A high-transmittance and high-fog light diffusion plate and a manufacturing method thereof
By adding an appropriate amount of silicone-type microsphere diffusant and titanium dioxide to the optical grade transparent resin, and using a specific molding process, a high light transmission and high haze light diffusion plate is prepared, which solves the light transmission in the prior art The problem of insufficient rate and haze achieves more efficient light diffusion effect and lower production costs.
Patent Information
- Application Number
- CN202111323646.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-11-09
AI Technical Summary
In the prior art, in order to pursue thinner light diffusion plates, the light diffusion effect of the diffusion plate is not ideal enough, especially when using high-brightness LED lamp beads and thinner products.
Optical grade transparent resin as the main material, combined with 0.1%-3% silicone microsphere diffuser and 0.015%-0.02% titanium dioxide, a thickness of 0.05mm-5mm was prepared through specific mixing and molding processes. High-transmittance and high-fog-type light diffusion plate, with a light transmittance of 75%-85%, haze ≥95%, and a light effect of 72%-80%.
While ensuring high light transmittance and haze, production costs are reduced, light diffusion effect is improved, and the problem of insufficient haze of traditional diffusion plates under high-brightness lamp beads and thin products is solved.
Smart Images

Figure BDA0003346130130000021 
Figure BDA0003346130130000031 
Figure BDA0003346130130000051
Abstract
Description
Technical field:
[0001] The present invention relates to the field of display technology, and in particular to a high-transmittance and high-fog light diffusion plate and a manufacturing method thereof. Background technology:
[0002] With the improvement of chip and LED molding technology, the brightness of LED lamp beads has increased from 80-100lm / w to 150-220lm / w high-brightness lamp beads are commonly used in recent years. Higher brightness requires materials with higher diffusion effects. At the same time, lighting and display products are pursuing thinner product thickness.
[0003] Traditional diffusers use transparent resins such as PC, PS, and PMMA, and achieve light diffusion through surface frosting or array structures, adding 2.0-3.0um silicone or polymethyl methacrylate diffusers inside, and adding a large amount of inorganic powder. The wavelength of visible light is 380-760nm, and the efficiency of scattering and refraction of light of different wavelengths at the same particle size varies greatly. Therefore, adding a single particle size diffuser to achieve a diffusion effect requires a large amount of addition, and the addition ratio of the diffuser to the resin reaches saturation between 1.6-1.8. Further addition does not improve the diffusion function, so ordinary diffusion materials usually further add 0.05-0.15 inorganic powder to reduce light transmittance; but these still cannot solve the problem of insufficient haze faced by diffusers in the lighting and display industries when using high-brightness lamp beads and thinner products. Summary of the invention:
[0004] The present invention aims to solve the problems of reduced light transmittance and insufficient haze caused by the pursuit of a thinner light diffuser in the prior art.
[0005] In view of the shortcomings of the prior art, the present invention provides a high-transmittance and high-fog light diffusion plate, which is made of optical grade transparent resin as the main material and includes the following components in percentage by mass:
[0006] Optical grade transparent resin: 97%-99.9%;
[0007] Diffusion aid: 0.1%-3%.
[0008] The optical grade transparent resin of the high-transmittance and high-fog light diffusion plate of the present invention is one or a mixture of polycarbonate, polyethylene terephthalate, copolymer resin and polystyrene.
[0009] The high-transmittance and high-fog light diffusion plate described in the present invention, wherein the diffusion aid is a silicone microsphere diffuser with a refractive index of 1.4-1.45, and is composed of 10%-30% of a 0.8-1.0um particle size diffusion aid, 50%-70% of a 1.6-1.9um particle size diffusion aid, 10%-20% of a 2.0-2.5um particle size light diffuser, and 0.015%-0.02% titanium dioxide.
[0010] The high-transmittance and high-fog light diffuser sheet of the present invention has a thickness of 0.05mm-5mm, a light transmittance of 75%-85%, a haze ≥95%, and a light efficiency of 72%-80%.
[0011] Another object of the present invention is to provide a method for manufacturing the high-transmittance and high-fog light diffusion sheet as described above, using optical grade transparent resin as the main material, which comprises the following method steps:
[0012] (1) Making masterbatch: A certain proportion of diffusion particles are fully mixed with optical grade transparent resin, and then put into a low shear high mixing special masterbatch machine, melted at high temperature, extruded through a melting pipe, cooled and cut into pellets as diffusion raw materials;
[0013] (2) Making titanium dioxide masterbatch: fully mix optical grade transparent resin and titanium dioxide in a certain proportion;
[0014] (3) Batching: fully mix the prepared masterbatch, titanium dioxide masterbatch and optical grade transparent resin according to the required proportion of the product;
[0015] (3) Melting: Add the mixed materials into the optical film extruder, and melt and further mix them evenly through the extruder;
[0016] (4) Casting: The molten resin flows out through a film die to form a hot film of a certain width;
[0017] (5) Microstructure and texture molding: The molten raw material flowing out of the mold flows into the calendering forming roller group, and is pressed into a diffusion plate with uniform thickness through several calendering rollers with adjusted gaps. One side of the diffusion plate has a texture with a microstructure diffusion structure, and the other side has a texture with a fine-grain structure.
[0018] Preferably, in step (1), the mass ratio of the optical grade transparent resin to the diffusion particles is 92:8.
[0019] Preferably, in step (2), the mass ratio of the optical grade transparent resin to the titanium dioxide is 99.5:0.5.
[0020] Preferably, in step (3), the color masterbatch comprises 0.8%-24%, the titanium dioxide masterbatch comprises 3%-4%, and the optical grade transparent resin comprises 72%-96.2%.
[0021] At the same haze, the high-transmittance and high-fog light diffuser sheet manufactured by the method of the present invention is compared with the diffuser sheet prepared by the traditional method. The results are shown in Table 1 below.
[0022] Table 1,
[0023]
[0024]
[0025] Conclusion: Under the condition of similar haze, the high-transmittance and high-fog light diffusion plate provided by the present invention has lower cost, higher light transmittance and better light effect.
[0026] The invention provides a high-transmittance and high-fog light diffusion plate and a manufacturing method thereof, which have the following beneficial effects compared with the prior art:
[0027] Compared with the common diffusion plates on the market that require thicker and higher proportion of diffusion materials or reduce the transparency of the materials, the present invention customizes the corresponding diffusion material combination according to the spectral distribution of the LED light source to achieve the best diffusion effect, uniform light transmittance, good diffusion effect, and low additive content, which reduces the production cost and solves the problem of insufficient haze faced by the diffusion plate when using high-brightness lamp beads and thinner products in the lighting and display industries. Specific implementation method:
[0028] The present invention is further described in detail below in conjunction with specific implementation modes.
[0029] The following examples will help to further understand the present invention, but do not limit the content of the present invention. Unless otherwise specified in the examples, all unspecified parts refer to mass or mass ratio.
[0030] The invention discloses a high-transmittance and high-fog light diffusion plate, which is mainly made of optical-grade transparent resin and includes the following components in percentage by mass:
[0031] Optical grade transparent resin: 97%-99.9%; the optical grade transparent resin is one or a mixture of polycarbonate, polyethylene terephthalate, copolymer resin, polystyrene;
[0032] Diffusion aid: 0.1%-3%; the diffusion aid is a silicone microsphere diffuser with a refractive index of 1.4-1.45, and is composed of 10%-30% of a 0.8-1.0um particle size diffusion aid, 50%-70% of a 1.6-1.9um particle size diffusion aid, 10%-20% of a 2.0-2.5um particle size light diffuser, and 0.015%-0.02% titanium dioxide.
[0033] The high-transmittance and high-fog light diffusion plate of the present invention has a thickness of 0.05 mm to 5 mm, a light transmittance of 75% to 85%, a haze of ≥95%, and a light efficiency of 72% to 80%.
[0034] Specific manufacturing method:
[0035] (1) Preparation of masterbatch: The diffusion particles and optical grade transparent resin are fully mixed in a mass ratio of 8:92, and then put into a low shear high mixing special masterbatch machine, melted at high temperature, extruded through a melting pipe, cooled and cut into pellets as diffusion raw materials;
[0036] (2) Preparation of titanium dioxide masterbatch: optical grade transparent resin and titanium dioxide are fully mixed in a mass ratio of 99.5:0.5;
[0037] (3) Ingredients: 0.8%-24% of the prepared masterbatch, 3%-4% of the titanium dioxide masterbatch and 72%-96.2% of the optical grade transparent resin are fully mixed;
[0038] (3) Melting: Add the mixed materials into the optical film extruder, and melt and further mix them evenly through the extruder;
[0039] (4) Casting: The molten resin flows out through a film die to form a hot film of a certain width;
[0040] (5) Microstructure and texture molding: The molten raw material flowing out of the mold flows into the calendering forming roller group, and is pressed into a diffusion plate with uniform thickness through several calendering rollers with adjusted gaps. One side of the diffusion plate has a texture with a microstructure diffusion structure, and the other side has a texture with a fine-grain structure.
[0041] The single-layer diffusion plate of the high-transmittance and high-fog light diffusion plate manufactured by the present invention is the most economical and efficient production method, but is not limited to the two-layer or three-layer composite co-extrusion of the listed materials.
[0042] The matters not described in the following embodiments are the same as those in the specific implementation mode.
[0043] Embodiment 1:
[0044] A high-transmittance and high-fog light diffusion plate and a manufacturing method thereof of the present invention are manufactured as follows:
[0045] (1) Preparation of masterbatch: The diffusion particles and optical grade transparent resin are fully mixed in a mass ratio of 8:92, and then put into a low shear high mixing special masterbatch machine, melted at high temperature, extruded through a melting pipe, cooled and cut into pellets as diffusion raw materials;
[0046] (2) Preparation of titanium dioxide masterbatch: optical grade transparent resin and titanium dioxide are fully mixed in a mass ratio of 99.5:0.5;
[0047] (3) Ingredients: 15% of the prepared masterbatch, 3% of the titanium dioxide masterbatch and 82% of the optical grade transparent resin are fully mixed;
[0048] (3) Melting: Add the mixed materials into the optical film extruder, and melt and further mix them evenly through the extruder;
[0049] (4) Casting: The molten resin flows out through a film die to form a hot film of a certain width;
[0050] (5) Microstructure and texture molding: The molten raw material flowing out of the mold flows into the calendering roller group, and is pressed into a diffusion sheet with a thickness of 0.5 mm by several calendering rollers with adjusted gaps. One side of the diffusion sheet has a texture with a microstructure diffusion structure, and the other side has a texture with a fine-grain structure.
[0051] Under the conditions of temperature 23℃ and humidity 55%RH, the tested data are as shown in Table 2:
[0052] Table 2,
[0053]
[0054] Embodiment 2:
[0055] A high-transmittance and high-fog light diffusion plate and a manufacturing method thereof in this example are manufactured as follows:
[0056] (1) Preparation of masterbatch: The diffusion particles and optical grade transparent resin are fully mixed in a mass ratio of 8:92, and then put into a low shear high mixing special masterbatch machine, melted at high temperature, extruded through a melting pipe, cooled and cut into pellets as diffusion raw materials;
[0057] (2) Preparation of titanium dioxide masterbatch: optical grade transparent resin and titanium dioxide are fully mixed in a mass ratio of 99.5:0.5;
[0058] (3) Ingredients: 6% of the prepared masterbatch, 3% of the titanium dioxide masterbatch and 91% of the optical grade transparent resin are fully mixed;
[0059] (3) Melting: Add the mixed materials into the optical film extruder, and melt and further mix them evenly through the extruder;
[0060] (4) Casting: The molten resin flows out through a film die to form a hot film of a certain width;
[0061] (5) Microstructure and texture molding: The molten raw material flowing out of the mold flows into the calendering forming roller group, and is pressed into a diffusion plate with a thickness of 2.0 mm by several calendering rollers with adjusted gaps. One side of the diffusion plate has a texture with a microstructure diffusion structure, and the other side has a texture with a fine-grain structure.
[0062] Under the conditions of temperature 23°C and humidity 55%RH, the tested data are shown in Table 3:
[0063] Table 3,
[0064]
[0065]
[0066] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the best embodiment, a person skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A high-transmittance and high-fog light diffusion sheet, characterized in that: It includes the following components in percentage by mass: Optical grade transparent resin: 97%-99.9%; Diffusion aid: 0.1%-3%; The optical grade transparent resin is one or a mixture of polycarbonate, polyethylene terephthalate, copolymer resin, and polystyrene; The diffusion aid is a silicone microsphere diffusion agent with a refractive index of 1.4-1.45, and is composed of 10%-30% of a 0.8-1.0um particle size diffusion aid, 50%-70% of a 1.6-1.9um particle size diffusion aid, 10%-20% of a 2.0-2.5um particle size light diffuser, and 0.015%-0.02% titanium dioxide; The high-transmittance and high-fog light diffusion plate has a thickness of 0.05mm-5mm, a light transmittance of 75%-85%, a haze ≥95%, and a light efficiency of 72%-80%.
2. A method for manufacturing a high-transmittance and high-fog light diffuser sheet as claimed in claim 1, characterized in that: The steps are as follows: (1) Making masterbatch: A certain proportion of diffusion particles are fully mixed with optical grade transparent resin, and then put into a low shear and high mixing special masterbatch machine, melted at high temperature, extruded through a melting pipe, cooled and cut into pellets as diffusion raw materials; (2) Preparation of titanium dioxide masterbatch: fully mix optical grade transparent resin and titanium dioxide in a certain proportion; (3) Batching: Fully mix the prepared masterbatch, titanium dioxide masterbatch and optical grade transparent resin according to the required proportion of the product; (4) Melting: Add the mixed materials into the optical film extruder, and then melt and further mix them evenly through the extruder; (5) Casting: The molten resin flows out through the film mold to form a hot film of a certain width; (6) Microstructure and texture molding: The molten raw material flowing out of the mold flows into the calendering roller group, and is pressed into a diffusion plate with uniform thickness through several calendering rollers with adjusted gaps. One side of the diffusion plate has a texture with a microstructure diffusion structure, and the other side has a texture with a fine grain structure; In step (1), the mass ratio of the optical grade transparent resin to the diffusion particles is 92:8; In step (2), the mass ratio of the optical grade transparent resin to the titanium dioxide is 99.5:0.5; In the step (3), the color masterbatch is 0.8%-24%, the titanium dioxide masterbatch is 3%-4%, and the optical grade transparent resin is 72%-96.2%.
Citation Information
Patent Citations
Light diffusion plate masterbatch, light diffusion plate and manufacturing method thereof
CN105001609A
Preparation method of high-transmittance high-haze light diffusion film
CN106405698A
Light diffusion plate and preparation method thereof
CN108841079A
Light diffusion plate and preparation method thereof
CN109438832A
Diffusion film for printing display and preparation method thereof
CN113504592A