Methods for dealing with layered structures
By using high-purity amorphous silicon discrete layer components as masks to etch the electrolyte layer, the problems of contamination, scratches and interface quality during the solid-state microbattery patterning process are solved, achieving high-quality discrete layer component formation and improving battery performance.
Patent Information
- Application Number
- CN202080020839.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-03-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-03-12
AI Technical Summary
Existing technologies easily lead to particle contamination, substrate scratching, and poor interface quality during the patterning process of solid-state microbatteries, especially in small-sized microbatteries, leading to poor alignment of discrete layer components and the presence of waste areas.
Using a second discrete layer element containing at least 95 atomic percent amorphous silicon as an etch mask, forming discrete layer elements by removing through-thickness portions of the first and second layers, and using these elements to etch the third layer to maintain interface quality , and trim the second discrete layer element when necessary to optimize its perimeter and form trenches to ensure effective isolation of the electrolyte layer.
It effectively avoids the contamination and degradation of the electrolyte layer, maintains the interface quality, reduces the risk of short circuit, improves the performance of the anode and the overall capacity ratio of the battery, and avoids the complex lithium-based electrode formation steps.
Smart Images

Figure CN113795960B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for processing a layered structure, in particular a layered structure in which the layers are provided by components of a battery. Background Art
[0002] Solid-state microbatteries typically include an active stack of thin layers. The active stack is formed by two electrodes (anode and cathode) separated by a solid electrolyte. Typically, the anode current collector is disposed on the face of the anode opposite the electrolyte, and the cathode current collector is disposed on the face of the cathode opposite the electrolyte.
[0003] Typically, solid-state microbatteries are formed by depositing individual thin layers on a wafer. For efficiency reasons, multiple microbatteries are typically formed on a single wafer. This requires that each battery component (e.g., cathode, anode, or electrolyte) be provided as a layer comprising multiple discrete elements, each discrete element providing a portion of a corresponding microbattery. The multiple discrete elements are typically formed into a regular array on the wafer surface.
[0004] The process of providing a layer comprising a plurality of discrete elements is known as "patterning" the layer. This can be achieved by depositing the layer through a shadow mask having a plurality of holes. The mask is placed on the surface of the substrate and remains in place throughout the deposition process. The shadow mask is then removed and the deposited layer exhibits the desired distribution of discrete elements, i.e. the desired pattern.
[0005] The disadvantage of this masking technique is that it may produce particle contamination on the substrate surface, which can adversely affect the performance of the microbattery. In addition, the process of placing the mask on the substrate may cause scratching of the substrate, which also has a detrimental effect on the battery performance. In addition, when the dimensions of the microbattery are small, masking can produce edge or shadow effects, resulting in poor alignment of discrete layer elements within a single stack and / or large wasted areas between stacks.
[0006] Therefore, it is often desirable to avoid masking techniques and use alternative patterning techniques, such as etching of deposited layers. Due to the different physical and chemical properties of the layers, this may require etching each layer individually. However, this process may have an adverse effect on the quality of the interface between the etched layer and the subsequently deposited layer.
[0007] It would therefore be desirable to provide a method of patterning layers of a stacked structure while reducing these adverse effects. Summary of the invention
[0008] In a first aspect, the present invention may provide a method of processing a stack of layers to provide a stack of discrete layer components, comprising the steps of:
[0009] A stack is provided, the stack comprising:
[0010] § a first layer provided by a first material;
[0011] § a third layer provided by a solid electrolyte; and
[0012] § a second layer located between the first and third layers, the second layer having a thickness of at least 500 nm and being provided by a second material comprising at least 95 atomic % amorphous silicon;
[0013] removing a through-thickness portion of the first layer to form a first discrete layer element provided by the first material;
[0014] removing a through-thickness portion of the second layer to form a second discrete layer element provided by a second material, the second discrete layer element being located between the first discrete layer element and the solid electrolyte; and
[0015] etching the third layer using the second discrete layer element as an etch mask to form a third discrete layer element provided by the solid electrolyte;
[0016] The first, second and third discrete layer components provide the stack of discrete layer components.
[0017] By using the second discrete layer element as a mask during etching of the third layer, the quality of the interface between the second and third layers can be maintained. Thus, contamination and / or degradation of the surface of the electrolyte layer that would normally occur if the electrolyte were etched prior to depositing the second layer (such contamination and / or degradation may occur, for example, through oxidation of the electrolyte surface or incomplete removal of the photoresist resin from the electrolyte surface) can be avoided.
[0018] For the avoidance of doubt, the step of using the second discrete layer elements as an etch mask refers to the fact that the dimensions of the mask are defined by the perimeter of the second discrete layer elements. It is contemplated that the first discrete layer elements are typically also present during the etching of the third layer, although their perimeter may not exactly correspond to the perimeter of the etch mask provided by the second discrete element layer.
[0019] Typically, the second material comprises at least 98 atomic % amorphous silicon, preferably at least 99 atomic % amorphous silicon. In some cases, the second material consists essentially of amorphous silicon. The term "amorphous" means that the silicon atoms of the second material do not exhibit long-range structural order.
[0020] Surprisingly, it has been found that when a discrete layer element comprising at least 95 atomic % amorphous silicon (hereinafter referred to as the "amorphous silicon layer element" and corresponding to the second discrete layer element) is used as a mask during etching of the electrolyte layer, the amorphous silicon material retains its ability to function as a cell anode. This is unexpected because it is well known that, for example, the performance of silicon solar cells deteriorates when the silicon is exposed to moisture (as a result, it is generally considered necessary to provide an encapsulation element to inhibit moisture from entering the cell).
[0021] Thus, the second layer can be deposited directly to provide the anode at a desired thickness of at least 500 nanometers. This is considered to be the minimum anode thickness to provide a working cell with useful capacity levels.
[0022] This minimum thickness is believed to help balance the capacity ratio between the battery's cathode and anode. That is, when the amorphous silicon material is used as an anode in a battery, the minimum thickness is believed to limit the relative volume expansion of the amorphous silicon material due to lithiation of the amorphous silicon material during battery charging.
[0023] The use of full thickness amorphous silicon elements as etching masks is in contrast to the method described in US 9,373,864, in which a pattern made of, for example, a silicon layer having a thickness between 5 and 100 nanometers is used as an etching mask for etching the electrolyte layer. After this etching process, a lithium-based layer is deposited on the pattern, and lithium atoms diffuse into the pattern, so that the lithium-based layer and the pattern form a lithium-based electrode.
[0024] The present invention avoids the complicated step of forming a lithium-based electrode after the etching process. In addition, the present invention can allow the current collector (as the first layer) to be deposited directly on the layer (i.e., the second layer) comprising at least 95 atomic % amorphous silicon before the step of etching the electrolyte. This may help maintain the interface quality between the second layer and the current collector.
[0025] The term "discrete layer element" is intended to refer to a portion of a layer having a defined perimeter and not in direct contact with any other portion of the layer. Discrete layer elements typically have a substantially square, rectangular or circular perimeter. Typically, each discrete layer element provides a component of a battery.
[0026] In some examples of the method of the present invention, the method may further include, after the step of etching the third layer, the step of modifying the second discrete layer element to provide a modified second discrete layer element.
[0027] Wherein the modified second discrete layer element has a perimeter enclosing an area that is smaller than an area enclosed by the perimeter of the second discrete layer element.
[0028] For example, the method of the present invention may further include the step of trimming the second discrete layer element around at least a portion of its periphery to provide a modified second discrete layer element after the step of etching the third layer.
[0029] The step of trimming the second discrete layer element may help remove any peripheral portions of the element that may have been damaged by the step of etching the third layer, thereby further improving the ability of the second discrete layer element to provide a high quality anode.
[0030] In some cases, it has been found that the step of etching the third layer using the second discrete layer element as an etch mask has the result that the etchant undercuts the etch mask. That is, the etchant removes electrolyte that was originally in contact with the mask at the periphery of the mask. When the stack of discrete layer elements is incorporated into a battery, this loss of electrolyte at the periphery of the second discrete layer element may result in the electrolyte no longer providing an effective separator between the cathode and anode, thereby causing a short circuit.
[0031] To help prevent this and help the electrolyte provide an effective separator between the cathode and anode, preferably, the step of trimming the second discrete layer element results in the modified second discrete layer element being completely within the boundaries defined by the perimeter of the third discrete layer element. For example, the modified second discrete layer element can have a perimeter that coincides with the third discrete layer element.
[0032] The step of trimming the second discrete layer element around at least a portion of its periphery may include an etching process. The etching may be performed using a dry etching process, such as a plasma etching process. The etching process may be mechanical (e.g., ion beam milling using, for example, an argon plasma) and / or chemical (e.g., reactive ion etching, in which substances such as SF6 are used because they are able to react with the first and / or second layer to produce volatile reaction products). For example, in some cases, the plasma etching process is performed using a plasma containing argon and / or SF6.
[0033] In other cases, trimming may be performed, for example, by laser ablation.
[0034] Typically, during the step of trimming the second discrete layer element, the first discrete layer element is also trimmed around at least a portion of its periphery to provide a modified first discrete layer element.
[0035] In some cases, the first and second discrete layer elements can be trimmed by an etching process in which a portion of the surface of the first discrete layer element facing away from the second discrete layer element is protected by a mask and an etchant removes exposed portions of the first discrete layer element and underlying portions of the second discrete layer element.
[0036] Typically, where the first and second discrete layer elements are trimmed in a single process, the process includes a photolithography process. In the process, a photoresist layer can be applied to the surface of the first discrete layer element and exposed to a pattern of light that causes chemical changes within certain portions of the photoresist layer. A solvent (i.e., a developer solution) can then be applied to the photoresist layer, the effect of which varies depending on the chemical changes caused by the light pattern (e.g., a positive photoresist layer becomes more soluble in the developer solution after exposure to ultraviolet light, while a negative photoresist layer becomes less soluble in the developer solution after exposure to ultraviolet light). Thus, a masking layer can be provided on the surface of the first discrete layer element, the masking layer exposing at least a portion of the first discrete layer element, the exposed portion of the first discrete layer element extending around at least a portion of the periphery of the first discrete layer element. Thus, selective etching of the first discrete layer element can be performed, followed by etching of the portion of the second discrete layer element exposed in the process.
[0037] In some cases, the second discrete layer element may be trimmed independently of the first discrete layer element. However, this is less preferred.
[0038] In other cases, the step of modifying the second discrete layer element may include the step of forming a groove in the second discrete layer element, the groove extending in a through-thickness direction of the second discrete layer element and defining a boundary between the modified second discrete layer element and an isolated portion of the second discrete layer element, the isolated portion extending around at least a portion of the periphery of the second discrete layer element.
[0039] Typically, in this case, the modified second discrete layer element is configured to allow it to be electrically connected to an external device, while the isolated portion of the second discrete layer element is configured to remain isolated from the external device. For example, the modified second discrete layer element may provide a portion of the anode contact pad.
[0040] Typically, the groove defines the entire perimeter of the modified second discrete layer element. In fact, in this case, the groove forms a closed loop. In this case, the isolated portion of the second discrete layer element typically extends around the entire perimeter of the second discrete layer element.
[0041] Typically, the trench has a base and sidewalls extending away from the base. The sidewalls are typically aligned with each other, but other configurations are possible, for example, the sidewalls may tend to converge in a direction toward the trench bottom (i.e., the trench may taper in a direction toward the trench bottom).
[0042] In some cases, the trench has a bottom that is in the same plane as the interface between the second discrete layer element and the third discrete layer element. In other cases, the trench extends into the third discrete layer element such that the bottom of the trench is within the third discrete layer element.
[0043] Typically, the trench passes through the first discrete layer element and the second discrete layer element.
[0044] Typically, the grooves are formed by an etching process. Etching can be performed using a dry etching process, such as a plasma etching process. The etching process can be mechanical (e.g., ion beam milling using, for example, an argon plasma) and / or chemical (e.g., reactive ion etching, in which substances such as SF6 are used because they can react with the first and / or second discrete layer elements to produce volatile reaction products). For example, in some cases, a plasma etching process is performed using a plasma containing argon and / or SF6.
[0045] In other cases, the grooves may be formed by laser ablation, for example.
[0046] The step of forming the groove may include a photolithography process. For example, a photoresist layer may be applied to the surface of the first discrete layer element and exposed to a pattern of light that causes chemical changes within certain portions of the photoresist layer. A solvent (i.e., a developer solution) is then typically applied to the photoresist layer, the effect of which varies depending on the chemical changes caused by the light pattern (e.g., a positive photoresist layer becomes more soluble in the developer solution after exposure to ultraviolet light, while a negative photoresist layer becomes less soluble in the developer solution after exposure to ultraviolet light). Therefore, a mask layer is typically provided on the surface of the first discrete layer element, which exposes at least a portion of the first discrete layer element corresponding to the proposed path of the groove. Thus, selective etching of the first discrete layer element can be performed, followed by etching of the portion of the second discrete layer element exposed in the process.
[0047] Typically, the width of the trenches is in the range of 1-100 microns.
[0048] Typically, the cathode layer is disposed on a face of the third discrete layer element opposite the second discrete layer element, and at least a portion of the trench is formed in a portion of the second discrete layer element directly opposite the cathode layer.
[0049] In certain examples of the present methods, the second discrete layer element can be modified by the step of trimming the second discrete layer element around at least a portion of its perimeter and by the step of forming a groove in the second discrete layer element.
[0050] Typically, in the method according to the first aspect of the invention, the steps of removing the through-thickness portion of the first layer to form the first discrete layer element and removing the through-thickness portion of the second layer to form the second discrete layer element are performed in a single process. This may help to improve the efficiency of the patterning process.
[0051] Typically, the step of removing the through-thickness portion of the first layer to form the first discrete layer element includes etching the first layer to expose a portion of the second layer. Typically, the step of removing the through-thickness portion of the second layer to form the second discrete layer element includes etching the second layer to expose a portion of the third layer. In some cases, the same etch can be applied to the first and second layers.
[0052] Typically, the step of removing the through-thickness portion of the first layer includes a photolithography step. That is, a photoresist layer is applied to the surface of the first layer and exposed to a light pattern that causes certain portions of the photoresist layer to undergo chemical changes. A solvent (i.e., a developer solution) is then applied to the photoresist layer, the effect of which varies depending on the chemical changes caused by the light pattern (e.g., a positive photoresist layer becomes more soluble in the developer solution after exposure to ultraviolet light, while a negative photoresist layer becomes less soluble in the developer solution after exposure to ultraviolet light). Thus, a mask layer is provided on the surface of the first layer, allowing selective etching of the first layer to be performed.
[0053] The first and / or second layer can be etched using a dry etching process, such as a plasma etching process. The etching process can be mechanical (e.g., ion beam milling using, for example, an argon plasma) and / or chemical (e.g., reactive ion etching, wherein substances such as SF6 are used because they can react with the first and / or second layer to produce volatile reaction products).
[0054] For example, in some cases, a plasma etching process is performed using a plasma containing argon and / or SF6. It is believed that the plasma exhibits good etching selectivity between amorphous silicon and the solid electrolyte, that is, it etches amorphous silicon at a significantly higher rate than the electrolyte, so that the electrolyte layer (i.e., the third layer) effectively acts as an etching stop layer.
[0055] In some cases, the plasma etch process is performed using a process gas selected from the group consisting of: argon; a mixture of HBr and Cl2; and SF6.
[0056] In other examples of methods according to the invention, the step of removing through-thickness portions of the second layer to form the second discrete layer elements is performed using laser ablation.
[0057] Typically, the step of etching the third layer is performed using an aqueous etchant. The etchant may have a neutral, alkaline or acidic pH. For example, the etchant may be water. In the case where the etchant is an acid, the etchant may be selected from phosphoric acid, sulfuric acid, hydrochloric acid and nitric acid. In the case where the etchant is alkaline, the etchant may be provided by an aqueous potassium hydroxide solution. It is believed that aqueous etchants exhibit good etching selectivity between amorphous silicon and solid electrolytes, that is, they can etch the electrolyte layer (i.e., the third layer) at a rate significantly higher than that of the amorphous silicon layer elements.
[0058] In some cases, the cathode layer is disposed on the face of the third layer opposite the second layer, the cathode layer being provided by a cathode material. For example, during formation of the stack, the electrolyte layer may be deposited on the cathode layer. The cathode material may include, for example, a crystalline oxide.
[0059] The solid electrolyte may be provided by any ionically conductive but electrically insulating material. Typically, the solid electrolyte is provided by a material selected from the group consisting of LiPON, LiSiPON, LiSiCON, Thio-LiSiCON, LiPBON, LiBON, amorphous lithium borosilicate compounds, and doped amorphous lithium borosilicate compounds.
[0060] The first material is typically selected from platinum, nickel, molybdenum, copper, titanium nitride, aluminum, gold and stainless steel. In the case where the first material is provided by a single metal element, the minimum purity of the first material is typically greater than 95 atomic%, preferably greater than 98 atomic%, more preferably greater than 99 atomic%. In this case, the first material can provide the anode current collector of a battery comprising a stack of discrete layer elements provided by the method of the present invention.
[0061] In some cases, the first material is selected from platinum and titanium nitride.
[0062] In some cases, the second layer can have a thickness of at least 700 nanometers. In some cases, the second layer can have a thickness of at least 900 nanometers. Typically, the second layer has a thickness of 2 micrometers or less. In some cases, the second layer has a thickness of 3 micrometers or less. In some cases, the second layer has a thickness of 5 micrometers or less. Thus, for example, the second layer can have a thickness of 500 nanometers to 5 micrometers. In some cases, the second layer can have a thickness of 500 nanometers to 3 micrometers. In some cases, the second layer can have a thickness of 700 nanometers to 3 micrometers. In some cases, the second layer can have a thickness of 900 nanometers to 3 micrometers.
[0063] Where the cathode layer is disposed on the face of the third layer opposite the second layer, the cathode layer may be at least twice as thick as the second layer, and in some cases at least three times as thick as the second layer. In some cases, the cathode layer may be up to ten times as thick as the second layer, and in some cases up to eight times as thick as the second layer. Thus, for example, the cathode layer may be 2-10 times as thick as the second layer, and in some cases 3-8 times as thick as the second layer.
[0064] The thickness ratio of the cathode layer and the second layer (comprising at least 95 atomic % amorphous silicon) is preferably selected so as to balance the capacity ratio between the anode and cathode of a battery comprising these layers. That is, when amorphous silicon is used as an anode in a battery, the thickness ratio is believed to limit the relative volume expansion of the amorphous silicon, which volume expansion is caused by lithiation of the amorphous silicon during battery charging.
[0065] Typically, the thickness of the third layer is in the range of 1-5 microns. In some cases, the thickness of the third layer is in the range of 2-4 microns.
[0066] Typically, the first layer has a thickness in the range of 100-500 nanometers. In some cases, the first layer has a thickness in the range of 200-400 nanometers.
[0067] Generally, the method of the invention may provide a stack of multiple discrete layer elements that are displaced from one another in the plane of the first, second and / or third layer. Typically, the multiple stacks of discrete layer elements are arranged in a regular array on a wafer.
[0068] In a second aspect, the present invention may provide an electrochemical cell comprising at least the following discrete layer elements stacked in the following order:
[0069] a first discrete layer element provided by a first material;
[0070] a second discrete layer element having a thickness of at least 500 nanometers and provided by a second material comprising at least 95 atomic % amorphous silicon;
[0071] a third discrete layer element provided by a solid electrolyte; and
[0072] a fourth discrete layer element comprising cathode active material;
[0073] wherein a groove is provided in the through-thickness direction of the second discrete layer element, the groove having a bottom located at the interface between the second and third discrete layer elements or within the third discrete layer element,
[0074] The trench defines a boundary between the modified second discrete layer element and an isolated portion of the second discrete layer element, the isolated portion extending around at least a portion of a perimeter of the second discrete layer element.
[0075] Typically, the trench defines the entire perimeter of the modified second discrete layer element.
[0076] Typically, the width of the trenches is in the range of 1-100 microns.
[0077] Typically, the trench also extends through the first discrete layer element.
[0078] Typically, the trench has side walls extending from a bottom, the side walls being aligned with each other.
[0079] Typically, at least a portion of the trench is disposed in a portion of the second discrete layer element directly opposite the fourth discrete layer element.
[0080] The solid electrolyte may be provided by any ionically conductive but electrically insulating material. Typically, the solid electrolyte is provided by a material selected from the group consisting of LiPON, LiSiPON, LiSiCON, Thio-LiSiCON, LiPBON, LiBON, amorphous lithium borosilicate compounds, and doped amorphous lithium borosilicate compounds.
[0081] The first material is usually selected from platinum, nickel, molybdenum, copper, titanium nitride, aluminum, gold and stainless steel. In the case where the first material is provided by a single metal element, the minimum purity of the first material is usually greater than 95 atomic%, preferably greater than 98 atomic%, and more preferably greater than 99 atomic%.
[0082] In some cases, the first material is selected from platinum and titanium nitride.
[0083] Typically, the first discrete layer element provides the anode current collector for the electrochemical cell.
[0084] Typically, the cathode active material is provided by a crystalline oxide.
[0085] Typically, the second material comprises at least 98 atomic % amorphous silicon, preferably at least 99 atomic % amorphous silicon. In some cases, the second material consists essentially of amorphous silicon. The term "amorphous" means that the silicon atoms of the second material do not exhibit long-range structural order.
[0086] In some cases, the second discrete layer elements can have a thickness of at least 700 nanometers. In some cases, the second discrete layer elements can have a thickness of at least 900 nanometers. Typically, the second discrete layer elements have a thickness of 2 micrometers or less. In some cases, the second discrete layer elements have a thickness of 3 micrometers or less. In some cases, the second discrete layer elements have a thickness of 5 micrometers or less. Thus, for example, the second discrete layer elements can have a thickness of 500 nanometers to 5 micrometers. In some cases, the second discrete layer elements can have a thickness of 500 nanometers to 3 micrometers. In some cases, the second discrete layer elements can have a thickness of 700 nanometers to 3 micrometers. In some cases, the second discrete layer elements can have a thickness of 900 nanometers to 3 micrometers.
[0087] In some cases, the fourth discrete layer element can be at least twice as thick as the second discrete layer element, and in some cases at least three times as thick as the second discrete layer element. In some cases, the fourth discrete layer element can be up to ten times as thick as the second discrete layer element, and in some cases up to eight times as thick as the second discrete layer element. Thus, for example, the fourth discrete layer element can be 2-10 times as thick as the second discrete layer element, and in some cases 3-8 times as thick as the second discrete layer element.
[0088] The thickness ratio of the fourth discrete layer element (comprising the cathode active material) and the second discrete layer element (comprising at least 95 atomic % amorphous silicon) is preferably selected so as to balance the capacity ratio between the anode and cathode of the electrochemical cell. That is, when the amorphous silicon is used as the anode of the cell, the thickness ratio is believed to limit the relative volume expansion of the amorphous silicon resulting from lithiation of the amorphous silicon during charging of the cell.
[0089] Typically, the third discrete layer element has a thickness in the range of 1-5 microns. In some cases, the third discrete layer element has a thickness in the range of 2-4 microns.
[0090] Typically, the first discrete layer element has a thickness in the range of 100-500 nanometers. In some cases, the first discrete layer element has a thickness in the range of 200-400 nanometers. BRIEF DESCRIPTION OF THE DRAWINGS
[0091] The present invention will now be described by way of example with reference to the following drawings, in which:
[0092] Figures 1 to 7 shows schematic cross-sectional views of assembled battery components at different stages of battery manufacturing incorporating a process of a first example of a method according to the invention;
[0093] Figure 8 shows a schematic cross-sectional view of a battery manufactured according to a process in conjunction with a first example of a method according to the invention;
[0094] Fig. 9 shows a schematic cross-sectional view of a battery manufactured according to a process in conjunction with a second example of a method according to the invention;
[0095] Fig.10 shows a schematic cross-sectional view of a battery manufactured according to a process incorporating a third example of a method according to the invention;
[0096] Fig.11 It is shown that from e.g. Figure 8 A graph of multiple charge and discharge cycles measured for a battery in, as a graph of voltage versus time;
[0097] Fig.12 It is shown that from e.g. Figure 8 The battery shown is a graph of battery capacity measured over multiple charge and discharge cycles. DETAILED DESCRIPTION
[0098] refer to Figure 1-8 , the manufacture of a battery incorporating a process according to a first example of the method of the present invention includes providing a substrate 10 and depositing a layer 12 on the surface of the substrate. The layer 12 includes an adhesive layer and a metal layer. The layer 12 is then etched by a photolithography process to provide a cathode current collector 12a. The photolithography process includes depositing a photoresist layer (not shown) onto the surface of the layer 12, processing the photoresist layer to form a mask, then etching using ion beam milling or wet chemical etching, and then removing the photoresist layer.
[0099] The substrate 10 is typically provided by a sapphire (aluminum oxide) wafer, but other materials such as silicon, glass or ceramics may also be used. When a silicon substrate is used, this may have a passivation layer such as silicon nitride or silicon oxide. The substrate may be provided by a wafer of a non-conductive, semi-conductive or conductive material. In the case where the substrate is provided by a wafer of a semiconductor or conductive material, it is preferred that the wafer surface in contact with the cathode current collector 12 is provided with a non-conductive film.
[0100] refer to Figure 3 and 4 , cathode layer 14 is deposited on cathode current collector 12a and the uncovered surface of substrate 10 (suitable cathode materials are known in the art). The cathode layer is then etched by a photolithography process to provide a cathode 14a having a similar footprint as cathode current collector 12a (e.g., the cathode can typically be slightly larger than the cathode current collector while leaving a portion of the cathode collector uncovered to provide contact pads to allow the battery to be connected to an external device). The photolithography process includes depositing a photoresist layer (not shown) on the surface of layer 14, processing the photoresist layer to form a mask, then etching layer 14, and removing the photoresist layer.
[0101] refer to Figure 5 , a LiPON electrolyte layer 16 is deposited onto the cathode 14a and any uncovered surfaces of the cathode current collector 12a and the substrate 10 by radio frequency sputtering to a thickness of 3 microns. An amorphous silicon (a-Si) layer 18 is deposited onto the electrolyte layer 16 to a thickness of 1 micron using electron beam physical vapor deposition from a target having a purity of at least 99 atomic %. A platinum layer 20 having a thickness of 300 nanometers is deposited onto the silicon layer 18 using direct current sputtering from a target having a purity of at least 99.99 atomic %. The LiPON electrolyte layer 16, the amorphous silicon layer 18, and the platinum layer 20 are deposited in sequence without removing the sample from the vacuum chamber. This helps prevent contamination of the interfaces between the layers 16, 18, and 20.
[0102] refer to Figure 6 , platinum layer 20 and amorphous silicon layer 18 are etched in a single photolithography process to provide anode current collector 20a and anode 18a, respectively. The photolithography process includes depositing a photoresist layer (not shown) on the surface of layer 20, treating the photoresist layer to form a mask, then performing reactive ion etching with an inductively coupled plasma containing SF6, and removing the photoresist layer. The footprint of current collector 20a and anode 18a on substrate 10 is greater than the footprint of cathode 14a.
[0103] refer to Figure 7 , the electrolyte layer 16 is etched using water as an etchant and the combined current collector 20a and anode 18a as a hard mask. The aqueous etchant tends to undercut the hard mask, so that the etched electrolyte layer 16a has a smaller footprint on the substrate 10 than the current collector 20a and the anode 18a. That is, the anode 18a tends to overhang the etched electrolyte layer 16a. However, the footprint of the etched electrolyte layer 16a remains greater than the footprint of the cathode 14a, so that the cathode 14a is completely surrounded by the cathode current collector 12a and the etched electrode layer 16a.
[0104] refer to Figure 8 , the current collector 20a and the anode 18a are trimmed using a photolithographic process to provide a trimmed current collector 20b and a trimmed anode 18b. Thus, the footprint of the current collector and the anode on the substrate is reduced to match the footprint of the etched electrolyte 16a (or, the footprint of the current collector and the anode on the substrate can be reduced to less than the footprint of the etched electrolyte, such as Fig. 9 16a). That is, the trimmed anode 20b no longer overhangs the etched electrolyte 16a. The trimming process includes depositing a photoresist layer (not shown) onto the surface of layer 20, treating the photoresist layer to form a mask, followed by reactive ion etching using an inductively coupled plasma containing SF6, and removing the photoresist layer.
[0105] The trimming process is believed to provide one or both of the following advantages:
[0106] reducing or eliminating the degree of overhang of anode 18a above etched electrolyte 16a, thereby reducing the risk of shorting between cathode 14a and trimmed anode 18b (which might otherwise occur, for example, through contact between anode 18a and cathode current collector 12a); and / or
[0107] • Material around the anode that may have been damaged by the action of the aqueous etchant may be partially or completely removed.
[0108] In another example of the method according to the present invention, the battery components are as described above with reference to Figure 1-7 Assemble and configure as described, then provide Fig.10 The battery shown.
[0109] refer to Fig.10 In an alternative example of the method according to the invention, grooves 22 are created in the current collector and the anode instead of trimming them. The grooves are located within the perimeter of the current collector 20a and the anode 18a (e.g. Figure 7 ) and form a closed loop, dividing each of the current collector and the anode into an active portion and an inactive portion. The active portions 18d, 20d of the anode and the current collector are contained in the closed loop provided by the groove, while the inactive portions 18e and 20e of the anode and the current collector are located outside the loop. Figure 7 As shown, the outer perimeter of the inactive portions 18e, 20e substantially coincides with the perimeter of the current collector 20a and anode 18a.
[0110] In effect, the grooves 22 define the outer periphery of the modified current collector and the modified anode.
[0111] The anode contact pad (not shown) of the cell is disposed within the groove ring so that when the cell is connected to an external device, the active portions 18d, 20d of the anode and current collector form part of an electrical circuit, while the inactive portions 18e, 20e of the anode and current collector are isolated from the electrical circuit. Thus, although portions 18e, 20e of the anode and current collector may overhang the etched electrolyte 16a, the risk of short circuits in the cell is reduced. Furthermore, although the material at the outer peripheral portion 18e of the anode may have been damaged by the action of the aqueous etchant during etching of the electrolyte layer, the material is isolated from the electrical circuit created when the cell is connected to an external device.
[0112] Typically, trench 22 is located directly opposite a portion of cathode 14a, although the portion of trench 22 that defines the contour of the anode contact pad (not shown) is not the case. That is, the majority of the trench is typically located within the footprint of cathode 14a.
[0113] By depositing a photoresist layer (not shown) onto the surface of the current collector 20a (eg Figure 7 The trench is formed by a process of forming a photoresist layer (as shown) and treating the photoresist layer to form a mask that defines the path the trench is to follow. Reactive ion etching is then performed using an inductively coupled plasma containing SF6 and the photoresist layer is removed.
[0114] The bottom of the groove is in the same plane as the interface between the anode and the electrolyte layer 16a. The side walls of the groove extend away from the electrolyte layer 16a and are aligned with each other. The width of the groove is typically 50 microns.
[0115] Fig.11 It is shown that from e.g. Figure 8 Graphs of multiple charge and discharge cycles measured for the battery of FIG. 1 are provided as graphs of voltage versus time. This confirms the good performance of the battery, indicating that the forming process used did not hinder or impair its operation. In particular, it is surprising that the use of the combined current collector 20a and anode 18a as a hard mask during the etching of the electrolyte layer 16 with water did not adversely affect the performance of the amorphous silicon anode.
[0116] Fig.12 A graph showing data from multiple cycles is shown, as for example Figure 8 Figure 2 shows a graph of the charge and discharge capacity measured over the course of a battery cell. The capacity remains at reasonable levels over the cycles with only minor drops, which is comparable to what would be expected from similar conventionally manufactured thin film batteries. This again confirms the good performance of the cell, indicating that the forming process used did not hamper or impair its operation.
[0117] • Anode current collector 20a provides an example of a first discrete layer element as formed in the method according to the first aspect of the invention;
[0118] • Anode 18a provides an example of a second discrete layer element as formed in the method according to the first aspect of the invention;
[0119] • The etched electrolyte layer 16a provides an example of a third discrete layer element as formed in the method according to the first aspect of the invention;
[0120] • The trimmed anode 18b provides an example of a modified second discrete layer element as formed in an alternative variation of the method according to the first aspect of the invention;
[0121] • The active portion 18d of the anode provides another example of a modified second discrete layer element as formed in another alternative variation of the method according to the first aspect of the invention.
Claims
1. A method of processing a stack of layers to provide a stack of discrete layer components, comprising the steps of: A stack is provided, the stack comprising: ■ a first layer provided by a first material; ■ a third layer provided by a solid electrolyte; and ■ a second layer located between the first and third layers, the second layer having a thickness of at least 500 nanometers and being provided by a second material comprising at least 95 atomic % amorphous silicon; removing a through-thickness portion of the first layer to form a first discrete layer element provided by the first material; removing a through-thickness portion of the second layer to form a second discrete layer element provided by a second material, the second discrete layer element being located between the first discrete layer element and the solid electrolyte; and etching the third layer using the second discrete layer element as an etch mask to form a third discrete layer element provided by the solid electrolyte; wherein the first, second and third discrete layer components provide the stack of discrete layer components, wherein the method further comprises the step of modifying the second discrete layer element to provide a modified second discrete layer element after the step of etching the third layer, wherein the perimeter of the modified second discrete layer element encompasses an area that is less than the area encompassed by the perimeter of the second discrete layer element, wherein the step of providing a modified second discrete layer element comprises forming a groove in the second discrete layer element, the groove extending in a through-thickness direction of the second discrete layer element and defining a boundary between the modified second discrete layer element and an isolated portion of the second discrete layer element, the isolated portion extending around at least a portion of a perimeter of the second discrete layer element, And further wherein the trench extends at least as far as the interface between the second discrete layer element and the third discrete layer element such that the bottom of the trench is either in the same plane as the interface between the second discrete layer element and the third discrete layer element or within the third discrete layer element.
2. The method of claim 1, wherein the groove defines the entire perimeter of the modified second discrete layer element.
3. The method according to claim 1, wherein: The trenches are formed by an etching process.
4. The method according to any one of claims 1 to 3, wherein: The width of the grooves is in the range of 1-100 microns.
5. The method according to any one of claims 1 to 3, wherein: The trench has a bottom and sidewalls, the bottom being aligned with the interface between the modified second discrete layer element and the third discrete layer element, and the sidewalls extending in a lateral direction relative to the bottom and aligned with each other.
6. The method according to any one of claims 1 to 3, wherein: A cathode layer is provided on a face of the third discrete layer element opposite the second discrete layer element, and at least a portion of the trench is formed in a portion of the second discrete layer element directly opposite the cathode layer.
7. The method according to any one of the preceding claims 1 to 3, wherein: The steps of removing through-thickness portions of the first layer to form a first discrete layer element and removing through-thickness portions of the second layer to form a second discrete layer element are performed in a single process.
8. The method according to any one of the preceding claims 1 to 3, wherein: The step of removing through-thickness portions of the first layer to form the first discrete layer element and / or removing through-thickness portions of the second layer to form the second discrete layer element comprises etching the respective layers.
9. The method according to claim 8, wherein: The step of removing the through-thickness portion of the first layer includes a photolithography process.
10. The method according to claim 8, wherein: The step of etching the respective layers includes using a dry etching process.
11. The method according to claim 10, wherein: The dry etching process is a plasma etching process.
12. The method according to claim 11, wherein: The plasma etching process is performed using plasma including argon and / or SF6.
13. The method according to any one of claims 1 to 3, wherein: The step of removing through-thickness portions of the second layer to form the second discrete layer elements is performed using laser ablation.
14. The method according to any one of the preceding claims 1 to 3, wherein: The step of etching the third layer is performed using an aqueous etchant having a neutral, alkaline or acidic pH value.
15. The method of claim 14, wherein the etchant is water.
16. The method according to any one of the preceding claims 1 to 3, wherein: The solid electrolyte is provided by a material selected from the group consisting of LiPON, LiSiPON, Thio-LiSiCON, LiBON, an amorphous lithium borosilicate compound, and a doped amorphous lithium borosilicate compound.
17. The method according to any one of the preceding claims 1 to 3, wherein The first material is selected from the group consisting of platinum, nickel, molybdenum, copper, titanium nitride, aluminum, gold, and stainless steel.
18. The method according to any one of the preceding claims 1 to 3, wherein: The second layer has a thickness of at least 700 nanometers.
19. The method according to any one of the preceding claims 1 to 3, wherein: The second layer has a thickness of at least 900 nanometers.
20. The method according to any one of the preceding claims 1 to 3, wherein: A plurality of stacked discrete layer elements are provided that are displaced from one another within the plane of the first, second and / or third layer.
21. The method according to claim 20, wherein: The stacked discrete layer elements are arranged in a regular array on a substrate.
22. An electrochemical cell comprising at least the following discrete layer elements stacked in the following order: a first discrete layer element provided by a first material; a second discrete layer element having a thickness of at least 500 nanometers and provided by a second material comprising at least 95 atomic % amorphous silicon; a third discrete layer element provided by a solid electrolyte; and a fourth discrete layer element comprising cathode active material; wherein a groove is provided in the through-thickness direction of the second discrete layer element, the groove having a bottom at the interface between the second and third discrete layer elements or within the third discrete layer element, The trench defines a boundary between the modified second discrete layer element and an isolated portion of the second discrete layer element, the isolated portion extending around at least a portion of a perimeter of the second discrete layer element.
23. The electrochemical cell of claim 22, wherein: The groove defines the entire perimeter of the modified second discrete layer element.
24. The electrochemical cell according to claim 22, wherein: The width of the grooves is in the range of 1-100 microns.
25. The electrochemical cell according to any one of claims 22 to 24, wherein: The trench additionally extends through the first discrete layer element.
26. The electrochemical cell according to any one of claims 22 to 24, wherein: The trench has side walls extending from the bottom, the side walls being aligned with each other.
27. The electrochemical cell according to any one of claims 22 to 24, wherein: At least a portion of the trench is disposed in a portion of the second discrete layer element that is located directly opposite the fourth discrete layer element.
Citation Information
Patent Citations
Lithium microbattery fabrication method
US9373864B2
Lithium microbattery and method for production thereof
CN102356493A
Thin film battery fabrication using laser shaping
WO2008134053A1