Thermal system management method for electric vehicle power battery, composite material and preparation method thereof
By using silicone rubber composite materials with automatic temperature adjustment in electric vehicle power batteries, the problem of coordination of thermal conductivity and thermal insulation functions is solved, the complex thermal system management of electric vehicle power batteries is realized, and the fire safety and energy density are improved.
Patent Information
- Application Number
- CN202010458917.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-05-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-05-27
AI Technical Summary
The prior art is difficult to coordinate the two functions of thermal conductivity and thermal insulation in electric vehicle power batteries, resulting in large space occupied by the system, low energy density, and insufficient fire safety performance.
A normal temperature thermal conductivity, high temperature heat insulation and fire-resistant silicone rubber composite material is used. This material consists of a silicone rubber matrix, thermal conductivity functional filler, foaming agent, porcelain functional filler and flame retardant. The thermal conductivity coefficient is automatically adjusted according to temperature changes, thereby achieving automatic realization of Heat dissipation, heat insulation and flame retardant fire resistance.
This material has high thermal conductivity at room temperature, automatically reduces the thermal conductivity coefficient at high temperature to achieve heat insulation, and turns into porous ceramic shape in high temperature or fire. It has fireproof and heat insulation function, improving the thermal system management capability of electric vehicle power batteries and fire safety.
Smart Images

Figure CN113745688B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of thermal system management methods and functional materials, and in particular to a thermal system management method for an electric vehicle power battery, a composite material and a preparation method thereof. Background Art
[0002] As new energy technologies continue to make breakthroughs, new energy vehicles have become a major change facing the automotive industry. Major safety accidents involving new energy vehicles have occurred one after another, making the fire safety of new energy vehicle power batteries the focus of industry attention. The causes of power batteries are complex and it is difficult to avoid them from the source at present. Lithium-ion batteries for power vehicles such as electric vehicles often require thousands of single cells to be used in groups. If some cells enter a thermal runaway state due to mechanical damage, thermal shock, internal short circuit, overcharging and other factors, the temperature of the surrounding cells will also rise, and then the thermal runaway will spread to the entire battery pack, eventually causing the catastrophic consequences of overall combustion and explosion.
[0003] There are currently two main means of dealing with thermal runaway in battery packs: one is the thermal management system, which includes a monitoring system and a heat dissipation system. Thermally conductive insulating thermal interface materials are a type of heat dissipation material commonly used in thermal management systems. The other is a thermal insulation and fire protection system, which is divided into active fire protection and passive fire protection. Foam, thermal insulation coatings, etc. are the most commonly used thermal insulation and fire protection materials. In order to solve the heat dissipation problem when the battery is working normally, the battery pack needs a high thermal conductivity interface material to dissipate the heat of the battery; on the other hand, in order to solve the fire safety problem, it is necessary to use thermal insulation materials to isolate each battery cell to delay the rapid spread of thermal runaway caused by thermal runaway of a single battery cell. The purposes and technical means of the two are exactly opposite, and are often difficult to achieve technically.
[0004] The existing methods for dealing with the fire safety problem of automotive power batteries, on the one hand, are only to improve the heat dissipation effect of the thermally conductive gasket material (a thermally conductive silicone pad for electric vehicle batteries CN209472079 U) or only involve foam and aerogel in the field of thermal insulation and fire prevention (a thermal insulation and fireproof material for new energy vehicle power batteries CN107914428A). On the other hand, the design of assembly components: thermal conductive blocks-barrier blocks-assembly buckles are designed in the gap between batteries (see an assembly component for heat dissipation of battery systems and prevention of thermal runaway propagation CN106532177A). This method still improves the safety problem of power batteries on two independent technical solutions of thermal conductivity and thermal insulation, but there are disadvantages such as contradictions between thermal conductivity and thermal insulation, large space occupied by the system, serious reduction of battery pack energy density, and low fire safety performance.
[0005] In the prior art, Chinese invention patent application No. 201711498849.6 discloses a dual-temperature safety silicone, the manufacturing materials of which include by weight: 100 parts of silicone rubber; 15-40 parts of white carbon black; 30-70 parts of thermal insulation filler; 15-40 parts of thermal conductive filler; 10-35 parts of flame retardant; 0.5-3 parts of coupling agent; 5-10 parts of structural control agent; 0.2-10 parts of high-temperature catalyst; 0-5 parts of other additives; 0.4-2 parts of vulcanizer. The invention has the functions of heat dissipation at room temperature and heat insulation under high temperature or fire. It is applied to fire-resistant wires and cables, bus ducts, engines and power batteries. When the components are operating normally, the heat generated by resistance, friction, and charging and discharging can be dispersed in time. At the same time, once the component overheats and causes high temperature or fire, this dual-temperature material can be quickly decomposed and phase-changed under the action of the catalyst to become a hard ceramic-like material with a porous structure.
[0006] However, the above dual-temperature safety silicone technical solution still has the following deficiencies: 1. The material controls the dual temperature by filling with thermal conductive fillers and thermal insulating fillers, but the thermal conductive filler has a high thermal conductivity, which is helpful for heat conduction; the thermal insulating filler has a low thermal conductivity, which is helpful for heat insulation. The two fillers have opposite effects and affect each other in the material, thereby affecting the realization of its room temperature heat dissipation or high temperature insulation effect. 2. The material cannot automatically produce structural changes according to the large changes in temperature. Therefore, when the temperature suddenly rises (especially when the temperature has not yet risen to the decomposition temperature of the material), the thermal conductivity of the material will not decrease in a gradient, and it cannot quickly change from heat conduction to heat insulation. Judging from the role of each filler in the specific embodiment, the thermal conductivity of the material at room temperature and high temperature is relatively small during the implementation of this solution, and it cannot realize the integration of the three functions of thermal conduction, thermal insulation, and flame retardancy and fire prevention. Therefore, it cannot meet the thermal management requirements of complex systems such as electric vehicle power batteries.
[0007] Therefore, it is necessary to study a new thermal system management method and composite material for electric vehicle power batteries that can integrate the three functions of thermal conductivity, thermal insulation, and flame retardancy and fire prevention, and automatically convert to meet the needs of complex thermal system management of electric vehicle power batteries. Summary of the invention
[0008] In view of the above technical problems, the purpose of the present invention is to focus on the dual needs of heat dissipation and fire safety of new energy vehicle batteries, and provide a thermal system management method for electric vehicle power batteries. By setting functional materials, it can integrate the three functions of thermal conductivity, thermal insulation, and flame retardancy and fire prevention, and can automatically switch according to changes in external temperature. It can meet the needs of complex thermal system management of electric vehicle power batteries, and effectively solve the current contradiction between heat dissipation and thermal insulation and fire prevention technologies in new energy vehicle power batteries.
[0009] The object of the present invention is also to provide a silicone rubber material for realizing the above method, which has the functions of heat conduction at room temperature, foaming and heat insulation at high temperature, and porcelain fire prevention during fire; the present invention also provides a method for preparing the silicone rubber composite material.
[0010] To achieve the above object, the technical solution of the present invention is:
[0011] A thermal system management method for an electric vehicle power battery, characterized in that it comprises the following steps:
[0012] (1) A room-temperature heat-conducting, high-temperature heat-insulating and fire-resistant silicone rubber composite material is prepared, and the material is placed in the gaps between the cells of the electric vehicle power battery. The material automatically changes the thermal conductivity of the material according to the temperature changes in the gaps between the battery cells, automatically adjusts the thermal system, ensures the safety of each battery cell, and has flame retardant and fire-resistant properties. According to the temperature changes, it automatically selects one of the following steps, or continuously changes according to the temperature changes, so as to realize the complex management of the thermal system of the electric vehicle power battery:
[0013] (2) Automatic heat dissipation: When the temperature is lower than 100°C, the material has a higher thermal conductivity of 0.5-3W / (m·K), achieving the function of automatic heat dissipation;
[0014] (3) Automatic thermal insulation: When the temperature is between 150 and 200°C, the thermal conductivity of the material gradually decreases to a low thermal conductivity of 0.2 to 0.02 W / (m·K), thus achieving the function of automatic thermal insulation;
[0015] (4) Automatic flame retardancy: When the temperature is further increased to 400-800°C, the material gradually changes from a soft rubber state to a porous ceramic state, and the shape and structural integrity are always maintained during the transformation process, thereby achieving the functions of fire prevention, heat insulation, and automatic flame retardancy.
[0016] A room temperature heat-conducting, high temperature heat-insulating and fire-resistant silicone rubber composite material for implementing the above method, characterized in that the material is made of the following components in parts by weight:
[0017] Silicone rubber matrix 100 parts;
[0018] 20-300 parts of thermal conductive filler;
[0019] 1-10 parts of foaming agent;
[0020] 10-20 parts of porcelain-forming functional filler;
[0021] Flame retardant 5-15 parts;
[0022] Other additives 1-5 parts.
[0023] The silicone rubber matrix is one of liquid two-component addition-type methyl vinyl silicone rubber, low-hardness solid high-temperature vulcanized silicone rubber, and room-temperature curing single-component liquid silicone rubber.
[0024] The heat-conducting functional filler is one or a combination of graphite, graphene, asphalt-based carbon fiber, hexagonal boron nitride, aluminum oxide, and zinc oxide whisker.
[0025] The ceramic functional filler is one or a combination of low melting point glass powder, zinc borate, feldspar, calcium silicate and boron oxide; the foaming agent is one or a combination of chemical foaming agent, physical foaming agent and expanded graphite.
[0026] The flame retardant is one or a combination of metal hydroxide, intumescent flame retardant and phosphorus-nitrogen flame retardant.
[0027] Other additives include vulcanizing agents, surface treatment agents, catalysts and other additives used for molding and processing.
[0028] A method for preparing the above-mentioned normal temperature heat-conducting, high temperature heat-insulating and fire-resistant silicone rubber composite material, characterized in that it comprises the following steps:
[0029] (1) Prepare or weigh the raw material components according to the following weight ratios:
[0030] 100 parts of silicone rubber matrix, 20-300 parts of thermal conductive filler, 1-10 parts of foaming agent,
[0031] 10-20 parts of ceramic functional filler, 5-15 parts of flame retardant, 1-5 parts of other additives;
[0032] (2) Mixing: Put silicone rubber, thermal conductive filler, foaming agent, ceramic filler, flame retardant and other additives into a kneading machine, and knead them uniformly and degas in vacuum;
[0033] (3) Vulcanization: Use a flat plate vulcanizer to perform hot pressing and vulcanization molding to obtain a room temperature thermal conductive and high temperature thermal insulating and fireproof silicone rubber composite material.
[0034] Wherein step (3) also includes: when performing vulcanization, on the basis of ensuring the vulcanization molding of the silicone rubber, the vulcanization process temperature of the silicone rubber is selected to be close to the lower limit, and the amount of the vulcanizing agent is selected to be close to the lower limit, so that the composite material has a higher foaming ratio at high temperature, greatly reduces the thermal conductivity coefficient at high temperature, and enables the composite material to have a functional transformation from thermal conductivity to thermal insulation.
[0035] Step (3) also includes: the temperature of the vulcanization process of the ceramic functional filler silicone rubber is lower than the lowest temperature at which the foaming agent starts to foam, so that the composite material has a higher thermal conductivity at room temperature.
[0036] The beneficial effects of the present invention are:
[0037] (1) The thermal system management method of the electric vehicle power battery provided by the present invention overcomes the technical contradiction between heat conduction and heat insulation in thermal system management. By setting a normal temperature heat-conducting and high temperature heat-insulating and fire-proof silicone rubber composite material, and setting the material in the gaps between the cells of the electric vehicle power battery, the material automatically changes the thermal conductivity of the material according to the temperature changes in the gaps between the battery cells, automatically adjusts the thermal system to ensure the safety of each battery cell, and has flame retardant and fireproof properties. According to the temperature changes, it automatically performs one of the steps of heat conduction, heat insulation, and flame retardant and fireproof, or continuously changes according to the temperature changes, so as to realize the complex management of the thermal system of the electric vehicle power battery and ensure the safety of the electric vehicle power battery system.
[0038] (2) The room-temperature heat-conducting, high-temperature heat-insulating and fire-resistant silicone rubber composite material provided by the present invention integrates the three functions of heat conduction, heat insulation and flame retardancy and fire prevention in one, and the material can automatically adjust its own thermal conductivity according to the temperature change of the battery cell. At normal use temperature, the thermal conductivity is high, which is conducive to heat dissipation between battery cells; when the battery cell heats up rapidly, the thermal conductivity decreases rapidly, and it changes from heat conduction to heat insulation, keeping the temperature of the surrounding batteries unaffected or less affected; when thermal runaway of the battery cell occurs, it can withstand high-temperature ablation of 500-800°C, thereby strictly limiting the fire to a small range, thereby improving the overall energy density and fire safety of the lithium-ion power battery pack.
[0039] (3) The room-temperature heat-conducting, high-temperature heat-insulating and fire-resistant silicone rubber composite material provided by the present invention overcomes the technical contradiction between heat conduction and heat insulation. The addition of thermal conductive fillers is only to improve its thermal conductivity at room temperature. When the temperature rises to 120-200°C, the thermal insulation depends on the action of the foaming agent at high temperature, which generates a large number of bubbles inside the material. The large number of bubbles in the material separate the thermal conductive fillers that were originally tightly connected, destroying the original good thermal conductive path, thereby reducing the thermal conductivity of the material and achieving the purpose of thermal insulation. At high temperature or fire, the material is transformed into porous inorganic ceramics under the action of the ceramic-forming agent, thereby having the functions of fire prevention and heat insulation. Therefore, it is a silicone rubber material that integrates the three functions of thermal conduction, heat insulation and flame retardancy and fire prevention. If divided according to temperature sections, it can be called "three-temperature" safety silicone rubber.
[0040] (4) The material and preparation method provided by the present invention, by adopting a unique combination and ratio of silicone rubber and thermal conductive functional filler, foaming agent and ceramic sintering aid, enable this polymer material to obtain the technical effects of good flame retardancy, maintaining a certain mechanical strength, and good weather resistance, room temperature thermal conductivity - high temperature thermal insulation and fire prevention, so that the silicone rubber composite material has a high thermal conductivity at room temperature, and begins to foam after the ambient temperature rises to the foaming temperature of the foaming agent, automatically reducing the thermal conductivity. As the temperature continues to rise, the ceramic functional filler enables the composite material to always maintain its shape and structural integrity, thereby achieving the function of preventing the rapid spread of flames or high temperatures and playing a fire prevention role.
[0041] (5) In actual application of the present invention, at room temperature, a large amount of heat-conducting functional fillers are interconnected in the polymer matrix to form a heat-conducting path. Although the foaming agent and the ceramic-forming auxiliary agent are not high-thermal conductivity fillers, they are connected to the heat-conducting functional fillers in a shell-to-shell manner to form a heat-conducting network, which not only does not reduce the thermal conductivity, but can improve the thermal conductivity of the silicone rubber material; at high temperatures, the foaming agent decomposes and foams, and the newly formed bubbles destroy the construction of the heat-conducting network at room temperature, thereby realizing the functional transformation of the heat-conducting silicone thermal interface material from heat conduction to heat insulation. When the temperature continues to rise, the high temperature decomposes the silicone matrix and melts the ceramic-forming auxiliary agent, further realizing the transformation from organic foamed silicone rubber to inorganic porous ceramic silicone rubber, playing a role in fireproofing and heat insulation, thereby perfectly meeting the requirements of heat dissipation of the current new energy vehicle power battery when working normally below 100°C, heat insulation to delay the spread of thermal runaway to surrounding cells when a single battery cell is in thermal runaway, and organizing the spread of flames and high temperatures when the battery cell is completely out of control and catches fire.
[0042] (6) The actual experimental test results of the present invention show that the room temperature thermal conductive and high temperature thermal insulating and fireproof silicone rubber composite material provided by the present invention has a tensile strength of >0.5MPa, an elongation at break >50%, a tear strength >1kN / m, a flame retardant grade of V-0, and a thermal conductivity of up to 2.0W / (m·K) at room temperature; the thermal conductivity after high temperature (150-200°C) foaming is reduced to 0.085W / (m·K); and as the temperature further increases, the structural integrity can be maintained, thereby preventing the rapid spread of flames and high temperatures. Compared with traditional single-function materials, the present invention integrates the three functions of thermal conductivity, thermal insulation and fireproofing, and can be widely used to deal with thermal runaway problems in new energy battery packs.
[0043] (7) The preparation method provided by the present invention has few steps, reasonable process, universal equipment, easy to realize batch production, and good product consistency.
[0044] The above is an overview of the technical solution of the invention. The present invention will be further described below in conjunction with specific implementation methods and drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 is a microscope image of a normal temperature heat-conducting, high temperature heat-insulating, and fire-resistant silicone rubber composite material according to an embodiment of the present invention; wherein Figure 1 (A) is a microscope image of the microstructure under normal temperature thermal conduction state. Figure 1 (B) is a microscope image of the microstructure under high temperature insulation state;
[0046] Figure 2 This is a graph showing the change in thermal conductivity of the normal-temperature heat-conducting, high-temperature heat-insulating, and fire-resistant silicone rubber composite material at different temperature stages in an embodiment of the present invention. DETAILED DESCRIPTION
[0047] See also Figure 1 , Figure 2 In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined purpose, the specific implementation methods of the present invention are described in detail below in combination with the preferred embodiments.
[0048] Example:
[0049] A thermal system management method for an electric vehicle power battery comprises the following steps:
[0050] (1) A room-temperature heat-conducting, high-temperature heat-insulating and fire-resistant silicone rubber composite material is prepared, and the material is placed in the gaps between the cells of the electric vehicle power battery. The material automatically changes the thermal conductivity of the material according to the temperature changes in the gaps between the battery cells, automatically adjusts the thermal system, ensures the safety of each battery cell, and has flame retardant and fire-resistant properties. According to the temperature changes, it automatically selects one of the following steps, or continuously changes according to the temperature changes, so as to realize the complex management of the thermal system of the electric vehicle power battery:
[0051] (2) Automatic heat dissipation: When the temperature is lower than 100°C, the material has a higher thermal conductivity of 0.5-3W / (m·K), achieving the function of automatic heat dissipation;
[0052] (3) Automatic thermal insulation: When the temperature is between 150 and 200°C, the thermal conductivity of the material gradually decreases to a low thermal conductivity of 0.2 to 0.02 W / (m·K), thus achieving the function of automatic thermal insulation;
[0053] (4) Automatic flame retardancy: When the temperature is further increased to 400-800°C, the material gradually changes from a soft rubber state to a porous ceramic state, and the shape and structural integrity are always maintained during the transformation process, thereby achieving the functions of fire prevention, heat insulation, and automatic flame retardancy.
[0054] A normal temperature heat-conducting, high temperature heat-insulating and fire-resistant silicone rubber composite material for implementing the above method, the material is made of the following components in parts by weight:
[0055] Silicone rubber matrix 100 parts;
[0056] 20-300 parts of thermal conductive filler;
[0057] 1-10 parts of foaming agent;
[0058] 10-20 parts of porcelain-forming functional filler;
[0059] Flame retardant 5-15 parts;
[0060] Other additives 1-5 parts.
[0061] The silicone rubber matrix is one of liquid two-component addition-type methyl vinyl silicone rubber, low-hardness solid high-temperature vulcanized silicone rubber, and room-temperature curing single-component liquid silicone rubber.
[0062] The heat-conducting functional filler is one or a combination of graphite, graphene, asphalt-based carbon fiber, hexagonal boron nitride, aluminum oxide, and zinc oxide whisker.
[0063] The ceramic functional filler is one or a combination of low melting point glass powder, zinc borate, feldspar, calcium silicate and boron oxide; the foaming agent is one or a combination of chemical foaming agent, physical foaming agent and expanded graphite.
[0064] The flame retardant is one or a combination of metal hydroxide, intumescent flame retardant and phosphorus-nitrogen flame retardant.
[0065] Other additives include vulcanizing agents, surface treatment agents, catalysts and other additives used for molding and processing.
[0066] A method for preparing the above-mentioned normal temperature heat-conducting, high temperature heat-insulating and fire-resistant silicone rubber composite material comprises the following steps:
[0067] (1) Prepare or weigh the raw material components according to the following weight ratios:
[0068] 100 parts of silicone rubber matrix, 20-300 parts of thermal conductive filler, 1-10 parts of foaming agent,
[0069] 10-20 parts of ceramic functional filler, 5-15 parts of flame retardant, 1-5 parts of other additives;
[0070] (2) Mixing: Put silicone rubber, thermal conductive filler, foaming agent, ceramic filler, flame retardant and other additives into a kneading machine, and knead them uniformly and degas in vacuum;
[0071] (3) Vulcanization: hot-press vulcanization molding is performed using a flat-plate vulcanizer to obtain a room-temperature thermally conductive and high-temperature thermally insulating and fireproof silicone rubber composite material; during the vulcanization, on the basis of ensuring the vulcanization molding of the silicone rubber, the vulcanization process temperature of the silicone rubber is selected to be close to the lower limit, and the amount of the vulcanizer is selected to be close to the lower limit, so that the composite material has a higher foaming ratio at high temperature, greatly reduces the thermal conductivity at high temperature, and enables the composite material to have a functional transformation from thermal conductivity to thermal insulation; the temperature of the vulcanization process of the ceramic functional filler silicone rubber is lower than the lowest temperature at which the foaming agent begins to foam, so that the composite material has a higher thermal conductivity at room temperature. Specific embodiment 1:
[0073] The room-temperature heat-conducting, high-temperature heat-insulating and fire-resistant silicone rubber composite material provided in an embodiment of the present invention is prepared from the following raw material components (by mass fraction):
[0074]
[0075] The method for preparing the above-mentioned normal temperature heat-conducting, high temperature heat-insulating and fire-resistant silicone rubber composite material comprises the following steps:
[0076] (1) Vacuum kneading: Put the above raw materials into a vacuum kneader according to proportion, mix and evenly mix, and degas;
[0077] (2) Vulcanization: The mixed material is placed on a flat plate and vulcanized using a flat plate vulcanizer at a pressure of 14 MPa and 100° C. for 30 min to obtain a room temperature thermally conductive, high temperature thermally insulating and fireproof silicone rubber composite material, i.e., a functional silicone rubber composite material. Specific embodiment 2:
[0079] The room-temperature heat-conducting, high-temperature heat-insulating and fire-resistant silicone rubber composite material provided in an embodiment of the present invention is prepared from the following raw material components (by mass fraction):
[0080]
[0081] The method for preparing the above-mentioned normal temperature heat-conducting, high temperature heat-insulating and fire-resistant silicone rubber composite material comprises the following steps:
[0082] (1) Vacuum kneading: Put the above raw materials into a vacuum kneader according to proportion, mix and evenly mix, and degas;
[0083] (2) Vulcanization: The mixed material is placed on a flat plate and vulcanized using a flat plate vulcanizer at a pressure of 14 MPa and 100° C. for 30 min to obtain a room temperature thermally conductive, high temperature thermally insulating and fireproof silicone rubber composite material, i.e., a functional silicone rubber composite material.
[0084] Embodiment 3:
[0085] The room temperature heat-conducting, high temperature heat-insulating and fire-resistant silicone rubber composite material provided in this embodiment is prepared from the following raw material components (by mass fraction):
[0086]
[0087]
[0088] The method for preparing the above-mentioned normal temperature heat-conducting, high temperature heat-insulating and fire-resistant silicone rubber composite material comprises the following steps:
[0089] (1) Vacuum kneading: Put the above raw materials into a vacuum kneader according to proportion, mix them evenly and degas;
[0090] (2) Vulcanization: The unvulcanized functional silicone rubber sheet obtained by mixing is placed in an oven and vulcanized at 125° C. for 20 min to obtain the room-temperature thermally conductive, high-temperature thermally insulating and fire-resistant silicone rubber composite material, i.e., the functional silicone rubber composite material. Specific embodiment 4:
[0092] The room-temperature heat-conducting, high-temperature heat-insulating and fire-resistant silicone rubber composite material provided in an embodiment of the present invention is prepared from the following raw material components (by mass fraction):
[0093]
[0094]
[0095] The method for preparing the above-mentioned normal temperature heat-conducting, high temperature heat-insulating and fire-resistant silicone rubber composite material comprises the following steps:
[0096] (1) Vacuum kneading: Put the above raw materials into a vacuum kneader according to proportion, mix them evenly and degas;
[0097] (2) Vulcanization: The unvulcanized functional silicone rubber sheet obtained by mixing is placed in an oven and vulcanized at 125° C. for 20 min to obtain a functional silicone rubber composite material.
[0098] like Figure 1 The figure shows the comparison of pictures and structures under a microscope of the material of Example 4 before and after the temperature rises. It can be clearly seen that the thermal conductive filler is distributed in the silicone rubber matrix when it is not foamed at room temperature, and when the temperature rises, the material foams, the thermal conductive filler and the silicone rubber are separated by spherical bubbles, and the heat conduction path is affected, thereby realizing the transition from room temperature heat conduction to high temperature heat insulation.
[0099] The normal temperature heat-conducting, high temperature heat-insulating and fire-resistant silicone rubber composite materials prepared in specific examples 1, 2, 3 and 4 were subjected to performance tests:
[0100] (1) Mechanical properties test
[0101] The prepared silicone rubber sheets were cut into dumbbell-shaped specimens of national standard using a cutting machine, and the mechanical properties of the specimens were measured using a ZWICK / Roell Z020 universal testing machine from the German ZWICK company. The test standard adopted was GB / T 528-2009.
[0102] (2) Determination of vertical burning grade
[0103] The test was conducted according to the vertical combustion standard GB / T 10707-2008 “Determination of combustion performance of rubber”.
[0104] (3) Thermal conductivity determination
[0105] The thermal conductivity of the composite material was tested using the LFA447 laser thermal conductivity tester from NETZSCH, Germany. The test sample had a diameter of 12.7 mm and a thickness of 0.8 to 3.5 mm, and the calculation model was the Cowan + pulse correction model.
[0106] (4) Fire resistance test
[0107] The sample was directly ablated with a propane flame at 1000℃-1200℃. The sample thickness was 2mm, the length was 135mm, the width was 125mm, and the ablation time was 30min. The test results are shown in the following table:
[0108]
[0109] See also Figure 2 , which is a graph of thermal conductivity of each formula at three temperature ranges: room temperature, high temperature and ignition. It can be seen that the thermal conductivity of the material is generally high at room temperature, and the thermal conductivity is good. This is due to the presence of thermal conductive fillers in the material and the construction of a good thermal conductive path. When the temperature rises, the material foams at high temperature, and a large number of bubbles separate the thermal conductive network formed between the thermal conductive fillers. Therefore, the thermal conductivity of the material drops sharply and changes from thermal conduction to thermal insulation. When on fire, due to the transformation of organic components to inorganic components in the material, the thermal conductivity of the material increases slightly, but it is still thermally insulating.
[0110] It can be seen that the room-temperature heat-conducting, high-temperature heat-insulating and fire-resistant silicone rubber composite material of the present invention has good heat dissipation function at room temperature, heat insulation and flame retardant functions at high temperature, and has good mechanical properties and thermal protection properties, and can realize safe management of complex thermal systems.
[0111] The present invention focuses on the dual needs of heat dissipation and fire safety of new energy vehicle batteries. By integrating three functional silicone rubber technologies: filled thermal conductive composite material technology, foamed rubber technology and porcelainizable silicone rubber technology, a room-temperature thermal conductive and high-temperature thermal insulating and fireproof silicone rubber composite material with the three functions of room-temperature thermal conductivity, high-temperature thermal insulation and flame retardancy and fireproofing is prepared. This material can effectively solve the problem of the contradiction between heat dissipation and thermal insulation and fireproofing technologies in the current new energy vehicle power batteries.
[0112] The room-temperature heat-conducting, high-temperature heat-insulating and fire-resistant silicone rubber composite material provided by the present invention obtains a functional silicone rubber composite material with good flame retardancy, excellent mechanical properties and good weather resistance through a unique ratio and preparation method of a heat-conducting functional filler, a foaming agent and a porcelain-forming sintering aid, overcomes the existing technical difficulties, and achieves good thermal conductivity at room temperature, heat insulation by high-temperature foaming, and will not burn into ash without strength during thermal runaway.
[0113] It should be noted that the selection of specific components and proportions of raw materials in the above embodiments only represents some examples. In other embodiments, other specific components and proportions can be selected as needed within the scope of the present invention, and the technical effects recorded in the present invention can be achieved. Therefore, the embodiments of the present invention will no longer list them one by one.
[0114] The above description is only a preferred embodiment of the present invention and does not limit the technical scope of the present invention. Therefore, technical features that are the same or similar to those of the above-mentioned embodiments of the present invention are within the protection scope of the present invention.
Claims
1. A thermal system management method for an electric vehicle power battery, characterized in that: It includes the following steps: (1) Prepare a room temperature thermal conductive, high temperature insulating and fireproof silicone rubber composite material, and place the material in the gap between each unit of the electric vehicle power battery. The material automatically changes the thermal conductivity of the material according to the temperature change of the gap between each battery unit, automatically adjusts the thermal system, ensures the safety of each battery unit, and has flame retardant and fireproof properties. According to the temperature change, it automatically selects one of the following steps, or continuously changes according to the temperature change, so as to realize the complex management of the thermal system of the electric vehicle power battery: (2) Automatic heat dissipation: When the temperature is lower than 100°C, the material has a higher thermal conductivity of 0.5-3W / (m·K), realizing the function of automatic heat dissipation; (3) Automatic thermal insulation: When the temperature is between 150 and 200 °C, the thermal conductivity of the material gradually decreases to a low thermal conductivity of 0.2 to 0.02 W / (m·K), thus achieving the function of automatic thermal insulation; (4) Automatic flame retardancy: When the temperature is further increased to 400-800°C, the material gradually changes from a soft rubber state to a porous ceramic state, and the shape and structure integrity are always maintained during the transformation process, thereby achieving the functions of fire prevention, heat insulation, and automatic flame retardancy; The room temperature heat-conducting, high temperature heat-insulating and fire-resistant silicone rubber composite material is made of the following components in parts by weight: Silicone rubber matrix 100 parts; 20-300 parts of thermal conductive filler; 1-10 parts of foaming agent; 10-20 parts of porcelain-forming functional filler; Flame retardant 5-15 parts; Other additives 1-5 parts; The silicone rubber matrix is one of liquid two-component addition-type methyl vinyl silicone rubber, low-hardness solid high-temperature vulcanized silicone rubber, and room-temperature curing single-component liquid silicone rubber; The thermal conductive filler is one or a combination of graphite, graphene, asphalt-based carbon fiber, hexagonal boron nitride, aluminum oxide, and zinc oxide whisker; The ceramic functional filler is one or a combination of low melting point glass powder, zinc borate, feldspar, calcium silicate and boron oxide; the foaming agent is one or a combination of chemical foaming agent, physical foaming agent and expanded graphite; The flame retardant is one or a combination of metal hydroxide, intumescent flame retardant, phosphorus-nitrogen flame retardant; The other additives are vulcanizing agents, surface treatment agents, and catalysts used for molding and processing.
2. A method for preparing the room temperature heat-conducting, high temperature heat-insulating and fire-resistant silicone rubber composite material according to claim 1, characterized in that: It includes the following steps: (1) Prepare or weigh the raw material components according to the following weight ratios: 100 parts of silicone rubber matrix, 20-300 parts of thermal conductive filler, 1-10 parts of foaming agent, 10-20 parts of ceramic functional filler, 5-15 parts of flame retardant, 1-5 parts of other additives; (2) Mixing: Put silicone rubber, thermal conductive filler, foaming agent, ceramic filler, flame retardant and other additives into a kneading machine, knead them evenly under vacuum and degas; (3) Vulcanization: Use a flat plate vulcanizer to perform hot pressing vulcanization molding to obtain a room temperature thermal conductive and high temperature thermal insulating and fireproof silicone rubber composite material.
3. The method for preparing the room temperature heat-conducting, high temperature heat-insulating and fire-resistant silicone rubber composite material according to claim 2, characterized in that: Wherein step (3) further comprises: when performing vulcanization, on the basis of ensuring the vulcanization molding of the silicone rubber, the vulcanization process temperature of the silicone rubber is selected to be close to the lower limit, and the amount of the vulcanizing agent is selected to be close to the lower limit, so that the composite material has a higher foaming ratio at high temperature, and the thermal conductivity coefficient at high temperature is greatly reduced, so that the composite material has the function of changing from thermal conductivity to thermal insulation.
4. The method for preparing the room temperature heat-conducting, high temperature heat-insulating and fire-resistant silicone rubber composite material according to claim 2, characterized in that: The step (3) also includes: the temperature of the vulcanization process of the ceramic functional filler silicone rubber is lower than the lowest temperature at which the foaming agent starts to foam, so that the composite material has a higher thermal conductivity at room temperature.