High solid content silica sol and its preparation method and application

By adjusting the pH value of silica sol at room temperature and adding silane coupling agent and acetic acid, the problem of solid content and stability of silica sol was solved, and a high-solid-content silica sol was prepared for use in ceramic coatings, achieving high density and good surface properties. Quartz composite ceramic slab of impressive quality.

CN113880096BActive Publication Date: 2024-10-22HUBEI SANJIANG HANGTIAN JIANGBEI MASCH ENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111209960.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-18
Publication Date
2024-10-22
Estimated Expiration
2041-10-18

AI Technical Summary

Technical Problem

Existing silica sol has low solid content, poor particle size uniformity, poor stability, and difficulty in long-term storage, which limits its application in fields such as coatings and catalysis.

Method used

By using magnetic stirring at room temperature, the pH value of the silica sol is gradually adjusted, and a silane coupling agent and acetic acid are added to form a high solid content silica sol to prevent particle agglomeration and improve the solid content and stability.

Benefits of technology

The prepared high-solid-content silica sol has high silica solid content, good particle size uniformity, strong stability, and long storage time. It is suitable for ceramic coatings and can form quartz composite ceramic slabs with high density and good apparent quality at high temperatures. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003308549280000061
    Figure BDA0003308549280000061
  • Figure BDA0003308549280000071
    Figure BDA0003308549280000071
Patent Text Reader

Abstract

The invention discloses a high-solid content silica sol and a preparation method and application thereof. The preparation method comprises S1, adding a certain amount of silica sol into a three-necked flask, stirring at room temperature to obtain liquid A; S2, dropping dilute ammonia water into liquid A under stirring, measuring the pH value of the solution while dropping, until the pH value of liquid A is adjusted to 8.1-8.4, to obtain liquid B; S3, adding a silane coupling agent with a mass ratio of 1:1 to the silica sol under stirring at room temperature, stirring to obtain liquid C; S4, dropping acetic acid into liquid C under magnetic stirring, measuring the pH value of the solution while dropping, until the pH value of liquid C is adjusted to 3.6-3.9, to obtain liquid D; S5, allowing liquid D to stand for reaction at room temperature for 8 hours, to obtain liquid E; S6, adding liquid E to the silica sol according to the designed mass ratio, mixing evenly at room temperature, to obtain a high-solid content silica sol. The silica sol obtained by the method has a high solid content, a theoretically uniform particle size distribution, and a simple preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of inorganic nanomaterials, and in particular to a high-solid content silica sol and a preparation method and application thereof. Background Art

[0002] Silica sol is a material system in which silicon dioxide nanoparticles with excellent performance are uniformly dispersed in water or organic solvents. Due to its network structure formed by countless micelles, it has the characteristics of large specific surface area, high dispersion, and high surface activity. It has been widely used in the coating industry, catalysis industry and other fields.

[0003] However, the currently widely used method for preparing silica sol has encountered great obstacles in practical application due to its low silicon dioxide solid content, poor particle size uniformity, poor stability, and difficulty in long-term storage.

[0004] Based on the above situation, the present invention proposes a high-solid content silica sol and a preparation method and application thereof, which can effectively solve the above problems. Summary of the invention

[0005] In view of the shortcomings of the prior art, the first purpose of the present invention is to provide a high-solid content silica sol, which has the advantages of high silicon dioxide solid content, good particle size uniformity, strong stability, long storage time, etc.

[0006] The second object of the present invention is to provide a method for preparing a high-solid content silica sol. The silica sol obtained by the method has a high solid content, a theoretically uniform particle size distribution and a simple preparation process.

[0007] The second object of the present invention is to provide an application of high solid content silica sol. By placing a ceramic flat plate in the colloidal solution for compounding, a ceramic flat plate with high density and good apparent quality can be obtained.

[0008] In order to solve the above technical problems, the present invention is implemented by the following technical solutions:

[0009] In one aspect, the present invention provides a method for preparing a high solid content silica sol, comprising the following steps:

[0010] S1. Add a certain amount of silica sol into a flask and stir it with magnetic force for a period of time at room temperature to obtain liquid A;

[0011] S2. Add dilute ammonia water dropwise into liquid A under magnetic stirring, and measure the pH value of the solution while adding, until the pH value of liquid A is adjusted to 8.1-8.4, to obtain liquid B;

[0012] S3, adding a silane coupling agent in a mass ratio of 1:1 to the silica sol under magnetic stirring at room temperature, stirring for a period of time, and obtaining liquid C;

[0013] S4, adding acetic acid dropwise into solution C under magnetic stirring, measuring the pH value of the solution while adding dropwise, until the pH value of solution C is adjusted to 3.6-3.9, to obtain solution D;

[0014] S5, leaving solution D to react for a period of time at room temperature to obtain solution E;

[0015] S6. Add liquid E into the silica sol according to the designed mass ratio, mix evenly at room temperature, and obtain a silica sol with a high solid content.

[0016] Preferably, the silica sol is acidic silica sol.

[0017] Preferably, the stirring time in steps S1 and S3 is both 15 minutes.

[0018] Preferably, the mass percentage of the dilute ammonia water in step S2 is 0.05-0.3%.

[0019] Preferably, the silane coupling agent in step S3 is methyltrimethoxysilane.

[0020] Preferably, the D solution in step S5 is allowed to react at room temperature for 8 hours.

[0021] Preferably, the mass percentage of acetic acid in step S4 is 2-4%.

[0022] Preferably, the E solution in step S6 is added to the silica sol in a mass ratio of (4-4.5):(21-22).

[0023] On the other hand, a high-solid content silica sol is provided, which is prepared by the preparation method in the above scheme.

[0024] In another aspect, there is provided an application of high solid content silica sol in ceramic coating, the application method comprising:

[0025] Take an untreated ceramic flat sheet and immerse it in high solid content silica sol, control the sol temperature at 60-80℃, and soak for 6-8h;

[0026] The ceramic flat plate was placed in a muffle furnace, heated to 120°C±10°C at 3°C / min and kept warm for 120min±10min, then heated to 1000°C±20°C at 3°C / min and kept warm for 120min±10min. After cooling to room temperature, the flat plate was taken out and the edges and corners were polished and trimmed according to the product size to obtain a quartz composite ceramic flat plate with a smooth surface and a high solid content.

[0027] Siloxane monomer and nano-SiO 2The reaction can be divided into four stages:

[0028] The first stage: Siloxane undergoes hydrolysis reaction under the action of acid catalyst, and multiple siloxane monomers in the reaction system begin to gradually undergo hydrolysis reaction to produce silanol;

[0029] The second stage: the silanol generated by hydrolysis of siloxane monomer undergoes random polycondensation through dehydration of silanol groups to generate small molecular weight chain oligomers and particles;

[0030] The third stage: small molecular weight chain oligomers and particles and nano-SiO in silica sol 2 The particles are bound together by random polycondensation of the silanol groups on the surface;

[0031] Stage 4: The system continues to generate chain oligomers with larger molecular weight and more nano-SiO 2 The particles undergo a condensation reaction and finally aggregate to form a three-dimensional network structure.

[0032] During the reaction process, the siloxane monomer will undergo a complex hydrolysis and polycondensation process. Factors such as the type and content of siloxane, hydrolysis pH value, type of catalyst, and hydrolysis reaction time will affect the reaction rate of the siloxane compound, and ultimately affect the structure and performance of the prepared high-solid content silica sol.

[0033] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0034] The modification of silica sol this time is to modify silica sol by silane coupling agent (linking inorganic Si and organic components), thus effectively preventing the agglomeration of silica sol particles. Its mechanism of action is: some reactive groups of silane coupling agent react with silanol groups on the surface of silica sol particles to form covalent bonds (introducing organic functional groups), so that the functional groups on the surface of the particles are no longer single, so the solid content of silica sol is improved. DETAILED DESCRIPTION

[0035] In order to enable those skilled in the art to better understand the technical solution of the present invention, the preferred implementation scheme of the present invention is described below in conjunction with specific embodiments, but it should not be understood as a limitation of this patent and is only used as an example.

[0036] The experimental methods or test methods described in the following examples are conventional methods unless otherwise specified; the reagents and materials are obtained from conventional commercial channels or prepared by conventional methods unless otherwise specified.

[0037] The present invention provides a method for preparing a high-solid content silica sol, comprising the following steps:

[0038] S1. Add a certain amount of silica sol into a flask and stir it with magnetic force for a period of time at room temperature to obtain liquid A.

[0039] Preferably, the flask is a three-necked flask, the silica sol is acidic silica sol, and the stirring time is 15 minutes.

[0040] S2. Add dilute ammonia water dropwise into liquid A under magnetic stirring, measuring the pH value of the solution while adding, until the pH of liquid A is adjusted to 8.1-8.4, to obtain liquid B.

[0041] Preferably, the mass percentage of the dilute ammonia water is 0.05-0.3%. The C solution obtained by adding the dilute ammonia water is alkaline, and the alkaline environment can serve as a buffer to prevent the solution from being over-acidic during the subsequent addition of acetic acid, resulting in agglomeration of siloxane when a large amount of hydrolysis occurs.

[0042] S3. Add a silane coupling agent at a mass ratio of 1:1 to the silica sol under magnetic stirring at room temperature, and stir for a period of time to obtain liquid C.

[0043] Preferably, the silane coupling agent is methyltrimethoxysilane (MTMS), and the stirring time is 15 minutes.

[0044] S4. Add acetic acid dropwise into liquid C under magnetic stirring, measuring the pH value of the solution while adding, until the pH of liquid C is adjusted to 3.6-3.9, to obtain liquid D.

[0045] Preferably, the mass percentage of the acetic acid is 2-4%.

[0046] S5. After leaving solution D to react for a period of time at room temperature, solution E is obtained.

[0047] Preferably, the D solution is allowed to react at room temperature for 8 hours.

[0048] S6. Add liquid E into the silica sol according to the designed mass ratio, mix evenly at room temperature, and obtain a silica sol with a high solid content.

[0049] Preferably, the E liquid is added to the silica sol in a mass ratio of (4-4.5):(21-22).

[0050] In addition, the present invention also provides a high-solid content silica sol prepared by the above method, which has the advantages of high silicon dioxide solid content, good particle size uniformity, strong stability, long storage time, etc.

[0051] The high solid content silica sol of the present invention can be applied to ceramic coatings, and the application method includes:

[0052] Take an untreated ceramic flat sheet and immerse it in high solid content silica sol, control the sol temperature at 60-80℃, and soak for 6-8h;

[0053] The ceramic flat plate was placed in a muffle furnace, heated to 120°C±10°C at 3°C / min and kept warm for 120min±10min, then heated to 1000°C±20°C at 3°C / min and kept warm for 120min±10min. After cooling to room temperature, the flat plate was taken out and the edges and corners were polished and trimmed according to the product size to obtain a quartz composite ceramic flat plate with a smooth surface and a high solid content.

[0054] It should be noted that the silica sol and silane coupling agent used in the following examples are all commercially available products.

[0055] Embodiment 1:

[0056] 1) Raw material preparation: methyltrimethoxysilane (MTMS), silica sol HP4010A, dilute ammonia water, acetic acid.

[0057] 2) Add 2 kg of silica sol HP4010A into a three-necked flask and stir with magnetic force for 15 min at room temperature to obtain liquid A;

[0058] 3) Add 0.1% by weight of dilute ammonia water into solution A under magnetic stirring, and measure the pH value of the solution while adding until the pH value of solution A is adjusted to 8.1 to obtain solution B;

[0059] 4) Add 2 kg of methyltrimethoxysilane (MTMS) under magnetic stirring at room temperature and stir for 15 min to obtain liquid C;

[0060] 5) Add 2% by weight acetic acid dropwise into solution C under magnetic stirring, and measure the pH value of the solution while adding until the pH value of solution C is adjusted to 3.6, to obtain solution D;

[0061] 6) Solution D was allowed to react at room temperature for 8 hours to obtain Solution E;

[0062] 7) Add liquid E to 21 kg of HP4010A high-purity silica sol and mix well at room temperature to obtain 25 kg of silica sol with high solid content.

[0063] The high solid content silica sol prepared above is applied to ceramic coatings, and the specific steps are as follows:

[0064] A 100×100×30mm ceramic flat blank was immersed in high solid content silica sol, the sol temperature was controlled at 80℃, and the sol was immersed for 8h;

[0065] The ceramic plate was placed in a muffle furnace, heated to 120°C at 3°C / min and kept warm for 120min±10min, then heated to 1000°C±20°C at 3°C / min and kept warm for 120min±10min. After cooling to room temperature, the plate was taken out and polished to obtain a high solid content quartz composite ceramic plate. The density of the ceramic plate was measured to be 1.86g / cm 3 The surface quality is good, without pits, slag, etc. The performance of the samples was tested, and the results are shown in Table 1.

[0066] Table 1 Performance test results

[0067]

[0068] Embodiment 2:

[0069] 1) Raw material preparation: methyltrimethoxysilane (MTMS), silica sol HP4010A, dilute ammonia water, acetic acid.

[0070] 2) Add 4 kg of silica sol HP4010A into a three-necked flask and stir with magnetic force for 15 min at room temperature to obtain liquid A;

[0071] 3) Add 0.2% by weight of dilute ammonia water into solution A under magnetic stirring, and measure the pH value of the solution while adding until the pH value of solution A is adjusted to 8.2 to obtain solution B;

[0072] 4) adding 4 kg of methyltrimethoxysilane (MTMS) under magnetic stirring at room temperature and stirring for 15 min to obtain liquid C;

[0073] 5) 3% by weight acetic acid was added dropwise into solution C under magnetic stirring, and the pH value of the solution was measured while adding the acetic acid, until the pH value of solution C was adjusted to 3.7, to obtain solution D;

[0074] 6) Solution D was allowed to react at room temperature for 8 hours to obtain Solution E;

[0075] 7) Add liquid E to 42 kg of HP4010A high-purity silica sol and mix well at room temperature to obtain 50 kg of silica sol with high solid content.

[0076] The high solid content silica sol prepared above is applied to ceramic coatings, and the specific steps are as follows:

[0077] A 100×100×30 mm ceramic flat sheet was immersed in a high solid content silica sol, the sol temperature was controlled at 70°C, and the sol was immersed for 7 hours.

[0078] The ceramic plate was placed in a muffle furnace, heated to 120°C ± 10°C at 3°C / min and kept warm for 120min ± 10min, then heated to 1000°C ± 20°C at 3°C / min and kept warm for 120min ± 10min, then cooled to room temperature and taken out, and the edges and corners were polished and trimmed according to the product size to obtain a quartz composite ceramic plate with high solid content. The density of the ceramic plate was measured to be 1.84g / cm 3 The surface quality is good, without pits, slag, etc. The performance of the samples was tested, and the results are shown in Table 2.

[0079] Table 2 Performance test results

[0080]

[0081] Embodiment 3:

[0082] 1) Raw material preparation: methyltrimethoxysilane (MTMS), silica sol HP4010A, dilute ammonia water, acetic acid;

[0083] 2) Add 2 kg of silica sol HP4010A into a three-necked flask and stir with magnetic force for 15 min at room temperature to obtain liquid A;

[0084] 3) Add 0.3% by mass of dilute ammonia water into solution A under magnetic stirring, and measure the pH value of the solution while adding, until the pH value of solution A is adjusted to 8.4, to obtain solution B;

[0085] 4) Add 2 kg of methyltrimethoxysilane (MTMS) under magnetic stirring at room temperature and stir for 15 min to obtain liquid C;

[0086] 5) 4% by weight acetic acid was added dropwise into solution C under magnetic stirring, and the pH value of the solution was measured while adding the acetic acid, until the pH value of solution C was adjusted to 3.9, to obtain solution D;

[0087] 6) Solution D was allowed to react at room temperature for 8 hours to obtain Solution E;

[0088] 7) Add liquid E to 21 kg of HP4010A high-purity silica sol and mix well at room temperature to obtain 25 kg of silica sol with high solid content.

[0089] The high solid content silica sol prepared above is applied to ceramic coatings, and the specific steps are as follows:

[0090] A 100×100×30 mm ceramic plate was immersed in high solid content silica sol, the sol temperature was controlled at 60°C, and the sol was immersed for 6 hours.

[0091] The ceramic plate was placed in a muffle furnace, heated to 120°C at 3°C / min and kept warm for 120min±10min, then heated to 1000°C±20°C at 3°C / min and kept warm for 120min±10min, then cooled to room temperature and taken out, and the ceramic plate after impregnation and compounding was polished and trimmed to obtain a quartz composite ceramic plate with high solid content. The density of the ceramic plate was measured to be 1.85g / cm 3 The surface quality is good, without pits, slag, etc. The performance of the samples was tested, and the results are shown in Table 3.

[0092] Table 3 Performance test results

[0093] Serial number project unit Test Results 1 density <![CDATA[g / cm 3 ]]> 1.85 2 Bending Strength MPa 66 3 Tensile Strength MPa 48 4 Linear expansion coefficient <![CDATA[×10 -6 / ℃]]> 0.24 5 Thermal conductivity W / m·k 0.51 6 Dielectric constant (15~17GHz) / 3.3 7 Loss tangent (15~17GHz) / 0.0004

[0094] The above are only preferred embodiments of the present invention. It should be noted that the above preferred embodiments should not be regarded as limiting the present invention, and the protection scope of the present invention should be based on the scope defined by the claims. For ordinary technicians in this technical field, several improvements and modifications can be made without departing from the spirit and scope of the present invention, and these improvements and modifications should also be regarded as the protection scope of the present invention.

Claims

1. An application of high solid content silica sol, characterized in that: The preparation method of high solid content silica sol comprises the following steps: S1. Add a certain amount of silica sol into a flask and stir it with magnetic force for a period of time at room temperature to obtain liquid A; S2, adding dilute ammonia water dropwise into liquid A under magnetic stirring, measuring the pH value of the solution while adding, until the pH value of liquid A is adjusted to 8.1-8.4, to obtain liquid B; the mass percentage of the dilute ammonia water in step S2 is 0.05-0.3%; S3, adding a silane coupling agent in a mass ratio of 1:1 to the silica sol under magnetic stirring at room temperature, stirring for a period of time, and obtaining liquid C; S4, adding acetic acid dropwise into solution C under magnetic stirring, measuring the pH value of the solution while adding dropwise, until the pH value of solution C is adjusted to 3.6-3.9, to obtain solution D; S5, leaving solution D to react for a period of time at room temperature to obtain solution E; S6. Adding liquid E to the silica sol according to the designed mass ratio, and mixing them evenly at room temperature to obtain a silica sol with a high solid content; the silica sol is an acidic silica sol; The application methods of high solid content silica sol in ceramic coatings include: Take an untreated ceramic flat sheet and immerse it in high solid content silica sol, control the sol temperature at 60-80℃, and soak for 6-8h; The ceramic flat plate was placed in a muffle furnace, heated to 120°C±10°C at 3°C / min and kept warm for 120min±10min, then heated to 1000°C±20°C at 3°C / min and kept warm for 120min±10min. After cooling to room temperature, the flat plate was taken out and the edges and corners were polished and trimmed according to the product size to obtain a quartz composite ceramic flat plate with a smooth surface and a high solid content.

2. The use of the high solid content silica sol according to claim 1, characterized in that: The stirring time in steps S1 and S3 is 15 minutes.

3. The use of the high solid content silica sol according to claim 1, characterized in that: The silane coupling agent in step S3 is methyltrimethoxysilane.

4. The use of the high solid content silica sol according to claim 1, characterized in that: The mass percentage of acetic acid in step S4 is 2-4%.

5. The use of the high solid content silica sol according to claim 1, characterized in that: The D solution in step S5 is allowed to react at room temperature for 8 hours.

6. The use of the high solid content silica sol according to claim 1, characterized in that: The E solution in step S6 is added to the silica sol in a mass ratio of (4-4.5):(21-22).

7. A high solid content silica sol, characterized in that: The preparation method is described in any one of claims 1 to 6.