Anisotropic bonded magnet and preparation method thereof
By stacking magnet preforms with different SmFeN contents and densities in high aspect ratio magnets, and adjusting the performance distribution during warm-pressure magnetic field orientation molding, the problem of axial density non-uniformity is solved and the performance of the magnets is improved. Uniformity and dimensional accuracy.
Patent Information
- Application Number
- CN202010483305.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-06-01
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-06-01
Smart Images

Figure CN113764148B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bonded magnet materials, and in particular to an anisotropic bonded magnet and a preparation method thereof. Background Art
[0002] Bonded permanent magnets have good processing properties, large shape freedom, high dimensional accuracy, and no need for secondary processing. They have become an indispensable component of modern high-tech products and are widely used in electronic information, computers, motors, automobiles, etc. Anisotropic bonded magnets have more excellent magnetic properties and can effectively promote the miniaturization, high efficiency, energy saving, and lightweight of electronic products, and have become the development direction of bonded permanent magnets.
[0003] The molding methods of bonded permanent magnets include compression molding, calendering molding, injection molding and extrusion molding. Among them, compression molding magnets are the most widely used due to their highest magnetic properties.
[0004] The basic process flow of preparing anisotropic bonded magnets by compression molding using thermosetting resin is as follows:
[0005] Magnetic powder is mixed with binder and additives to obtain composite magnetic powder → orientation pressing → demagnetization → curing → anti-corrosion treatment → performance testing, where additives refer to lubricants, coupling agents, etc.: binders generally use thermosetting resins such as epoxy resins and phenolic resins. The orientation forming process can be carried out in three ways: room temperature forming, warm pressing forming and multi-step forming. The preparation of anisotropic bonded magnets by room temperature forming has low magnetic properties due to the low density and poor orientation of the magnets. During the warm pressing forming process, the high temperature softens the binder and melts it into a viscous flow state. Its low viscosity plays a certain lubricating role, achieving the purpose of reducing the rotation resistance of the magnetic powder particles during orientation and the friction resistance between the magnetic powder and the mold wall, thereby effectively improving the orientation and density of the magnet. At present, warm pressing forming technology is widely used in the preparation of anisotropic bonded magnets. Therefore, improving the orientation and density is the key to preparing anisotropic bonded permanent magnets.
[0006] In the prior art, CN101599333A provides a method for manufacturing a dry-pressed anisotropic multipolar magnetic ring, which comprises wet-crushing magnetic powder, adding one or more adhesives and lubricants to the dried magnetic powder; then pre-pressing and pre-magnetizing, and then mixing with a high-speed crusher, and finally double-sided isostatic pressing of the aforementioned powder in a radial magnetic field.
[0007] CN101814368A provides a method for preparing anisotropic magnets: adjusting the powder particle size, wherein the first mixture is composed of a first magnetic powder with a particle size greater than 20μm and less than 150μm, a thermosetting resin with an addition amount of less than 2.0wt% in the anisotropic bonded magnet, and a first additive, and the second mixture is composed of a second magnetic powder with a particle size greater than 1μm and less than 20μm and a second additive, which is used to improve the density and magnetic properties of the magnet, but the magnetic field strength at the center of the magnet differs by more than 5% from that at the end.
[0008] CN103489621A provides a method for preparing a molded anisotropic bonded magnet, which adopts a two-step molding process, namely, room temperature preforming and orientation densification warm pressing molding process to prepare the anisotropic bonded magnet. During the orientation densification process, there will be a phenomenon of highly directional magnetic field orientation and uneven density, resulting in a phenomenon of low in the middle and high on both sides.
[0009] CN107393709A provides a method for preparing a highly oriented anisotropic bonded magnet by cold isostatic pressing, wherein a thermosetting resin and a curing agent are made into a binder, anisotropic bonded magnetic powder is added to the binder solution, and the mixture is fully stirred and then injected into a silicone mold, which is vacuum sealed and oriented in a 1.5T to 2T magnetic field, and then cold isostatic pressing is performed to prepare the magnet.
[0010] In industrial production, for magnetic rings with high aspect ratio, the existing technology of directly filling the high-temperature magnetic field cavity with magnetic powder will result in a high height of the magnetic powder in the cavity, which is easy to cause uneven magnetic field orientation along the height direction. In addition, the mixed magnetic powder is heated during high-temperature filling, which is easy to cause the magnetic powder to stick to the wall, making it difficult to ensure the uniformity of the filling, affecting the uniformity of the magnetic properties and dimensional accuracy of the magnet. Summary of the invention
[0011] The purpose of the present invention is to address the problem of uneven performance caused by low density in the middle and high density at both ends or at the periphery in the axial direction during the preparation of a high aspect ratio magnet, by stacking multiple magnets and mixing SmFeN powder into the magnets, wherein the SmFeN powder content in the middle is high and the SmFeN powder content at both ends or at the periphery is low, so as to compensate for the performance deviation caused by the density difference during the pressing process and improve the uniformity of the performance of the magnet in the axial direction.
[0012] In order to achieve the above purpose, the present invention adopts the following scheme:
[0013] A first aspect of the present invention provides an anisotropic bonded magnet, comprising RTB permanent magnet powder and SmFeN permanent magnet powder.
[0014] Among them, in the RTB permanent magnet powder, the content of R is 28-31wt.%, the content of B is 0.9-1.1wt.%, and the balance is T; R is selected from one or more rare earth elements, T is Fe or FeCo and transition metals, and B is boron;
[0015] The weight content of SmFeN permanent magnet powder is 3% to 40% of the RTB permanent magnet powder;
[0016] The anisotropic bonded magnet is formed by pressing a plurality of different preformed bodies, and the density deviation of the obtained anisotropic bonded magnet along the pressing direction is less than 2%.
[0017] Furthermore, the plurality of different preforms include preforms having different contents of SmFeN permanent magnet powder.
[0018] Furthermore, R is one or more elements selected from the group consisting of Y, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Ho, Er, Tm, Yb, and Lu, and is preferably Nd or PrNd.
[0019] Furthermore, the bonded magnet is a bonded magnetic ring, the aspect ratio of the bonded magnetic ring is greater than 0.6, preferably 1.0-10, more preferably 2-8; the wall thickness is greater than 1 mm, preferably 1-20 mm, more preferably 1-5 mm.
[0020] Furthermore, the particle size of the SmFeN permanent magnet powder is 1 to 30 μm, preferably 3 to 10 μm.
[0021] A second aspect of the present invention provides a method for preparing anisotropic bonded magnets, comprising the following steps:
[0022] Step 1, preparing bonded magnet raw materials: the raw materials include RTB permanent magnet powder, SmFeN permanent magnet powder, thermosetting resin binder, coupling agent and lubricant; wherein the weight content of RTB permanent magnet powder and SmFeN permanent magnet powder is 100, and SmFeN permanent magnet powder is 3% to 40% of the weight content of RTB permanent magnet powder; the weight content of binder is 1.0% to 6.0% of RTB permanent magnet powder and SmFeN permanent magnet powder, preferably 2.5% to 3.5%, the weight content of coupling agent is 0.05% to 1.0% of RTB permanent magnet powder and SmFeN permanent magnet powder, preferably 0.1% to 0.3%, and the weight content of lubricant is 0.05% to 2.0% of RTB permanent magnet powder and SmFeN permanent magnet powder, preferably 0.05% to 0.50%;
[0023] Step 2, mixing: uniformly mixing the RTB permanent magnet powder and SmFeN permanent magnet powder in the raw materials with the thermosetting resin binder, coupling agent and lubricant to obtain composite magnetic powder;
[0024] Step 3: Preforming at room temperature: Place the dried composite magnetic powders with different magnetic properties in the first mold and place them in a magnetic field H. 1 A variety of different preforms are obtained by press forming, wherein the pressing pressure is 100-600 MPa, and the magnetic field H 1 Less than 0.15T, pressing temperature is room temperature;
[0025] Step 4: Warm-press magnetic field orientation molding: Place a stack of several different preforms in a second mold and place them in a magnetic field H. 2 The magnet is oriented by medium temperature pressing, and then pressed again; then demagnetized, cooled, and demolded to obtain anisotropic bonded magnets oriented by temperature pressing magnetic field; wherein the magnetic field intensity H 2 The temperature is 0.6~3T, the pressing pressure is 300~1000MPa, and the molding temperature is 60~200℃;
[0026] Step 5, curing: heating the anisotropic bonded magnet formed by warm-pressing magnetic field orientation to a certain temperature and then keeping it warm, the warming temperature is 100-200° C., preferably 120-180° C.; the warming time is 0.5-2 hours.
[0027] Furthermore, the step 2 comprises:
[0028] The coupling agent measured in the above step is dissolved in the corresponding organic solvent, and then mixed evenly with the RTB permanent magnet powder and the SmFeN permanent magnet powder. After the organic solvent is volatilized and removed, the coupling agent is evenly coated on the surface of the permanent magnet powder. Then, the measured binder and lubricant are dissolved in the corresponding organic solvent, and mixed evenly with the RTB permanent magnet powder and the SmFeN permanent magnet powder coated with the coupling agent. After the organic solvent is removed, the composite magnetic powder required for preparing the bonded magnet is obtained.
[0029] Furthermore, the plurality of different preformed bodies include a first preformed body and a second preformed body; the first preformed body is made of composite magnetic powder with a low content of SmFeN permanent magnetic powder, and the second preformed body is made of composite magnetic powder with a high content of SmFeN permanent magnetic powder; wherein the mass percentage of SmFeN in the composite magnetic powder with a low content of SmFeN permanent magnetic powder is 3 to 15%, preferably 5 to 13%, and the mass percentage of SmFeN in the composite magnetic powder with a high content of SmFeN permanent magnetic powder is 15 to 40%, preferably 15 to 30%.
[0030] Furthermore, the density of the first preform is less than the density of the second preform, and the ratio of the density of the first preform is 1:1.1 to 1:1.5.
[0031] Furthermore, in step 4, stacking a plurality of different preforms into the second mold includes: a second preform in the middle, first preforms at both ends, and the length of the second preform in the middle is less than the length of the first preforms at both ends.
[0032] Furthermore, in step 4, stacking a plurality of different preformed bodies and placing them in the second mold includes: the center is the second preformed body and the periphery is the first preformed body.
[0033] Furthermore, stacking a plurality of different preforms into the second mold includes: the density and / or SmFeN content of the preforms arranged from the middle to the two ends gradually decreases; or the density and / or SmFeN content of the preforms arranged from the center to the periphery gradually decreases.
[0034] Furthermore, in step 4, the gap ratio between the preformed body and the warm-pressing magnetic field orientation forming die is 0.5% to 40%, preferably 3.5% to 25%.
[0035] Furthermore, the first preformed body and the second preformed body are magnetic cylinders or magnetic rings of the same shape, and the number ratio of the first preformed body to the second preformed body is 1:1 to 10:1.
[0036] In summary, the present invention provides an anisotropic bonded magnet and a method for preparing the same. By stacking magnets with different SmFeN contents and / or densities, the magnets in the middle have high performance and the magnets at both ends and / or the periphery have low performance, thereby compensating for the performance deviation caused by density differences during the pressing process and improving the performance uniformity of the magnet in the axial direction. This method solves the problem of highly directional magnetic field orientation and uneven density during the orientation and densification process, as well as the problem of low in the middle and high on both sides. The anisotropic bonded magnet prepared by this method has the characteristic of a density deviation of less than 2% along the pressing direction, which effectively improves the orientation and density of the magnet, as well as the uniformity and dimensional accuracy of the magnetic properties of the magnet. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a schematic flow chart of a method for preparing anisotropic bonded magnets according to an embodiment of the present invention. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0039] The first aspect of the present invention provides an anisotropic rare earth bonded magnet. The bonded magnet comprises RTB permanent magnet powder and SmFeN permanent magnet powder prepared by the HDDR method, wherein the content of R in the RTB permanent magnet powder is 28-31wt.%; the content of B is 0.9-1.1wt.%, and the balance is T; R is selected from one or more rare earth elements, T is Fe or FeCo and a small amount of transition metals, and the content of transition metals is less than 3%; B is boron. The weight content of SmFeN permanent magnet powder is 5% to 30% of the RTB permanent magnet powder; the anisotropic bonded magnet is formed by pressing a plurality of different preforms, and the density deviation of the obtained anisotropic bonded magnet along the pressing direction is less than 2%.
[0040] Furthermore, the plurality of different preforms include preforms having different contents of SmFeN permanent magnet powder.
[0041] Furthermore, the rare earth element R constituting the RTB permanent magnet powder of the present invention can be one or more selected from Y, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Ho, Er, Tm, Yb, and Lu. From the perspective of cost and magnetic properties, Nd or PrNd is preferably used.
[0042] The element T constituting the RTB rare earth magnet powder of the present invention is Fe or FeCo. The T amount of the average composition of the powder is the remainder after removing other elements constituting the powder. In addition, the Curie temperature can be increased by adding Co as an element replacing Fe, but too much will cause the residual magnetic flux density of the powder to decrease. Adding transition elements as elements replacing Fe can increase the residual magnetic flux density Br, but too much will passivate the hydrogenation reaction in the HDDR process and affect the magnetic properties.
[0043] Furthermore, the bonded magnet can have various shapes. The following is a further explanation using a bonded magnetic ring as an example, but it is not limited to a bonded magnetic ring. The density of the bonded magnetic ring determines its magnetic properties. For a magnetic ring with a length-to-diameter ratio, the pressing process of the magnetic ring determines that the axial density will have deviations. The density deviation will cause the magnetic ring to have uneven axial magnetic properties, thereby affecting the output stability of the motor after the magnetic ring is assembled. The density deviation of the bonded magnetic ring of the present invention along the pressing direction is less than 2%, which fully guarantees the performance uniformity of the magnetic ring and the output stability of the motor after assembly. The bonded magnetic ring constituting the present invention has an aspect ratio greater than 0.6, preferably 1.0-10, and more preferably 2-8, because for a magnetic ring with a small aspect ratio (less than 0.6), the density deviation in the pressing direction is small, which can be accomplished in the prior art. If the aspect ratio of the magnetic ring is too large (greater than 10), it will bring greater difficulties to the molding of the magnetic ring and the subsequent equipment process.
[0044] Furthermore, the wall thickness of the bonded magnetic ring constituting the present invention is greater than 1 mm, preferably 1-20 mm, and more preferably 1-5 mm. If the wall thickness of the magnetic ring is too thin (less than 1 mm), the preparation process of the magnetic ring is difficult and it is easy to be damaged; if the wall thickness of the magnetic ring is too thick (greater than 20 mm), the bonding strength is too weak due to the lack of radial compression. Too thick a wall thickness is not conducive to the overall molding of the magnetic ring. At the same time, too thick a wall thickness does not conform to the trend of lightweighting, which limits its assembly process and application areas.
[0045] Furthermore, the particle size of the SmFeN permanent magnet powder is 1 to 30 μm, preferably 3 to 10 μm. If the particle size of the SmFeN permanent magnet powder is too fine (less than 1 μm), the magnetic properties will be significantly reduced, and the preparation will be difficult and easy to oxidize. If the particle size of the SmFeN permanent magnet powder is too coarse (>30 μm), it will not be able to effectively fill the gaps between the NdFeB powders during the pressing process, resulting in a low pressing density.
[0046] The second aspect of the present invention provides a method for preparing anisotropic bonded magnets, which is used to make the above-mentioned anisotropic bonded magnets. The method adopts a two-step molding process, namely room temperature preforming and oriented warm pressing to prepare anisotropic bonded magnetic rings (hereinafter, the anisotropic bonded magnets in the present invention use magnetic rings as specific embodiments, but are not limited to magnetic ring structures), wherein the room temperature preforming process prepares several pre-pressed magnetic rings with different properties, and in the oriented warm pressing process, multiple pre-pressed magnetic rings are stacked and pressed, wherein the magnetic ring in the middle has high performance and the performance of the two sides is low. Specifically, it includes the following process steps, such as Figure 1 As shown:
[0047] Step 1: Prepare the raw materials for bonding magnetic rings:
[0048] The raw materials of bonded magnetic rings are RTB permanent magnet powder, SmFeN permanent magnet powder, thermosetting resin binder, coupling agent and lubricant.
[0049] The rare earth element R constituting the RTB permanent magnet powder of the present invention can be selected from one or more of Y, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Ho, Er, Tm, Yb, and Lu. In view of cost and magnetic properties, Nd or PrNd is preferably used. The element T constituting the RTB rare earth magnet powder is Fe or FeCo; the thermosetting resin binder is a thermosetting resin such as epoxy resin and phenolic resin; the coupling agent is a silane coupling agent, titanate, etc. The lubricant is paraffin, stearate, silicone oil, etc.
[0050] Taking the weight content of RTB permanent magnet powder and SmFeN permanent magnet powder as 100, SmFeN permanent magnet powder accounts for 3% to 40% of the weight content of RTB permanent magnet powder; the weight content of binder accounts for 1.0% to 6.0% of RTB permanent magnet powder and SmFeN permanent magnet powder, preferably 2.5% to 3.5%; the weight content of coupling agent accounts for 0.05% to 1.0% of RTB permanent magnet powder and SmFeN permanent magnet powder, preferably 0.1% to 0.3%; the weight content of lubricant accounts for 0.05% to 2.0% of RTB permanent magnet powder and SmFeN permanent magnet powder, preferably 0.05% to 0.50%.
[0051] Step 2, mixing: uniformly mixing the RTB permanent magnet powder and SmFeN permanent magnet powder in the raw materials with the thermosetting resin binder, coupling agent and lubricant to obtain composite magnetic powder.
[0052] Specifically, the coupling agent measured in the above step is dissolved in a corresponding organic solvent, and then mixed evenly with the RTB permanent magnet powder and the SmFeN permanent magnet powder. After the organic solvent is evaporated and removed, the coupling agent is evenly coated on the surface of the anisotropic magnetic powder. Subsequently, the measured binder and lubricant are dissolved in a corresponding solvent, and then mixed evenly with the RTB permanent magnet powder coated with the coupling agent. After the organic solvent is removed, the composite magnetic powder used to prepare the bonded magnet can be obtained.
[0053] A variety of composite magnetic powders with different magnetic properties (different SmFeN contents) and / or densities are produced.
[0054] Step 3: Preforming at room temperature:
[0055] The dried composite magnetic powders are placed in the mold cavity and placed in the magnetic field H. 1 A variety of different preforms are obtained by pressing, wherein the pressing pressure is 100-600 MPa, and the magnetic field H 1 Less than 0.15T, the molding temperature is room temperature;
[0056] The preform body density is 3.6-5.0 g / cm 3 Since the strength of the preform decreases with the decrease of density, when the density is lower than 3.6g / cm 3 When the density is higher than 5.0g / cm 3 It is difficult to obtain a high degree of orientation in the subsequent temperature-pressure magnetic field orientation process.
[0057] Specifically, the preformed compacts are divided into two categories, one is a composite magnetic powder with a low SmFeN permanent magnetic powder content, and the other is a composite magnetic powder with a low SmFeN permanent magnetic powder content. The SmFeN content of the composite magnetic powder with a low SmFeN content is 3% to 15%, preferably 5 to 13%, and the SmFeN content of the composite magnetic powder with a high SmFeN content is 15% to 40%, preferably 15 to 30%.
[0058] Specifically, the preformed bodies are divided into two categories, including a first preformed body and a second preformed body; the density of the first preformed body is less than the density of the second preformed body, and the ratio of the two densities is 1:1.1 to 1:1.5.
[0059] Furthermore, the first preformed body and the second preformed body are magnetic cylinders or magnetic rings of the same shape, and the number ratio of the first preformed body to the second preformed body is 1:1 to 10:1.
[0060] Step 4: Warm-pressing magnetic field orientation molding:
[0061] A stack of several demoulded preforms of different types is placed in another mold and placed in a magnetic field H. 2 The medium temperature pressing orientation is performed, wherein the middle part is a green body with high performance and the two sides are green bodies with low performance; or the center part is a green body with high performance and the periphery part is a green body with low performance, and the pressing is performed again. Specifically, the density and / or SmFeN content of the preformed green bodies arranged from the middle to the two ends gradually decreases; or the density and / or SmFeN content of the preformed green bodies arranged from the center to the periphery gradually decreases.
[0062] During the stacking process of the preformed bodies, they are positioned by mutual magnetic attraction.
[0063] During the preform stacking process, the length of the middle preform is smaller than the upper and lower preforms; specifically, the length of the middle preform is smaller than the length of the preforms at each end.
[0064] Wherein, the magnetic field strength H 2The temperature is 0.6-3T, the pressing pressure is 300-1000MPa, the molding temperature is 60-200°C, the gap ratio is 0.5-40%, and the gap between the preformed body and the warm-pressing magnetic field orientation molding die is preferably 3.5%-25% in terms of the two-step operation process and the improvement of magnetic properties;
[0065] Subsequently, demagnetization, cooling, and demoulding are performed to obtain anisotropic bonded magnetic rings. The demagnetization method is one of AC pulse demagnetization and reverse pulse demagnetization.
[0066] Step 5: Curing:
[0067] The curing process is: heating the final formed body to a certain temperature and then keeping it warm to further improve the strength of the bonded magnetic ring, wherein the warming temperature is generally 100-200°C, preferably 120-180°C; the warming time is generally 0.5-2 hours, which can be appropriately adjusted according to the size of the magnetic ring.
[0068] Specific embodiments of the present invention are described below, but the present invention is by no means limited to the described embodiments.
[0069] Example 1
[0070] (1) Prepare the raw materials for bonding magnetic rings
[0071] NdFeB anisotropic permanent magnet powder with a Nd content of 29.5 wt.%, SmFeN anisotropic permanent magnet powder, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate are prepared.
[0072] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, there are two batches of SmFeN anisotropic permanent magnet powder with different contents, the first batch has a SmFeN mass percentage content of 9%, and the second batch has a SmFeN mass percentage content of 23%. Taking the total weight content of NdFeB and SmFeN anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3%, the weight content of silane is 0.2%, and the weight content of zinc stearate is 0.25%.
[0073] (2) Rubber mixing
[0074] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of anisotropic permanent magnetic powders with different SmFeN contents, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the anisotropic permanent magnetic powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.
[0075] (3) Room temperature preforming
[0076] The two composite magnetic powders prepared above are dried and placed in a mold cavity under a magnetic field H. 1 =0 to obtain different preforms, wherein the pressing pressure is 350 MPa, and the SmFeN contents in the first and second preforms are 9% and 23% respectively.
[0077] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 2 mm. According to actual conditions, the quantity ratio of the first preformed bodies to the second preformed bodies is 2:1.
[0078] (4) Warm pressure magnetic field orientation molding:
[0079] The above different preforms are stacked in another mold and placed in a magnetic field H. 2 (2.5T) Medium temperature pressing orientation, the pressing pressure is 700MPa, the forming temperature is 150℃, the gap rate between the blank and the mold cavity is 5%, the middle one is the second preformed blank with high performance and higher density, the two sides are the first preformed blanks with lower performance and density, and the height of the first preformed blank is greater than that of the second preformed blank. The blanks are positioned by mutual magnetic adsorption for warm pressing orientation pressing.
[0080] Subsequently, demagnetization, cooling and demoulding are performed to obtain anisotropic bonded magnetic rings.
[0081] (5) Curing:
[0082] The final molded body obtained above is heated to 160° C. for curing and kept at this temperature for 1 hour, thereby completing the preparation of the anisotropic magnetic ring.
[0083] Example 2
[0084] (1) Prepare the raw materials for bonding magnetic rings
[0085] NdFeB anisotropic permanent magnet powder with a Nd content of 29.5 wt.%, SmFeN anisotropic permanent magnet powder, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate are prepared.
[0086] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, there are two batches of SmFeN anisotropic permanent magnet powder with different contents, the first batch has a SmFeN mass percentage content of 5%, and the second batch has a SmFeN mass percentage content of 23%. Taking the total weight content of NdFeB and SmFeN anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3%, the weight content of silane is 0.2%, and the weight content of zinc stearate is 0.25%.
[0087] (2) Rubber mixing
[0088] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of anisotropic permanent magnetic powders with different SmFeN contents, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the anisotropic permanent magnetic powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.
[0089] (3) Room temperature preforming
[0090] The two composite magnetic powders prepared above are dried and placed in a mold cavity under a magnetic field H. 1 =0 to obtain different preforms, wherein the pressing pressure is 350 MPa, and the SmFeN contents in the first and second preforms are 5% and 23% respectively.
[0091] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 2 mm. According to actual conditions, the quantity ratio of the first preformed bodies to the second preformed bodies is 2:1.
[0092] The other steps are the same as those in Example 1
[0093] Example 3
[0094] (1) Prepare the raw materials for bonding magnetic rings
[0095] NdFeB anisotropic permanent magnet powder with a Nd content of 29.5 wt.%, SmFeN anisotropic permanent magnet powder, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate are prepared.
[0096] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, there are two batches of SmFeN anisotropic permanent magnet powder with different contents, the mass percentage of SmFeN in the first batch is 15%, and the mass percentage of SmFeN in the second batch is 23%. Taking the total weight content of NdFeB and SmFeN anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3% of the weight of NdFeB anisotropic permanent magnet powder; the weight content of silane is 0.2% of the weight of NdFeB anisotropic permanent magnet powder, and the weight content of zinc stearate is 0.25% of the weight of NdFeB anisotropic permanent magnet powder.
[0097] (2) Rubber mixing
[0098] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of anisotropic permanent magnetic powders with different SmFeN contents, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the anisotropic permanent magnetic powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.
[0099] (3) Room temperature preforming
[0100] The two composite magnetic powders prepared above are dried and placed in a mold cavity under a magnetic field H. 1 =0 to obtain different preforms, wherein the pressing pressure is 350 MPa, and the SmFeN contents in the first and second preforms are 15% and 23% respectively.
[0101] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 2 mm. According to actual conditions, the quantity ratio of the first preformed bodies to the second preformed bodies is 2:1.
[0102] The other steps are the same as those in Example 1
[0103] Example 4
[0104] (1) Prepare the raw materials for bonding magnetic rings
[0105] NdFeB anisotropic permanent magnet powder with a Nd content of 29.5 wt.%, SmFeN anisotropic permanent magnet powder, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate are prepared.
[0106] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, there are two batches of SmFeN anisotropic permanent magnet powder with different contents, the first batch has a SmFeN mass percentage content of 9%, and the second batch has a SmFeN mass percentage content of 15%. Taking the total weight content of NdFeB and SmFeN anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3%, the weight content of silane is 0.2%, and the weight content of zinc stearate is 0.25%.
[0107] (2) Rubber mixing
[0108] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of anisotropic permanent magnetic powders with different SmFeN contents, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the anisotropic permanent magnetic powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.
[0109] (3) Room temperature preforming
[0110] The two composite magnetic powders prepared above are dried and placed in a mold cavity under a magnetic field H. 1 =0 to obtain different preforms, wherein the pressing pressure is 350 MPa, and the SmFeN contents in the first and second preforms are 9% and 15% respectively.
[0111] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 2 mm. According to actual conditions, the quantity ratio of the first preformed bodies to the second preformed bodies is 2:1.
[0112] The other steps are the same as those in Example 1
[0113] Example 5
[0114] (4) Prepare the raw materials for bonding magnetic rings
[0115] NdFeB anisotropic permanent magnet powder with a Nd content of 29.5 wt.%, SmFeN anisotropic permanent magnet powder, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate are prepared.
[0116] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, there are two batches of SmFeN anisotropic permanent magnet powder with different contents, the first batch has a SmFeN mass percentage content of 9%, and the second batch has a SmFeN mass percentage content of 25%. Taking the total weight content of NdFeB and SmFeN anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3%; the weight content of silane is 0.2%, and the weight content of zinc stearate is 0.25%.
[0117] (5) Rubber mixing
[0118] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of anisotropic permanent magnetic powders with different SmFeN contents, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the anisotropic permanent magnetic powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.
[0119] (6) Room temperature preforming
[0120] The two composite magnetic powders prepared above are dried and placed in a mold cavity under a magnetic field H. 1 =0 to obtain different preforms, wherein the pressing pressure is 350 MPa, and the SmFeN contents in the first and second preforms are 9% and 25% respectively.
[0121] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 2 mm. According to actual conditions, the quantity ratio of the first preformed bodies to the second preformed bodies is 2:1.
[0122] The other steps are the same as those in Example 1
[0123] Example 6
[0124] (1) Prepare the raw materials for bonding magnetic rings
[0125] NdFeB anisotropic permanent magnet powder with a Nd content of 29.5 wt.%, SmFeN anisotropic permanent magnet powder, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate are prepared.
[0126] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, there are two batches of SmFeN anisotropic permanent magnet powder with different contents, the first batch has a SmFeN mass percentage content of 9%, and the second batch has a SmFeN mass percentage content of 23%. Taking the total weight content of NdFeB and SmFeN anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 1%; the weight content of silane is 0.2%, and the weight content of zinc stearate is 0.25%.
[0127] The other steps are the same as those in Example 1
[0128] Example 7
[0129] (2) Prepare the raw materials for bonding magnetic rings
[0130] NdFeB anisotropic permanent magnet powder with a Nd content of 29.5 wt.%, SmFeN anisotropic permanent magnet powder, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate are prepared.
[0131] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, there are two batches of SmFeN anisotropic permanent magnet powder with different contents, the first batch has a SmFeN mass percentage content of 9%, and the second batch has a SmFeN mass percentage content of 23%. Taking the total weight content of NdFeB and SmFeN anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 5%, the weight content of silane is 0.2%, and the weight content of zinc stearate is 0.25%.
[0132] The other steps are the same as those in Example 1
[0133] Example 8
[0134] (1) Prepare the raw materials for bonding magnetic rings
[0135] NdFeB anisotropic permanent magnet powder with a Nd content of 29.5 wt.%, SmFeN anisotropic permanent magnet powder, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate are prepared.
[0136] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, there are two batches of SmFeN anisotropic permanent magnet powder with different contents, the first batch has a SmFeN mass percentage content of 9%, and the second batch has a SmFeN mass percentage content of 23%. Taking the total weight content of NdFeB and SmFeN anisotropic permanent magnet powder as 100, and the total weight content of NdFeB and SmFeN anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3%; the weight content of silane is 0.2%, and the weight content of zinc stearate is 0.25%.
[0137] (2) Rubber mixing
[0138] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of anisotropic permanent magnetic powders with different SmFeN contents, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the anisotropic permanent magnetic powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.
[0139] (3) Room temperature preforming
[0140] The two composite magnetic powders prepared above are dried and placed in a mold cavity under a magnetic field H. 1 =0 to obtain different preforms, wherein the pressing pressure is 350 MPa, and the SmFeN contents in the first and second preforms are 9% and 23% respectively.
[0141] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 2 mm. According to actual conditions, the quantity ratio of the first preformed bodies to the second preformed bodies is 2:1.
[0142] (4) Warm pressure magnetic field orientation molding:
[0143] The above different preforms are stacked in another mold and placed in a magnetic field H. 2 (2.5T) Medium temperature pressing orientation, the pressing pressure is 700MPa, the forming temperature is 150℃, the gap rate between the blank and the mold cavity is 5%, the middle one is the second preformed blank with high performance and higher density, the two sides are the first preformed blanks with lower performance and density, and the height of the first preformed blank is greater than that of the second preformed blank. The blanks are positioned by mutual magnetic adsorption for warm pressing orientation pressing.
[0144] Subsequently, demagnetization, cooling and demoulding are performed to obtain anisotropic bonded magnetic rings.
[0145] (5) Curing:
[0146] The final molded body obtained above is heated to 120° C. for curing and kept at this temperature for 1 hour to complete the preparation of the anisotropic magnetic ring.
[0147] The other steps are the same as those in Example 1
[0148] Example 9
[0149] (1) Prepare the raw materials for bonding magnetic rings
[0150] NdFeB anisotropic permanent magnet powder with a Nd content of 29.5 wt.%, SmFeN anisotropic permanent magnet powder, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate are prepared.
[0151] Taking the weight content of NdFeB anisotropic permanent magnet powder as 100, there are two batches of SmFeN anisotropic permanent magnet powder with different contents, the first batch has a SmFeN mass percentage content of 9%, and the second batch has a SmFeN mass percentage content of 23%. Taking the total weight content of NdFeB and SmFeN anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3%, the weight content of silane is 0.2%, and the weight content of zinc stearate is 0.25%.
[0152] (2) Rubber mixing
[0153] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of anisotropic permanent magnetic powders with different SmFeN contents, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the anisotropic permanent magnetic powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.
[0154] (3) Room temperature preforming
[0155] The two composite magnetic powders prepared above are dried and placed in a mold cavity under a magnetic field H. 1 =0 to obtain different preforms, wherein the pressing pressure is 350 MPa, and the SmFeN contents in the first and second preforms are 5% and 13% respectively.
[0156] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 2 mm. According to actual conditions, the quantity ratio of the first preformed bodies to the second preformed bodies is 2:1.
[0157] (4) Warm pressure magnetic field orientation molding:
[0158] The above different preforms are stacked in another mold and placed in a magnetic field H. 2 (2.5T) Medium temperature pressing orientation, the pressing pressure is 700MPa, the forming temperature is 150℃, the gap rate between the blank and the mold cavity is 5%, the middle one is the second preformed blank with high performance and higher density, the two sides are the first preformed blanks with lower performance and density, and the height of the first preformed blank is greater than that of the second preformed blank. The blanks are positioned by mutual magnetic adsorption for warm pressing orientation pressing.
[0159] Subsequently, demagnetization, cooling and demoulding are performed to obtain anisotropic bonded magnetic rings.
[0160] (5) Curing:
[0161] The final molded body obtained above is heated to 180° C. for curing and kept at this temperature for 1 hour to complete the preparation of the anisotropic magnetic ring.
[0162] The other steps are the same as those in Example 1
[0163] Comparative Example 1
[0164] (1) Prepare the raw materials for bonding magnetic rings
[0165] NdFeB anisotropic permanent magnet powder with a Nd content of 29.5 wt.%, SmFeN anisotropic permanent magnet powder, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate are prepared.
[0166] Based on the weight content of NdFeB anisotropic permanent magnet powder as 100, the mass percentage content of SmFeN is 3%. Based on the total weight content of NdFeB and SmFeN anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3%, the weight content of silane is 0.2%, and the weight content of zinc stearate is 0.25%.
[0167] (2) Rubber mixing
[0168] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of anisotropic permanent magnetic powders with different SmFeN contents, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the anisotropic permanent magnetic powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.
[0169] (3) Room temperature preforming
[0170] The two composite magnetic powders prepared above are dried and placed in a mold cavity under a magnetic field H. 1 =0 and press-formed to obtain a preformed body, wherein the pressing pressure is 350 MPa and the content of SmFeN in the preformed body is 5%.
[0171] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 2 mm. According to actual conditions, the quantity ratio of the first preformed bodies to the second preformed bodies is 2:1.
[0172] The other steps are the same as those in Example 1
[0173] Comparative Example 2
[0174] (4) Prepare the raw materials for bonding magnetic rings
[0175] NdFeB anisotropic permanent magnet powder with a Nd content of 29.5 wt.%, SmFeN anisotropic permanent magnet powder, thermosetting resin binder epoxy resin, coupling agent silane and lubricant zinc stearate are prepared.
[0176] Based on the weight content of NdFeB anisotropic permanent magnet powder as 100, the mass percentage content of SmFeN is 40%. Based on the total weight content of NdFeB and SmFeN anisotropic permanent magnet powder as 100, the weight content of epoxy resin is 3%, the weight content of silane is 0.2%, and the weight content of zinc stearate is 0.25%.
[0177] (5) Rubber mixing
[0178] The measured silane is dissolved in the organic solvent acetone, and then placed in a vacuum mixer with the two batches of anisotropic permanent magnetic powders with different SmFeN contents, and mixed evenly. After the acetone evaporates, the silane is evenly coated on the surface of the magnetic powder. Then the measured epoxy resin and zinc stearate are dissolved in acetone, respectively, and mixed evenly with the anisotropic permanent magnetic powder coated with silane. After the acetone evaporates, two batches of composite magnetic powders for bonded magnets with different properties can be prepared.
[0179] (6) Room temperature preforming
[0180] The two composite magnetic powders prepared above are dried and placed in a mold cavity under a magnetic field H. 1 =0 and press-formed to obtain a preformed body, wherein the pressing pressure is 350 MPa and the content of SmFeN in the preformed body is 13%.
[0181] The aspect ratio of the pressed magnetic ring in this example is 1.25, and the wall thickness is 2 mm. According to actual conditions, the quantity ratio of the first preformed bodies to the second preformed bodies is 2:1.
[0182] The other steps are the same as those in Example 1
[0183] After magnetizing the prepared magnetic ring, the surface magnetic distribution and radial crushing force at the upper, middle and lower ends were tested, and then the magnetic ring was cut into three sections to obtain the density and performance data at the two ends and the middle, and to evaluate the uniformity of the density and performance along the axial distribution, as shown in Table 1.
[0184] Table 1
[0185]
[0186] In summary, the present invention provides an anisotropic bonded magnet and a method for preparing the same. By stacking magnets with different SmFeN contents and / or densities, the magnets in the middle have high performance and the magnets at both ends and / or the periphery have low performance, thereby compensating for the performance deviation caused by density differences during the pressing process and improving the performance uniformity of the magnet in the axial direction. This method solves the problem of highly directional magnetic field orientation and uneven density during the orientation and densification process, as well as the problem of low in the middle and high on both sides. The anisotropic bonded magnet prepared by this method has the characteristic of a density deviation of less than 2% along the pressing direction, which effectively improves the orientation degree and density of the magnet, as well as the uniformity and dimensional accuracy of the magnetic properties of the magnet.
[0187] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
Claims
1. Anisotropic bonded magnet, It is characterized in that Including RTB permanent magnet powder and SmFeN permanent magnet powder, Among them, in the RTB permanent magnet powder, the content of R is 28-31wt.%, the content of B is 0.9-1.1wt.%, and the balance is T; R is selected from one or more rare earth elements, T is Fe or FeCo, and B is boron; The weight content of SmFeN permanent magnet powder is 5% to 30% of the RTB permanent magnet powder; The anisotropic bonded magnet is formed by pressing a plurality of different preformed bodies, and the density deviation of the obtained anisotropic bonded magnet along the pressing direction is less than 2%; The plurality of different preforms include a first preform and a second preform; The first preformed body is made of composite magnetic powder with a low content of SmFeN permanent magnetic powder, and the second preformed body is made of composite magnetic powder with a high content of SmFeN permanent magnetic powder; wherein the mass percentage of SmFeN in the composite magnetic powder with a low content of SmFeN permanent magnetic powder is 3-15%, and the mass percentage of SmFeN in the composite magnetic powder with a high content of SmFeN permanent magnetic powder is 15-40%; or, The density of the first preformed body is less than that of the second preformed body. Putting a plurality of different preformed bodies into a mold for pressing comprises: the second preformed body is in the middle and the first preformed bodies are at both ends or the periphery.
2. The anisotropic bonded magnet according to claim 1, It is characterized in that R is one or more elements selected from the group consisting of Y, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Ho, Er, Tm, Yb, and Lu.
3. The anisotropic bonded magnet according to claim 2, It is characterized in that R is Nd, or Pr and Nd.
4. The anisotropic bonded magnet according to claim 1, It is characterized in that The bonded magnet is a bonded magnetic ring, the aspect ratio of the bonded magnetic ring is greater than 0.6, and the wall thickness is greater than 1 mm.
5. The anisotropic bonded magnet according to claim 4, It is characterized in that The bonded magnetic ring has an aspect ratio of 1.0-10 and a wall thickness of 1-20 mm.
6. The anisotropic bonded magnet according to claim 5, It is characterized in that The bonded magnetic ring has an aspect ratio of 2-8 and a wall thickness of 1-5 mm.
7. The anisotropic bonded magnet according to claim 1, It is characterized in that The particle size of the SmFeN permanent magnet powder is 1 to 30 μm.
8. The anisotropic bonded magnet according to claim 7, It is characterized in that The particle size of the SmFeN permanent magnet powder is 3-10 μm.
9. A method for preparing anisotropic bonded magnets, It is characterized in that The steps include: Step 1, preparing bonded magnet raw materials: the raw materials include RTB permanent magnet powder, SmFeN permanent magnet powder, thermosetting resin binder, coupling agent and lubricant; wherein the weight content of RTB permanent magnet powder and SmFeN permanent magnet powder is 100, and SmFeN permanent magnet powder is 3% to 40% of the weight content of RTB permanent magnet powder; the weight content of binder is 1.0% to 6.0% of RTB permanent magnet powder and SmFeN permanent magnet powder, the weight content of coupling agent is 0.05% to 1.0% of RTB permanent magnet powder and SmFeN permanent magnet powder, and the weight content of lubricant is 0.05% to 2.0% of RTB permanent magnet powder and SmFeN permanent magnet powder; Step 2, mixing: uniformly mixing the RTB permanent magnet powder and SmFeN permanent magnet powder in the raw materials with the thermosetting resin binder, coupling agent and lubricant to obtain composite magnetic powder; Step 3: Preforming at room temperature: Place the dried composite magnetic powders with different magnetic properties in the first mold and place them in a magnetic field H. 1 A variety of different preforms are obtained by press forming, wherein the pressing pressure is 100-600 MPa, and the magnetic field H 1 Less than 0.15T, the pressing temperature is room temperature; the plurality of different preforms include a first preform and a second preform; The first preformed body is made of composite magnetic powder with a low content of SmFeN permanent magnetic powder, and the second preformed body is made of composite magnetic powder with a high content of SmFeN permanent magnetic powder; wherein the mass percentage of SmFeN in the composite magnetic powder with a low content of SmFeN permanent magnetic powder is 3-15%, and the mass percentage of SmFeN in the composite magnetic powder with a high content of SmFeN permanent magnetic powder is 15-40%; or, The density of the first preform is less than the density of the second preform; Step 4: Warm-press magnetic field orientation molding: Place a stack of different preforms in a second mold and place them in a magnetic field H. 2 The magnet is oriented by medium temperature pressing and pressed again; then demagnetized, cooled and demolded to obtain anisotropic bonded magnets oriented by temperature pressing and magnetic field; wherein the magnetic field H 2 The pressure is 0.6-3T, the pressing pressure is 300-1000MPa, and the molding temperature is 60-200°C; wherein, when the density of the first preformed body is less than the density of the second preformed body, a plurality of different preformed bodies are stacked and placed in a mold for pressing, including: the middle is the second preformed body, and the two ends or the periphery are the first preformed bodies; Step 5, curing: heating the anisotropic bonded magnet formed by warm-pressing magnetic field orientation to a certain temperature and then keeping it warm, the warming temperature is 100-200° C. and the warming time is 0.5-2 hours.
10. The method according to claim 9, It is characterized in that The step 2 comprises: The coupling agent measured in the above step is dissolved in the corresponding organic solvent, and then mixed evenly with the RTB permanent magnet powder and the SmFeN permanent magnet powder. After the organic solvent is volatilized and removed, the coupling agent is evenly coated on the surface of the permanent magnet powder. Then, the measured binder and lubricant are dissolved in the corresponding organic solvent, and mixed evenly with the RTB permanent magnet powder and the SmFeN permanent magnet powder coated with the coupling agent. After the organic solvent is removed, the composite magnetic powder required for preparing the bonded magnet is obtained.
11. The method according to claim 9, It is characterized in that The mass percentage of SmFeN in the composite magnetic powder with a lower content of SmFeN permanent magnetic powder is 5-13%, and the mass percentage of SmFeN in the composite magnetic powder with a higher content of SmFeN permanent magnetic powder is 15-30%.
12. The method according to claim 11, It is characterized in that The ratio of the density of the first preform to the density of the second preform is 1:1.1 to 1:1.
5.
13. The method according to claim 11 or 12, It is characterized in that In step 4, stacking a plurality of different preforms into the second mold further comprises: the length of the middle second preform is smaller than the lengths of the first preforms at both ends.
14. The method according to claim 9, It is characterized in that The stacking of the various preforms into the second mold includes: the density and / or SmFeN content of the preforms arranged from the middle to the two ends gradually decreases; or the density and / or SmFeN content of the preforms arranged from the center to the periphery gradually decreases.
15. The method according to any one of claims 9 to 12, It is characterized in that In the step 4, the gap ratio between the preformed body and the warm-pressing magnetic field orientation forming die is 0.5 to 40%.
16. The method according to claim 15, It is characterized in that The gap ratio is 3.5%-25%.
17. The method according to claim 9, It is characterized in that The first preformed body and the second preformed body are magnetic cylinders or magnetic rings of the same shape, and the number ratio of the first preformed body to the second preformed body is 1:1 to 10:
1.
18. The method according to claim 9, It is characterized in that The weight content of the binder is 2.5% to 3.5% of the RTB permanent magnet powder and the SmFeN permanent magnet powder, the weight content of the coupling agent is 0.1% to 0.3% of the RTB permanent magnet powder and the SmFeN permanent magnet powder, and the weight content of the lubricant is 0.05% to 0.50% of the RTB permanent magnet powder and the SmFeN permanent magnet powder; In step 5, the insulation temperature is 120-180°C.
Citation Information
Cited By
Centrifugal auxiliary curing bonded magnet radial gradient magnetic powder distribution device and method
CN120190352A
A method for preparing a bonded magnet with radial gradient magnetic powder distribution through centrifugal assisted solidification
CN120190352B