A method for recovering a particle mixture produced by an abrasive wire cutting method
By using a sacrificial carrier made of biodegradable polymer materials for abrasive wire cutting, the problem of silicon powder pollution is solved, and the recycling of high-purity silicon powder and low-cost production is achieved.
Patent Information
- Application Number
- CN202080033661.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-05-06
- Filing Date
- 2020-04-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-04-30
AI Technical Summary
In the existing abrasive wire cutting technology, silicon powder is seriously polluted, especially the pollution caused by metal elements and light elements such as carbon and oxygen in the cutting carrier is difficult to effectively remove, affecting the purity and recycling efficiency of silicon powder.
A sacrificial carrier made of a solvent-soluble biodegradable polymer material is cut by fixing the component to be cut on this carrier and after cutting, the polymer material is dissolved with a solvent to clean and recover the silicon powder.
It significantly reduces powder contamination during cutting, improves the purity and recycling efficiency of silicon powder, reduces production costs, and does not require the use of hazardous chemicals and produces less waste.
Smart Images

Figure CN113853284B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the general field of cutting or sawing by abrasive wire, and more particularly to the field of diamond wire cutting.
[0002] The present invention relates to a sacrificial carrier for cutting a component by an abrasive wire.
[0003] The invention also relates to a method for abrasive wire cutting by using such a carrier and a method for recovering the powder mixture produced by such a cutting method.
[0004] The invention finds application in many industrial fields, in particular in the manufacture of photovoltaic cells, since it makes it possible to obtain thin slices of substrates (called "wafers" or more generally in English "wafers"), for example made of crystalline silicon.
[0005] The present invention is particularly attractive because it allows the production of abrasive wire sawing-generated silicon powder ("kerf") having extremely high purity without increasing production costs. Background Art
[0006] Currently, in the field of photovoltaic cells, 90% to 95% of single-crystalline silicon wafers are cut from silicon ingots using abrasive wire (especially diamond wire) sawing technology.
[0007] The silicon ingot is placed on a so-called sacrificial carrier and cut in the presence of a cutting fluid containing a lubricant that limits heating of the silicon ingot and / or the abrasive wire.
[0008] The ingot slicing is caused by the longitudinal motion of the diamond wire, most commonly a reciprocating motion (with periodic reversals of direction).
[0009] Typically, to perform this operation, the abrasive wire is wound hundreds or even thousands of times around a cylindrical rotating guide with grooves that define the path spacing, forming a wire sheet. In photovoltaic applications, the path spacing is 150 to 300 μm in order to obtain a silicon wafer with a thickness of about 180 μm.
[0010] Each cut uses hundreds or even thousands of meters of cutting wire, which reciprocates in the ingot to be cut, with a low renewal rate per cycle (about 1% to 3% at most). Currently, it takes 2 to 3 hours to saw a silicon block with a side length of 156 mm, which is equivalent to 0.5 to 5 meters per cut silicon wafer.
[0011] During cutting, a large amount of silicon powder (called "kerf") is entrained and suspended in the liquid. For example, using an 80μm abrasive wire to cut a 600mm long silicon ingot into 156×156mm, 180μm thick silicon wafers, the liquid will contain 12kg of silicon chips (seront) at the end of cutting, that is, the mass concentration in the liquid is about 5%. It is estimated that about 36% of the silicon is lost during the cutting process.
[0012] After sawing, this liquid with entrained silicon powder is disposed of as industrial waste. Conventionally, the silicon powder is recovered by filtration and / or centrifugation. The extracted powder can then be reused, for example by recrystallization. In order to address the photovoltaic market, the purity of the silicon powder produced by sawing should be as high as possible.
[0013] However, the silicon powder produced by this cutting method is contaminated by metal elements and light elements such as carbon and oxygen, which affects subsequent crystallization.
[0014] Metallic contamination originates from the cutting carrier. Most cutting carriers contain a polymer resin in which particles are loaded, most commonly aluminum oxide (Al2O3). In order to limit this contamination, one solution is to cut silicon parts on a carrier containing or made of silicon (EP3424663 A1).
[0015] Carbon and oxygen contamination may come from lubricants added to the cutting fluid. In this case, these light elements are present in the form of grafts and can be easily removed by flushing, simple chemical etching (HCl) and / or heat treatment.
[0016] Carbon and oxygen contamination can also come from the polymer resin that forms the cutting carrier. The latter type of contamination is extremely difficult to remove, since most resins do not degrade even in acidic solutions. One solution to avoid this type of contamination is to stop the centrifuge or any other filtration system to collect the powder in-line before the cutting wire cuts into the carrier. However, this solution is not very practical in an industrial environment, since there are usually multiple machines running at the same time and using a centralized cutting fluid supply system. Therefore, it is very difficult to implement or even impossible to manage the filtration stop of multiple equipment to avoid "contaminated" cutting fluid from contaminating the "clean" cutting fluid. Summary of the invention
[0017] An object of the present invention is to propose a sacrificial carrier for abrasive wire sawing that can limit or even eliminate the powder contamination generated during the cutting process, thereby recovering this powder.
[0018] To this end, the invention proposes a sacrificial carrier for cutting a component, preferably made of silicon, by means of an abrasive wire, the sacrificial carrier being made of a biodegradable polymer material soluble in a solvent.
[0019] The fundamental difference between the present invention and the prior art is the use of a sacrificial carrier made of a biodegradable polymer material soluble in a solvent. When using such a carrier, the contamination of powders generated by cutting is significantly reduced compared to the methods of the prior art, so that it is easy to recover these powders. In addition, it is easy to clean and / or peel the cut wafers from the sacrificial carrier, because only the carrier substrate needs to be partially or completely dissolved in a suitable solvent.
[0020] "Carrier" refers to an element having sufficient thickness to be self-supporting.
[0021] According to the EN NF 13432 standard, a "biodegradable polymer" is a polymer material that can be degraded by the enzymatic action of microorganisms into carbon dioxide, inorganic compounds, new biomass and water (in the presence of oxygen) or methane (in the absence of oxygen).
[0022] "Soluble" means that the polymer material contains more than 10% by weight of soluble components, preferably more than 25% by weight, and even more preferably more than 50% by weight in a given solvent and at a given temperature (advantageously, the given temperature is selected in the range of 5° C. to 80° C.) within a period of less than 2 hours, such as less than 1 hour, preferably less than 30 minutes. The polymer material can be completely soluble in a given solvent (i.e., the soluble components are 100%).
[0023] According to a first advantageous embodiment, the biodegradable polymer material is a synthetic polymer (material known as a “biopolymer”).
[0024] Advantageously, the synthetic biodegradable polymer material is PVA or PLA.
[0025] According to a second advantageous embodiment, the biodegradable polymer material is a natural polymer (material known as “agropolymer”), such as an oligosaccharide or a polysaccharide.
[0026] Advantageously, the biodegradable polymeric material is water soluble.
[0027] According to other advantageous embodiments, the biodegradable polymer material can be dissolved in alcohols and / or ketones. It can also be dissolved in so-called green solvents, such as glycerol or fatty acid esters.
[0028] Advantageously, the sacrificial carrier contains a powder dispersed uniformly or non-uniformly. Advantageously, the powder will be selected to be of the same material as the part to be cut on the sacrificial carrier. Advantageously, it is recycled silicon powder. This allows the powder to be recycled ("kerf") while limiting contamination of the part to be cut.
[0029] Advantageously, the sacrificial carrier comprises a longitudinal channel for the passage of the cleaning liquid. Therefore, the cleaning liquid nozzle can be passed in the longitudinal channel, so that the liquid can flow between each wafer, thereby obtaining better cleanliness.
[0030] Advantageously, the sacrificial carrier comprises grooves for mechanical fixing to the plate, in particular to a steel plate. Compared to simple gluing, the mechanical retention of the sacrificial carrier on the plate is improved and the phenomenon of the carrier detaching from the steel plate is avoided.
[0031] Advantageously, the sacrificial support is porous. The porosity will be selected so that the sacrificial support can mechanically support the part to be cut while limiting the amount of material used. In addition, the dissolution kinetics of such a material will be faster than those of a non-porous material, which means that for a large-scale implementation of the process considerable time is saved.
[0032] The invention relates to the use of a carrier as defined above for abrasive wire sawing of a component to be cut, said component preferably being made of silicon.
[0033] The present invention also relates to a method for abrasive wire cutting of a first material component, comprising the following consecutive steps:
[0034] fixing the part to be cut made of a first raw material, preferably silicon, on a sacrificial support of a solvent-soluble, biodegradable polymer material as defined above,
[0035] The component is cut with an abrasive wire, preferably a diamond wire, until a notch is formed in the sacrificial carrier, thereby obtaining a sheet of the first material and a mixture comprising first particles of the first material and second particles of the biodegradable polymer material.
[0036] The cutting method using such a carrier is simple to implement and uses a carrier made of a biodegradable polymer material. Even if particles of the biodegradable polymer material are deposited on the slice, they can be easily removed by dissolving in a solvent such as a washing liquid, for example, water or alcohol at a temperature of 5° C. to 80° C., and preferably at room temperature.
[0037] The present invention also relates to a method for recovering a particle mixture produced by an abrasive wire cutting method, comprising the following consecutive steps:
[0038] providing a mixture of first particles comprising a first material (referred to as key particles) and second particles of a solvent-soluble biodegradable polymer material obtained according to the cutting method as defined above,
[0039] adding a solvent capable of dissolving the second particles of the biodegradable material to the mixture, thereby obtaining a solid phase consisting of the first particles of the first material and a liquid phase comprising the solvent in which the biodegradable polymer material is dissolved,
[0040] The solid phase is separated from the liquid phase, in particular by a centrifugation or filtering step, thereby obtaining a granular powder of the first material.
[0041] Advantageously, the solvent is water.
[0042] Advantageously, the solvent temperature is between 5°C and 80°C.
[0043] Advantageously, the method comprises a subsequent step during which the granular powder of the first material crystallizes, for example in the form of an ingot. The ingot can then be cut with an abrasive wire to form new slices.
[0044] The biodegradable polymer material particles are easily removed by dissolving in a solvent. Advantageously, it is a flushing liquid. At the end of the recovery process, the dissolved polymer material can be resolidified and reused to form a new sacrificial carrier. Solidification can be achieved in a so-called non-solvent fluid (i.e., in which the polymer material is not soluble) and / or by reducing the temperature.
[0045] The recovery method of the key particles is economically attractive. The recovery cost is relatively low, the yield is high, and no hazardous chemicals need to be used, so there is no need to deal with the waste generated by the recovery method. The method generates very little waste.
[0046] With this method, it is easy to purify critical powders, such as silicon. The resulting powder is of better quality and can be reused to make new silicon ingots. This is not possible with silicon powder that is contaminated with elements such as carbon and oxygen, as this would lead to the formation of silicon carbide and silicon oxide during the silicon melting process.
[0047] The powder recovered at the end of the recovery process has a high purity (usually at least 99.99%) and a low carbon and oxygen content (usually [C] < 0.07%, [O] < 0.2%, preferably [C] < 0.004%, [O] < 0.2%) relative to metallic impurities. The ingots obtained with this powder are of good quality.
[0048] The invention also relates to a method for manufacturing a sacrificial carrier as defined above, comprising the step of shaping the biodegradable polymer material, for example by 3D printing or by moulding.
[0049] Other features and advantages of the invention emerge from the further description which follows.
[0050] Obviously, this further description is intended only as an illustration of the object of the present invention and should not be interpreted as limiting this object in any case. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] The invention will be better understood by describing non-limiting embodiments given by way of example only and with reference to the accompanying drawings, in which:
[0052] Figure 1A and Figure 1B Different sacrificial carriers for cutting a component by means of an abrasive wire according to different embodiments of the invention are shown in partial elevational views,
[0053] Figure 2 According to a specific embodiment of the present invention, a component including a sacrificial carrier according to the present invention is shown in a partial front view, wherein the sacrificial carrier is assembled with a plate and supports a part to be cut.
[0054] Figure 3A and Figure 3B The step of cutting the silicon material placed on the sacrificial carrier according to different embodiments of the present invention is shown in perspective view.
[0055] Figure 4 is a graph showing the change in sugar dissolution time as a function of water temperature.
[0056] Figure 5A , Figure 5B , Figure 5C The steps of pressing, trimming and cutting silicon materials according to different embodiments of the present invention are shown in perspective views.
[0057] Figure 6 FIG. 5 is a graph showing the change in volume percentage of PVA dissolved in 80° C. water over time.
[0058] Fig. 7A and Figure 7B Pictures of a sugar sacrificial substrate before and after cutting with diamond wire, respectively, according to one embodiment.
[0059] Fig. 8A and Figure 8B Figures 1 and 2 are pictures of a silicon block mounted on a sugar sacrificial substrate, which itself is placed on a resin plate, before and after cutting with a diamond wire according to one embodiment of the present invention.
[0060] Fig. 9 According to a specific embodiment of the present invention, Fig. 8A Picture of thin silicon slices obtained after cutting of silicon block shown.
[0061] Fig.10 FIG. 1 is a picture of a silicon block fixed on a PVA sacrificial substrate without adhesive according to a specific embodiment of the present invention.
[0062] Fig.11 According to a specific embodiment of the present invention, Fig.10Picture of thin silicon slices obtained after cutting of silicon block shown.
[0063] In order to make the drawings clearer, the various parts shown in the drawings are not necessarily to the same scale.
[0064] The various possibilities (variations and embodiments) are to be understood as not being mutually exclusive and being combinable with one another.
[0065] Additionally, in the following description, directional words such as “above” and “below” the structure are used in consideration of the orientation of the structure as shown in the drawings. DETAILED DESCRIPTION
[0066] In the following, even if the description refers to the wire sawing of crystalline silicon components, preferably single-crystalline silicon components, the invention can also be transferred to the sawing of other material components, for example other semiconductor material components.
[0067] Although this is by no means limiting, the present invention is particularly applicable to the photovoltaic and semiconductor fields.
[0068] Method for cutting the silicon component 30:
[0069] The cutting method comprises the following consecutive steps:
[0070] Providing a sacrificial carrier 10 made of a biodegradable polymer material soluble in a solvent,
[0071] The silicon component 30 to be cut is fixed on the sacrificial carrier 10,
[0072] In the presence of cutting fluid, the crystalline silicon component 30 is cut with an abrasive wire (cutting wire) 20 until a notch is formed on the sacrificial carrier, thereby obtaining a silicon wafer and a mixture of crystalline silicon particle powder and sacrificial carrier 10 particle powder.
[0073] The sacrificial carrier 10 (also referred to as a "beam") used in the wire sawing process is made of a specific material.
[0074] The sacrificial carrier 10 comprises and preferably consists of a biodegradable polymer material 11 ( Figure 1A )constitute.
[0075] Biodegradable polymer material complies with NF EN 13432 standard.
[0076] Biodegradable polymeric materials can be natural polymers. For example, they can be polysaccharides or oligosaccharides, i.e., polymers or oligomers comprising several monosaccharide molecules. Monosaccharides can be, for example, trioses, tetroses, pentoses, hexoses or heptoses. Preferably, they are hexoses, especially fructose or glucose. For example, disaccharides (or disaccharides) will be selected, such as sucrose (commonly referred to as sugar). This can be another processed form of sugar obtained by heating sugar. For example, it can be caramel or charcoal sugar.
[0077] Biodegradable polymeric materials can be synthetic polymers. For example, polyvinyl acetate (PVA), polyglycolic acid (PGA), polylactic-glycolic acid copolymer (PLGA), polyester or copolyester such as polycaprolactone (PCL), polylactic acid (PLA), polybutylene succinate (PBS), poly (butylene succinate-co-adipate) (PBSA), poly (butylene adipate-co-terephthalate) (PBAT). It can also be a copolymer thereof. In PLA, poly-L-lactide (PLLA) and poly-D-lactide (PDLA) can be selected.
[0078] This material has the special property of being able to dissolve in so-called rinsing fluids, which are used to rinse away the silicon dust (also known as “kerf”) produced during the cutting process and recover it for reuse.
[0079] Biodegradable polymer materials are soluble in organic solvents (preferably alcohols or ketones) and / or in water (water-soluble). Advantageously, materials soluble in so-called green solvents such as glycerol or fatty acid esters can be selected. Advantageously, materials soluble in solvents that are extremely low in harm to humans and the environment will be selected.
[0080] Advantageously, the material is soluble in a temperature range of 20°C to 80°C.
[0081] Without contact with a solution in which it is soluble, a material will be selected that is solid at a temperature less than or equal to 50°C, particularly at room temperature (typically 20°C to 25°C). Solid means that it can act as a support during the cutting process and can be cut by diamond wire.
[0082] The sacrificial carrier 10 may also contain particles 12, preferably in contact with the part 30 to be cut ( Figure 1B ). More specifically, the particles 12 are made of a semiconductor material or a semiconductor-based material (that is, their mass ratio in the semiconductor material is at least 50%). According to an advantageous embodiment, the sacrificial carrier 10 is composed of a biodegradable polymer material 11 and particles 12.
[0083] A particle is an element of a shape such as spherical, elongated, ellipsoidal, etc. In the case of spherical particles, the largest dimension corresponds to the diameter. This size can be determined by photon correlation spectroscopy.
[0084] Silicon particle crushed matter having a larger size of 200 μm to 500 μm may be selected.
[0085] Advantageously, recycled silicon particles 12 will be selected from silicon powder collected after cutting with the associated abrasive wire. Such particles have a larger size of less than 10 μm, for example 100 nm to 10 μm, preferably 1 μm to 10 μm.
[0086] The silicon particles 12 combined with the water-soluble material 11 , such as sugar, can advantageously slow down the dissolution of the sacrificial carrier 10 .
[0087] The sacrificial carrier 10 may be porous. For example, it has a porosity of 5% to 50% and / or a pore size of 0.5 μm to 1 mm, preferably 0.1 mm to 0.5 mm. The individual pores may form an interconnected network. The individual pores are open on at least one outer surface of the sacrificial carrier 10.
[0088] The thickness of the sacrificial carrier 10 is between 5 mm and 30 mm, for example, 10 mm to 20 mm. Its length can be between 250 mm and 800 mm, and its width is between 125 mm and 170 mm. The size will be selected according to the size of the part 30 to be cut.
[0089] like Figure 1A , Figure 1B and Figure 2 As shown, the sacrificial carrier 10 may include longitudinal channels 13. The longitudinal channels 13 through which the cleaning liquid passes can effectively clean the silicon wafer. The channels 13 may be arranged to form a honeycomb structure.
[0090] The sacrificial carrier 10 may also comprise mechanical fixing grooves 14 for fixing the sacrificial carrier 10 to a plate 50, in particular a steel plate 50. The steel plate may feed the sacrificial carrier 10 into the wire cutting device. Advantageously, these fixing grooves 6 may allow the carrier 10 to be easily assembled to the plate 50.
[0091] The sacrificial carrier 10, the plate 50 and the part to be cut 30 constitute an assembly 40 ( Figure 2 ).
[0092] The wire-cut sacrificial carrier 10 according to the present invention may include one or more of the above-mentioned features, which may be used alone or in combination according to any feasible technique.
[0093] according to Figure 3AIn the illustrated embodiment, during the cutting process, the component 30 to be cut may be positioned above the sacrificial substrate 10 .
[0094] according to Figure 3B In another embodiment shown, the component 30 to be cut may be placed under the sacrificial substrate 10 .
[0095] The sacrificial substrate 10 may be fixed to the part to be cut 30 by means of glue. The glue will advantageously be chosen so as to limit contamination as much as possible.
[0096] According to another embodiment, the sacrificial substrate 10 can be fixed to the part to be cut 30 without additional adhesive. For example, the sacrificial substrate 10 can be simply wetted with water, the part to be cut 30 is placed on the sacrificial substrate 10, and then dried. After drying, the sacrificial substrate 10 and the part to be cut 30 are connected.
[0097] According to another embodiment, the sacrificial substrate 10 is molded around the part to be cut 30. This embodiment is particularly advantageous because the sacrificial substrate 10 is in direct contact with the part to be cut. There are no intermediate elements, which can reduce contamination.
[0098] Advantageously, the cutting fluid used is an aqueous solution. The aqueous solution may contain a surfactant for cooling and / or lubrication.
[0099] For example, the temperature of the cutting fluid is between 10° C. and 80° C. Advantageously, the temperature of the cutting fluid is room temperature (20° C. to 25° C.).
[0100] When the sacrificial carrier 10 is soluble in the cutting fluid at room temperature, the temperature of the cutting fluid can be lowered to reduce the solubility. For example, for a sugar sacrificial carrier, using a temperature of 10°C during the cutting process will extend the time required for the sugar carrier to dissolve in the cutting fluid by 67% ( Figure 4 ).
[0101] According to a specific embodiment, the surface of the sacrificial carrier 10 can be covered with a thin layer of material, advantageously a hydrophilic material that does not pollute seriously, so as to protect the sacrificial carrier when it is soluble in the cutting fluid. Advantageously, this material blocks the passage of the cutting line 20 at the end of the cut.
[0102] The wire sawing method can be used in all the silicon cutting steps carried out from the simple ingot stage to the substrate (or "wafer" in English) forming stage, the purpose of which is to manufacture photovoltaic cells. Therefore, more precisely, these steps include in sequence:
[0103] i) a briquetting step (also called "squaring"), which corresponds to cutting the ingot 31 into ingots 32 of standardized cross-section by cutting lines 20 arranged in a matrix ( Figure 5A );
[0104] ii) a trimming step (also called "cropping"), which consists in removing the top and bottom of each ingot 32, which contain impurity precipitation resulting from crystallization, which is undesirable in subsequent manufacturing steps ( Figure 5B );
[0105] iii) a step of cutting the ingot 32 (also known as "wafering" or "slicing" in English), which can eventually form a substrate 33 or "slice", wherein the ingot is cut from the top and bottom thereof and has a thickness between 100 μm and 300 μm ( Figure 5C ).
[0106] Wire cutting refers to at least one of the three embodiments of wire cutting, namely: it can be a layer of several wires represented by the term "nappe de fils", including several different cutting wires that are all generally parallel to each other, each wire forming a coil around a rotating member; it can be a single wire forming a single turn; it can also be a single wire wound several times to form a coil of multiple rotating members, thereby defining a layer composed of multiple strands, all of which are generally parallel to each other, and the strand layer is represented by the term "nappe de fil", "Fil" being the singular. Therefore, it is selected according to the type of wire cutting device.
[0107] Wire cutting can be loose abrasive cutting or bonded abrasive cutting.
[0108] In loose abrasive cutting, abrasive particles, usually silicon carbide, are added to a specific solution, such as polyethylene glycol (PEG), to form a cutting fluid (known as "slurry" in English). This cutting fluid is then poured between the cutting wire (usually steel) and the part to be cut. The abrasive particles are set in motion by the relative sliding of these two objects, thereby abrading the material through multiple micro-indentations caused by the abrasive particles rolling on the part to be cut.
[0109] In fixed abrasive sawing, abrasive particles, usually diamond (hence the common term "diamond wire sawing"), are fixed to a sawing wire surface and then drawn across the component material to be cut. This type of sawing would be advantageously chosen for sawing single crystal silicon.
[0110] The silicon powder obtained at the end of the wire sawing process has, for example, a flake-like morphology.
[0111] The mixture of silicon powder and biodegradable polymer material powder is then collected to recover the silicon powder.
[0112] Silicon powder recovery method:
[0113] A method for recovering silicon fume ("kerf") containing particles of biodegradable polymer material, comprising the following consecutive steps:
[0114] providing a mixture comprising silicon powder and particles of a biodegradable polymer material obtained according to the method as defined above,
[0115] adding a solvent capable of dissolving the biodegradable polymer material particles to the mixture, thereby obtaining a solid phase consisting of the first material powder and a liquid phase containing the solvent in which the biodegradable polymer material is dissolved,
[0116] Optionally, the solid phase is separated from the liquid phase, in particular by a centrifugation or filtration step, thereby obtaining a powder of particles of the first material.
[0117] Advantageously, the solvent is a flushing liquid. The solvent is preferably water. No additional fluid needs to be added to dissolve the biodegradable polymer material.
[0118] According to another alternative, the biodegradable polymer material is insoluble in the flushing liquid. Then a solvent needs to be added to the flushing liquid to dissolve the biodegradable polymer material. It can be an organic solvent, such as an alcohol or a ketone.
[0119] The temperature of the solvent and / or the washing liquid is, for example, between 5° C. and 80° C. Preferably, the temperature is between 20° C. and 60° C., for example, at room temperature (ie, 20° C. to 25° C.).
[0120] As an example, for PVA, the solvent may be water. A PVA block with a size of 30×20×5 mm dissolves quickly (in less than 30 minutes) in water at 80°C. Figure 6 ).
[0121] Method for manufacturing sacrificial carrier 10:
[0122] The sacrificial carrier 10 may be manufactured by a three-dimensional printing method (commonly referred to as 3D printing).
[0123] The method consists in locally melting biodegradable polymer threads through a nozzle and depositing them on a substrate, forming mutually adherent threads.
[0124] Alternatively, the sacrificial carrier 10 may be formed by molding.
[0125] Non-limiting illustrative examples of implementations:
[0126] In this example, the substrate 10 is obtained by mixing sucrose mass, dehydrated glucose syrup and water in a volume ratio of 12-4.5-4. The mixture is heated to 150°C to obtain a sugar called barley sugar. The mixture is then poured into individual silicone molds. After cooling, the sugar becomes hard and transparent ( Fig. 7A ). Through the diamond wire 20 ( Figure 7B ) can easily cut the sugar sacrificial carrier 10.
[0127] The substrate 10 was used to cut a silicon block 30 (50×40×40 mm). To this end, the substrate 10 was placed in a research and development diamond wire sawing device (TAKATORI). In this device, the wire sheet 20 was placed above the block to be cut and the block was raised during the cutting process (as described above). Figure 2 ).
[0128] The equipment includes three nozzles: two lateral nozzles spray the wire sheets on both sides of the silicon block, and an upper / central nozzle sprays the silicon block in large quantities. The cutting water is a mixture of tap water and a coolant called Blaser DWS500 with a volume content of 2%.
[0129] The silicon block 30 is bonded to the sugar carrier 10, which itself is bonded to a standard carrier which is fixed to a steel plate 50 of the TAKATORI apparatus by means of adhesive tape (see Fig. 8A ). The glue used in these tests is a glue commonly used in cutting methods, and its trade name is DELO RM885.
[0130] After bonding and drying, the silicon blocks were cut by diamond wire 20 according to the parameters given in the following table:
[0131] Routing speed 500m / min Turntable speed 1.5mm / min Forward / reverse length 200m Line Update 1m / min
[0132] The cutting proceeded smoothly, and the central nozzle stopped a few minutes before the end of the cutting. When there was a lot of lubricant, part of the sugar substrate dissolved in the cutting water flowing under the silicon block ( Figure 8B ). However, the silicon block remains bonded to the sugar sacrificial carrier 10, which itself remains bonded to the substrate to which it is fixed.
[0133] The cutting line tip is removed ( Fig. 9 ).
[0134] The PVA substrate 10 is also manufactured by 3D printing. The surface of the substrate 10 is moistened by spraying a small amount of water, and a silicon block 30 (50×40×40 mm) is placed on the substrate 10. After drying, the silicon block adheres to the substrate 10 ( Fig.10 ). No glue was used in this assembly.
[0135] The silicon block was cut by diamond wire 20 in a TAKATORI machine according to the parameters given in the table below:
[0136] Routing speed 500m / min Turntable speed 1.0mm / min Forward / reverse length 200m Line Update 1m / min
[0137] We obtained high-quality chips ( Fig.11 ).
Claims
1. A method for recovering a particle mixture produced by a method for cutting an abrasive wire (20), comprising the following consecutive steps: A mixture is provided comprising first particles of a first material and second particles of a solvent-soluble biodegradable polymer material (11) obtained by a cutting method of cutting a component (30) of the first material using an abrasive wire (20) comprising the following consecutive steps: A part to be cut (30) made of a first material is fixed on a sacrificial carrier (10) made of a biodegradable polymer material (11) soluble in a solvent, wherein the first material is silicon. cutting the component (30) with the abrasive wire (20), the cutting being carried out until a notch is formed in the sacrificial carrier (10), thereby obtaining a sheet of the first material and a mixture comprising first particles of the first material and second particles of the biodegradable polymer material (11); adding a solvent capable of dissolving the second particles of the biodegradable polymer material (11) to the mixture, thereby obtaining a solid phase consisting of the first particles of the first material and a liquid phase containing the solvent in which the biodegradable polymer material (11) is dissolved; The solid phase is separated from the liquid phase, thereby obtaining a granular powder of the first material.
2. The recycling method according to claim 1, characterized in that: The abrasive wire (20) is a diamond wire.
3. The recycling method according to claim 1, characterized in that: The solid phase is separated from the liquid phase by a centrifugation or filtration step.
4. The recycling method according to claim 1, characterized in that: The solvent is water.
5. The recycling method according to claim 1, characterized in that: The solvent temperature is between 5°C and 80°C.
6. The recycling method according to claim 1, characterized in that: The method comprises a subsequent step during which the granular powder of the first material is crystallized into the form of an ingot.
7. The recovery method according to any one of claims 1 to 6, characterized in that: The recycling method comprises a step of manufacturing the sacrificial carrier (10), wherein the biodegradable polymer material is shaped by 3D printing or by molding.
8. The recovery method according to any one of claims 1 to 6, characterized in that: The biodegradable polymer material (11) is a synthetic polymer.
9. The recycling method according to claim 8, characterized in that: The synthetic polymer is PVA or PLA.
10. The recovery method according to any one of claims 1 to 6, characterized in that: The biodegradable polymer material (11) is a natural polymer.
11. The recycling method according to claim 10, characterized in that: The natural polymers are oligosaccharides.
12. The recovery method according to any one of claims 1 to 6, characterized in that: The biodegradable polymer material (11) is water-soluble.
13. The recovery method according to any one of claims 1 to 6, characterized in that: The sacrificial carrier comprises a powder (12).
14. The recycling method according to claim 13, characterized in that: The powder (12) is a powder of the same material as the component to be cut by abrasive wire.
15. The recovery method according to any one of claims 1 to 6, characterized in that: The sacrificial carrier comprises a longitudinal channel (13) for the passage of a cleaning liquid.
16. The recovery method according to any one of claims 1 to 6, characterized in that: The sacrificial carrier includes a mechanical fixation to the plate (50).
17. The recycling method according to claim 16, characterized in that: The plate (50) is a steel plate.
18. The recovery method according to any one of claims 1 to 6, characterized in that: The sacrificial carrier (10) is porous.
Citation Information
Patent Citations
Wire cutting support for bonded abrasives comprising an assembly of different materials, system comprising such a support and wire cutting methods
EP3424663A1
Pad strip for cutting solar silicon wafer
CN102371631A
Method for increasing utilization rate of crystal bars for crystal plate
CN108724490A
Surface grinding method and surface grinding device using multiwire saw
JP2000288903A
Method of dividing semiconductor wafer
JP2011198875A