Wound core and method for manufacturing the same
By stacking multiple bending bodies in the thickness direction of the rolled core and controlling the temperature gradient between the bending area and the flat area, the problems of deformation twins and film damage during the bending process are solved, and low iron loss rolled core manufacturing is achieved .
Patent Information
- Application Number
- CN202080030690.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-04-25
- Filing Date
- 2020-04-27
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-04-27
AI Technical Summary
The existing rolled core has problems such as a large number of deformation twins and film damage during the bending process, resulting in increased iron loss.
By stacking multiple bending bodies in the plate thickness direction, the bending bodies are made of directional electromagnetic steel plates. The temperature gradient between the bending area and the flat area is controlled within the range of 45°C to 500°C and less than 400°C/mm to ensure that the film The soundness rate reaches more than 90% to avoid film damage and deformation twins.
It effectively suppresses the iron loss of the rolled core, reduces the peeling of the film and the number of deformation twins in the bending area, and improves the performance of the rolled core.
Smart Images

Figure CN113785370B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a wound core and a method for manufacturing the same.
[0002] This application claims priority based on Japanese Patent Application No. 2019-084634 filed in Japan on April 25, 2019, the contents of which are incorporated herein by reference. Background Art
[0003] Wound cores are widely used as magnetic cores for transformers, reactors, noise filters, etc. In the past, reducing the iron loss generated in the core has become one of the important issues from the viewpoint of improving efficiency, and the reduction of iron loss has been studied from various viewpoints.
[0004] As one of the methods for manufacturing a wound core, for example, the method described in Patent Document 1 is widely known. In this method, after a steel plate is rolled into a cylindrical shape, the steel plate is pressed so that the corner portion has a constant curvature, and the steel plate is formed into a roughly rectangular shape. Thereafter, the steel plate is annealed to eliminate stress of the steel plate and maintain its shape. In the case of this manufacturing method, the radius of curvature of the corner portion varies depending on the size of the wound core. However, the radius of curvature is generally greater than 4 mm, and the corner portion becomes a gentle curved surface with a large radius of curvature.
[0005] On the other hand, as another method for manufacturing a wound core, the following method of laminating steel plates to form a wound core has been studied. In this method, portions of steel plates that will become corners of the wound core are bent in advance, and the bent steel plates are stacked.
[0006] According to this manufacturing method, the above-mentioned pressing process is unnecessary. In addition, since the steel plate is bent, the shape is maintained, and the shape maintenance by the above-mentioned annealing process is not an essential process. Therefore, there is an advantage of easy manufacturing. In this manufacturing method, since the steel plate is bent, a bending area with a curvature radius of less than 3 mm, that is, a bending area with a small curvature radius, is formed in the processed part.
[0007] As a wound core manufactured by a manufacturing method including bending, the following wound core structure is disclosed in Patent Document 2, for example. The wound core is formed by stacking a plurality of steel plates of different lengths bent into a ring shape in the outer circumferential direction. The end faces of the steel plates facing each other are evenly offset by predetermined dimensions in the stacking direction of the plurality of steel plates, and the joints of the end faces are stepped.
[0008] Patent document 3 discloses the following method for manufacturing a wound core. In this manufacturing method, a directional electromagnetic steel sheet with a coating having a phosphorus-containing coating on its surface is bent into a bent body, and a plurality of bent bodies are stacked in the direction of the plate thickness to manufacture a wound core. When the directional electromagnetic steel sheet with a coating is bent, the bending is performed so that the portion of the bent body that becomes the bending area is at a temperature of 150°C to 500°C. The plurality of bent bodies obtained are stacked in the direction of the plate thickness. By this method, the number of deformation twins present in the bending area of the bent body can be suppressed, and a wound core with suppressed iron loss can be obtained.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Publication No. 2005-286169
[0012] Patent Document 2: Japanese Utility Model Registration No. 3081863
[0013] Patent Document 3: International Publication No. 2018 / 131613 Summary of the invention
[0014] Problems to be solved by the invention
[0015] An object of the present disclosure is to provide a wound core with suppressed iron loss and a method for manufacturing the same.
[0016] Means for solving problems
[0017] The summary of the present disclosure is as follows.
[0018] <1> A wound core is formed by laminating a plurality of bent bodies in a plate thickness direction, wherein the plurality of bent bodies are formed by forming a coated grain-oriented electromagnetic steel sheet having a coating formed on at least one surface of the grain-oriented electromagnetic steel sheet so that the coating is on the outside.
[0019] The bent body includes: a bent region formed by bending the grain-oriented electromagnetic steel sheet with a coating; and a flat region adjacent to the bent region.
[0020] In side view, the number of deformation twins present in the curved region is 5 or less per 1 mm length of the center line in the plate thickness direction in the curved region,
[0021] The strain affected area is an area 40 times the thickness of the directional electromagnetic steel sheet with a coating on both sides of the circumference from the center of the bending area on the outer peripheral surface of the bent body. For any position along the circumference in the flat area within the strain affected area, the proportion of the area where the coating is not damaged is more than 90%.
[0022] <2> According to the above <1> The wound core, wherein, in the strain influence area, a plurality of micro-areas divided every 0.5 mm along the circumferential direction are specified, and the ratio of each of the plurality of micro-areas in each of the plurality of bent processed bodies is specified as a local soundness ratio that serves as a basis, and in different bent processed bodies, when the average value of the local soundness ratios that serve as a basis in each of the micro-areas that are at the same position in the circumferential direction is taken as an average local soundness ratio, the average local soundness ratio in all the micro-areas that are at different circumferential positions is greater than 90%, and all the local soundness ratios that serve as a basis are greater than 50%.
[0023] <3> Manufacturing the above <1> or <2> The method for manufacturing a wound core comprises the following steps:
[0024] a steel sheet preparation step of preparing the grain-oriented electromagnetic steel sheet with a coating;
[0025] a bending process, which is a process of forming the coated grain-oriented electromagnetic steel sheet into the bent body, in which the portion of the bent body to be the bent region is heated to 45° C. to 500° C., and the bending process is performed on the coated grain-oriented electromagnetic steel sheet to form the bent body under the condition that the absolute value of the local temperature gradient at any position in the length direction of the coated grain-oriented electromagnetic steel sheet is less than 400° C. / mm in the flat region within the strain influence region;
[0026] A stacking step of stacking a plurality of the bent bodies in a plate thickness direction.
[0027] <4> According to the above <3> In the method for manufacturing a wound core, in the bending step, the bending is performed under the condition that the product of the thickness of the grain-oriented electromagnetic steel sheet with a coating and the absolute value of the local temperature gradient is less than 100°C.
[0028] <5> According to the above <3> or <4> The method for manufacturing a wound core may include a steel sheet heating step of heating the grain-oriented electromagnetic steel sheet with a coating after the steel sheet preparing step and before the bending step.
[0029] <6> A method for implementing the above <5> The wound core manufacturing method adopts a wound core manufacturing device, which comprises:
[0030] a heating device for heating the grain-oriented electromagnetic steel sheet with a coating; and
[0031] A bending device is provided for bending the grain-oriented electromagnetic steel sheet with coating conveyed from the heating device.
[0032] <7> According to the above <6> The device for manufacturing a wound core, wherein the grain-oriented electromagnetic steel sheet with a coating unwound from a coil is conveyed to the heating device,
[0033] The bending device performs bending after cutting the grain-oriented electromagnetic steel sheet with a coating.
[0034] <8> According to the above <7> The above-mentioned wound core manufacturing device further comprises a pinch roller for conveying the coated grain-oriented electromagnetic steel sheet to the heating device.
[0035] <9> According to the above <6> In the above-mentioned wound core manufacturing apparatus, the heating device heats the coil and the grain-oriented electromagnetic steel sheet with coating that is unwound from the coil and conveyed to the bending device.
[0036] <10> According to the above <6> ~ <9> In the apparatus for manufacturing a wound core as described in any one of the above, the heating device heats the grain-oriented electromagnetic steel sheet with a coating by induction heating or irradiation with high-energy rays.
[0037] Effects of the Invention
[0038] According to the present disclosure, a wound core with suppressed iron loss and a method for manufacturing the same can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 This is a perspective view showing an example of a wound core.
[0040] Figure 2 for Figure 1 Side view of the wound core.
[0041] Figure 3 To express Figure 1 A side view of a first variation of the wound core.
[0042] Figure 4 To express Figure 1 A side view of a second variation of the wound core.
[0043] Figure 5 For the general Figure 1A side view obtained by enlarging the corner portion of the wound core.
[0044] Figure 6 For the general Figure 3 A side view showing an enlarged view of the vicinity of a corner portion of the wound core of the first modified example.
[0045] Figure 7 For the general Figure 4 A side view showing an enlarged view of the vicinity of a corner portion of the wound core of the second modified example.
[0046] Figure 8 This is a side view showing an enlarged example of a curved region.
[0047] Fig. 9 for Figure 1 A side view of a bent body of a wound core.
[0048] Fig.10 To express Fig. 9 A side view of a deformation example of a bent body.
[0049] Fig.11 To express Fig. 9 A side view of another modified example of the bent body.
[0050] Fig.12 This is an explanatory diagram showing an example of a bending process in a method of manufacturing a wound core.
[0051] Fig.13 It is an explanatory diagram showing a first example of a wound core manufacturing apparatus used in a wound core manufacturing method.
[0052] Fig.14 It is an explanatory diagram showing a second example of the manufacturing apparatus of the wound core used in the manufacturing method of the wound core.
[0053] Fig.15 To express the use Fig.12 An explanatory diagram of the dimensions of a wound core manufactured by the manufacturing method.
[0054] Fig.16 It is a plan view for explaining a bent region forming portion as a heated region, a flat region forming portion in which a temperature gradient is generated by heating the bent region forming portion, and a region affected by strain generated by bending.
[0055] Fig.17 This is an optical microscope photograph showing stripe-shaped deformation twins generated in the bending region of a conventional bent body. DETAILED DESCRIPTION
[0056] Hereinafter, the wound core and the method for manufacturing the same according to the present disclosure will be described.
[0057] It should be noted that the terms such as "parallel", "perpendicular", "same", or the values of lengths and angles used in the present disclosure to define the shapes or geometric conditions and their extent are not limited to strict meanings, but are interpreted within the range of the extent that the same function can be expected. In addition, in the present disclosure, approximately 90° means that an error of ±3° is allowed, meaning a range of 87° to 93°.
[0058] In addition, the element content of a component composition may be expressed as an element amount (for example, C amount, Si amount, etc.).
[0059] In addition, regarding the element content of a component composition, "%" means "mass %".
[0060] The term "process" refers not only to an independent process but also to a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process can be achieved.
[0061] In addition, the numerical range expressed using "to" means a range including the numerical values described before and after "to" as the lower limit and the upper limit.
[0062] Before the wound core and the method for manufacturing the same according to the present disclosure were completed, some of the inventors of the present invention discovered the following matters (see Patent Document 3).
[0063] That is, in the method for manufacturing a wound core of Patent Document 3, a directional electromagnetic steel sheet having a phosphorus-containing film on its surface is bent into a bent body, and a plurality of bent bodies are stacked to manufacture a wound core. At this time, the directional electromagnetic steel sheet is bent and the portion of the bent body that becomes the bending region (sometimes referred to as the "bending region forming portion" in this disclosure) is bent at a temperature of 150°C to 500°C. Thus, the number of deformation twins present in the bending region can be suppressed. By setting such a structure in which a plurality of bent bodies are stacked in the direction of the plate thickness, iron loss can be suppressed.
[0064] However, subsequent research has revealed that even if the temperature of the bending area forming portion is adjusted to 150°C to 500°C for bending, damage to the film may occur near the boundary between the bending area and the flat area adjacent to the bending area. The damage occurs locally on the flat area side near the boundary. Here, "damage" means that in mild cases, it is identified as a rupture of the film (cracks occur in the film); in severe cases, it is detected as peeling of the film. In the case of cracks in the film (mild cases), the following conditions exist: (1) the front end of the crack stays in the film and does not reach the mother steel plate; (2) the crack reaches the mother steel plate. In the case of peeling of the film (severe cases), the following conditions exist: (1) the film is completely peeled off so that the mother steel plate is exposed; (2) only the upper area of the film is peeled off and damaged, but the lower area covers the mother steel plate. In the present disclosure, these conditions are collectively described as "damage".
[0065] Even when the curved region forming portion is heated to 150°C to 500°C as in the method disclosed in Patent Document 3, a temperature gradient is generated near the boundary between the curved region forming portion and the portion that becomes a flat region adjacent to the curved region forming portion (sometimes referred to as "flat region forming portion" in this disclosure). This temperature gradient changes continuously at a temperature lower than the heating (soaking) temperature. It was found that when this temperature gradient is severe, strain is introduced into the flat region forming portion, causing damage to the film of the flat region forming portion.
[0066] Then, the inventors of the present invention found that the introduction of strain in the flat region forming portion and the damage of the tension coating are causes of deterioration of the iron loss.
[0067] As a result of further repeated studies to solve the above-mentioned problems, the inventors of the present invention found the following matters and completed the wound core and the method for manufacturing the wound core of the present disclosure.
[0068] When bending a grain-oriented electromagnetic steel sheet with a coating (sometimes referred to as a "steel sheet with a coating" or simply a "steel sheet" in the present disclosure), the bending is performed by heating in such a manner that the temperature of (1) the portion that becomes the bending area (bending area forming portion) and the temperature gradient of (2) the portion that becomes the flat area adjacent to the bending area forming portion that is bent (flat area forming portion) are respectively within specific ranges. As a result, (a) the generation of deformation twins in the bending area is suppressed, thereby avoiding deterioration of iron loss in the bending area. Furthermore, in addition to this advantage, (b) even in the flat area adjacent to the bending area, the peeling of the coating is suppressed. Moreover, (c) a bent body with less strain in the processed portion can be obtained. The inventors of the present invention have found that by stacking a plurality of bent bodies manufactured in this way in such a manner that the individual steel sheets overlap, a wound core with suppressed iron loss can be obtained.
[0069] [Coiling core]
[0070] The wound core disclosed in the present invention is a wound core formed by stacking a plurality of bent bodies in the plate thickness direction, wherein the plurality of bent bodies are formed by forming a coated directional electromagnetic steel sheet having a coating formed on at least one surface of the directional electromagnetic steel sheet in such a manner that the coating is located on the outside, wherein the bent body comprises: a bent region formed by bending the directional electromagnetic steel sheet with the coating; and a flat region adjacent to the bent region,
[0071] In side view, the number of deformation twins present in the curved region is 5 or less per 1 mm length of the center line in the plate thickness direction in the curved region,
[0072] The area from the center of the bending area at the outer peripheral surface of the bent body to both sides of the circumference, which is 40 times the thickness of the directional electromagnetic steel plate with coating, is taken as the strain affected area. For any position along the circumference in the flat area within the strain affected area, the proportion of the area where the coating is not damaged (local soundness of the coating) is greater than 90%.
[0073] In the wound core disclosed in the present invention, the local soundness of the coating is 90% or more at any position along the circumferential direction in the flat area within the strain influence zone. That is, in the bent body, local damage to the coating in the flat area formed on the outer peripheral surface of the directional electromagnetic steel sheet is suppressed. The wound core is composed of such a bent body. Therefore, in the wound core disclosed in the present invention, the deterioration of iron loss is suppressed compared to a wound core composed of a bent body in which the coating in the flat area is locally damaged. Although the mechanism is uncertain, the wound core disclosed in the present invention is based on the following understanding.
[0074] (Overview of Inhibition of Film Peeling)
[0075] The inventors of the present invention have repeatedly conducted in-depth studies on the causes of damage to the film pre-formed on the surface of the grain-oriented electrical steel sheet and deterioration of the iron loss of the wound core. As a result, it is believed that the temperature during the bending process of the grain-oriented electrical steel sheet with the film may affect the film, and the soundness of the film may affect the iron loss.
[0076] In the case of room temperature bending, although the soundness of the film can be ensured in the flat region, the soundness of the film is greatly reduced in the curved region.
[0077] Even in the case of heated bending, if the temperature gradient in the circumferential direction of the bent body is severe, strain will be introduced into the flat region forming portion. As a result, during heated bending, the film will be damaged in the flat region near the boundary between the bent region and the flat region, and the soundness of the film will be greatly reduced.
[0078] On the other hand, even in the case of heat bending, if the temperature gradient in the circumferential direction of the bent body is moderated (gentle), introduction of strain into the flat region forming portion can be suppressed, and the soundness of the film of the flat region forming portion can be ensured.
[0079] The inventors of the present invention have repeatedly conducted intensive studies and found that if a steel sheet is bent to form a bent body under the following conditions (1) and (2), the soundness of the film in the entire flat portion of the bent body reaches 90% or more.
[0080] (1) The temperature of the steel sheet in the bending region, which will be the highest temperature, is controlled to be between 45°C and 500°C. (2) The temperature gradient (local temperature gradient) at any position (all positions) in the length direction of the steel sheet (equivalent to the circumferential direction of the bent body) of the flat region forming portion adjacent to the heated bending region forming portion is less than 400°C / mm.
[0081] Then, it is considered that by stacking a plurality of bent bodies having a high film soundness rate throughout the flat portion in the plate thickness direction to form a wound core, unevenness of the film in the circumferential direction can be suppressed, and degradation of iron loss due to local damage to the film can be suppressed.
[0082] That is, local damage to the film is likely to occur in each area of the strain influence area that is at the same distance from the bending area in each of the multiple stacked bent bodies. In addition, in each bent body, if local damage to the film occurs, the interlayer resistance at the damaged position of the film in each bent body is reduced. In this way, after the steel plate is sheared (bent), if these bent bodies are stacked to manufacture a wound core, it is possible that the damaged position of the film overlaps in the direction of the plate thickness, and the interlayer resistance is reduced in the entire plate thickness direction. As a result, eddy currents increase and iron loss deteriorates. Therefore, it is believed that by improving the soundness of the film, the deterioration of this iron loss can be suppressed.
[0083] In addition, even if the damaged positions of the film do not overlap in the thickness direction, when the film is locally damaged, strain is generated locally in the film, so that the shape of the surface layer of the steel plate becomes locally rough, which becomes the cause of melt adhesion when the steel plates are stacked. If melt adhesion occurs, the appropriate film tension is lost and the iron loss is greatly deteriorated. Therefore, it is believed that by improving the soundness of the film, the deterioration of this iron loss can also be suppressed.
[0084] In addition, Fig.16 In the figure, a bending region forming portion as a heated region during bending and a flat region forming portion that generates a temperature gradient by heating the bending region forming portion are schematically shown in a plan view. The inventors of the present invention have found that when a bending region is formed by bending a grain-oriented electromagnetic steel sheet with a coating, the region from the center position in the length direction of the bending region forming portion to 40 times the plate thickness is a region that is greatly affected by strain caused by the bending process. Therefore, the inventors of the present invention define the region from the center position of the bending region forming portion to 40 times the plate thickness before and after in the steel sheet before processing as a strain affected region caused by the bending process (sometimes referred to as "strain affected region" in this disclosure).
[0085] The fact that the strain influence region to be considered in the present disclosure is 40 times the plate thickness is believed to be related to the fact that the contribution of strain to elastic deformation in this region is also taken into account (e.g. "Physics of Bending Deformation" p96-97, written by Fumio Hibino and Kabushi Sho).
[0086] In addition, Fig.16As can be seen, when a nominal plate thickness is set for the steel plate, the value of the plate thickness can be the value of the nominal plate thickness. When the nominal plate thickness is not set, for example, the following value can be used as the value of the plate thickness: the thickness of the wound core is measured at any 10 locations, and the average measurement result is divided by the number of bent processed bodies that form the wound core. In addition, before the manufacture of the wound core, for example, it can also be obtained in the following way: 10 sheets of oriented electromagnetic steel sheets with coatings are stacked, and the thickness of the stacked steel sheets is measured at any 10 locations, and the measurement result is divided by 10. The thickness of the wound core or the thickness of the stacked steel sheets can be measured using a micrometer. As the arbitrary 10 locations, for example, 10 locations obtained by equally spacing the full width in a specific position along the length direction of the steel plate (the circumferential direction of the wound core) can be set.
[0087] In addition, Fig.16 In the embodiment, the case where the curved region forming portion is used as the heated region is exemplified, but it is of course possible to also heat the flat region forming portion.
[0088] Hereinafter, the grain-oriented electromagnetic steel sheet with coating and the wound core of the present disclosure will be specifically described.
[0089] (Coated grain-oriented electrical steel sheet)
[0090] The grain-oriented electromagnetic steel sheet with coating in the present disclosure includes at least a grain-oriented electromagnetic steel sheet (sometimes referred to as a “parent steel sheet” in the present disclosure) and a coating formed on at least one surface of the parent steel sheet.
[0091] The grain-oriented electrical steel sheet with a coating has at least a primary coating as the coating, and may further have other layers as necessary. Examples of the other layers include a secondary coating provided on the primary coating.
[0092] Hereinafter, the structure of the grain-oriented electrical steel sheet with a coating will be described.
[0093] <Oriented Magnetic Steel Sheet>
[0094] In the coated grain-oriented electromagnetic steel sheet constituting the wound core 10 of the present disclosure, the parent steel sheet has a grain orientation in the range of {110} <001> A steel plate with highly concentrated orientation. The parent steel plate has excellent magnetic properties in the rolling direction.
[0095] The mother steel sheet used in the wound core of the present disclosure is not particularly limited. As the mother steel sheet, a known grain-oriented electromagnetic steel sheet can be appropriately selected and used. An example of a preferred mother steel sheet is described below, but the mother steel sheet is not limited to the following example.
[0096] The chemical composition of the base steel sheet is not particularly limited, and for example, it preferably contains, by mass%, Si: 0.8% to 7%, C: higher than 0% and 0.085% or less, acid-soluble Al: 0% to 0.065%, N: 0% to 0.012%, Mn: 0% to 1%, Cr: 0% to 0.3%, Cu: 0% to 0.4%, P: 0% to 0.5%, Sn: 0% to 0.3%, Sb: 0% to 0.3%, Ni: 0% to 1%, S: 0% to 0.015%, Se: 0% to 0.015%, and the remainder is composed of Fe and impurities.
[0097] The chemical composition of the mother steel sheet is controlled so that the crystal orientation is {110} <001> The Goss texture is oriented and concentrated, so it is the preferred chemical composition.
[0098] Among the elements in the mother steel sheet, Si and C are basic elements (essential elements) except Fe, and acid-soluble Al, N, Mn, Cr, Cu, P, Sn, Sb, Ni, S and Se are optional elements (arbitrary elements). Since these optional elements can be contained according to their purpose, there is no need to control the lower limit value, and they may not be substantially contained. In addition, even if these optional elements are contained as impurity elements, the effects of the present disclosure will not be impaired. The remainder of the basic elements and optional elements of the mother steel sheet is composed of Fe and impurity elements.
[0099] Among them, when the Si content of the base steel sheet is 2.0% or more by mass%, it is preferred because the conventional eddy current loss of the product can be suppressed. The Si content of the base steel sheet is more preferably 3.0% or more.
[0100] In addition, when the Si content of the base steel sheet is 5.0% or less in mass%, it is preferred because the steel sheet is less likely to break during hot rolling and cold rolling. The Si content of the base steel sheet is more preferably 4.5% or less.
[0101] The term "impurity elements" refers to elements that are accidentally mixed into the steel sheet from raw materials such as ores and scraps or from the manufacturing environment when the base steel sheet is manufactured industrially.
[0102] In addition, for grain-oriented electrical steel sheets, purification annealing is usually performed during secondary recrystallization. During purification annealing, inhibitor-forming elements are discharged out of the system. In particular, the concentration of N and S decreases significantly, becoming less than 50 ppm. Under normal purification annealing conditions, it is less than 9 ppm, and further less than 6 ppm. If purification annealing is performed sufficiently, it reaches a level that cannot be detected by general analysis (less than 1 ppm).
[0103] The chemical composition of the mother steel plate can be measured by a general analysis method for steel. For example, the chemical composition of the mother steel plate can be measured by ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry). Specifically, for example, it can be determined by the following method: a 35 mm square test piece is obtained from the central position in the width direction of the mother steel plate after the film is removed, and the test piece is measured by ICPS-8100 (measuring device) manufactured by Shimadzu Corporation under conditions based on a pre-made calibration curve. In addition, C and S can be measured by the combustion-infrared absorption method, and N can be measured by the inert gas melting-heat conduction method.
[0104] The chemical composition of the mother steel sheet is a composition obtained by analyzing the composition of a steel sheet obtained by removing a glass film and a phosphorus-containing film described later from a grain-oriented electrical steel sheet by a method described later.
[0105] The method for manufacturing the parent steel sheet is not particularly limited, and a method for manufacturing a conventionally known grain-oriented electromagnetic steel sheet can be appropriately selected. As a preferred specific example of the manufacturing method, for example, the following method can be cited: a slab having a C content of 0.04 to 0.1 mass % and other chemical compositions having the chemical compositions of the parent steel sheet is heated to 1000°C or higher for hot rolling, and then annealing the hot-rolled sheet as required, and then cold-rolling is performed once or twice or more with intermediate annealing to form a cold-rolled steel sheet, and the cold-rolled steel sheet is heated to 700 to 900°C in a wet hydrogen-inert gas atmosphere for decarburization annealing, and further nitriding annealing is performed as required, and final annealing is performed at about 1000°C.
[0106] The thickness of the base steel plate is not particularly limited, and may be, for example, 0.1 mm to 0.5 mm.
[0107] Furthermore, it is preferable to use a steel sheet whose magnetic domain is refined by imparting local strain on the surface or forming grooves on the surface as the grain-oriented electromagnetic steel sheet. By using such a steel sheet, the iron loss can be further suppressed.
[0108] <Primary film>
[0109] The primary coating is a coating formed directly on the surface of the grain-oriented electromagnetic steel sheet as the mother steel sheet without any other layer or film, and an example of the primary coating is a glass coating. Examples of the glass coating include a coating having a crystalline solid selected from forsterite (Mg2SiO4), spinel (MgAl2O4) and cordierite (Mg2Al4Si5O 16 )A film of one or more oxides.
[0110] The method for forming the glass film is not particularly limited and can be appropriately selected from known methods. For example, the following method can be cited: in a specific example of the method for manufacturing the mother steel sheet, after applying an annealing separator containing one or more selected from magnesium oxide (MgO) and aluminum oxide (Al2O3) on the cold-rolled steel sheet, final annealing is performed. In addition, the annealing separator also has the effect of inhibiting the steel sheets from sticking to each other during the final annealing. For example, when the annealing separator containing magnesium oxide is applied for final annealing, the silicon oxide contained in the mother steel sheet reacts with the annealing separator to form a glass film containing forsterite (Mg2SiO4) on the surface of the mother steel sheet.
[0111] In addition, instead of forming a glass film on the surface of the grain-oriented electrical steel sheet, for example, a phosphorus-containing film described later may be formed as a primary film.
[0112] The thickness of the primary film is not particularly limited, but is preferably 0.5 μm to 3 μm, for example, from the viewpoint of forming the primary film on the entire surface of the base steel sheet and suppressing separation.
[0113] <Other films>
[0114] The grain-oriented electromagnetic steel sheet with coating may also have a coating other than the primary coating. For example, as a secondary coating on the primary coating, it is preferable to have a phosphorus-containing coating in order to mainly impart insulation. The phosphorus-containing coating is a coating formed on the outermost surface of the grain-oriented electromagnetic steel sheet, and is formed on the primary coating when the grain-oriented electromagnetic steel sheet has a glass coating or an oxide coating as a primary coating. By forming the phosphorus-containing coating on the glass coating formed on the surface of the mother steel sheet as the primary coating, high adhesion can be ensured.
[0115] The phosphorus-containing film can be appropriately selected from conventionally known films. As the phosphorus-containing film, a phosphate-based film is preferred, and a film containing one or more of aluminum phosphate and magnesium phosphate as a main component and one or more of chromium and silicon oxide as a secondary component is particularly preferred. The phosphate-based film can provide tension to the steel sheet while ensuring the insulation of the steel sheet, and is also excellent in reducing iron loss.
[0116] The method for forming the phosphorus-containing film is not particularly limited and can be appropriately selected from known methods. For example, a method in which a coating liquid in which the film composition is dissolved is applied to a mother steel plate and then sintered is preferably used. Preferred specific examples are described below, but the method for forming the phosphorus-containing film is not limited thereto.
[0117] A coating liquid containing 4 to 16% by weight of colloidal silica, 3 to 24% by weight of aluminum phosphate (calculated as aluminum dihydrogen phosphate), and a total of 0.2 to 4.5% by weight of one or more of chromic anhydride and dichromate is prepared. Then, the coating liquid is applied to a mother steel plate or to other films such as a glass film formed on the mother steel plate, and sintered at a temperature of about 350°C or above. Thereafter, a phosphorus-containing film can be formed by heat treatment at 800°C to 900°C. The film thus formed can impart tension to the steel plate while having insulating properties, and can improve iron loss and magnetostrictive properties.
[0118] The thickness of the phosphorus-containing film is not particularly limited, but is preferably 0.5 μm to 3 μm from the viewpoint of ensuring insulation properties.
[0119] <Plate thickness>
[0120] The thickness of the grain-oriented electrical steel sheet with a coating is not particularly limited and may be appropriately selected depending on the intended use, and is generally in the range of 0.10 mm to 0.50 mm, preferably 0.13 mm to 0.35 mm, and more preferably 0.15 mm to 0.23 mm.
[0121] (Constitution of wound core)
[0122] An example of the structure of the wound core disclosed in the present invention is as follows: Figure 1 , Figure 2 The winding core 10 is taken as an example for explanation. Figure 1 is a three-dimensional diagram of the wound core 10, Figure 2 for Figure 1 A side view of the wound core 10 is shown.
[0123] In the present disclosure, the term "side view" refers to the width direction ( Figure 1 A side view is a view showing a shape recognized by side observation ( Figure 1 The plate thickness direction refers to the plate thickness direction of the oriented electromagnetic steel sheet with a coating, and refers to the direction perpendicular to the peripheral surface of the wound core when the wound core is formed into a rectangular shape. The direction perpendicular to the peripheral surface here refers to the direction perpendicular to the peripheral surface when the peripheral surface is viewed from the side. When the peripheral surface is curved when viewed from the side, the direction perpendicular to the peripheral surface (plate thickness direction) refers to the direction perpendicular to the tangent of the curve formed by the peripheral surface.
[0124] The wound core 10 is formed by stacking a plurality of bent bodies 1 in the thickness direction thereof. Figure 1 , Figure 2As shown in the figure, it has a substantially rectangular stacked structure formed of a plurality of bent bodies 1. The wound core 10 can be used as it is. The wound core 10 can also be fixed using a known fastening tool such as a cable tie as needed. In addition, the bent body 1 is formed of a coated grain-oriented electromagnetic steel sheet having a coating formed on at least one surface of a grain-oriented electromagnetic steel sheet as a mother steel sheet.
[0125] like Figure 1 and Figure 2 As shown, each bent body 1 is formed into a rectangular shape by alternating four flat portions 4 and four corner portions 3 along the circumferential direction. The angle between two flat portions 4 adjacent to each corner portion 3 is approximately 90°. Here, the circumferential direction refers to the direction around the axis of the wound core 10.
[0126] like Figure 2 As shown in the figure, in the wound core 10, the corner portion 3 of the bent body 1 has two bending regions 5. The bending region 5 is a region having a curved shape in a side view of the bent body 1, and a more specific definition will be described below. The following contents will also be described below. With respect to the two bending regions 5, the total bending angle in a side view of the bent body 1 is approximately 90°.
[0127] The corners 3 of the bent body 1 can also be formed as follows: Figure 3 As shown in the first modified example of the wound core 10A, three bending areas 5 are provided at one corner portion 3. Figure 4 Like the wound core 10B of the second modified example, one corner portion 3 has one bent region 5. That is, each corner portion 3 of the bent body 1 only needs to have one or more bent regions 5 so that the steel plate is bent by approximately 90 degrees.
[0128] As Figure 2 As shown, the bent body 1 has a flat region 8 adjacent to the bent region 5. The flat region 8 adjacent to the bent region 5 includes two flat regions 8 shown in the following (1) and (2).
[0129] (1) A flat region 8 located between the curved regions 5 and 5 (between two curved regions 5 adjacent to each other in the circumferential direction) at one corner portion 3 and adjacent to each curved region 5 .
[0130] (2) The flat regions 8 adjacent to the respective curved regions 5 as the flat portions 4 .
[0131] Figure 5 For the general Figure 1 FIG. 1 is an enlarged side view of the vicinity of the corner portion 3 in the wound core 10. FIG.
[0132] like Figure 5 As shown, in the case where a corner portion 3 has two bending areas 5a and 5b, the bending area 5a (curved portion) is continuous from the flat portion 4a (straight portion) which is a flat area of the bending processed body 1, and in front of it, the flat area 7a (straight portion), the bending area 5b (curved portion) and the flat portion 4b (straight portion) which is a flat area are continuous.
[0133] In the wound core 10, Figure 5 The area from line segment A-A' to line segment B-B' in is the corner portion 3. Point A is the end point on the side of the flat portion 4a in the bending area 5a of the innermost bending body 1a arranged on the wound core 10. Point A' is the intersection of a straight line passing through point A and being perpendicular to the plate surface of the bending body 1a (in the direction of plate thickness) and the outermost surface of the wound core 10 (the outer peripheral surface of the outermost bending body 1 arranged on the wound core 10). Similarly, point B is the end point on the side of the flat portion 4b in the bending area 5b of the innermost bending body 1a arranged on the wound core 10. Point B' is the intersection of a straight line passing through point B and being perpendicular to the plate surface of the bending body 1a (in the direction of plate thickness) and the outermost surface of the wound core 10. In Figure 5 In the example, the angle formed by the two adjacent flat portions 4a and 4b through the corner portion 3 (the angle formed by the intersection of the extended lines of the flat portions 4a and 4b) is θ. Figure 5 In the example of FIG. 5 , the angle θ is approximately 90°. The bending angles of the bending regions 5a and 5b will be described below. Figure 5 The total of the bending angles of the middle bending regions 5a and 5b, φ1+φ2, is approximately 90°.
[0134] Next, a case where one corner portion 3 has three curved regions 5 will be described. Figure 6 For the general Figure 3 The side view of the vicinity of the corner portion 3 in the wound core 10A of the first modified example is enlarged. Figure 6 Zhong Ye and Figure 5 Likewise, the area from line segment AA' to line segment BB' is the corner portion 3. Figure 6 In the figure, point A is the endpoint of the curved region 5a closest to the flat portion 4a on the flat portion 4a side. Point B is the endpoint of the curved region 5b closest to the flat portion 4b on the flat portion 4b side. When there are three or more curved regions 5, there are flat regions between the curved regions. Figure 6 In the example, the total of the bending angles of the bending regions 5a, 5b, and 5c, φ1+φ2+φ3, is approximately 90°. Generally speaking, when the corner portion 3 has n bending regions 5, the total of the bending angles of the bending regions 5, φ1+φ2+...+φn, is approximately 90°.
[0135] Next, a case where one corner portion 3 has one curved region 5 will be described. Figure 7 For the general Figure 4 The side view of the corner portion 3 and the vicinity of the wound core 10B of the second modified example is enlarged. Figure 7 Zhong Ye and Figure 5 and Figure 6 Likewise, the area from line segment AA' to line segment BB' is the corner portion 3. Figure 7 In FIG. 5 , point A is the end point on the flat portion 4a side of the curved region 5. Point B is the end point on the flat portion 4b side of the curved region 5. Figure 7 In the example of FIG. 5 , the bending angle φ1 of the bending region 5 is approximately 90°.
[0136] In the present disclosure, since the angle θ of the corner portion is approximately 90°, the bending angle φ of one bending area is approximately 90° or less. From the perspective of suppressing the peeling of the steel plate film and suppressing the iron loss, the bending angle φ of one bending area is preferably 60° or less, and more preferably 45° or less. Therefore, it is preferred that one corner portion 3 has two or more bending areas 5. However, it is difficult to form four or more bending areas 5 at one corner portion 3 in terms of the constraints of the manufacturing equipment design, so it is preferred that the number of bending areas 5 in one corner portion is three or less.
[0137] like Figure 5 In the case where a corner portion 3 has two bending areas 5a and 5b, as in the wound core 10 shown in the figure, it is preferably set to φ1=45° and φ2=45° from the perspective of suppressing the peeling of the coating and reducing the iron loss, but it can also be set to φ1=60° and φ2=30°, or to φ1=30° and φ2=60°, etc.
[0138] In addition, if Figure 6 When one corner portion 3 has three curved regions 5a, 5b, 5c as in the wound core 10A of the first modified example, it is preferable to set φ1=30°, φ2=30°, and φ3=30° from the viewpoint of reducing iron loss.
[0139] Furthermore, from the perspective of production efficiency, it is preferred that the bending angles in the bending regions are equal. Therefore, when one corner portion 3 has two bending regions 5a and 5b ( Figure 5 ), preferably set to φ1 = 45° and φ2 = 45°, in the case where a corner portion 3 has three curved regions 5a, 5b, 5c ( Figure 6 ), from the perspective of suppressing film peeling and reducing iron loss, it is preferably set to φ1=30°, φ2=30° and φ3=30°.
[0140] In reference Figure 8At the same time, the bending area 5 is described in more detail. Figure 8 : is a side view of an example of an enlarged bending region 5 of the bending work body 1. The bending angle φ of the bending region 5 refers to the angle difference between the flat region on the rear side of the bending direction and the flat region on the front side of the bending direction in the bending region 5 of the bending work body 1. Specifically, the bending angle φ of the bending region 5 is expressed in the form of an angle φ of the supplementary angle formed by the following two imaginary lines Lb extension line 1 and Lb extension line 2 in the bending region 5, wherein the two imaginary lines Lb extension line 1 and Lb extension line 2 are obtained by extending the straight line portions that are respectively continuous with both sides (point F and point G) of the curved portion included in the line Lb representing the outer surface of the bending work body 1.
[0141] The bending angle of each bending region 5 is approximately 90° or less, and the total bending angle of all the bending regions 5 present in one corner portion 3 is approximately 90°.
[0142] The bending area 5 refers to an area surrounded by the following lines when points D and E on the line La representing the inner surface of the bending body 1 and points F and G on the line Lb representing the outer surface of the bending body 1 are defined as follows in the side view of the bending body 1: (1) a line divided by points D and E on the line La representing the inner surface of the bending body 1; (2) a line divided by points F and G on the line Lb representing the outer surface of the bending body 1; (3) a straight line connecting the point D and the point G; and (4) a straight line connecting the point E and the point F.
[0143] Here, point D, point E, point F, and point G are defined as follows.
[0144] In the side view, a straight line AB is obtained by connecting the center point A of the curvature radius at the curved portion included in the line La representing the inner surface of the bent body 1 and the intersection point B of the two imaginary lines Lb extension line 1 and Lb extension line 2 obtained by extending the straight line portions adjacent to both sides of the curved portion included in the line Lb representing the outer surface of the bent body 1, and the point where the straight line AB intersects with the line La representing the inner surface of the bent body 1 is set as the origin C;
[0145] A point D is set as a point that is away from the origin C in one direction along the line La representing the inner surface of the bent body 1 by a distance m expressed by the following equation (2);
[0146] A point E is set as a point that is a distance m from the origin C along the line La representing the inner surface of the bent body in other directions;
[0147] The intersection of the straight line portion of the straight line portion of the line Lb representing the outer surface of the bent body, the straight line portion facing the point D, and an imaginary line drawn perpendicular to the straight line portion facing the point D and passing through the point D is set as point G;
[0148] The intersection of the straight line portion facing the point E among the straight line portions included in the line Lb representing the outer surface of the bent body and an imaginary line drawn perpendicular to the straight line portion facing the point E and passing through the point E is set as point F.
[0149] m=r×(π×φ / 180) (2)
[0150] In formula (2), m represents the distance from the origin C, and r represents the distance from the center point A to the origin C (curvature radius).
[0151] That is, r represents the radius of curvature when the curve near the origin C is regarded as an arc, and represents the radius of curvature of the inner surface side in the side view of the curved region 5. The smaller the radius of curvature r, the sharper the curvature of the curved portion of the curved region 5, and the larger the radius of curvature r, the gentler the curvature of the curved portion of the curved region 5.
[0152] Even when the curved region 5 having a curvature radius r of 3 mm or less is formed by bending, peeling of the coating in the curved region 5 is suppressed, so that a wound core with low iron loss can be obtained.
[0153] Fig. 9 for Figure 1 A side view of a bent body 1 of a wound core 10. Fig. 9 As shown in the figure, the bent body 1 is obtained by bending a grain-oriented electromagnetic steel sheet with a coating, and has four corner portions 3 and four flat portions 4, so that one grain-oriented electromagnetic steel sheet with a coating is formed into a substantially rectangular ring in a side view. More specifically, the bent body 1 is set to have the following structure: a gap 6 is provided in one flat portion 4, where two end surfaces of the grain-oriented electromagnetic steel sheet with a coating face each other in the longitudinal direction, and the other three flat portions 4 do not contain the gap 6.
[0154] However, the wound core 10 may have a laminated structure that is substantially rectangular in shape when viewed from the side. Fig.10 As shown, the bent body 1A has two flat portions 4 including the voids 6 and the other two flat portions 4 not including the voids 6. In this case, the bent body is constituted by two coated grain-oriented electromagnetic steel sheets.
[0155] As a further modification example of the case where the bent body is formed of two coated grain-oriented electromagnetic steel sheets, a method such as Fig.11As shown in the figure, a bent body 1B is formed in which one flat portion 4 includes two gaps 6 and the other three flat portions 4 do not include gaps 6. That is, the bent body 1B is formed by combining a grain-oriented electromagnetic steel sheet with a coating that is bent in a manner corresponding to three sides of a substantially rectangular shape and a grain-oriented electromagnetic steel sheet with a coating that is flat (straight in side view) in a manner corresponding to the remaining side. In the case where the bent body is formed of two or more grain-oriented electromagnetic steel sheets with a coating, the bent body of the steel sheet and the flat (straight in side view) steel sheet may be combined.
[0156] Preferably, in any case, when manufacturing the wound core, no gap is generated between two adjacent layers in the plate thickness direction. Therefore, in the two adjacent layers of bent bodies, the length of the steel plate and the position of the bent region are adjusted so that the outer circumference of the flat portion 4 of the bent body arranged on the inner side and the inner circumference of the flat portion 4 of the bent body arranged on the outer side become equal.
[0157] <Number of deformation twins in the bent portion>
[0158] In the wound core 10 of the present disclosure, the number of deformation twins present in the bent region 5 is 5 or less per 1 mm length of the center line in the plate thickness direction of the bent region 5 in a side view.
[0159] That is, when the length of the center line in the plate thickness direction of "all the bent areas 5 contained in a corner portion 3 of a bent processed body 1 of the wound iron core 10" is set to LTotal (mm) and the number of deformation twins contained in "all the bent areas 5 contained in a corner portion 3 of a bent processed body 1 of the wound iron core 10" is set to NTotal (roots), the value of NTotal / LTotal (roots / mm) is less than 5.
[0160] The number of deformation twins present in the bent region 5 is preferably 4 or less, more preferably 3 or less per 1 mm length of the center line in the plate thickness direction in the bent region 5 . Fig.17 FIG. 1 shows deformation twins generated in a bent region of a bent body formed from a grain-oriented electromagnetic steel sheet constituting a conventional wound core, and stripe-shaped deformation twins 7 are observed from the surface of the steel sheet toward the inside.
[0161] Regarding the number of deformation twins present in the bending region 5 in the side view, an optical microscope is used to photograph the cross section of the bending region 5 along the circumferential direction of the bent body (equivalent to the length direction of the electromagnetic steel sheet with film orientation) and the thickness direction of the plate, and the number of stripe-shaped deformation twins 7 from the surface of the steel plate toward the inside is counted. Deformation twins are formed on the outer peripheral surface of the rolled core of the steel plate and the inner peripheral surface of the rolled core. In the present disclosure, the deformation twins formed on the outer peripheral surface and the deformation twins formed on the inner peripheral surface are summed. In addition, the existence of deformation twins can be confirmed by analyzing and evaluating using a scanning electron microscope and crystal orientation analysis software (EBSD: Electron BackScatter Diffraction). In addition, for deformation twins, when the magnification in the cross-sectional observation is set to 100 times, the deformation twin that meets the following two requirements is regarded as one deformation twin.
[0162] (1) A line extending from the plate thickness surface side (outside) to the plate thickness center of a cross section and having a color different from that of the base steel plate.
[0163] (2) The length of the line is 10 μm or more and the width of the line is 3 μm or more. In addition, the length of the line is preferably set to 180 μm or less.
[0164] Here, a method for preparing a sample for cross-sectional observation of the curved region 5 will be described by taking the wound core 10 of the present disclosure as an example.
[0165] The cross-sectional observation sample of the curved region 5 is processed into a mirror surface by, for example, SiC grinding paper and diamond grinding in the same manner as the general cross-sectional structure observation. Finally, in order to erode the structure, the sample is weakly immersed in a solution prepared by adding 2 to 3 drops of picric acid and hydrochloric acid to 3% nitric acid for 20 seconds to erode the structure. In this way, the cross-sectional observation sample of the curved region 5 is prepared.
[0166] In addition, the center line length of the plate thickness of the grain-oriented electromagnetic steel sheet (bent body 1) is Figure 8 The length of the curve KJ in is specifically determined as follows. The point where the straight line AB defined as described above intersects the line representing the outer peripheral surface of the directional electromagnetic steel sheet (bending body 1) is set as point H, and the midpoint of the point H and the origin C is set as point I. At this time, the distance (radius of curvature) from the center point A to the point I is set to r', and m' is calculated by the following formula (2'). At this time, the center line length of the directional electromagnetic steel sheet (bending body 1) in the plate thickness direction becomes twice (2m') of m'. In addition, point K is the midpoint of the line segment EF, and point J is the midpoint of the line segment GD.
[0167] Formula (2'): m' = r' × (π × φ / 180)
[0168] In formula (2'), m' represents the length from point I to point K and point J, and r' represents the distance from the center point A to point I (curvature radius).
[0169] In the present disclosure, the number of deformation twins is determined for at least 10 bending regions of one wound core, and the average thereof is used as the number of deformation twins to be evaluated.
[0170] <Healthy rate of membrane>
[0171] In the present disclosure, the soundness of the coating is specified in the circumferential direction (corresponding to the longitudinal direction of the grain-oriented electromagnetic steel sheet with the coating) of the outer peripheral surface of the bent body constituting the wound core.
[0172] In the present disclosure, the flat area within the strain influence zone at the outer peripheral surface of the bent processed body is divided into fine micro-areas, and the "soundness" within the micro-areas is defined. The "soundness" within the micro-areas can be used to evaluate the soundness change or local peak value within a continuous and wide strain influence zone. In the present disclosure, the "soundness" within the micro-area is referred to as the "local soundness". In addition, regarding the "(local) soundness of the film" in the present disclosure, when only one film is formed on the directional electromagnetic steel sheet, it refers to the soundness of the primary film; when other films are formed on the primary film, it refers to the soundness of the film including the primary film and other films on the primary film. The "local soundness" is explained below.
[0173] In the present disclosure, in the flat area in the strain influence area at the outer peripheral surface of the bending processing body, the micro-area is divided into areas with a width of 0.5mm (circumferential length) relative to the circumference of the outer peripheral surface of the bending processing body. At this time, the area with a width of 0.5mm is divided from the side close to the bending area. It is divided sequentially from the side close to the bending area. When the flat area in the strain influence area on the side away from the bending area becomes less than 0.5mm in width, the width is set to 0.5mm and a micro-area is set outside the flat area in the strain influence area. For example, when the circumferential length of the flat area in the strain influence area is 6.3mm, 12 micro-areas with a width of 0.5mm are divided inside the flat area in the strain influence area, and one micro-area extending 0.2mm to the outer area of the flat area in the strain influence area is further set. In this case, a total of 13 micro-areas are set.
[0174] Then, the case where the local soundness at any position (micro area) in the flat area within the strain influence area on the outer peripheral surface of the bent body is 90% or more is a preferred mode. As can be seen from the above division, the local soundness is a value determined at intervals of 0.5 mm in the above flat area, and the value at any position (local soundness in all micro areas) reaches 90% or more. It is preferably 95% or more, more preferably 98% or more, and 100% is undoubtedly the best state.
[0175] <Measurement of health rate>
[0176] In order to determine the soundness, it is necessary to identify the area where the coating covers the base steel sheet and the area where the coating is damaged on the surface of the grain-oriented electrical steel sheet with coating (the outer peripheral surface of the bent body). The method is described below.
[0177] In the present disclosure, the condition of membrane damage is determined by surface observation using a digital camera and the color tone (shade) of the observed image. The following is used: the area where the membrane is damaged is observed in a brighter tone than the area where the membrane is not damaged. More specifically, in the present disclosure, (1) the image brightness in the area where damage has occurred; and (2) the image brightness in the area where damage has occurred are obtained in advance. Then, (3) an image of the area to be evaluated is obtained, and (4) based on the two brightnesses obtained in advance, it is determined whether the image of the area to be evaluated has damage, and the soundness rate (area ratio without damage) of each micro-area is calculated.
[0178] Specifically, (1) first obtain the image brightness in the area where the film is not damaged. At this time, observe more than 5 flat areas A (flat areas A that are sufficiently far away from the bending area) where the film is not damaged, and find the average brightness BA of the image. At this time, there is no problem as long as the flat area A is an area that is more than 40 times the thickness of the steel plate in the circumferential direction from the bending area. In addition, when observing more than 5 locations, when there are more than 5 bent bodies (steel plates) forming the wound core, it is preferred that the areas with equal circumferential positions are observed in each of the 5 or more different bent bodies. As such 5 or more bent bodies, it is preferred to select the following 5 or more bent bodies: including the outermost bent body in the plate thickness direction (stacking direction) and the innermost bent body, and arranged at equal intervals in the plate thickness direction. In this case, the position in the plate width direction of each bent body that is the object of obtaining the image is preferably the center in the plate width direction. In addition, the size of the image is preferably a square with a side of 0.5 mm.
[0179] In addition, (2) the image brightness in the area where the film is not damaged is obtained. At this time, the image brightness is obtained, for example, on the basis of preparing a sample of the damaged area. The sample of the damaged area is prepared as follows. First, a damaged sample is cut out from a flat area (a flat area sufficiently far away from the bending area) of the bent body where the film is not damaged. As a damaged sample, a square with a side of 20 mm can be exemplified. For example, the sample is subjected to bending processing with a radius of 3 mm using a type II bending resistance tester (cylindrical mandrel method) manufactured by TP Giken (Co., Ltd.) by the method described in JIS K-5600. Furthermore, for the bent portion, the inner and outer sides are bent back in opposite directions. The bending and bending operations are performed more than 3 times to obtain a sample in which the film is fully damaged. In this sample, more than 5 parts of the bent-bent area B are observed to obtain the average brightness BB of the image. When observing five or more locations, when there are five or more bent bodies (steel plates) forming the wound core, it is preferred that samples be cut out from regions at equal circumferential positions in the five or more different bent bodies for observation. The method for selecting the five or more bent bodies, the positions in the plate width direction from which the samples are obtained, and the size of the images are preferably the same as those exemplified in (1) above.
[0180] Furthermore, (3) observe the flat areas in the strain influence area at the outer peripheral surface of the bent body to be evaluated in the present disclosure at more than 5 locations. That is, as in the above (1) and (2), first select more than 5 bent bodies. Observe all the micro-areas set in the strain influence area in each selected bent body. Thus, all the micro-areas (i.e., flat areas) in the strain influence area are observed at more than 5 locations. In addition, the position in the plate width direction of each micro-area that is the object of obtaining the image is preferably the center in the plate width direction. In addition, the size of the image is preferably a square with a side of 0.5 mm.
[0181] The observations of these (1) to (3) themselves do not depend on the observation machine. For example, as a general commercially available digital camera, the PowerShot SX710 HS (BK) manufactured by Canon can be cited. The resolution of the image observation is set in such a way that the spatial resolution of each pixel of the magnetic domain image reaches less than 20 μm. In addition, from the perspective of operating hours, it is preferred to stop at the observation of 5 locations (5 sheets) in any of the above (1) to (3). In addition, in the case where the bent processed body (steel plate) forming the rolled iron core is less than 5 sheets, etc., multiple locations can also be observed in one bent processed body.
[0182] Next, (4) each image of the strain-affected region is processed using the concentration change measurement software "Gray-val" (manufactured by Library Co., Ltd.). The image is binarized with the average brightness of brightness BA and brightness BB (i.e., (BA+BB) / 2) as the boundary, and the area darker than the boundary value (lower brightness) is set as a healthy area where the film is not damaged, and its area ratio is calculated. In the present disclosure, the above-mentioned "local soundness" is calculated for each of the strain-affected regions at more than 5 locations, and the measurements at more than 5 locations are averaged to obtain the "local soundness" in the flat area within the strain-affected region. That is, first, the "local soundness" of more than 5 locations is calculated for all the micro-regions within the strain-affected region. In other words, at this stage, the local soundness (basic local soundness) of (total number of micro-regions) × (more than 5 locations) is calculated. Furthermore, the average local soundness (average local soundness) is calculated for each of all the micro-regions within the strain-affected region. That is, in five or more bent bodies, the average value of the "basic local soundness" calculated for the corresponding micro regions is calculated. In other words, the same number of local soundness as the total number of micro regions is obtained at this stage.
[0183] In the wound core of the present disclosure, the “average local soundness” of all the micro regions in the strain influence region reaches 90% or more as described above.
[0184] [Manufacturing method of wound core]
[0185] Next, a method for manufacturing the wound core of the present disclosure will be described.
[0186] The method for manufacturing the wound core of the present disclosure is not particularly limited, but the wound core can be preferably manufactured by the method for manufacturing the wound core of the present disclosure described below.
[0187] That is, the method for manufacturing a wound core of the present disclosure includes the following steps:
[0188] a steel sheet preparing step of preparing a grain-oriented electrical steel sheet with a coating formed on at least one surface of the grain-oriented electrical steel sheet;
[0189] a bending process step, which is a process of forming the grain-oriented electromagnetic steel sheet with a coating into a bent body having a bent region formed by bending in a manner so that the coating is on the outside and a flat region adjacent to the bent region, heating the portion of the bent body that becomes the bent region to 45°C to 500°C, and defining regions adjacent to the portion that becomes the heated bent region and having a thickness of 40 times that of the grain-oriented electromagnetic steel sheet with a coating from the center of the bent region to both sides in the circumferential direction as strain-affected regions, and subjecting the grain-oriented electromagnetic steel sheet with a coating to the bending process to form the bent body under the condition that the temperature gradient at any position in the length direction of the portion that becomes the flat region within the strain-affected region is less than 400°C / mm;
[0190] A stacking step of stacking a plurality of the bent bodies in a plate thickness direction.
[0191] (Steel plate preparation process)
[0192] First, a grain-oriented electromagnetic steel sheet with a coating formed on at least one side of the grain-oriented electromagnetic steel sheet is prepared. The grain-oriented electromagnetic steel sheet with a coating can be manufactured or a commercial product can be obtained. The structure of the mother steel sheet, the structure of the coating, the manufacturing method, etc. of the grain-oriented electromagnetic steel sheet with a coating are as described above, so the description here is omitted.
[0193] (Bending process)
[0194] Next, the grain-oriented electromagnetic steel sheet with a coating is cut into a desired length as needed, and then formed into a ring-shaped bent body in a manner such that the coating is on the outside. At this time, the grain-oriented electromagnetic steel sheet with a coating is bent to form a bent body under the following conditions (1) and (2).
[0195] (1) A portion of the bent body that is to become a bent region (bend region forming portion) is heated to 45°C to 500°C.
[0196] (2) In the flat region adjacent to the bent region forming portion heated as in (1) above and located within the strain influence region, the temperature gradient at any position in the longitudinal direction of the grain-oriented electromagnetic steel sheet with coating is less than 400°C / mm.
[0197] The coated grain-oriented electromagnetic steel sheet is formed into a bent body 1 in a manner that satisfies the above conditions. As described above, the bent body has a bent region formed by bending and a flat region adjacent to the bent region. In the bent body 1, the flat portion and the corner portion are alternately continuous. In each corner portion, the angle between two adjacent flat portions is approximately 90°.
[0198] The bending method will be described with reference to the drawings. Fig.12 It is an explanatory diagram showing an example of a bending method of a grain-oriented electromagnetic steel sheet with a coating in a method of manufacturing the wound core 10 .
[0199] The structure of the processing machine (hereinafter also referred to as the bending processing device 20) is not particularly limited. Fig.12 As shown in (A), it usually has a die 22 and a punch 24 for pressing, and further has a guide device 23 for fixing the coated grain-oriented electromagnetic steel sheet 21. The coated grain-oriented electromagnetic steel sheet 21 is conveyed in the conveying direction 25 and is fixed at a predetermined position ( Fig.12 (B)) Next, by pressing with a predetermined force set in advance to a predetermined position in the pressing direction 26 using the punch 24, the bent body 1 having a bending region having a desired bending angle φ is obtained.
[0200] - Heating around the bending area -
[0201] In the method for manufacturing a wound core disclosed in the present invention, in such a bending process, the temperature of the bending region forming portion of the grain-oriented electromagnetic steel sheet with a coating is adjusted to an appropriate range. Furthermore, the local temperature gradient in the longitudinal direction at any position in the strain-affected region is made to be within an appropriate range. On this basis, the grain-oriented electromagnetic steel sheet with a coating is bent to form a bent body.
[0202] The method for heating the above-mentioned area is not particularly limited. For example, the following general methods for heating metal plates can be applied: (1) heating in contact with a heated metal mold; (2) heating in a high-temperature furnace; (3) induction heating; (4) electric heating; (5) heating by irradiating high-energy rays (such as infrared rays) such as halogen heaters. As an example of a manufacturing method that includes this heating method, there is the following method. This method, for example, Fig.13As shown in the first example of the wound core manufacturing device 40A shown in the figure, it basically includes a process of appropriately heating the steel plate in the heating device 30A (heating furnace) provided immediately before the bending device 20. Furthermore, the method includes a process of conveying the heated steel plate to the bending device 20 and bending the steel plate in a high temperature state. That is, using the heating device 30A, not only the bending area forming part of the directional electromagnetic steel plate 21 is heated, but also the flat area forming part adjacent to the bending area forming part in the length direction is heated. As a result, when the bending area forming part is bent, the temperature gradient in the strain-affected area can be moderated. However, when the heated metal mold is directly used as the processing metal mold in the method of heating in contact with the metal mold, the step equivalent to conveying from the heating device 30A to the bending device 20 is omitted.
[0203] In addition, use Fig.13 The method for manufacturing a wound core of the wound core manufacturing apparatus 40A of the first example shown in FIG. 1 includes a steel sheet heating step after the steel sheet preparing step and before the bending step. The steel sheet heating step is a step of heating the grain-oriented electromagnetic steel sheet 21 with a coating.
[0204] The wound core manufacturing device 40A includes an uncoiler 50 , a pinch roll 60 , a heating device 30A, and a bending device 20 .
[0205] The uncoiler 50 unwinds the coated grain-oriented electromagnetic steel sheet 21 from the coil 27 of the coated grain-oriented electromagnetic steel sheet 21. The coated grain-oriented electromagnetic steel sheet 21 unwound from the uncoiler 50 is conveyed toward the heating device 30A and the bending device 20.
[0206] The heating device 30A heats the grain-oriented electromagnetic steel sheet 21 with a coating. The grain-oriented electromagnetic steel sheet 21 with a coating unwound from the coil 27 is conveyed to the heating device 30A. The heating device 30A preferably heats the grain-oriented electromagnetic steel sheet 21 with a coating, for example, by induction heating or irradiation with high-energy rays. As the heating device 30A, for example, a heating furnace such as a so-called induction heating method or an infrared heating method can be cited. The heating device 30A heats the grain-oriented electromagnetic steel sheet 21 with a coating that is about to be conveyed to the bending processing device 20.
[0207] The pinch rollers 60 convey the coated grain-oriented electromagnetic steel sheet 21 to the heating device 30A. The pinch rollers 60 adjust the conveying direction of the coated grain-oriented electromagnetic steel sheet 21 to be supplied to the heating device 30A. The pinch rollers 60 adjust the conveying direction of the coated grain-oriented electromagnetic steel sheet 21 to the horizontal direction and then supply the coated grain-oriented electromagnetic steel sheet 21 to the heating device 30A. In addition, the pinch rollers 60 may not be provided.
[0208] The bending device 20 performs bending on the coated grain-oriented electromagnetic steel sheet 21 conveyed from the heating device 30A. The bending device 20 includes the die 22, the punch 24, the guide 23, and a cover 28. The cover 28 covers the die 22, the punch 24, and the guide 23. The bending device 20 performs bending after cutting the coated grain-oriented electromagnetic steel sheet 21.
[0209] The bending apparatus 20 further includes a cutter (not shown) for cutting the coated grain-oriented electromagnetic steel sheet 21 into predetermined lengths.
[0210] In addition, you can also use Fig.14 The wound core manufacturing apparatus 40B of the second example shown in FIG. Fig.13 40A of the manufacturing apparatus of the wound core of the first example shown in FIG. In the manufacturing apparatus 40B of the second example, the heating apparatus 30B is different from the heating apparatus 30A of the first example. The heating apparatus 30B heats the coil 27 and the grain-oriented electromagnetic steel sheet 21 with a coating which is unwound from the coil 27 and conveyed to the bending apparatus 20. In addition, the heating apparatus 30B does not heat the bending apparatus 20.
[0211] According to the manufacturing apparatus 40A, 40B of the wound core of the first example and the second example, and the manufacturing method of the wound core implemented by each manufacturing apparatus 40A, 40B, the grain-oriented electromagnetic steel sheet 21 with a coating is heated before the bending process. Therefore, the entire region to be bent in the grain-oriented electromagnetic steel sheet 21 with a coating can be heated. In other words, in the grain-oriented electromagnetic steel sheet 21 with a coating, not only the portion with which the metal mold (die 22, punch 24) contacts during the bending process can be preheated, but also the portion adjacent to the portion can be preheated. Thus, the above-mentioned matters can be performed: the grain-oriented electromagnetic steel sheet 21 with a coating is bent on the basis of making the local temperature gradient in the longitudinal direction at any position in the strain influence region into an appropriate range.
[0212] The heating temperature (reaching temperature) of the bending area can be controlled, for example, by the output power (furnace temperature, current value, etc.) of the heating devices 30A and 30B or the holding time during heating. In addition, the temperature gradient of the strain-affected area can be controlled by appropriately changing the heating power itself (i.e., the intensity of the heating power), adjusting the conveying speed of the steel plate or the length of the furnace body (soaking zone length) to change the residence time of the steel plate in the heating devices 30A and 30B. At this time, it is also necessary to consider the heat conduction from the heating area to the non-heating area. These specific conditions are of course different depending on the steel plate, heating device 30A, 30B, etc. used, and are not intended to uniformly show and stipulate quantitative conditions. Therefore, in the present disclosure, it is set to stipulate the heating state by the temperature distribution obtained by the temperature measurement described later. However, regarding such control, as long as a person skilled in the art who performs heat treatment of the steel plate in a normal operation, based on the measurement data of the steel plate temperature as described later, according to the steel plate and the heating device 30A and 30B used, it is easy to reproduce the desired temperature state within a practical range, and it will not hinder the implementation of the wound core and its manufacturing method disclosed in the present disclosure.
[0213] -Temperature measurement around the bending area-
[0214] Here, the temperature of the grain-oriented electromagnetic steel sheet with coating during the bending process specified in the present disclosure is measured as follows.
[0215] Basically, the temperature is measured in the process of conveying the grain-oriented electromagnetic steel sheet with coating from the heating device to the bending device. Specifically, a radiation thermometer for micro-point measurement (as an example, TMHX-CSE0500 (H) manufactured by JAPAN SENSOR Corporation) is set between the heating device and the bending device, and the temperature of the grain-oriented electromagnetic steel sheet with coating is continuously measured in the longitudinal direction with a response speed of 0.01 seconds and an area Φ of 0.7 mm. At this time, the conveying speed of the steel sheet and the scanning speed of the measuring point of the thermometer are adjusted, and the measurement is performed in a manner that the measurement interval in the longitudinal direction of the steel sheet becomes 0.5 mm (i.e., the same as the width of the micro area). The obtained temperature measurement value can be used to evaluate the heating temperature of the bending area and the temperature gradient of the strain-affected area.
[0216] At this time, the measurement points at intervals of 0.5 mm are set with the center of the bending area as the starting point. If the measurement points are set sequentially from the center point, it is possible that the temperature gradient cannot be determined only by the measurement points inside the flat area in the strain influence area at the boundary between the flat area and the external area in the strain influence area. In this case, the temperature gradient is determined using the temperature of a measurement point at an interval of 0.5 mm toward the outside of the flat area in the strain influence area. For example, at the boundary of the flat area in the strain influence area, the temperature gradient of the area including the boundary is determined by the temperature of two points at an interval of 0.5 mm, 0.3 mm from the inner side of the boundary and 0.2 mm from the outer side of the boundary.
[0217] In addition, in the method of using the heated metal mold directly as the processing metal mold, since the temperature measurement during the above-mentioned "transport process" cannot be performed, the temperature of the steel plate just after the processing is completed and it is transported out of the processing device is measured under the same conditions.
[0218] -Temperature control around the bending area-
[0219] In the manufacturing method disclosed in the present invention, the temperature of the bending region forming part of the grain-oriented electromagnetic steel sheet with a coating is adjusted to 45°C to 500°C. It is believed that there is a temperature fluctuation in the bending region in the above-mentioned temperature measurement, but the average temperature in the bending region is used in the present invention. When the temperature is less than 45°C, the generation of deformation twins in the bending region cannot be suppressed. It is preferably above 100°C, and more preferably above 150°C. In addition, if it exceeds 500°C, the coating is deteriorated and the melt adhesion of the laminated steel sheets becomes obvious, and at the same time, the appropriate coating tension is lost, so that the iron loss is greatly reduced. It is preferably below 400°C, and more preferably below 300°C. By setting it to this temperature range, the following well-known advantages can be obtained: the generation of deformation twins in the bending region is suppressed to avoid the deterioration of the iron loss in the bending region. In addition, if the grain-oriented electromagnetic steel sheet that achieves low iron loss by refining the magnetic domain, that is, the so-called non-heat-resistant magnetic domain control material (ZDKH), is heated to a temperature exceeding 300°C, the magnetic domain control effect may disappear. Therefore, when a non-heat-resistant magnetic domain control steel sheet is used as the grain-oriented electromagnetic steel sheet with a coating, the upper limit of the temperature of the curved region forming portion is preferably controlled to 300° C. or less.
[0220] Furthermore, the temperature gradient in the longitudinal direction of the grain-oriented electromagnetic steel sheet with coating in the strain-affected region is appropriately controlled. Thus, when the steel sheet is heated and bent to form a bent region, it is possible to suppress coating peeling in a flat region adjacent to the bent region.
[0221] What should be controlled in the present disclosure is the local temperature gradient at any position within the strain region. In the present disclosure, using the temperature distribution at 0.5 mm intervals obtained by the measurement described above, for the temperature gradient at 0.5 mm intervals, the maximum value of the absolute value of the temperature gradient (local temperature gradient) is set to less than 400°C / mm. In the strain-affected region, if the maximum value is above 400°C / mm, the film peeling caused by the temperature gradient in the flat portion becomes obvious. The temperature gradient is preferably less than 350°C / mm, more preferably less than 250°C / mm, and further preferably less than 150°C / mm. In addition, the temperature gradient is preferably greater than 3°C / mm, more preferably greater than 5°C / mm. The preferred range of the temperature gradient is set by appropriately combining these preferred upper and lower limits.
[0222] In addition, the local temperature gradient can be controlled more preferably by considering the influence of the thickness of the applied directional electromagnetic steel sheet. In the present disclosure, it is defined as the product of the thickness of the directional electromagnetic steel sheet with coating and the absolute value of the local temperature gradient. By setting the product to less than 100°C, the damage to the coating can be significantly suppressed. Preferably, it is less than 90°C, more preferably less than 60°C, and further preferably less than 40°C. The product is preferably above 1°C, more preferably above 2°C. The preferred range of the product is set by appropriately combining these preferred upper and lower limits.
[0223] The reason why such control is possible is not clear, but it is believed to be as follows. As described above, the temperature gradient in the present disclosure is a factor for avoiding damage to the coating associated with strain occurring in the strain influence zone. It is believed that at this time, the magnitude of the strain caused by processing in the strain influence zone depends on the thickness of the steel plate being bent. In other words, it is believed that the thicker the plate thickness, the greater the strain on the outer surface side, especially in the outermost area where the coating exists. Therefore, it is believed that the following situation occurs: the thicker the plate thickness, the lower the temperature gradient should be controlled. The inventors of the present invention believe that this point can be defined as the product of the thickness of the oriented electromagnetic steel plate with coating and the absolute value of the local temperature gradient.
[0224] In addition, in manufacturing Figure 2 , Figure 3 In the case of a bent body having two or more bending regions at one corner 3, such as the wound core shown in , there may be a region where the strain influence regions of the respective bending regions overlap. When manufacturing a bent body having two or more bending regions at one corner 3, the bending process may be performed so that the temperature gradient in all the strain influence regions including such overlapping regions satisfies the above-mentioned content.
[0225] (Lamination process)
[0226] The plurality of bent bodies obtained through the bending process as described above are stacked in the plate thickness direction in such a manner that the coating of each bent body is on the outside. That is, for the bent body 1, the corner portions 3 are aligned with each other, overlapped and stacked in the plate thickness direction, and a stacked body 2 having a substantially rectangular shape in a side view is formed. Thus, the wound core with low iron loss disclosed in the present invention can be obtained. The wound core obtained can also be fixed using a known tie or fastening tool as needed.
[0227] It should be noted that, in the above description, a case where four bent bodies 1 are stacked is described, but the number of the stacked bent bodies 1 is not limited.
[0228] In this way, the wound core of the present invention can suppress the peeling of the coating in the flat region adjacent to the curved region in addition to the curved region, so that the iron loss can be reduced. Therefore, according to one embodiment of the present invention, the wound core can be preferably used for any of the conventionally known uses such as magnetic cores such as transformers, reactors, and noise filters.
[0229] The present disclosure is not limited to the above-described embodiments. The above-described embodiments are merely examples, and all those having substantially the same configuration and exhibiting the same functions and effects as the technical concept described in the claims of the present disclosure are included in the technical scope of the present disclosure.
[0230] Example
[0231] The following examples (experimental examples) are described, but the wound core and the method for manufacturing the same disclosed in the present invention are not limited to the following examples. The wound core and the method for manufacturing the same disclosed in the present invention may adopt various conditions as long as they do not deviate from the main purpose of the present invention and achieve the purpose of the present invention. In addition, the conditions of the following examples are condition examples adopted to confirm the feasibility and effect.
[0232] [Manufacturing of wound core]
[0233] A glass film (1.0 μm thick) containing forsterite (Mg2Sio4) as a primary film and a secondary film (2.0 μm thick) containing aluminum phosphate were sequentially formed on a mother steel sheet having the above chemical composition. Furthermore, a plurality of directional electromagnetic steel sheets with finer magnetic domains were prepared by irradiating the steel sheet surface with laser light at intervals of 4 mm in the rolling direction and in a direction perpendicular to the rolling direction.
[0234] The bent region forming portion of these grain-oriented electromagnetic steel sheets with coatings was controlled within a temperature range of 25° C. to 600° C. and a bending process was performed while controlling the temperature gradient of the strain-affected region, thereby obtaining a bent body having a bent region.
[0235] Table 1 shows the plate thickness of the steel plate, the radius of curvature of one bending region, the bending angle of one bending region, the heating temperature of the bending region (local region temperature), and the local temperature gradient.
[0236] The steel sheet was heated in an induction heating coil (heating device) installed before the processing device, and the temperature of the steel sheet was measured by the above method while being conveyed to the bending processing device after heating.
[0237] Next, the bent bodies are stacked in the plate thickness direction to obtain Fig.15 The number of layers depends on the thickness of the steel plate used. For 0.23 mm steel plate, there are 200 layers; for 0.50 mm steel plate, there are 90 layers; for 0.15 mm steel plate, there are 306 layers; and for 0.35 mm steel plate, there are 131 layers. Fig.15 The winding core with a bending angle of 45° in the bending region is shown. Figure 1 and Figure 2 However, in this embodiment, a wound core 10 with a bending angle of 90° is also manufactured with the same size. Figure 4 The wound core 10B).
[0238] Experiments No. 1 to 29 are examples of heating to form a gentle temperature gradient in the entire strain influence region. Experiments No. 30 to 49 are examples of heating to cause a temperature change in a specific region within the strain influence region.
[0239] [evaluate]
[0240] <Number of deformation twins in the bending region>
[0241] As described above, the number of deformation twins is measured by cross-sectional microstructure observation.
[0242] <Fusion Adhesion of Film>
[0243] The stacked steel sheets of the wound core were peeled off, and the presence or absence of fusion bonding of the coating was evaluated in five stages. Regarding the ratio of the fusion bonding area at the bent portion, the case of more than 80% was evaluated as "5", the case of less than 80% and more than 60% was evaluated as "4", the case of less than 60% and more than 40% was evaluated as "3", the case of less than 40% and more than 20% was evaluated as "2", and the case of less than 20% was evaluated as "1".
[0244] In addition, as an indirect method for evaluating melt adhesion, a method of measuring the dissolved P of the steel plate as described in the above-mentioned Patent Document 3 can be cited. However, this time, the melt adhesion of the steel plate film was directly evaluated. As the reason, it is because: due to the excessive temperature gradient, the strain is locally and unevenly retained in the film, so that the shape of the surface layer of the steel plate becomes locally rough, which becomes the cause of melt adhesion when the steel plates are stacked. That is, this is because: it is natural that the damage of the film affects the melt adhesion of the film, and the microscopic shape of the film also affects the melt adhesion of the film. Therefore, as a comprehensive indicator including these effects, a direct evaluation is preferred.
[0245] <Measurement of film soundness>
[0246] The surface (outer peripheral surface) of the bent body was photographed with a digital camera (PowerShot SX710 HS (BK) manufactured by Canon), and the concentration change measurement software "Gray-val" was used to determine the damaged area and sound area of the film as described in the above-mentioned <Determination of Soundness> to obtain the soundness of the film.
[0247] Specifically, first, five bent bodies are selected from a plurality of bent bodies forming the wound core. As the five bent bodies, the following five bent bodies are selected: including a bent body located at the outermost side in the plate thickness direction (stacking direction) and a bent body located at the innermost side, and arranged at equal intervals in the plate thickness direction. Then, with these five bent bodies as objects, the average brightness BA described in (1) and the average brightness BB described in (2) are obtained. Furthermore, as described in (3), images are obtained in all micro-regions in each of the five bent bodies. On this basis, as described in (4), after the local soundness in the micro-region image obtained in (3) (hereinafter referred to as "basic local soundness") is measured, the average local soundness of all micro-regions (hereinafter referred to as "average local soundness") is obtained. The total number of the basic local soundness is 5 times the number of micro-regions (5 pieces). The total number of the average local soundness is the total number of micro-regions.
[0248] Here, in Table 1 and Table 2, the first local soundness ratio and the second local soundness ratio are described as the soundness ratio of the film.
[0249] The first local health rate is the lowest value among all the average local health rates. That is, if the first local health rate is 90% or more, the average local health rate of all the micro regions reaches 90% or more.
[0250] The second local soundness ratio represents the lowest value among all the basic local soundness ratios. That is, if the second local soundness ratio is 50% or more, the basic local soundness ratios of all the micro regions reach 50% or more.
[0251] In addition, for some samples in which fusion bonding was severe, the soundness ratio could not be appropriately measured (marked with "-" in Tables 1 and 2).
[0252] <Determination of Iron Loss Value of Wound Core>
[0253] The wound core of the experimental example was measured at a frequency of 50 Hz and a magnetic flux density of 1.7 T using the exciting current method in the method for measuring the magnetic properties of an electromagnetic steel strip using an Epstein tester described in JIS C2550-1 to obtain the iron loss value W. A .
[0254] [Table 1]
[0255]
[0256] [Table 2]
[0257]
[0258] From the results of Tables 1 and 2, it can be seen that the deterioration of iron loss is suppressed in the wound core using the following bending work body, wherein the bending region forming part is heated to 45°C to 500°C and the temperature gradient is appropriately controlled in the flat region within the strain influence region. In addition, when evaluating the iron loss, it should be noted that the absolute value level of the iron loss is greatly different due to the difference in the thickness of the steel plate, so the comparison should be made under the condition of the same plate thickness.
[0259] In addition, in Experiments No. 34 to 49, if the effects of the local temperature gradient caused by the difference in steel plate thickness on the characteristic change behavior are compared, it can be seen that a more preferable result can be obtained by appropriately controlling the temperature gradient taking the plate thickness into account (local temperature gradient × plate thickness).
[0260] Furthermore, in experiments No. 36, 36-(a), 36-(b) and No. 48, 48-(a), 48-(b), if the effect of the second local soundness on the characteristic change behavior is compared, it can be seen that by setting the second local soundness to be greater than 50%, and then greater than 60%, greater than 70%, greater than 80%, and greater than 90%, more preferable results can be obtained in the order described.
[0261] Industrial Applicability
[0262] According to the present disclosure, iron loss can be suppressed, and thus the industrial applicability is great.
[0263] Explanation of symbols
[0264] 1.1a Bending body
[0265] 2 Laminated body
[0266] 3 Corner
[0267] 4, 4a, 4b Flat part
[0268] 5, 5a, 5b, 5c Bending area
[0269] 6. Gap
[0270] 8 Flat Area
[0271] 10 coils of core
[0272] 20 Bending device
[0273] 30A, 30B Heating device
[0274] 40A, 40B Manufacturing Equipment
[0275] 21. Grain-oriented electrical steel sheet with coating
[0276] 22 Mould
[0277] 23 Guide device
[0278] 24 Punch
[0279] 25 Transport direction
[0280] 26 Pressurization direction
Claims
1. A method for manufacturing a wound core, comprising the following steps: A steel sheet preparation process for preparing a grain-oriented electromagnetic steel sheet with a coating; a bending process step, which is a process of forming the grain-oriented electromagnetic steel sheet with a coating into a bent body having a bending region and a flat region adjacent to the bending region, in which the portion of the bent body to become the bending region is heated to 45°C to 500°C, and regions from the center of the bending region at the outer peripheral surface of the bent body to both sides in the circumferential direction that are 40 times the thickness of the grain-oriented electromagnetic steel sheet with a coating are used as strain-affected regions, and in the flat region within the strain-affected region, the grain-oriented electromagnetic steel sheet with a coating is formed into the bent body by the bending process under the condition that the absolute value of the local temperature gradient at any position in the longitudinal direction of the grain-oriented electromagnetic steel sheet with a coating is 3°C / mm or more and less than 400°C / mm; A stacking step of stacking a plurality of the bent bodies in a plate thickness direction.
2. The method for manufacturing a wound core according to claim 1, wherein: In the bending step, the bending is performed under the condition that a product of a thickness of the grain-oriented electromagnetic steel sheet with a coating and an absolute value of the local temperature gradient is less than 100°C.
3. The method for manufacturing a wound core according to claim 1 or 2, wherein: After the steel sheet preparing step and before the bending step, a steel sheet heating step of heating the grain-oriented electromagnetic steel sheet with a coating is provided.
4. A wound core manufacturing device for use in implementing the wound core manufacturing method according to claim 3, comprising: a heating device for heating the grain-oriented electromagnetic steel sheet with a coating; and A bending device is provided for bending the grain-oriented electromagnetic steel sheet with coating conveyed from the heating device.
5. The wound core manufacturing device according to claim 4, wherein: The grain-oriented electromagnetic steel sheet with coating unwound from a coil is conveyed to the heating device, The bending device performs bending after cutting the grain-oriented electromagnetic steel sheet with a coating. 6 . The wound core manufacturing apparatus according to claim 5 , further comprising a pinch roll for conveying the coated grain-oriented electromagnetic steel sheet to the heating device.
7. The wound core manufacturing device according to claim 4, wherein: The heating device heats the coil and the grain-oriented electromagnetic steel sheet with a coating that is unwound from the coil and conveyed to the bending device.
8. The wound core manufacturing device according to any one of claims 4 to 7, wherein: The heating device heats the coated grain-oriented electromagnetic steel sheet by induction heating or irradiation with high-energy rays.