Semiconductor structure and method for forming the same
By covering the protective layer before the mask stack in semiconductor manufacturing and performing rework operations when removing the mask stack, the problem of material loss during photoresist layer and anti-reflective coating removal is solved, and the graphics transfer is improved reliability and graphical accuracy.
Patent Information
- Application Number
- CN202010473015.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-05-29
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2040-05-29
AI Technical Summary
During the semiconductor manufacturing process, bubble defects are easily formed during the removal of the photoresist layer and the anti-reflective coating, resulting in damage to the pattern transfer material layer and affecting the reliability of the pattern transfer.
Before forming the mask stack, cover the protective layer of the pattern transfer material layer, isolate the process environment when the pattern transfer material layer is removed from the mask stack through the protective layer, reduce material losses, and rework operations until the detection reference is met, ensuring that Accuracy of graphic openings.
It improves the reliability of graphics transfer, reduces the loss of graphics transfer material layer and metal hard mask layer, and ensures the graphics accuracy and material preservation of subsequent processes.
Smart Images

Figure CN113745150B_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present invention relate to the field of semiconductor manufacturing, and in particular to a semiconductor structure and a method for forming the same. Background Art
[0002] Photolithography is a crucial technology in semiconductor manufacturing. It can transfer the required pattern from the mask to the silicon wafer to form a semiconductor product that meets the design requirements. Specifically, photolithography transfers the pattern by exposing it to the photoresist layer (the material is a light-sensitive resist) on the silicon wafer.
[0003] With the continuous development of integrated circuits, in order to meet the requirements of photolithography, in addition to the continuous upgrading of photolithography equipment, people also use other technologies to improve the quality and accuracy of photolithography, and the use of antireflective coating (ARC) technology is one of them. The function of forming an antireflective coating is to prevent the exposure light from reflecting at the substrate interface after passing through the photoresist layer, because the reflected light returning to the photoresist will interfere with the incident exposure light, resulting in uneven exposure of the photoresist.
[0004] However, in an actual production process, when the photoresist layer formed on the anti-reflective coating does not meet the pattern detection benchmark, the product needs to be reworked to remove the photoresist layer and the anti-reflective coating. Summary of the invention
[0005] The problem solved by the embodiments of the present invention is to provide a semiconductor structure and a method for forming the same, so as to improve the reliability of pattern transmission.
[0006] To solve the above problems, an embodiment of the present invention provides a method for forming a semiconductor structure, comprising: providing a substrate, on which a pattern transfer material layer is formed; forming a protective layer covering the pattern transfer material layer; forming a mask stack covering the protective layer, the mask stack comprising an anti-reflective coating and a photoresist layer stacked in sequence from bottom to top; patterning the photoresist layer to form a pattern opening penetrating the photoresist layer; detecting the pattern opening to determine whether the pattern opening meets a pattern detection benchmark; when the detection result does not meet the pattern detection benchmark, performing a rework operation until the detection result meets the pattern detection benchmark, the rework operation comprising: removing the mask stack and the protective layer in sequence; when the detection result meets the pattern detection benchmark, using the remaining photoresist layer as a mask, etching the anti-reflective coating and the protective layer along the pattern opening to expose the pattern transfer material layer.
[0007] Correspondingly, an embodiment of the present invention also provides a semiconductor structure, comprising: a substrate, on which a pattern transfer material layer is formed; a protective layer, covering the pattern transfer material layer; a mask stack, covering the protective layer, the mask stack comprising an anti-reflective coating and a photoresist layer stacked in sequence from bottom to top.
[0008] Compared with the prior art, the technical solution of the embodiment of the present invention has the following advantages:
[0009] In the formation method provided by the embodiment of the present invention, before forming the mask stack, a protective layer covering the graphic transfer material layer is formed. When the product needs to be reworked (i.e., when the mask stack needs to be removed), due to the existence of the protective layer, the protective layer can protect the graphic transfer material layer and isolate the graphic transfer material layer from the process environment when the mask stack is removed. In the process of removing the mask stack, the probability of the graphic transfer material layer being damaged is low. Therefore, after the mask stack is removed through the rework operation, the graphic transfer material layer is helped to be preserved intact, thereby helping to improve the reliability of subsequent graphic transfer. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figures 1 to 5 It is a schematic structural diagram corresponding to each step in a method for forming a semiconductor structure;
[0011] Figure 6 is a flow chart of an embodiment of a method for forming a semiconductor structure of the present invention;
[0012] Figures 7 to 16 It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor structure of the present invention. DETAILED DESCRIPTION
[0013] At present, the reliability of pattern transmission still needs to be improved. Now, the reasons why its performance needs to be improved are analyzed in combination with a method for forming a semiconductor structure.
[0014] Figures 1 to 5 The present invention is a schematic structural diagram corresponding to each step in a method for forming a semiconductor structure.
[0015] refer to Figure 1 , a substrate (not shown) is provided, on which an interlayer dielectric layer 10 is formed. The interlayer dielectric layer 10 is used to form interconnection holes.
[0016] Continue to refer Figure 1 , a metal hard mask layer 20 is formed on the interlayer dielectric layer 10 ; a buffer oxide layer 30 is formed on the metal hard mask layer 20 ; and a pattern transfer material layer 40 is formed on the buffer oxide layer 30 .
[0017] As an example, the material of the pattern transfer material layer 40 is amorphous silicon (a-Si).
[0018] Continue to refer Figure 1 A mask stack 90 is formed on the pattern transfer material layer 40 , wherein the mask stack 90 includes a spin-on carbon layer 50 , an anti-reflective coating layer 60 on the spin-on carbon layer 50 , and a photoresist layer 70 on the anti-reflective coating layer 60 .
[0019] After forming the mask stack 90 , the method further includes: patterning the photoresist layer 70 to form a graphic opening (not shown) penetrating the photoresist layer 70 ; and detecting the graphic opening to determine whether the graphic opening meets a graphic detection benchmark.
[0020] Combined with reference Figure 2 and Figure 3 When the inspection result does not meet the pattern inspection benchmark, a rework operation is performed, and the rework operation includes: removing the mask stack 90 (such as Figure 1 After removing the mask stack 90, the pattern transfer material layer 40 is cleaned using a hydrofluoric acid solution.
[0021] After the rework operation, the processes of forming the mask stack 90, patterning the photoresist layer 70, and inspecting the pattern opening are performed again in sequence until the inspection result meets the pattern inspection benchmark.
[0022] refer to Figure 4 After the rework operation, when the inspection result meets the graphic inspection benchmark, the remaining photoresist layer 70 is used as a mask to etch the anti-reflective coating 60 and the spin-coated carbon layer 50 along the graphic opening to expose the graphic transfer material layer; the exposed graphic transfer material layer 40 is doped to improve the etching resistance of the graphic transfer material layer 40, and the graphic transfer material layer 40 after the doping treatment is used as a shielding layer 40d.
[0023] refer to Figure 5 After forming the shielding layer 40d, the remaining pattern transfer material layer 40 is removed.
[0024] For example, if the material of the pattern transfer material layer 40 is amorphous silicon, the remaining pattern transfer material layer 40 is wet-etched using an ammonia solution.
[0025] The subsequent process also includes: using the blocking layer 40d as a mask, etching the metal hard mask layer 20 to form a mask opening in the metal hard mask layer 20; etching the interlayer dielectric layer 10 below the mask opening to form an interconnect opening in the interlayer dielectric layer 10; and forming a conductive structure in the interconnect opening.
[0026] However, if Figure 1As shown in FIG. 1 , since the anti-reflective coating 60 and the photoresist layer 70 are formed by a coating process and are affected by the materials of the anti-reflective coating 60 and the photoresist layer 70 themselves, when forming the mask stack 90, bubble defects 80 are easily formed in one or both of the anti-reflective coating 60 and the photoresist layer 70, and the process of removing the mask stack 90 is performed by controlling a preset time (by time), therefore, as shown in FIG. Figure 2 As shown, in the process of removing the mask stack 90, the pattern transfer material layer 40 below the bubble defect 80 is first exposed. Accordingly, after removing the mask stack 90, the pattern transfer material layer 40 at the position corresponding to the bubble defect 80 is easily damaged, thereby easily forming a pin hole 45 in the pattern transfer material layer 40. Moreover, in the process of cleaning, the cleaning solution (i.e., the hydrofluoric acid solution) is easy to contact and react with the buffer oxide layer 30 through the pin hole 45, thereby causing damage to the buffer oxide layer 30 and exposing the metal hard mask layer 20.
[0027] like Figure 5 As shown, when the metal hard mask layer 20 is exposed, when the remaining pattern transfer material layer 40 is wet-etched, the etching solution easily contacts the metal hard mask layer 20 through the perforation 45, thereby causing part of the metal hard mask layer 20 to be consumed, which easily causes large-area collapse (peeling) of the metal hard mask layer 20, and further causes the layout of the interconnect opening to fail to meet the process design.
[0028] In particular, when the material of the pattern transfer material layer 40 is amorphous silicon, the etching solution correspondingly includes ammonia water (NH 4 OH), and the ammonia water easily reacts with the metal hard mask layer 20 , thereby consuming the metal hard mask layer 20 .
[0029] In order to solve the technical problem, an embodiment of the present invention provides a method for forming a semiconductor structure, comprising: providing a substrate, on which a pattern transfer material layer is formed; forming a protective layer covering the pattern transfer material layer; forming a mask stack covering the protective layer, the mask stack comprising an anti-reflective coating and a photoresist layer stacked in sequence from bottom to top; patterning the photoresist layer to form a pattern opening penetrating the photoresist layer; detecting the pattern opening to determine whether the pattern opening meets a pattern detection benchmark; when the detection result does not meet the pattern detection benchmark, performing a rework operation until the detection result meets the pattern detection benchmark, the rework operation comprising: removing the mask stack and the protective layer in sequence; when the detection result meets the pattern detection benchmark, using the photoresist layer as a mask, etching the anti-reflective coating and the protective layer along the pattern opening to expose the pattern transfer material layer.
[0030] In the formation method provided by the embodiment of the present invention, before forming the mask stack, a protective layer covering the graphic transfer material layer is formed. When the product needs to be reworked (i.e., when the mask stack needs to be removed), due to the existence of the protective layer, the protective layer can protect the graphic transfer material layer and isolate the graphic transfer material layer from the process environment when the mask stack is removed. In the process of removing the mask stack, the probability of the graphic transfer material layer being damaged is low. Therefore, after the mask stack is removed through the rework operation, the graphic transfer material layer is helped to be preserved intact, thereby helping to improve the reliability of subsequent graphic transfer.
[0031] In order to make the above-mentioned purposes, features and advantages of the embodiments of the present invention more obvious and understandable, specific embodiments of the present invention are described in detail below with reference to the accompanying drawings.
[0032] Combined with reference Figures 6 to 16 , Figure 6 is a flow chart of an embodiment of a method for forming a semiconductor structure of the present invention, Figures 7 to 16 It is a schematic structural diagram corresponding to each step in an embodiment of a method for forming a semiconductor structure of the present invention.
[0033] Combined with reference Figure 6 and Figure 7 , perform step S1, provide a substrate 100, and a pattern transfer material layer 230 is formed on the substrate 100.
[0034] The substrate 100 provides a process operation basis for subsequent processes.
[0035] According to actual process conditions, the base 100 includes a substrate and a functional structure formed on the substrate. For example, the functional structure may include semiconductor devices such as MOS field effect transistors, resistor structures, etc.
[0036] In this embodiment, the base 100 includes a substrate (not shown) and an interlayer dielectric layer 110 located on the substrate.
[0037] The interlayer dielectric layer 110 is used to form an interconnect opening. As an example, the interconnect opening is used to form a source-drain plug (CT) connected to the source-drain doped region. In other embodiments, the interconnect opening can also be used to form a metal interconnect structure in a back-end process, and the metal interconnect structure includes a metal interconnect line or a through-hole interconnect structure.
[0038] The material of the interlayer dielectric layer 110 is an insulating material. In this embodiment, the material of the interlayer dielectric layer 110 is silicon oxide. In other embodiments, the material of the interlayer dielectric layer may also be a dielectric material such as silicon nitride or silicon oxynitride. In other embodiments, the material of the interlayer dielectric layer may also be an ultra-low-k dielectric material (an ultra-low-k dielectric material refers to a dielectric material with a relative dielectric constant less than 2.6).
[0039] In this embodiment, a metal hard mask layer 200 is further formed on the substrate 100 , and the pattern transfer material layer 230 is located on the metal hard mask layer 200 .
[0040] The patterned metal hard mask layer 200 is used as a mask for etching the substrate 100 , that is, after a mask opening is subsequently formed in the metal hard mask layer 200 , the substrate 100 exposed by the mask opening is etched.
[0041] The substrate 100 and the metal hard mask layer 200 have a high selectivity. The metal hard mask layer 200 is selected to improve the yield of pattern transfer, for example, the target pattern formed in the substrate 100 has a higher morphology quality and a smoother side wall.
[0042] In this embodiment, the material of the metal hard mask layer 200 is TiN. In other embodiments, the material of the metal hard mask layer may also be Ti, Ta or TaN.
[0043] After the pattern transfer material layer 230 is patterned, a shielding layer is formed, and the shielding layer is used as a mask for patterning the metal hard mask layer 200. The patterned pattern transfer material layer 230 is used to transfer the pattern to the metal hard mask layer 200, and then the patterned metal hard mask layer 200 is used to transfer the pattern to the substrate 100, which is beneficial to improve the dimensional accuracy of the target pattern formed in the substrate 100.
[0044] Therefore, there is a high etching selectivity ratio between the metal hard mask layer 200 and the pattern transfer material layer 230. In this embodiment, the metal hard mask layer 200 and the pattern transfer material layer 230 are made of different materials.
[0045] In this embodiment, the material of the pattern transfer material layer 230 is amorphous silicon. By selecting amorphous silicon, the pattern transfer material layer 230 can be doped later to improve the etching resistance of part of the pattern transfer material layer 230, and the doped pattern transfer material layer 230 is used as a shielding layer. This facilitates the subsequent removal of the remaining pattern transfer material layer 230 by maskless etching, retaining the shielding layer, thereby improving the process window for forming the shielding layer.
[0046] It should be noted that a buffer layer 210 is formed between the metal hard mask layer 200 and the pattern transfer material layer 230. The buffer layer 210 has good adhesion to the metal hard mask layer 200, and the buffer layer 210 also has good adhesion to the pattern transfer material layer 230.
[0047] In this embodiment, the material of the buffer layer 210 is silicon oxide. Specifically, the buffer layer 210 is a plasma enhanced oxide layer (plasma enhanced oxide), and the buffer layer 210 is formed by plasma enhanced CVD (PECVD) process.
[0048] Continue to refer Figure 6 , and combined with reference Figure 8 , perform step S2 to form a protective layer 300 covering the graphic transfer material layer 230; perform step S3 to form a mask stack 400 covering the protective layer 300, the mask stack 400 comprising an anti-reflective coating 420 and a photoresist layer 430 stacked in sequence from bottom to top.
[0049] After the pattern opening penetrating the photoresist layer 430 is subsequently formed, the pattern opening is inspected to determine whether the pattern opening meets the pattern inspection benchmark, and when the inspection result does not meet the pattern inspection benchmark, a rework operation is performed to remove the mask stack 400. When the product needs to be reworked, due to the existence of the protective layer 300, the protective layer 300 can protect the pattern transfer material layer 230, and isolate the pattern transfer material layer 230 from the process environment when removing the mask stack 400. In the process of removing the mask stack 400, the probability of damage to the pattern transfer material layer 230 is low, which can correspondingly reduce the probability of damage to the metal hard mask layer 200. Therefore, after removing the mask stack 400 through the rework operation, it is beneficial to keep the pattern transfer material layer 230 and the metal hard mask layer 200 intact, so that the pattern can be accurately transferred to the pattern transfer material layer 230 and the metal hard mask layer 200 using the pattern opening, which is beneficial to improve the reliability of subsequent pattern transfer.
[0050] Therefore, when removing the mask stack 400 , the process of removing the mask stack 400 causes less loss to the protection layer 300 .
[0051] In this embodiment, the material of the protective layer 300 is an inorganic material. The material of the mask stack 400 is an organic material. When removing the mask stack 400, the etching rate of the protective layer 300 is very small or negligible, thereby reducing the loss of the protective layer 300 in the process of removing the mask stack 400.
[0052] Furthermore, the protective layer 300 is located at the bottom of the mask stack 400 . Therefore, when the photoresist layer 430 is exposed, the protective layer 300 has little effect on the exposure light, thereby having little effect on the patterning effect of the mask stack 400 .
[0053] In addition, the protective layer 300 will be etched or removed later, so there is a high etching selectivity between the protective layer 300 and the pattern transfer material layer 230, thereby reducing the damage to the pattern transfer material layer 230 caused by the process of etching the protective layer 300 or removing the protective layer 300. Specifically, the etching selectivity between the protective layer 300 and the pattern transfer material layer 230 is greater than 30.
[0054] In this embodiment, the material of the protection layer 300 is silicon oxide. The side effects of the silicon oxide removal process are small, and the etching selectivity of silicon oxide and silicon is relatively high. When the protection layer 300 is subsequently removed, the pattern transfer material layer 230 is less damaged.
[0055] In this embodiment, the protective layer 300 is formed by a plasma enhanced chemical vapor deposition process, which is beneficial to improving the formation rate of the protective layer 300 .
[0056] In this embodiment, the thickness of the protective layer 300 is greater than or equal to the thickness of the mask stack 400. By making the thickness of the protective layer 300 greater than or equal to the thickness of the mask stack 400, when the product needs to be reworked, the thickness of the protective layer 300 is sufficient to protect the pattern transfer material layer 230, and even if the ratio of the removal rate of the mask stack 400 to the removal rate of the protective layer 300 is 1, the probability of the process of removing the mask stack 400 continuing to remove the exposed pattern transfer material layer 230 is low, thereby increasing the process window of the process of removing the mask stack 400, and effectively reducing the probability of the pattern transfer material layer 230 being damaged during the process of removing the mask stack 400.
[0057] It should be noted that the difference between the thickness of the protective layer 300 and the thickness of the mask stack 400 should not be too large. If the difference is too large, it will not only lead to waste of production capacity, but also the subsequent removal of the protective layer 300 will take a long time, and the probability of damage to the pattern transfer material layer 230 will increase accordingly. Therefore, in this embodiment, the difference between the thickness of the protective layer 300 and the thickness of the mask stack 400 is 0 to 1000.
[0058] The patterned mask stack 400 is used to define the size, shape and position of a target pattern subsequently formed in the substrate 100 .
[0059] In this embodiment, the mask stack 400 includes an anti-reflective coating 420 and a photoresist layer 430 stacked in sequence from bottom to top.
[0060] During the photolithography process of the photoresist layer 430 , the anti-reflective coating 420 is used to reduce the reflection effect during exposure, thereby improving the transfer accuracy of the pattern.
[0061] Specifically, the anti-reflective coating 420 is a silicon-containing anti-reflective coating (Si-ARC). The Si-ARC layer is beneficial for increasing the exposure depth of field (DOF) during the photolithography process and improving the exposure uniformity. Moreover, the Si-ARC layer is rich in silicon, so it is also beneficial for improving the hardness of the anti-reflective coating 420, thereby further improving the transfer accuracy of the pattern, making the pattern in the photoresist layer 430 less likely to be deformed or defective.
[0062] It should be noted that the anti-reflective coating 420 and the photoresist layer 430 are both formed by a coating process, and are affected by the materials of the anti-reflective coating 420 and the photoresist layer 430 themselves. During the coating process, bubble defects 440 are easily formed in one or two layers of the anti-reflective coating 420 and the photoresist layer 430.
[0063] like Figure 8 As shown, as an example, it is shown that the bubble defect 440 is located in the anti-reflective coating 420 and the photoresist layer 430.
[0064] In this embodiment, the mask stack 400 further includes a cover layer 410 located between the anti-reflection coating 420 and the protection layer 300 .
[0065] The cover layer 410 provides a flat process platform for the formation and patterning of the anti-reflective coating 420 and the photoresist layer 430 , and is also helpful in avoiding damage to the underlying film layers when patterning the photoresist layer 430 and the anti-reflective coating 420 and improving the exposure effect of the photoresist layer 430 .
[0066] In this embodiment, the material of the cover layer 410 is a spin on carbon (SOC) material. In other embodiments, the material of the cover layer may also be an organic dielectric layer (ODL) material.
[0067] Continue to refer Figure 6 , and combined with reference Fig. 9 , perform step S4, pattern the photoresist layer 430, and form a pattern opening 431 (such as Fig.10 shown).
[0068] The pattern opening 431 is used to define a region that is subsequently exposed in the pattern transfer material layer 230 .
[0069] Specifically, the photoresist layer 430 is subjected to exposure and development processes to pattern the photoresist layer 430 .
[0070] As an example, a pattern opening 431 is formed in the photoresist layer 430 at a position corresponding to the bubble defect 440. In other embodiments, the position of the pattern opening may also be separated from the position of the bubble defect.
[0071] Continue to refer Figure 6 , execute step S5 to detect the graphic opening 431 and determine whether the graphic opening 431 meets the graphic detection standard.
[0072] By judging whether the graphic opening 431 meets the graphic detection benchmark, it is determined whether the shape, size or position of the graphic opening 431 meets the product requirements.
[0073] In this embodiment, in the step of detecting the graphic opening 431, the detection includes line width (critical dimension, CD) detection or alignment (overlay) deviation detection. For example, when the actual line width of the graphic opening 431 exceeds the preset line width range, it is determined that the graphic opening 431 does not meet the graphic detection benchmark; or when the actual alignment deviation of the graphic opening 431 exceeds the preset alignment deviation range, it is determined that the graphic opening 431 does not meet the graphic detection benchmark.
[0074] In other embodiments, the detection may also include defect detection, for example, particle defect detection on the surface of the photoresist layer, or morphology defect detection of the pattern opening.
[0075] Continue to refer Figure 6 When the inspection result does not meet the graphic inspection benchmark, step S7 is executed to perform a rework operation until the inspection result meets the graphic inspection benchmark, and the rework operation includes: removing the mask stack 400 and the protection layer 300 in sequence.
[0076] In the process of removing the mask stack 400, the protective layer 300 can protect the pattern transfer material layer 230. Even if a bubble defect 440 is formed in the mask stack 400, the probability of damage to the pattern transfer material layer 230 below the bubble defect 440 is low, which can correspondingly reduce the probability of damage to the metal hard mask layer 200. Therefore, after removing the mask stack 400 through the rework operation, it is beneficial to keep the pattern transfer material layer 230 and the metal hard mask layer 200 intact, thereby facilitating the improvement of the reliability of subsequent pattern transfer.
[0077] Moreover, the rework operation will also remove the protective layer 300. Even if the protective layer 300 is damaged during the process of forming the graphic opening 431, the protective layer 300 will be re-formed after the protective layer 300 is removed. Therefore, the subsequent process is less affected.
[0078] In addition, the protective layer 300 and the pattern transfer material layer 230 have a high etching selectivity ratio, so when the protective layer 300 is removed, the loss of the pattern transfer material layer 230 is small.
[0079] In this embodiment, the mask stack 400 includes a covering layer 410, an anti-reflective coating 420 located on the covering layer 410, and a photoresist layer 430 located on the anti-reflective coating 420, wherein the covering layer 410 is a spin-on carbon layer, and the anti-reflective coating 420 is a silicon-containing anti-reflective coating. Therefore, the reaction gas used to remove the mask stack 400 includes O2, CHF3, CF4, N2 and H2.
[0080] Specifically, O2 is used to remove the photoresist layer 430, a mixed gas of CHF3 and CF4 is used to remove the anti-reflective coating 420, and a mixed gas of N2 and H2 is used to remove the capping layer 410.
[0081] It should be noted that the process of removing the mask stack 400 is carried out by controlling a preset time (by time). If the graphic transfer material layer 230 is exposed to the reaction gas environment of removing the mask stack 400, the reaction gas is likely to affect the graphic transfer material layer 230, and the probability of the graphic transfer material layer 230 being mistakenly etched is relatively high. Therefore, by forming a protective layer 300 located between the graphic transfer material layer 230 and the mask stack 400, the graphic transfer material layer 230 is isolated from the process environment when removing the mask stack 400.
[0082] In this embodiment, a wet etching process is used to remove the protective layer 300. Specifically, the material of the protective layer 300 is silicon oxide, and the etching solution used in the wet etching process is a diluted hydrofluoric acid solution.
[0083] The wet etching process can also play a cleaning role, thereby reducing or removing the residue of the mask stack 400 .
[0084] In this embodiment, after removing the mask stack 400 and the protective layer 300 in sequence, the processes of forming a protective layer, forming a mask stack, patterning a photoresist layer, and detecting the pattern opening are performed again in sequence until the detection result meets the pattern detection benchmark.
[0085] Continue to refer Figure 6 , and combined with reference Fig.10 and Fig.11 When the detection result meets the pattern detection benchmark, step S6 is executed to etch the anti-reflective coating 420 and the protective layer 300 along the pattern opening 431 using the remaining photoresist layer 430 as a mask to expose the pattern transfer material layer 230 .
[0086] By exposing a portion of the pattern transfer material layer 230 , preparation is made for subsequent patterning of the pattern transfer material layer 230 .
[0087] Specifically, Fig.10 As shown, after the photoresist layer 430 is patterned, the anti-reflective coating 420 and the cover layer 410 are sequentially etched using the remaining photoresist layer 430 as a mask; Fig.11 As shown, after etching the cover layer 410 , the exposed protection layer 300 is further etched.
[0088] It should be noted that, when etching the bubble defect 440 (such as Figure 8 When the anti-reflective coating 420 and the covering layer 410 at the position corresponding to the bubble defect 440 are etched, the total etching amount of the remaining mask stack 400 (i.e., the anti-reflective coating 420 and the covering layer 410) at this position is less than the total etching amount of the remaining mask stack 400 at other positions. Therefore, the protective layer 300 under the graphic opening 431 corresponding to the bubble defect 440 is exposed first.
[0089] As an example, Fig.10 As shown, the protective layer 300 below the pattern opening 431 corresponding to the bubble defect 440 is easily etched and lost. The protective layer 300 protects the pattern transfer material layer 230, and the probability of the pattern transfer material layer 230 being lost is small.
[0090] In this embodiment, a dry etching process (e.g., an anisotropic dry etching process) is used to sequentially etch the anti-reflective coating 420, the cover layer 410, and the protective layer 300 along the pattern opening 431. The dry etching process has the characteristic of anisotropic etching, which is beneficial to improving the morphology quality of the cross-section obtained after etching. Moreover, by changing the etching gas, the anti-reflective coating 420, the cover layer 410, and the protective layer 300 can be sequentially etched in the same etching equipment.
[0091] It should be noted that, in this embodiment, the exposed portion of the pattern transfer material layer 230 is subsequently retained. In other embodiments, the exposed portion of the pattern transfer material layer is subsequently removed.
[0092] refer to Fig.12 After etching the protective layer 300 along the pattern opening 431 to expose the pattern transfer material layer 230, the forming method further includes: removing the remaining mask stack 400 (such as Fig. 9 shown).
[0093] The subsequent process also includes doping the exposed graphic transfer material layer 230. Compared with the groove surrounded by the remaining mask stack 400, the protective layer 300 and the graphic transfer material layer 230, the aspect ratio of the groove surrounded by the protective layer 300 and the graphic transfer material layer 230 is smaller. Therefore, by removing the mask stack 400 first, it is helpful to reduce the process difficulty of the subsequent doping treatment.
[0094] refer to Fig.13 The exposed pattern transfer material layer 230 is subjected to a doping treatment 231, and the pattern transfer material layer 230 after the doping treatment 231 serves as a shielding layer 230d. The doping treatment 231 is suitable for improving the etching resistance of the shielding layer 230d.
[0095] Compared with the pattern transfer material layer 230 that has not been doped 231, the shielding layer 230d has a higher etching resistance, that is, there is a larger etching selectivity ratio between the pattern transfer material layer 230 and the shielding layer 230d, thereby significantly improving the process window for subsequent patterning of the pattern transfer material layer 230. For example, the remaining pattern transfer material layer 230 can be removed by maskless etching.
[0096] In the process of the doping treatment 231 , the protective layer 300 acts as a mask, thereby defining the area to be doped in the pattern transfer material layer 230 .
[0097] In this embodiment, the graphic transfer material layer 230 that has undergone the doping treatment 231 is used as a shielding layer 230d. Through the doping treatment 231, impurity ions are doped into a partial area of the graphic transfer material layer 230, so that the microstructures of the shielding layer 230d and the graphic transfer material layer 230 are different.
[0098] Specifically, the impurity ions doped by the doping treatment 231 reduce the grain boundary gap of silicon in the material of the shielding layer 230d, thereby improving the thermal stability and chemical stability of the shielding layer 230d. The improvement in stability is correspondingly beneficial to improving the corrosion resistance of the shielding layer 230d, thereby improving the etching resistance of the graphic transfer material layer 230.
[0099] In this embodiment, the material of the pattern transfer material layer 230 is amorphous silicon, and therefore, the doping ions of the doping treatment 231 are B ions. By doping B ions into part of the amorphous silicon, the material of the shielding layer 230d is changed to boron-doped silicon, thereby significantly improving the etching selectivity between the shielding layer 230d and the pattern transfer material layer 230. Moreover, the stability of B atoms is relatively high, which is beneficial to improving the thermal stability and chemical stability of the shielding layer 230d. In addition, B ions are commonly used doping ions in the semiconductor field and have high process compatibility.
[0100] In this embodiment, an ion implantation process is used to perform the doping treatment 231. The ion implantation process is relatively simple, and by adjusting the implantation dose, it is easy to adjust the etching selectivity ratio between the shielding layer 230d and the pattern transfer material layer 230.
[0101] refer to Fig.14 , remove the remaining protective layer 300 (such as Fig.13 shown).
[0102] The remaining protection layer 300 is removed to expose the pattern transfer material layer 230 that has not been doped 231 , thereby preparing for the subsequent removal of the remaining pattern transfer material layer 230 .
[0103] In this embodiment, a wet etching process is used to remove the remaining protection layer 300. Specifically, the material of the protection layer 300 is silicon oxide, and the etching solution used in the wet etching process is a diluted hydrofluoric acid (DHF) solution.
[0104] In this embodiment, the etching selectivity between the protective layer 300 and the graphic transfer material layer 230 is relatively high, the etching resistance of the shielding layer 230d is greater than that of the graphic transfer material layer 230, and the etching selectivity between the protective layer 300 and the shielding layer 230d is also relatively high. Therefore, the process of removing the protective layer 300 has little effect on the graphic transfer material layer 230 and the shielding layer 230d.
[0105] It should be noted that, in this embodiment, after removing the mask stack 400, the exposed pattern transfer material layer 230 is subjected to a doping treatment 231. In other embodiments, the exposed pattern transfer material layer may be subjected to a doping treatment and then the mask stack is removed; and after removing the mask stack, the protective layer is removed.
[0106] refer to Fig.15 After removing the protective layer 300 , the remaining pattern transfer material layer 230 is removed.
[0107] The remaining pattern transfer material layer 230 is removed, and the shielding layer 230 d is retained. The shielding layer 230 d is used as a mask for subsequent patterning of the metal hard mask layer 200 .
[0108] In this embodiment, a wet etching process is used to remove the remaining pattern transfer material layer 230. The wet etching process removes the remaining pattern transfer material layer 230 by chemical reaction, which is beneficial to reduce the probability of other film layers under the pattern transfer material layer 230 being damaged.
[0109] Specifically, the material of the pattern transfer material layer 230 is amorphous silicon, and the etching solution used in the wet etching process includes ammonia water (NH4OH).
[0110] refer to Fig.16 , remove the remaining pattern transfer material layer 230 (such as Fig.12 As shown in the figure), the metal hard mask layer 200 is etched with the blocking layer 230d as a mask to form a mask opening 201 in the metal hard mask layer 200.
[0111] The metal hard mask layer 200 having the mask opening 201 is used as a mask for etching the substrate 100 . The mask opening 201 is used to define the shape, size and position of the target pattern in the substrate 100 .
[0112] In this embodiment, the metal hard mask layer 200 having the mask opening 201 is used as a mask for etching the interlayer dielectric layer 110 , thereby forming an interconnect opening in the interlayer dielectric layer 110 , and the interconnect opening is used as a target pattern.
[0113] Specifically, the buffer layer 210 and the metal hard mask layer 200 are etched in sequence using the blocking layer 230d as a mask.
[0114] It should be noted that the shielding layer 230d is also susceptible to loss during the etching of the metal hard mask layer 200. As an example, after the mask opening 201 is formed in the metal hard mask layer 200, a portion of the thickness of the shielding layer 230d is retained. In other embodiments, after the mask opening is formed in the metal hard mask layer, the shielding layer is completely removed.
[0115] It should also be noted that the pattern opening 431 (eg Figure 8 After that, when the product needs to be reworked (ie, the mask stack 400 needs to be removed), the protective layer 300 can be applied to the pattern transfer material layer 230 (as shown in FIG. Fig.12 The protective layer 300 is formed between the mask stack 400 and the pattern transfer material layer 230 to protect the pattern transfer material layer 230. In the process of removing the mask stack 400, the probability of forming a pinhole in the pattern transfer material layer 230 is low. Accordingly, after the blocking layer 230d is formed, when removing the remaining pattern transfer material layer 230, the probability of the etching solution contacting and reacting with the metal hard mask layer 200 is low, which can reduce the probability of the metal hard mask layer 200 being consumed. Therefore, in this embodiment, by forming the protective layer 300 between the mask stack 400 and the pattern transfer material layer 230, both the pattern transfer material layer 230 and the metal hard mask layer 200 can be preserved intact, so as to accurately transfer the pattern to the metal hard mask layer 200 through the pattern opening 431, thereby improving the reliability of the pattern transfer. For example, the pattern accuracy of the interconnection opening in the interlayer dielectric layer 110 is improved.
[0116] Subsequent processes will also form an interconnect structure (eg, a contact plug or a metal interconnect structure) in the interconnect opening. The pattern accuracy of the interconnect opening in the interlayer dielectric layer 110 is relatively high, which in turn ensures the performance of the interconnect structure, thereby improving the performance of the semiconductor structure.
[0117] Accordingly, an embodiment of the present invention further provides a semiconductor structure. Figure 8 , showing a schematic structural diagram of an embodiment of a semiconductor structure of the present invention.
[0118] The semiconductor structure includes: a substrate 100, on which a pattern transfer material layer 230 is formed; a protective layer 300, covering the pattern transfer material layer 230; a mask stack 400, covering the protective layer 300, and the mask stack 400 includes an anti-reflective coating 420 and a photoresist layer 430 stacked in sequence from bottom to top.
[0119] In the process of forming the semiconductor structure, the photoresist layer 430 will be patterned to form a pattern opening that penetrates the photoresist layer 430, and the pattern opening will be inspected to determine whether the pattern opening meets the pattern inspection benchmark. When the inspection result does not meet the pattern inspection benchmark, a rework operation is required to remove the mask stack 400. When the product needs to be reworked, due to the existence of the protective layer 300, the protective layer 300 can protect the pattern transfer material layer 230 and isolate the pattern transfer material layer 230 from the process environment when removing the mask stack 400. In the process of removing the mask stack 400, the probability of the pattern transfer material layer 230 being damaged is low. Therefore, after removing the mask stack 400 through the rework operation, it is beneficial to keep the pattern transfer material layer 230 intact, so that the pattern can be accurately transferred to the pattern transfer material layer 230 through the pattern opening, which is beneficial to improve the reliability of subsequent pattern transfer.
[0120] The substrate 100 provides a process operation basis for subsequent processes.
[0121] According to actual process conditions, the base 100 includes a substrate and a functional structure formed on the substrate. For example, the functional structure may include semiconductor devices such as MOS field effect transistors, resistor structures, etc.
[0122] In this embodiment, the base 100 includes a substrate (not shown) and an interlayer dielectric layer 110 located on the substrate.
[0123] The interlayer dielectric layer 110 is used to form an interconnect opening. As an example, the interconnect opening is used to form a source-drain plug (CT) connected to the source-drain doped region. In other embodiments, the interconnect opening can also be used to form a metal interconnect structure in a back-end process, and the metal interconnect structure includes a metal interconnect line or a through-hole interconnect structure.
[0124] The material of the interlayer dielectric layer 110 is an insulating material. In this embodiment, the material of the interlayer dielectric layer 110 is silicon oxide. In other embodiments, the material of the interlayer dielectric layer may also be a dielectric material such as silicon nitride or silicon oxynitride. In other embodiments, the material of the interlayer dielectric layer may also be an ultra-low-k dielectric material (an ultra-low-k dielectric material refers to a dielectric material with a relative dielectric constant less than 2.6).
[0125] In this embodiment, a metal hard mask layer 200 is further formed on the substrate 100 , and the pattern transfer material layer 230 is located on the metal hard mask layer 200 .
[0126] The patterned metal hard mask layer 200 is used as a mask for etching the substrate 100, that is, after a mask opening is formed in the metal hard mask layer 200, the substrate 100 exposed by the mask opening is etched. There is a high selectivity between the substrate 100 and the metal hard mask layer 200. By selecting the metal hard mask layer 200, it is beneficial to improve the yield of pattern transfer, for example, the target pattern formed in the substrate 100 has a higher pattern morphology quality and a smoother side wall of the target pattern.
[0127] In this embodiment, the material of the metal hard mask layer 200 is TiN. In other embodiments, the material of the metal hard mask layer may also be Ti, Ta or TaN.
[0128] The patterned pattern transfer material layer 230 is used as a mask for the patterned metal hard mask layer 200. The patterned pattern transfer material layer 230 is used to transfer the pattern to the metal hard mask layer 200, and then the patterned metal hard mask layer 200 is used to transfer the pattern to the substrate 100, which is beneficial to improve the dimensional accuracy of the target pattern formed in the substrate 100.
[0129] Therefore, there is a high etching selectivity ratio between the metal hard mask layer 200 and the pattern transfer material layer 230. In this embodiment, the metal hard mask layer 200 and the pattern transfer material layer 230 are made of different materials.
[0130] In this embodiment, the material of the pattern transfer material layer 230 is amorphous silicon. By selecting amorphous silicon, the pattern transfer material layer 230 can be doped later to improve the etching resistance of the pattern transfer material layer 230 in some areas, and the doped pattern transfer material layer 230 is used as a shielding layer. This facilitates the subsequent removal of the remaining pattern transfer material layer 230 by maskless etching, retaining the shielding layer, thereby increasing the process window of the patterned pattern transfer material layer 230.
[0131] It should be noted that a buffer layer 210 is formed between the metal hard mask layer 200 and the pattern transfer material layer 230. The buffer layer 210 has good adhesion to the metal hard mask layer 200, and the buffer layer 210 also has good adhesion to the pattern transfer material layer 230.
[0132] In this embodiment, the material of the buffer layer 210 is silicon oxide. Specifically, the buffer layer 210 is a plasma enhanced oxide layer.
[0133] In this embodiment, the material of the protective layer 300 is an inorganic material. The material of the mask stack 400 is an organic material. When removing the mask stack 400, the etching rate of the protective layer 300 is very small or negligible, thereby reducing the loss of the protective layer 300 in the process of removing the mask stack 400.
[0134] Furthermore, the protective layer 300 is located at the bottom of the mask stack 400 . Therefore, when the photoresist layer 430 is exposed, the protective layer 300 has little effect on the exposure light, thereby having little effect on the patterning effect of the mask stack 400 .
[0135] Specifically, the material of the protection layer 300 is silicon oxide. The side effects of the silicon oxide removal process are small, and the etching selectivity of silicon oxide and silicon is relatively high. When the protection layer 300 is subsequently removed, the pattern transfer material layer 230 is less damaged.
[0136] In this embodiment, the thickness of the protective layer 300 is greater than or equal to the total thickness of the mask stack 400. By making the thickness of the protective layer 300 greater than or equal to the thickness of the mask stack 400, when the product needs to be reworked, the thickness of the protective layer 300 is sufficient to protect the pattern transfer material layer 230, and even if the ratio of the removal rate of the mask stack 400 to the removal rate of the protective layer 300 is 1, the probability of the process of removing the mask stack 400 continuing to remove the exposed pattern transfer material layer 230 is low, thereby increasing the process window of the process of removing the mask stack 400, and effectively reducing the probability of the pattern transfer material layer 230 being damaged during the process of removing the mask stack 400.
[0137] It should be noted that the difference between the thickness of the protective layer 300 and the thickness of the mask stack 400 should not be too large. If the difference is too large, it will not only lead to waste of production capacity, but also the subsequent removal of the protective layer 300 will take a long time, and the probability of damage to the pattern transfer material layer 230 will increase accordingly. Therefore, in this embodiment, the difference between the thickness of the protective layer 300 and the thickness of the mask stack 400 is 0 to 1000.
[0138] The patterned mask stack 400 is used to define the size, shape and position of the target pattern subsequently formed in the substrate 100. In this embodiment, the mask stack 400 includes an anti-reflective coating 420 and a photoresist layer 430 stacked in sequence from bottom to top.
[0139] During the photolithography process of the photoresist layer 430 , the anti-reflective coating 420 is used to reduce the reflection effect during exposure, thereby improving the transfer accuracy of the pattern.
[0140] Specifically, the anti-reflective coating 420 is a silicon-containing anti-reflective coating. The Si-ARC layer is beneficial to increasing the exposure depth of field during the photolithography process and improving the exposure uniformity. Moreover, the Si-ARC layer is rich in silicon, so it is also beneficial to improve the hardness of the anti-reflective coating 420, thereby further improving the transfer accuracy of the pattern, making the pattern in the photoresist layer 430 less likely to be deformed or defective.
[0141] It should be noted that the anti-reflective coating 420 and the photoresist layer 430 are both formed by a coating process and are affected by the materials of the anti-reflective coating 420 and the photoresist layer 430. Therefore, during the coating process, bubble defects 440 are easily formed in one or both of the anti-reflective coating 420 and the photoresist layer 430. Figure 8 As shown, as an example, it is shown that the bubble defect 440 is located in the anti-reflective coating 420 and the photoresist layer 430.
[0142] In this embodiment, the mask stack 400 further includes a cover layer 410 located between the anti-reflection coating 420 and the protection layer 300 .
[0143] The cover layer 410 provides a flat process platform for the formation and patterning of the anti-reflective coating 420 and the photoresist layer 430 , and is also helpful in avoiding damage to the underlying film layers when patterning the photoresist layer 430 and the anti-reflective coating 420 and improving the exposure effect of the photoresist layer 430 .
[0144] In this embodiment, the material of the cover layer 410 is a spin-on carbon layer material. In other embodiments, the material of the cover layer may also be an organic dielectric layer material.
[0145] It should be noted that after the graphic opening penetrating the photoresist layer 430 is subsequently formed, when the product needs to be reworked, the mask stack 400 needs to be removed, and the process of removing the mask stack 400 is carried out by controlling a preset time (bytime). In the process of removing the mask stack 400, the film layer below the bubble defect 440 is exposed first.
[0146] Therefore, by forming the protective layer 300 between the mask stack 400 and the pattern transfer material layer 230, the protective layer 300 can protect the pattern transfer material layer 230. In the process of removing the mask stack 400, the pattern transfer material layer 230 is not easily damaged, and the probability of forming a pin hole in the pattern transfer material layer 230 is low. Accordingly, in each process before patterning the metal hard mask layer 200, the probability of the metal hard mask layer 200 being consumed is low. Therefore, in this embodiment, the pattern transfer material layer 230 and the metal hard mask layer 200 can be preserved intact, which is conducive to accurately transferring the pattern to the metal hard mask layer 200 through the pattern opening, thereby helping to improve the reliability of the pattern transfer. For example, the pattern accuracy of the interconnection opening in the interlayer dielectric layer 110 is improved.
[0147] As an example, subsequent processes will also form an interconnect structure (for example, a contact plug or a metal interconnect structure) in the interconnect opening. The pattern accuracy of the interconnect opening in the interlayer dielectric layer 110 is relatively high, which in turn ensures the performance of the interconnect structure, thereby improving the performance of the semiconductor structure.
[0148] The semiconductor structure can be formed by the formation method described in the above embodiment, or by other formation methods. For the specific description of the semiconductor structure described in this embodiment, reference can be made to the corresponding description in the above embodiment, and this embodiment will not be repeated here.
[0149] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.
Claims
1. A method for forming a semiconductor structure, characterized in that: include: Providing a substrate, on which a pattern transfer material layer is formed; forming a protective layer covering the pattern transfer material layer; forming a mask stack covering the protective layer, wherein the mask stack comprises an anti-reflective coating layer and a photoresist layer stacked sequentially from bottom to top; Patterning the photoresist layer to form a pattern opening penetrating the photoresist layer; Detecting the graphic opening to determine whether the graphic opening meets a graphic detection benchmark; When the inspection result does not meet the graphic inspection benchmark, performing a rework operation until the inspection result meets the graphic inspection benchmark, the rework operation comprising: removing the mask stack and the protective layer in sequence; When the detection result meets the pattern detection benchmark, the anti-reflective coating and the protective layer are etched along the pattern opening using the remaining photoresist layer as a mask to expose the pattern transfer material layer; The protective layer is configured to isolate the pattern transfer material layer from a process environment when the mask stack is removed, and an etching selectivity ratio between the protective layer and the pattern transfer material layer is greater than 30.
2. The method for forming a semiconductor structure according to claim 1, wherein: In the step of detecting the pattern opening, the detection includes line width detection or alignment deviation detection.
3. The method for forming a semiconductor structure according to claim 1, wherein: In the step of forming a protective layer on the pattern transfer material layer, the material of the protective layer is an inorganic material.
4. The method for forming a semiconductor structure according to claim 3, wherein: The material of the protection layer includes silicon oxide.
5. The method for forming a semiconductor structure according to claim 1, wherein: In the step of forming a protective layer on the pattern transfer material layer, the thickness of the protective layer is greater than or equal to the thickness of the mask stack.
6. The method for forming a semiconductor structure according to claim 5, wherein: The difference between the thickness of the protective layer and the thickness of the mask stack is 0 to 7. The method for forming a semiconductor structure according to claim 1, wherein: The material of the pattern transfer material layer includes amorphous silicon.
8. The method for forming a semiconductor structure according to claim 1, wherein: A metal hard mask layer is also formed on the substrate; the pattern transfer material layer is located on the metal hard mask layer; After etching the protective layer along the pattern opening to expose the pattern transfer material layer, the forming method further comprises: removing the mask stack; After removing the mask stack, removing the protective layer; Performing a doping treatment on the exposed pattern transfer material layer, wherein the pattern transfer material layer after the doping treatment serves as a shielding layer, and the doping treatment is suitable for improving the etching resistance of the shielding layer; After forming the shielding layer, removing the remaining pattern transfer material layer; After removing the remaining pattern transfer material layer, the metal hard mask layer is etched using the shielding layer as a mask to form a mask opening in the metal hard mask layer.
9. The method for forming a semiconductor structure according to claim 8, wherein: After removing the mask stack, the exposed pattern transfer material layer is doped; or, After the exposed pattern transfer material layer is doped, the mask stack is removed.
10. The method for forming a semiconductor structure according to claim 1, wherein: During the rework operation, the reaction gases used to remove the mask stack include O2, CHF3, CF4, N2 and H2.
11. The method for forming a semiconductor structure according to claim 1, wherein: During the rework operation, a wet etching process is used to remove the protective layer, and an etching solution used in the wet etching process includes a diluted hydrofluoric acid solution.
12. The method for forming a semiconductor structure according to claim 8, wherein: In the step of performing doping treatment on the exposed pattern transfer material layer, the doping ions include B ions.
13. The method for forming a semiconductor structure according to claim 8, wherein: The remaining pattern transfer material layer is removed by using a wet etching process, wherein the etching solution used in the wet etching process includes ammonia water.
14. A semiconductor structure, characterized in that: include: A substrate, a pattern transfer material layer is formed on the substrate, a metal hard mask layer is also formed on the substrate, and the pattern transfer material layer is located on the metal hard mask layer; A protective layer covering the graphic transfer material layer; A mask stack covering the protective layer, wherein the mask stack comprises an anti-reflective coating layer and a photoresist layer stacked in sequence from bottom to top; The protective layer is configured to isolate the pattern transfer material layer from a process environment when the mask stack is removed during a rework operation, and an etching selectivity ratio between the protective layer and the pattern transfer material layer is greater than 30.
15. The semiconductor structure according to claim 14, wherein: The material of the protective layer is an inorganic material.
16. The semiconductor structure according to claim 15, wherein: The material of the protection layer includes silicon oxide.
17. The semiconductor structure according to claim 14, wherein: The thickness of the protection layer is greater than or equal to the thickness of the mask stack.
18. The semiconductor structure according to claim 17, wherein: The difference between the thickness of the protective layer and the thickness of the mask stack is 0 to 19. The semiconductor structure according to claim 14, wherein: The material of the pattern transfer material layer includes amorphous silicon.