Soft magnetic metal flat powder, resin composite sheet using the same, and resin composite compound for molding

By adjusting the Fe-Al-Si composition and optimizing the processing technology, the problem of insufficient permeability stability of soft magnetic metal flat powder in the range of -40-85℃ is solved, and soft with high permeability and low coercivity is achieved Magnetic metal flat powder and resin composite sheet meet the improvement of electromagnetic wave noise suppression and magnetic shielding performance in electronic equipment.

CN113748471BActive Publication Date: 2024-12-06株式会社每德
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202180002865.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-01-11
Filing Date
2021-01-08
Publication Date
2024-12-06
Estimated Expiration
2041-01-08

AI Technical Summary

Technical Problem

The existing soft magnetic metal flat powder has insufficient permeability stability within the actual temperature range (-40~85℃), and the coercive force is difficult to maintain low to meet the requirements of high permeability, especially in thinner and small sizes. Electromagnetic wave noise suppression and magnetic shielding performance in transformed electronic devices are limited.

Method used

By adjusting the Fe-Al-Si composition, ensure that the magnetic permeability shows a positive temperature coefficient in the range of -40℃~85℃, and the coercive force is controlled to be less than 70A/m. A specific flat processing and molding process is adopted, combined with resin Composite material, optimize the composition and structure of soft magnetic metal flat powder and resin composite sheet.

Benefits of technology

A soft magnetic metal flat powder and resin composite sheet with high magnetic permeability and low coercivity in the range of -40-85℃ is realized, which meets the requirements of electromagnetic wave noise suppression and magnetic shielding performance in electronic equipment and increases temperature Stability and magnetic permeability overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113748471B_ABST
    Figure CN113748471B_ABST
Patent Text Reader

Abstract

The present invention provides a soft magnetic flat metal powder having high magnetic permeability and adjusted temperature coefficient of magnetic permeability, a resin composite sheet using the material, and a resin composite composition for molding. The soft magnetic flat metal powder is characterized in that the temperature coefficient K of the magnetic permeability of the soft magnetic flat metal powder composed of Fe-Al-Si satisfies the following formula (1), (2), (3) in the range of -40°C to 85°C, and the coercive force is 70A / m or less. K=(μ(0℃)-μ(-40℃)) / μ(-40℃)>0(1)K=(μ(40℃)-μ(0℃)) / μ(0℃)>0(2)K=(μ(85℃)-μ(40℃)) / μ(40℃)>0(3)K: temperature coefficient, μ: magnetic permeability (μ': real magnetic permeability, μ": imaginary magnetic permeability) In addition, a resin composite sheet, a resin composite composition for injection molding and extrusion molding are provided, and the resin composite sheet is characterized in that the above-mentioned soft magnetic metal flat powder is composed of resin and has a coercive force of less than 80A / m.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a soft magnetic metal flat powder, a resin composite sheet using the powder, and a resin composite composition for molding processing. The soft magnetic metal flat powder is used for noise suppression components used to prevent unnecessary electromagnetic waves generated in communication equipment and various electronic devices from leaking to the outside and interfering between internal circuits, and the influence of malfunctions caused by external electromagnetic waves, pen input of mobile devices using electromagnetic induction, and magnetic shielding components used in non-contact charging modules. Background Art

[0002] Unnecessary electromagnetic waves are generated from communication equipment and various electronic devices, and equipment failure and communication barriers caused by external and internal interference have become a problem. Although various countermeasures have been taken, the problem has become more prominent with the popularization of 5G and WiFi6 communication methods.

[0003] In addition, as communication equipment and various electronic devices are becoming thinner and smaller, the mounting density of electronic components has increased significantly. As a result, problems caused by electromagnetic interference between components or circuit boards frequently occur. For this reason, electronic components or flexible magnetic sheets (resin composite sheets) for noise countermeasures are used.

[0004] On the other hand, the effective use of electromagnetic waves is developing, pen input and contactless charging of mobile devices using electromagnetic induction are becoming more and more popular, and in order to prevent interference with metal parts and effectively use the magnetic field, magnetic shielding materials are used in combination with coil parts.

[0005] Soft magnetic metal flat powder is used in flexible magnetic sheets (resin composite sheets) or extrusion and injection molded products used to suppress electromagnetic wave noise and magnetic shielding. This is because, by processing into a flat shape, the anti-magnetic field coefficient becomes smaller and the magnetic permeability in the in-plane direction becomes higher. In addition, exceeding the Snoek limit can maintain the magnetic permeability to a higher frequency. In order to suppress electromagnetic wave noise, the imaginary magnetic permeability μ ", which represents the magnetic loss of the magnetic permeability, is used, and the real magnetic permeability μ ' is used in magnetic shielding.

[0006] However, due to the development of thinner and smaller devices in recent years, the installation space for suppressing electromagnetic wave noise and magnetic shielding components has been limited. To date, the demand for soft magnetic metal flat powders and flexible magnetic sheets (resin composite sheets) with high magnetic permeability and resin composite compositions for molding processing has become higher.

[0007] At present, as a soft magnetic metal flat powder using Fe-based alloy powder, it is known that the flat powder of Fe-Al-Si composition, which is called aluminum silicon sendust, has high magnetic permeability. In particular, the composition of Fe-Al-Si, in which both crystal magnetic anisotropy and magnetostriction are zero, is Al: 5.4wt%, Si: around 9.6wt%, and the remainder is Fe and inevitable impurities. Therefore, there is patent No. 3722391 (patent document 1) that takes into account the surface oxidation of flat powder to adjust the composition. On the other hand, patent No. 6592424 (patent document 2) and patent publication 2005-281783 (patent document 3) propose that by actively adjusting the composition of Al and Si, a higher magnetic permeability can be obtained.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: Japanese Patent No. 3722391

[0011] Patent Document 2: Japanese Patent No. 6592424

[0012] Patent Document 3: Japanese Patent Application Laid-Open No. 2005-281783 Summary of the invention

[0013] Problems to be solved by the invention

[0014] When communication equipment and various electronic devices are actually used, there are changes in the surrounding temperature or heat generation, and there is a requirement for performance assurance of -40 to 150°C in automobiles and -40 to 85°C in other applications. Therefore, it is necessary to ensure stable electromagnetic wave noise suppression and magnetic shielding performance in the temperature range of -40 to 85°C at least. However, the measurement of magnetic permeability is usually performed only at room temperature, and there is no record related to stably obtaining high magnetic permeability in the actual use temperature range as mentioned in the present invention in Patent Documents 1, 2 and 3.

[0015] In addition, Patent Document 2 describes that the magnetic permeability is improved by adjusting the composition from Fe-5.4wt%Al-9.6wt%Si. Generally, in order to improve the magnetic permeability, it is effective to increase the diameter-to-thickness ratio to reduce the diamagnetic field and reduce the coercive force, but by adjusting the composition, the coercive force increases to more than 100A / m (applied magnetic field 144kA / m), and it is difficult to meet the requirements of further high magnetic permeability in the prior art. In addition, the contents of the total content of Al+Si and the coercive force mentioned in the present invention are not described in the examples of Patent Documents 2 and 3. In addition, the diameter-to-thickness ratio varies in each powder measured due to different flattening processing degrees, so if the size of the long side direction of the measured powder is not specified, it is meaningless, but there is no record related to these. In addition, if only the diameter-to-thickness ratio is concerned, there is a problem of over-crushing, increasing the proportion of fine powder, and increasing coercive force, but there is no record related to this.

[0016] The present invention has been developed in view of the above problems and aims to provide a soft magnetic flat metal powder and resin composite sheet and a resin composite composition for molding which exhibit a positive temperature coefficient of magnetic permeability in the range of -40°C to 85°C and maintain a low coercive force and high magnetic permeability.

[0017] The present invention solves the problems of the above-mentioned conventional soft magnetic flat metal powder composed of Fe—Al—Si, and the resin composite sheet and the resin composite composition for molding using the same.

[0018] Technical solutions to solve problems

[0019] According to the present invention, a soft magnetic flat metal powder is obtained, characterized in that the temperature coefficient K of the magnetic permeability of the soft magnetic flat metal powder composed of Fe-Al-Si satisfies the following formulas (1), (2), (3) in the range of -40°C to 85°C, and the coercive force is less than 70 A / m.

[0020] K=(μ(0℃)-μ(-40℃)) / μ(-40℃)>0(1)

[0021] K=(μ(40℃)-μ(0℃)) / μ(0℃)>0(2)

[0022] K=(μ(85℃)-μ(40℃)) / μ(40℃)>0(3)

[0023] K: temperature coefficient, μ: magnetic permeability (μ': real magnetic permeability, μ": imaginary magnetic permeability)

[0024] In addition, according to the present invention, a soft magnetic flat metal powder is obtained, characterized in that, in the above-mentioned soft magnetic flat metal powder, the powder with a particle size near the average particle size D50 is flat with an aspect ratio of 20 to 200, and its composition contains Al: 6 to 7.5wt%, Si: 8.5 to 9.5wt%, and the remainder: a component composed of Fe and inevitable impurities, wherein the total content of Al and Si is 15 to 16.5wt%.

[0025] According to the present invention, there is obtained a resin composite sheet characterized by comprising the above-mentioned flat soft magnetic metal powder and a resin and having a coercive force of 80 A / m or less.

[0026] According to the present invention, there is obtained a resin composite composition for injection molding and extrusion molding, characterized in that it is composed of the above-mentioned soft magnetic flat metal powder and a resin.

[0027] Effects of the Invention

[0028] The present invention aims to provide a soft magnetic flat metal powder and a resin composite sheet having high magnetic permeability and an adjusted temperature coefficient of magnetic permeability, and a resin composite composition for molding. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The graph shows the temperature dependency of the real magnetic permeability of a resin composite sheet in which a flat soft magnetic metal powder having a composition of 50 vol % Fe-5.4 wt % Al-9.6 wt % Si is blended and the flat soft magnetic metal powders having different grades of magnetic permeability are mixed.

[0030] Figure 2 This is a graph showing the temperature dependency of the real magnetic permeability when the soft magnetic flat metal powder has a composition of Fe-5.4 wt % Al-9.6 wt % Si and a composition of Fe-4.5 wt % -9.0 wt % Si. DETAILED DESCRIPTION

[0031] Hereinafter, the best mode of the present invention will be described specifically.

[0032] The soft magnetic alloy raw material powder of the Fe—Al—Si composition can be produced by various generally known methods such as a water atomization method, a gas atomization method, an ingot pulverization method, etc., but is not particularly limited.

[0033] The soft magnetic alloy raw material powder of the Fe-Al-Si composition preferably contains Al: 6-7.5wt%, Si: 8.5-9.5wt%, and the total content of Al and Si is 15-16.5wt%. The range of 15.5-16wt% is more preferred. When the total content of Al and Si is less than 15wt%, the coercive force increases, so the magnetic permeability becomes lower. When it exceeds 16.5wt%, the temperature coefficient of the magnetic permeability at 85°C becomes negative. In addition, in addition to Fe-Al-Si, the soft magnetic alloy raw material powder can also be added with trace components such as Mn, Mo, Ca, O, and C as needed.

[0034] Flattening is not particularly limited, and can be implemented using a grinder, ball mill, vibration mill, etc. in the presence of distilled water or an organic solvent. As an organic solvent, toluene, hexane, alcohol, ethylene glycol, etc. can be used, and the atmosphere in the device can also be adjusted during processing. In addition, as a flattening aid, stearic acid, etc. can also be added. In addition, the soft magnetic alloy raw material powder can also be used after heat treatment before flattening.

[0035] After the flattening treatment, heat treatment is preferably performed in an inert atmosphere to remove the crystal strain generated during processing, and the heat treatment temperature is preferably 500 to 900° C. This is because if it is below 500° C., the strain removal is insufficient, and if it exceeds 900° C., local aggregation or sintering occurs.

[0036] The aspect ratio of the powder near the average particle size D50 of the soft magnetic metal flat powder is preferably 20 to 200, more preferably 30 to 150. If the aspect ratio is less than 20, the magnetic permeability decreases when the resin composite sheet and the resin composite composition for molding are made due to the influence of the reverse magnetic field, and when it exceeds 200, the processability decreases.

[0037] In addition, the bulk density / true density is preferably in the range of 0.036 to 0.086. When it becomes smaller than 0.036, it is too flat and becomes difficult to handle. On the other hand, when it exceeds 0.086, the flattening is insufficient, so the magnetic permeability decreases. The measurement of bulk density is implemented based on JIS Z2504. The true density is measured using AccuPyc 1330 manufactured by Shimadzu Corporation.

[0038] The average particle size D50 of the flat powder is measured using R4 in HELOS / BR-multi manufactured by Sympatec. Flat powders with a particle size range of ±10% are extracted by air classification relative to the average particle size D50 obtained, embedded in epoxy resin and mirror-polished to obtain a sample for thickness measurement. The diameter-to-thickness ratio is the major diameter / thickness of the flat powder, but the major diameter is taken as the value of the average particle size D50, and the thickness of the powder flat powder is measured by a scanning electron microscope to obtain the diameter-to-thickness ratio. The diameter-to-thickness ratio can also be obtained by embedding a resin composite magnetic sheet or molded part in epoxy resin and measuring the average major diameter and thickness by a scanning electron microscope.

[0039] The coercivity was measured using an automatic coercivity meter K-HC1000 manufactured by Tohoku Special Steel in an applied magnetic field of 148 kA / m. About 10 mg of the flat powder was wrapped with a non-magnetic tape so as not to scatter to prepare a sample for measurement. The sample for magnetic permeability measurement was used in the coercivity measurement of the resin composite sheet and the molded product of the resin composition.

[0040] The magnetic permeability was measured using an impedance analyzer E4991B, a magnetic material test fixture 16454A and a heat resistance test assembly manufactured by Keysight, in a constant temperature and humidity chamber at a temperature range of -40°C to 85°C.

[0041] As the measurement samples, a resin composite sheet and an article obtained by injection molding the resin composite composition for molding were used.

[0042] As for the resin composite sheet, it is also possible to combine the soft magnetic metal flat powder and the polymer material, and make it into ink-like by various known methods, and make the sheet-like articles by blade coating, comma coating, screen printing, etc., and further compress it by various rollers or presses. In addition, it can be kneaded by a kneading machine and made by roller forming, and it can also be further compressed by pressing. When making the sheet, a magnetic field is applied and the orientation of the soft magnetic metal flat powder is controlled, thereby, the magnetic permeability can be improved.

[0043] The coercive force of the resin composite sheet is preferably 80A / m or less. More preferably, it is 70A / m or less. Preferably, the content of the soft magnetic metal flat powder is 35vol% to 65vol% relative to the total solid content. More preferably, it is 40vol% to 55vol%. When it is less than 35vol%, the magnetic permeability will decrease even if the coercive force is 80A / m or less. When it exceeds 65vol%, it becomes difficult to form a sheet and the magnetic permeability decreases.

[0044] As the polymer resin, polyurethane, acrylic, silicon, epoxy, chlorinated polyethylene, chloroprene rubber, etc. can be used alone or in combination, but are not limited thereto. Thermoplasticity and thermosetting properties are also not limited. In addition, various surface treatments can be performed as needed by coupling agents, dispersants, rust inhibitors, etc., or various additives such as antioxidants, pigments, non-magnetic fillers, and thermal conductive fillers can be added as needed within the scope of not damaging the purpose of the present invention.

[0045] The resin composite composition is prepared by mixing a soft magnetic flat metal powder and a polymer resin and kneading them by a kneader or a biaxial mixer, but it is not particularly limited and can be carried out by various known methods, but the content of the soft magnetic flat metal powder is preferably 35 vol% to 65 vol% relative to the total solid content. More preferably, it is 45 vol% to 55 vol%. When it is less than 35 vol%, the magnetic permeability of the molded product becomes low, and when it exceeds 65 vol%, molding becomes difficult and the magnetic permeability decreases.

[0046] As the polymer material, thermosetting epoxy resins, acrylic resins, urea resins, etc. and thermoplastic polyamide resins, aromatic polyamide resins, polyphenylene sulfide resins, fluorine resins, polyether resins, polyester resins, etc. can be used alone or in combination, but are not limited thereto. In addition, various surface treatments can be performed as needed by coupling agents, dispersants, rust inhibitors, etc., or various additives such as antioxidants, pigments, non-magnetic fillers, and thermal conductive fillers can be added as needed within the scope of not damaging the purpose of the present invention.

[0047] The resin composite composition can be molded into various shapes using an extrusion molding machine, an extrusion molding machine, etc. During the molding, the molding can also be performed while applying a magnetic field.

[0048] Example

[0049] Hereinafter, the present invention will be specifically described by way of examples.

[0050] For the soft magnetic metal flat powder used in Examples 1 to 14 and Comparative Examples 1 to 8, a raw material powder composed of Fe-Al-Si with an average particle size D50 = 100 μm produced by an ingot pulverization method was used, and flattening was performed using a grinding mill in a manner to achieve a specified bulk density / true density. In Examples 1 to 14, the processing conditions were adjusted in a manner such that the coercive force was 70 A / m or less. Flattening was performed using ethanol under wet conditions. After flattening, the ethanol was removed by drying, and a heat treatment for strain removal was performed at 800°C for 2 hours in an Ar atmosphere.

[0051] Using the soft magnetic metal flat powder obtained in Examples 1 to 12 and Comparative Examples 1 to 6, a thermosetting polyurethane resin is dispersed in a resin solution diluted with toluene in a manner of 50 vol% relative to the total solid content. The dispersion is applied to a thickness of 100 μm by a comma coater, oriented in a magnetic field, and then dried at 50°C to remove the solvent. The dried sheets are stacked and hot pressed at 150°C and a pressure of 10 MPa to obtain a resin composite sheet with a thickness of 200 μm for performance evaluation. Next, it is cut into a ring with an outer shape of 20 mm and an inner diameter of 10 mm, and the coercive force and magnetic permeability are measured.

[0052] The composition, coercive force, average particle size D50, aspect ratio, bulk density / true density of the flat powders of Examples 1 to 12 and Comparative Examples 1 to 6, and the coercive force, real magnetic permeability at 0°C, imaginary magnetic permeability at 0°C, and temperature coefficient in each temperature range in the resin composite sheet are collectively shown in Table 1. The real magnetic permeability is set to the value at 1 MHz, and the imaginary magnetic permeability is set to the value at 500 MHz.

[0053] The soft magnetic flat metal obtained in Examples 13 to 14 and Comparative Examples 7 to 8 and polyamide 12 were used and heated and kneaded using a biaxial kneading machine to obtain a resin composite composition. The soft magnetic flat powder used was one that had been surface-treated in advance with a silane coupling agent. Next, an injection molding machine was used to mold it into a ring shape with an outer shape of 20 mm, an inner diameter of 10 mm, and a thickness of 1 mm, and the coercive force and magnetic permeability were measured.

[0054] The flat powder composition, coercive force, aspect ratio, and flat powder dosage in the resin composite composition used in the above-mentioned Examples 13 to 14 and Comparative Examples 7 to 8, the coercive force in the molded body, the real magnetic permeability at 0°C, the imaginary magnetic permeability at 0°C, and the temperature coefficient in each temperature range are collectively shown in Tables 2 and 3.

[0055] Table 1

[0056]

[0057] According to Table 1, in Examples 1 to 12, the temperature coefficient K of the real and imaginary permeabilities is positive at -40°C to 85°C, and the real and imaginary permeabilities are higher than those of Comparative Examples 1 to 5 at 0°C. In the Fe-5.4wt%Al-9.6wt%Si composition of Comparative Example 6, the real and imaginary permeabilities are high at 0°C, but when it exceeds 0°C, the temperature coefficient becomes negative, and the real and imaginary permeabilities decrease sharply. In addition, in the Fe-5.4wt%Al-9.6wt%Si composition, Figure 1 As shown, the higher the real permeability at 0°C, the more significant the decrease in the real permeability at 85°C.

[0058] When comparing the real permeabilities at 85°C, Examples 1 to 12 all have a real permeability of 200 or more, but Comparative Example 6 has a real permeability of 145, which is a large difference. Figure 2 As shown, even if the Fe—Al—Si alloy composition is adjusted outside the range of this embodiment, the temperature coefficient of the real magnetic permeability can be adjusted, but the real magnetic permeability at 0° C. is too low to meet the demand for higher magnetic permeability.

[0059] Table 2

[0060]

[0061] Table 3

[0062]

[0063] According to Tables 2 and 3, in the injection molded bodies of the resin composite compositions, the temperature coefficients K of the real and imaginary magnetic permeabilities of Examples 13 to 14 are positive at -40°C to 85°C. In addition, when the temperature exceeds 0°C, Fe-5.4wt%Al-9.6wt%Si of Comparative Example 7 exhibits a negative temperature coefficient, and therefore the magnetic permeability at 85°C decreases to 70. The powder blending amount of Comparative Example 8 is too large to be molded, and thus it is described as being unmoldable.

Claims

1. A soft magnetic metal flat powder, characterized in that: It is a soft magnetic flat metal powder composed of Fe-Al-Si, the temperature coefficient K of its magnetic permeability satisfies the following formula (1), (2), (3) in the range of -40°C to 85°C, the coercive force is less than 70 A / m, The powder having a particle size near the average particle size D50 is flat with an aspect ratio of 20 to 200, and its composition contains Al: 6 to 7.5 wt%, Si: 8.5 to 9.5 wt%, and the remainder is composed of Fe and inevitable impurities, wherein the total content of Al and Si is 15 to 16.5 wt%, The ratio of bulk density / true density is in the range of 0.036 to 0.086; K=(μ(0℃)-μ(-40℃)) / μ(-40℃)>0 (1) K=(μ(40℃)-μ(0℃)) / μ(0℃)>0 (2) K=(μ(85℃)-μ(40℃)) / μ(40℃)>0 (3) K is the temperature coefficient, μ is the magnetic permeability and includes the real magnetic permeability μ' and the imaginary magnetic permeability μ".

2. The soft magnetic flat metal powder according to claim 1, characterized in that: In the soft magnetic flat metal powder, the aspect ratio of the powder having a particle size near the average particle size D50 is 30 to 150, and the total content of Al and Si is 15.5 to 16 wt %.

3. A resin composite sheet, characterized in that , The invention comprises the flat soft magnetic metal powder according to any one of claims 1 and 2 and a resin, and has a coercive force of 80 A / m or less.

4. A resin composite composition for injection molding and extrusion molding, characterized in that: The invention comprises the flat soft magnetic metal powder according to any one of claims 1 and 2 and a resin.

Citation Information

Patent Citations

  • Soft magnetic powder for noise suppression, production method therefor and noise suppression sheet using the same

    JP2005281783A

  • Improvements in or relating to magnetic dust cores

    GB527874A

  • Magnetic element and its manufacturing method

    JP2002093612A

  • Flat soft magnetic material, and manufacturing method thereof

    JP2009266960A

  • Method for producing flattened soft magnetic powder, flattened soft magnetic powder and electromagnetic wave absorber

    JP2010196123A