cooled, and then removed from the furnace. Optical inspection showed the presence of carbon nanotubes on the carbon pellets. The extent of nanotube formation was assessed as follows: 0 = no nanotubes; 1 = nanotubes present on some particles; 2 = nanotubes present on many particles; 3 = nanotubes present on most particles.

[0093] SEM examination showed that the coating was composed of a large number of carbon nanotubes, each of which was nucleated by a gold particle. Figure 3 The nanotube formation degree of this embodiment is 3.

[0094] Embodiment 3: The catalyst is prepared according to the invention.

[0095] The catalyst was prepared as described in Example 1, except that 0.58 g of an additive in the form of sodium metasilicate pentahydrate was dissolved in HAuCl 4 Thereafter, the procedure was the same as in Example 1.

[0096] Embodiment 4: The catalyst is prepared according to the invention.

[0097] The catalyst was prepared as described in Example 1, except that 0.58 g of an additive in the form of sodium tetraborate was dissolved in HAuCl 4 Thereafter, the procedure was the same as in Example 1.

[0098] Embodiment 5: The catalyst is prepared according to the invention.

[0099] The catalyst was prepared as described in Example 1, except that 0.58 g of boric acid was dissolved in HAuCl 4 Thereafter, the procedure was the same as in Example 1. Figure 2 is a SEM image of the fresh boric acid treated catalyst.

[0100] Embodiment 6: The catalyst is prepared according to the invention.

[0101] The catalyst was prepared as described in Example 1, except that 0.58 g of trisodium orthophosphate was dissolved in HAuCl 4 Thereafter, the procedure was the same as in Example 1.

[0102] Embodiment 7: The catalysts according to the invention were tested for nanotube formation.

[0103] Catalysts prepared as described in Examples 3-6 were tested for nanotube formation over time periods ranging from two to five days according to the method given in Example 2. In all cases, carbon nanotube formation was either completely prevented (degree of nanotube formation = 0) or was present only on a few microscopic areas of the pellet (degree of nanotube formation = 1). Figure 4 is a SEM image of the boric acid treated catalyst of Example 5 after testing according to the method of Example 2; here it can be seen that the gold particle size increased, but there was no discernible nanotube growth. The degree of nanotube formation for this example was zero.

[0104] Embodiment 8 (comparison): The 0.05% Au catalyst was prepared according to the prior art.

[0105] The catalyst was prepared as described in Example 1, except that 0.071 g of HAuCl containing 41% Au was used. 4 Solution to prepare diluted HAuCl 4 solution; and 0.093 g of sodium thiosulfate was used to prepare the thiosulfate solution. The resulting catalyst contained approximately 0.05% Au.

[0106] Embodiment 9: The 0.05% Au catalyst was prepared according to the present invention.

[0107] The catalyst was prepared as described in Example 8, except that 0.58 g of sodium metasilicate pentahydrate was dissolved in HAuCl 4 Thereafter, the procedure was the same as in Example 8.

[0108] Embodiment 10: Testing of 0.05% Au catalysts according to the present invention resulted in increased activity.

[0109] The 0.05% Au catalyst with silicate additive according to Example 9 was subjected to the conversion test described in Example 2. The conversion is shown in Figure 6 , where it can be seen that a significant increase in conversion to VCM is obtained with the catalyst comprising silicate relative to the catalyst in which no silicate is present. For the material prepared in Example 9, there was no nanotube formation after six days, as shown in FIG. Figure 5 Visible in.

[0110] Figure 5 The conversion to VCM of two untreated catalysts (one containing 0.1% Au and the other containing 0.05% Au) according to Example 2 at 220°C but over a longer period of time (up to 6 days instead of 48 hours) is shown compared to 0.05% Au when treated with sodium silicate addition as described above. Figure 5In the Figure 5, it can be clearly seen that the addition of sodium silicate allows the catalyst containing lower (0.05%) Au to achieve selectivity comparable to the catalyst containing higher (0.1%) Au (but untreated).

[0111] For the 0.1% Au catalyst, the conversion improvement exhibited by the catalyst containing 0.05% Au and silicate in Example 10 did not occur as clearly, but nanotube formation was advantageously suppressed. Thus, the present invention is particularly applicable and desirable for catalysts having less than 0.1% gold.

[0112] Examples 11-17

[0113] HAuCl containing 0.100 g Au was diluted with a specified amount of deionized water (DI). 4 Separately, solutions of sulfur-containing ligands and additives were prepared with the indicated amounts of deionized (DI) water. The solutions were combined in the order indicated to prepare the gold-containing impregnation solution. This solution was then added to 100 g (dry weight) of commercially available activated carbon pellets via an incipient impregnation technique with stirring. The impregnated material was allowed to stand for approximately 30 minutes, during which time all of the added solution was adsorbed. The material was then heated at 105 ℃ The catalyst was dried overnight at 4 °C to obtain a catalyst containing approximately 0.1% Au.

[0114] In the case of Example 17, pH adjustment was performed as follows. HAuCl containing 0.100 g Au was diluted with 30 ml of deionized water. 4 Solution. About 5% KOH solution was prepared by dissolving 5 g of NaOH in 100 ml of deionized water. About 1 ml of KOH solution was added dropwise to the gold-containing solution to form a solution with a pH of about 6.8. 0.336 g of ammonium thiosulfate was separately dissolved in 30 ml of deionized water. The gold-containing solution was then added to the ammonium thiosulfate solution under stirring to obtain a mixed solution of the prepared gold complex. The resulting solution was then used in the initial impregnation technique according to the above procedure.

[0115] XPS analysis of Examples 11-16 indicated the presence of SiO in the materials formed after drying overnight at 105 °C. 2 .

[0116] The catalysts were tested for carbon nanotube formation according to the procedure in Example 2.

[0117]

[0118] Table 1

[0119] Zr, Ce and La Precursors

[0120] Embodiment 18 (Compare)

[0121] Dilute HAuCl containing 0.100 g Au with 12 ml of deionized water. 4 Solution. 4 g of NaOH was dissolved in 100 ml of deionized water to prepare an approximately 1 M NaOH solution. 1.60 g of the prepared 1 M NaOH solution was added dropwise to the gold-containing solution to form a solution having a pH of approximately 6.5. 0.336 g of sodium thiosulfate was separately dissolved in 12 ml of deionized water. The gold-containing solution was then added to the sodium thiosulfate solution under stirring to obtain a mixed solution of the prepared gold complex having a pH of approximately 11.2. Another 12 ml of the pre-prepared 1 M NaOH solution and 22 ml of deionized water were added to the gold-containing solution to obtain a solution of the prepared gold complex having a pH of approximately 12.3. The resulting gold-containing solution was then added to 100 g (dry weight) of commercially available activated carbon pellets via an initial impregnation technique under stirring. The impregnated material was allowed to stand for approximately 30 minutes, during which time all of the added solution was adsorbed. The material was then heated at 105 ℃ The catalyst was dried overnight at 400 °C to give an Au / C catalyst containing approximately 0.1% Au. The catalyst was tested as described in Example 2. The degree of carbon nanotube formation was 1.

[0122] Embodiment 19

[0123] The 0.1% Au / C catalyst was prepared as described in Example 18. Separately, 1.467 g zirconium oxynitrate dihydrate [ZrO(NO 3 ) 2 .2H 2 O] was dissolved in 30 ml of deionized water and the solution was added to 50 g of dry gold-containing carbon pellets via an initial impregnation technique. After the material was allowed to stand for about 30 minutes, the material was heated at 105 ℃ The catalyst was dried overnight at 40 °C to obtain a catalyst containing approximately 0.1% Au and 1% Zr.

[0124] Embodiment 20

[0125] The 0.1% Au / C catalyst was prepared as described in Example 18. Separately, 1.550 g of cerium nitrate hexahydrate [Ce(NO 3 ) 3 .6H 2 O] was dissolved in 30 ml of deionized water and the solution was added to 50 g of dry gold-containing carbon pellets via an initial impregnation technique. After the material was allowed to stand for about 30 minutes, the material was heated at 105 ℃The catalyst was dried overnight at 400 °C to obtain a catalyst containing approximately 0.1% Au and 1% Ce. The catalyst was tested as described in Example 2. The degree of carbon nanotube formation was 1.

[0126] Embodiment 21

[0127] The 0.1% Au / C catalyst was prepared as described in Example 18. Separately, 1.335 g of lanthanum chloride heptahydrate [LaCl 3 .7H 2 O] was dissolved in 30 ml of deionized water and the solution was added to 50 g of dry gold-containing carbon pellets via an initial impregnation technique. After the material was allowed to stand for about 30 minutes, the material was heated at 105 ℃ The catalyst was dried overnight at 40 °C to obtain a catalyst containing approximately 0.1% Au and 1% La.

[0128] It will be appreciated by those skilled in the art that the above embodiments are described by way of example only and not in any limiting manner, and that various changes and modifications may be made without departing from the scope of the present invention as defined in the appended claims.

[0129] The present invention also includes the following embodiments:

[0130] 1. A catalyst comprising a complex of gold and a sulfur-containing ligand on a carrier and an inorganic salt or acid.

[0131] 2. The catalyst according to embodiment 1, comprising between 10 wt% and 0.1 wt% of an inorganic salt or acid, based on the total weight of the catalyst.

[0132] 3. The catalyst according to embodiment 1, comprising between 5 wt% and 0.1 wt% of an inorganic salt or acid, based on the total weight of the catalyst.

[0133] 4. The catalyst according to embodiment 1, comprising between 3 wt% and 0.5 wt% of an inorganic salt or acid, based on the total weight of the catalyst.

[0134] 5. The catalyst according to any preceding embodiment, wherein the inorganic acid or salt is an inorganic acid selected from boric acid, phosphoric acid or sulfuric acid.

[0135] 6. The catalyst according to any one of embodiments 1 to 4, wherein the inorganic acid or salt is an inorganic salt selected from ammonium salts, silicates, borates or phosphates.

[0136] 7. The catalyst according to embodiment 6, wherein the inorganic salt is sodium silicate, sodium borate or sodium phosphate.

[0137] 8. The catalyst according to embodiment 7, wherein the inorganic salt is selected from sodium metasilicate pentahydrate, sodium tetraborate, boric acid and trisodium orthophosphate.

[0138] 9. The catalyst according to embodiment 6, wherein the inorganic salt is an ammonium salt.

[0139] 10. The catalyst according to any preceding embodiment, comprising less than 1.0 wt% gold, based on the total weight of the total catalyst.

[0140] 11. The catalyst according to any preceding embodiment, comprising no more than 0.1 wt. % gold, based on the total weight of the total catalyst.

[0141] 12. The catalyst according to any preceding embodiment, comprising no more than 0.05 wt. % gold, based on the total weight of the catalyst.

[0142] 13. The catalyst according to any preceding embodiment, wherein the support comprises carbon.

[0143] 14. The catalyst according to any preceding embodiment, wherein the support is in the form of powder, granules or shaped units.

[0144] 15. The catalyst according to any preceding embodiment, wherein at least some of the gold is in a positive oxidation state.

[0145] 16. The catalyst according to any preceding embodiment, wherein the sulfur-containing ligand is an oxidized ligand comprising sulfur in a positive oxidation state.

[0146] 17. The catalyst according to embodiment 16, wherein the sulfur-containing ligand is selected from sulfonates, thiosulfates, thiocyanates, thioureas, thionyl chloride, thiopropionic acid, and thiomalic acid.

[0147] 18. The catalyst according to any preceding embodiment, comprising sulfur in the range of about 0.005 wt % to 15 wt % based on the total weight of the total catalyst.

[0148] 19. The catalyst according to any preceding embodiment, further comprising a metal or a compound of a metal selected from the group consisting of cobalt, copper, lanthanum, cerium, lithium, sodium, potassium, rubidium, cesium, magnesium, calcium, strontium and barium.

[0149] 20. A method for producing a catalyst according to any one of embodiments 1 to 19, wherein:

[0150] i) providing a gold solution,

[0151] ii) providing a solution of a sulfur-containing ligand,

[0152] iii) providing a solution of an inorganic salt or an acid,

[0153] iv) mixing the gold solution with the sulfur-containing ligand solution to provide a gold complex impregnation solution,

[0154] v) impregnating a catalyst support with the gold complex impregnation solution and then drying the impregnated support,

[0155] vi) impregnating the catalyst support with the inorganic salt or acid and then drying the impregnated support.

[0156] 21. A method for producing a catalyst according to any one of embodiments 1 to 19, characterized in that

[0157] i) providing a gold solution,

[0158] ii) providing a solution of a sulfur-containing ligand,

[0159] iii) before step iv), adding an inorganic salt or an acid to the gold solution or the sulfur-containing ligand solution

[0160] iv) mixing the gold solution with the sulfur-containing ligand solution to provide an impregnation solution comprising a gold complex and an inorganic salt or acid, wherein the gold solution or the sulfur-containing ligand solution further comprises the inorganic salt or acid,

[0161] v) impregnating a catalyst support with said impregnation solution comprising a gold complex and an inorganic salt or acid, and then drying the impregnated support.

[0162] 22. A method according to embodiment 20 or 21, wherein the inorganic salt or acid is derived from a precursor that has been transformed.

[0163] 23. A method according to embodiment 22, wherein the precursor is transformed by thermal degradation or chemical degradation.

[0164] 24. The method according to any one of embodiments 20 to 23, further comprising an activation step.

[0165] 25. A chemical process comprising reacting at least one chemical substrate in the presence of a catalyst according to any one of embodiments 1 to 19 or a catalyst prepared by a process according to embodiment 20 or 21.

[0166] 26. The chemical method of embodiment 23, comprising oxidation of the chemical substrate.

[0167] 27. A process for the hydrochlorination of an alkyne comprising reacting the alkyne with hydrogen chloride in the presence of a catalyst according to any one of embodiments 1 to 19.

[0168] 28. A process for the hydrochlorination of alkynes according to embodiment 25, comprising the step of treating the catalyst with hydrogen chloride in the absence of acetylene.

Claims

1. A catalyst comprising the following on a carbon-containing support: a complex of gold and a sulfur-containing ligand, wherein the sulfur-containing ligand is a thiosulfate; and additives, wherein the additives are selected from: oxides, hydroxides, oxygen-containing salts or oxygen-containing acids of silicon, wherein the catalyst contains less than 0.5 wt % gold based on the total weight of the catalyst; and The catalyst has a silicon content of 0.1% to 10% by weight, based on the total weight of the catalyst. 2 . The catalyst according to claim 1 , wherein the catalyst has a silicon content of 0.5 to 10% by weight. The catalyst according to claim 1 , wherein the additive is silicic acid. The catalyst according to claim 1 , wherein the additive is sodium metasilicate pentahydrate.

5. The catalyst of claim 1, wherein the catalyst comprises no more than 0.1 wt% gold based on the total weight of the total catalyst.

6. The catalyst of claim 1, wherein the catalyst comprises no more than 0.05 wt% gold, based on the total weight of the catalyst.

7. A method of making a catalyst comprising: a complex of gold and a sulfur-containing ligand, wherein the sulfur-containing ligand is a thiosulfate; and additives, wherein the additives are selected from: oxides, hydroxides, oxygen-containing salts or oxygen-containing acids of silicon, wherein the catalyst contains less than 0.5 wt % gold based on the total weight of the catalyst; and wherein the catalyst has a silicon content of 0.1% to 10% by weight, based on the total weight of the catalyst, in, i) providing a gold solution, ii) providing a solution of a sulfur-containing ligand, wherein the sulfur-containing ligand is a thiosulfate, iii) providing a solution of an additive or a precursor thereof, wherein the additive is selected from oxides, hydroxides, oxygen-containing salts or oxygen-containing acids of silicon, iv) mixing the gold solution with the sulfur-containing ligand solution to provide a gold complex impregnation solution, and vi) impregnating a catalyst support with the gold complex impregnation solution and then drying the impregnated support, then impregnating with the solution from (iii) and then drying the impregnated support, or v-ii) impregnating the catalyst support with the solution from step (iii) and then drying the impregnated support, and then impregnating with the gold complex impregnation solution and then drying the impregnated support.

8. A method of making a catalyst comprising: a complex of gold and a sulfur-containing ligand, wherein the sulfur-containing ligand is a thiosulfate; and additives, wherein the additives are selected from: oxides, hydroxides, oxygen-containing salts or oxygen-containing acids of silicon, wherein the catalyst contains less than 0.5 wt % gold based on the total weight of the catalyst; and wherein the catalyst has a silicon content of 0.1% to 10% by weight, based on the total weight of the catalyst, in, i) providing an impregnation solution, wherein the impregnation solution comprises a complex of gold and a sulfur-containing ligand and an additive or a precursor thereof, wherein the sulfur-containing ligand is a thiosulfate, and the additive is selected from silicon oxides, hydroxides, oxygen-containing salts or oxygen-containing acids; ii) impregnating a catalyst support with the solution from step (i) to produce an impregnated support, and then drying the impregnated support.

9. A process according to claim 7 or claim 8, wherein the catalyst is as defined in any one of claims 1 to 6.

10. A method according to claim 7 or claim 8, wherein an additive precursor is used and is converted to an oxide, hydroxide, oxy-salt or oxy-acid of silicon via thermal or chemical degradation.

11. A process for the hydrochlorination of an alkyne, the process comprising reacting the alkyne with hydrogen chloride in the presence of a catalyst according to any one of claims 1 to 6.