A vanadium-based MXene-based sericin memristor and its preparation method
By introducing vanadium-based MXene material into sericin memristors, the problems of poor cycle stability and high energy consumption are solved, and the sericin memristor with low power consumption and high stability is realized, which is suitable for brain-like computing systems low energy consumption and high density storage applications.
Patent Information
- Application Number
- CN202111148583.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-09-29
AI Technical Summary
The existing sericin-based memristors have problems such as poor cyclic stability, slow information storage and rewritten speed and high working energy consumption, and are costly, making it difficult to meet the needs of brain-like computing systems.
Vanadium-based MXene material is introduced into the resistive layer of the sericin memristor, and a vanadium-based MXene film is prepared by magnetron sputtering and spin coating technology to regulate the on and off of conductive filaments and improve the performance of the device.
It realizes low power consumption, good stability and low cost sericin memristor, has good biocompatibility and high integration, and is suitable for low energy consumption and high density integrated storage electronic devices.
Smart Images

Figure CN113889575B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a vanadium-based MXene-based sericin memristor and a preparation method thereof, belonging to the technical field of microelectronic devices. Background Art
[0002] In this era of big data, traditional von Neumann computing systems have encountered some technical bottlenecks, such as storage and computing separation, high energy consumption and poor computing power. Therefore, brain-like computer systems have great potential in replacing traditional von Neumann computing systems due to their advantages such as parallel computing, low power consumption and high energy efficiency. Many different types of electronic devices, such as memristors, are used to simulate synapses and neurons in the human brain to build the basic unit of brain-like computing systems. Memristors are the fourth basic passive circuit element besides resistors, capacitors and inductors proposed by Professor Cai Shaotang from the perspective of circuit theory completeness. Memristors are nonlinear devices that can switch back and forth between high and low resistance states under the action of an external electric field, and their current-voltage relationship forms a typical figure-eight hysteresis curve. It has a simple structure, high operating speed, low power consumption and can be used for high-density three-dimensional integration. It can realize data calculation and storage at the same time, so it is expected to be applied to brain-like computing systems to break through the limitations of the "von Neumann architecture".
[0003] In the past, the resistive layer of memristors was generally made of various semiconductor and insulator materials, such as halogen oxide, tantalum oxide, silicon oxide, etc. However, using semiconductor and insulator materials as resistive materials is costly, difficult to recycle, and has low sustainable utilization rates. Some of these materials are also toxic and have negative effects on the environment and human body.
[0004] Therefore, in order to cater to the application trend of information electronic devices in the fields of flexible wearable and implantable in the body in the new era, organic protein devices are increasingly favored because of their good biocompatibility, adjustable biodegradability, diverse regenerative morphology and excellent mechanical properties. When organic protein materials, such as silk materials, are used to construct memristors, these protein-based memristors often have problems such as poor cycle stability, slow information storage and erasing speed, and high working energy consumption, which cannot be used in practice. Among them, most organic protein materials, such as silk materials, are expensive to construct memristors.
[0005] Sericin is a polymer material that is cheap and readily available, and has the same excellent properties as other organic proteins, such as good biocompatibility, controllable biodegradability, diverse regenerative morphological structures, and excellent mechanical properties. However, the sericin-based memristors in the existing technology have no obvious advantages over other protein-based memristors. The development of high-performance sericin memristors will have broad application prospects. Summary of the invention
[0006] In view of the defects of the prior art or the need for improvement, in order to improve the problem of poor cyclic stability of sericin-based memristors, the present invention provides a sericin memristor based on vanadium-based MXene and a preparation method thereof. A new two-dimensional material vanadium-based MXene is introduced into the resistive switching layer of the sericin memristor to regulate the rapid and stable switching of conductive filaments, thereby improving the key performance of the sericin memristor. The prepared sericin memristor has low power consumption, good stability and low cost.
[0007] The vanadium-based MXene belongs to the MXene class of materials, which is a new type of two-dimensional material with a specific chemical composition of transition metal carbonitrides. The synthesis of MXene materials is obtained by etching MAX phase materials. MXene materials have outstanding performance in hydrophilicity, conductivity and oxidation resistance, have a unique layered structure, and are highly surface modifiable. They can be widely used in multiple fields. Currently, the material has been widely used in supercapacitors, lithium-ion batteries, field effect transistors, and memristor devices. According to research, the insertion of MXene in oxide-based memristor devices can reduce the randomness of conductive filaments, reduce the mobility of metal conductive filaments, and regulate the rapid and stable on and off of the memristor, thereby improving the performance of the memristor.
[0008] To achieve the above object, the present invention adopts the following technical solutions:
[0009] In the first aspect, the present invention provides a sericin memristor based on vanadium-based MXene, which comprises, from top to bottom, an upper electrode, a resistive switching layer, a lower electrode and a substrate, wherein the lower electrode is sputtered through a first mask opening, the resistive switching layer is composed of a double-layer material of a sericin dielectric layer and a vanadium-based MXene film spin-coated thereon, and above the vanadium-based MXene film is an upper electrode sputtered using a second mask opening, the sericin dielectric layer is spin-coated on top of the lower electrode, and the bottom of the lower electrode is in contact with the substrate.
[0010] Furthermore, the upper electrode can be selected from one of aluminum, molybdenum, niobium, copper, gold, palladium, platinum, ruthenium, ruthenium oxide, silver, tantalum nitride, titanium nitride, tungsten and tungsten nitride, and the thickness of the upper electrode is preferably 80nm.
[0011] Furthermore, the lower electrode can be selected from one of aluminum, molybdenum, niobium, copper, gold, palladium, platinum, ruthenium, ruthenium oxide, silver, tantalum nitride, titanium nitride, tungsten and tungsten nitride, and the thickness of the lower electrode is preferably 80nm.
[0012] Furthermore, the vanadium-based MXene material is preferably V2C.
[0013] Furthermore, the substrate is preferably a silicon substrate layer.
[0014] In a second aspect, the present invention further provides a method for preparing the above-mentioned vanadium-based MXene-based sericin memristor, comprising the following steps:
[0015] S1. Prepare a lower electrode layer on a substrate, attach a first mask to the substrate, then fix the substrate on a target table of a sputtering system, evacuate the sputtering chamber, put the lower electrode material into a target gun as a sputtering source, and deposit the lower electrode obtained by a magnetron sputtering instrument on top of the substrate;
[0016] S2, subjecting the lower electrode deposited in step S1 to ultraviolet irradiation;
[0017] S3, preparing a sericin aqueous solution, placing sericin powder and deionized water in a centrifuge tube according to the required concentration, mixing, and then performing ultrasonic oscillation for 20 minutes to 40 minutes;
[0018] S4, taking the prepared sericin aqueous solution, dropping it on the center of the lower electrode after irradiation in step S2, and spin coating it for a certain period of time, and naturally drying the thin film obtained after spin coating, so that a uniform and flat sericin medium layer can be obtained above the lower electrode;
[0019] S5. Prepare a vanadium-based MXene suspension, put the vanadium-based MXene material and deionized water into a centrifuge tube according to the required concentration, mix them, and then perform ultrasonic oscillation for 50 minutes to 80 minutes.
[0020] S6. Take the prepared vanadium-based MXene suspension and drop it on the obtained sericin dielectric layer, then spin coat it through a spin coating device such as a spinner. Naturally dry the thin film obtained after spin coating to obtain a uniform vanadium-based MXene thin film on the sericin dielectric layer, thereby completing the preparation of the resistive layer.
[0021] S7. Fit the second mask tightly on top of the vanadium-based MXene film, and then fix it on the target of the sputtering system. Evacuate the sputtering chamber, take the upper electrode material and put it into the target gun as a sputtering source, and deposit it through a magnetron sputtering device to obtain the upper electrode located above the resistive layer, thereby preparing a vanadium-based MXene-based sericin memristor.
[0022] Furthermore, in step S1, tungsten is selected as the sputtering source, the power of the magnetron sputtering instrument is set to 30 W, the sputtering is heated at 100° C., and the sputtering time for depositing the lower electrode is 40 minutes.
[0023] Furthermore, the lower electrode deposited in step S1 is subjected to ultraviolet irradiation for 30 minutes to enhance the hydrophilicity and adsorption of the lower electrode.
[0024] Furthermore, the concentration of the sericin powder in S3 after mixing with deionized water is 20 mg / ml, and the duration of ultrasonic oscillation is 30 min.
[0025] Furthermore, the rotation speed of the spin coating equipment such as the glue spinner in S4 is first set to 1000 r / min, and the coating is carried out at this speed for 40 seconds. After the coating is completed, the rotation speed of the spin coating equipment is set to 2000 r / min, and the coating is carried out at this speed for 2 minutes.
[0026] Furthermore, the vanadium-based MXene material selected in S5 is V2C, the concentration of V2C and deionized water after mixing is 10 mg / ml, and the duration of ultrasonic oscillation is 1 h.
[0027] Furthermore, in S6, the V2C MXene suspension is first dropped onto the sericin medium layer and allowed to stand for 30 seconds. Then, the rotation speed of the spin coating equipment is set to 1500 r / min, and the spin coating is performed at this speed for 2 minutes to obtain a uniform and dense MXene film.
[0028] Furthermore, in S7, silver is selected as the sputtering source, the power of the magnetron sputtering instrument is set to 100 W, the sputtering process does not require heating, and the sputtering time of the entire deposition of the upper electrode is 3 minutes and 29 seconds.
[0029] The present invention proposes a sericin memristor based on vanadium-based MXene, which introduces two-dimensional MXene materials into the resistive switching layer of sericin memristor for the first time to improve the resistive switching performance of sericin memristor devices. The prepared device can measure the memristive effect under voltage stimulation, and has the advantages of low power consumption, good stability and biocompatibility; it lays a foundation for the application of two-dimensional MXene materials in sericin memristors, provides design ideas for the development of more new multifunctional memristive devices, and also provides a new thinking direction for manufacturing memristive devices with better performance.
[0030] The vanadium-based MXene used in the present invention is inserted into the sericin memristor, which can not only achieve the effect of reducing the randomness and mobility of the conductive filaments and regulating the rapid and stable switching of the memristor similar to the insertion of MXene into the oxide-based memristor; it can also reduce the potential barrier for the silver ions to transition to the bottom electrode and accelerate the migration speed of the silver ions, thereby reducing the threshold voltage of the device and improving the switching performance of the device.
[0031] Beneficial effects:
[0032] (1) The present invention provides a method for preparing a vanadium-based MXene-based sericin memristor. The preparation method is simple and easy to operate. The prepared sericin memristor has high sensitivity. The sensitivity here refers to the degree of response of the device to an external signal. The threshold voltage is less than 1V, the power consumption is low, and the conversion from volatile to non-volatile state can be achieved under different current limits (1μA, 500μA and 1mA), and the non-volatile state has a large switching ratio;
[0033] (2) The present invention provides a method for preparing a vanadium-based MXene-based sericin memristor, which has a wide range of applications. The prepared device has stable signal transmission, which is specifically manifested in that the IV curve has a small fluctuation amplitude. The device adopts a crossbar array structure, which makes the device have a higher degree of integration and is expected to be applied in the field of low-energy and high-density integrated storage electronic devices.
[0034] (3) The present invention provides a vanadium-based MXene-based sericin memristor. Compared with traditional inorganic or organic synthetic materials, the biomaterial has the advantages of good biocompatibility, biodegradability, sustainability and green environmental protection. In addition, the present invention uses sericin as the dielectric layer to achieve the reuse of waste. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 Schematic diagram of the structure of the sericin memristor according to the present invention.
[0036] Figure 2 This is an array diagram of the sericin memristor prepared in Example 1 of the present invention under a metallographic microscope.
[0037] Figure 3 This is an XRD physical characterization diagram of the MXene (V2C) material in the sericin memristor prepared in Example 1 of the present invention.
[0038] Figure 4 3 is an IV diagram of the sericin memristor prepared in Example 1 of the present invention under 1 μA current limiting.
[0039] Figure 5 This is an IV diagram of the sericin memristor prepared in Example 1 of the present invention under a current limit of 500 μA.
[0040] Figure 6 3 is an IV diagram of the sericin memristor prepared in Example 1 of the present invention under 1 mA current limiting. DETAILED DESCRIPTION
[0041] In order to more clearly illustrate the specific method of the present invention, the preparation method of the present invention is further described in detail below in conjunction with the accompanying drawings. It should be understood that the specific examples described herein are only used to explain the present invention and do not constitute a limitation on the scope of protection of the present invention.
[0042] The present invention provides a vanadium-based MXene-based sericin memristor, the structure of which is as follows: Figure 1 As shown, the memristor is built on a substrate 5, which is a silicon substrate. The entire memristor structure is composed of an upper electrode 1, a resistive switching layer, and a lower electrode 4 from top to bottom. The resistive switching layer is a double-layer structure composed of a two-dimensional MXene material 2 and a sericin material 3. The two-dimensional MXene material is V 1.5 Nb 0.5 For vanadium-based MXenes such as V2C or V2C, the upper and lower electrodes are used to connect to an external power source. They can be made of the same material or different materials. They are one of aluminum, molybdenum, niobium, copper, gold, palladium, platinum, ruthenium, ruthenium oxide, silver, tantalum nitride, titanium nitride, tungsten and tungsten nitride.
[0043] The sericin dielectric layer 3 and the MXene film 2 are both made by spin coating. The sericin dielectric layer is spin coated on the top of the lower electrode 4 by a spin coating device, and the two-dimensional MXene material V2C is spin coated on the top of the dielectric layer sericin 3 by a spin coating device.
[0044] The lower electrode 4 is a tungsten metal layer with a preferred thickness of 80 nm, which is sputtered on top of the substrate 5 through the opening of the first mask plate; the upper electrode 1 is a silver layer with a preferred thickness of 80 nm, which can also be sputtered on top of the MXene film in the resistive layer through the opening of the second mask plate.
[0045] The present invention provides a method for preparing a sericin memristor based on two-dimensional MXene material regulation. The preparation method is as follows:
[0046] S1: Prepare the lower electrode on the substrate, fit the first mask tightly on the substrate, and fix the substrate on the target of the sputtering system. Select the lower electrode material as the sputtering source. Deposit the lower electrode by magnetron sputtering in a vacuum environment so that the lower electrode is plated on the substrate.
[0047] S2: subjecting the lower electrode deposited in step S1 to ultraviolet irradiation for 30 minutes;
[0048] S3: Spin-coat a sericin aqueous solution on the lower electrode, mix sericin powder and deionized water at a concentration of 20 mg / ml, and then perform ultrasonic oscillation for 20 minutes to 40 minutes. Take the sericin solution after oscillation and drop it on the center of the lower electrode, and then spin-coat by setting the speed and time of the spin coating equipment. Naturally dry the thin film obtained after spin coating to obtain a sericin medium layer uniformly covering the upper surface of the lower electrode;
[0049] S4: Spin-coat the MXene suspension on the sericin medium layer, mix the two-dimensional material MXene and deionized water at a concentration ratio of 10 mg / ml, and then perform ultrasonic oscillation for 50 minutes to 80 minutes. Drop the MXene suspension after oscillation on the center of the sericin medium layer, and then perform spin coating by setting the rotation speed and time of the spin coating equipment. Naturally dry the film after spin coating to obtain a uniform MXene film on the top of the sericin film;
[0050] S5: Prepare an upper electrode on the resistive layer, closely attach a second mask on the MXene film, and fix it on a sputtering target, select the upper electrode material as a sputtering source, and sputter to obtain an upper electrode on the MXene film, thereby obtaining a sericin memristor based on two-dimensional MXene material regulation;
[0051] It can be seen that the above preparation method is simple, efficient and low-cost. In order to further illustrate the sericin memristor based on two-dimensional MXene material regulation and its preparation method provided by the present invention, a specific example is now described as follows:
[0052] Embodiment 1
[0053] A method for preparing a memristor device having a structure of silver / vanadium carbide / sericin / tungsten comprises the following preparation steps:
[0054] S1) In a vacuum environment, the first mask is tightly attached to the substrate and fixed on the target stage of the sputtering system. Tungsten is selected as the sputtering source, and a tungsten electrode with a thickness of 80 nm is obtained by magnetron sputtering deposition, so that the tungsten electrode is successfully plated on the substrate;
[0055] S2) subjecting the lower electrode deposited in step S1 to ultraviolet irradiation for 30 minutes to enhance the hydrophilicity and adsorption of the lower electrode;
[0056] S3) Mix sericin powder and deionized water at a concentration of 20 mg / ml, and then perform ultrasonic oscillation for 30 minutes. Take the vibrated sericin solution and drop it on the center of the lower electrode. First, set the spin coating equipment speed to 1000 r / min, rotate for 40 seconds, and then set the spin coating equipment speed to 2000 r / min, and spin coat at this speed for 2 minutes;
[0057] S4) The film obtained after spin coating in step S3 is dried naturally to obtain a uniform sericin medium layer. Then, the two-dimensional MXene material V2C and deionized water are mixed at a concentration of 10 mg / ml, and then ultrasonically vibrated for 1 hour. The vibrated MXene suspension is dropped on the center of the sericin medium layer and allowed to stand for 30 seconds. After the end, the spin coating equipment speed is set to 1500 r / min, and the spin coating is performed at this speed for 2 minutes;
[0058] S5) The film produced after spin coating in step S4 is dried naturally to obtain a uniform and dense MXene film. A second mask is tightly attached to it and fixed on a sputtering target. Silver is selected as a sputtering source to obtain a silver electrode located above the MXene film with a thickness of 80 nm, thereby obtaining a memristor device with a structure of silver / vanadium carbide / sericin / tungsten.
[0059] Figure 2 This is the array diagram of the sericin memristor array device in this example under a metallographic microscope. Figure 2 The cross-array node is a single silver / vanadium carbide / sericin / tungsten memristor device. The metal pads in the figure are the bottom electrode and the top electrode. Checking the device at the array node is a single silver / vanadium carbide / sericin / tungsten memristor device. It can be seen that the cross-array structure of the array memristor device in this example is obvious, and it has the potential to realize high-density large-scale memristor array devices.
[0060] The two-dimensional material MXene (V2C) is prepared based on the precursor V2AlC. The synthesized V2AlC raw material is added to a hydrochloric acid and lithium fluoride solution and heated and stirred for 72 hours. The reaction solution is washed with water until neutral to obtain multilayer V2C, and then ultrasonically dispersed to obtain a single layer of V2C. Figure 3 From the XRD diffraction pattern of the prepared V2C nanosheets, it can be seen that the two-dimensional single-layer V2C material has been successfully prepared, and the characteristic peak of Al in the original V2AlC has been etched away.
[0061] The present invention performs a volt-ampere curve test on the device, and the testing instrument is Keithley4200A-SCS. Figure 4 This is a typical IV curve of the memristor device of the present invention under bidirectional voltage stimulation of 0 to 1V and current limiting of 1μA. The SET voltage of the device is about 0.75V, and the device exhibits obvious resistance change characteristics. Under stimulation of 0 to 0.75V, the current of the device rises slowly at first. When the device reaches the SET voltage, the conductive filaments of the device are formed under the stimulation of the voltage, and the current of the device undergoes a sudden change, reaching the current limit. When the device is stimulated by a voltage of 1 to 0V, the current drops rapidly, the conductive filaments are gradually disconnected, and the device resistance returns to the initial state. The device exhibits volatile characteristics under the current limiting of 1μA, and the resistance state cannot be maintained.
[0062] Figure 5This is a typical IV curve of the memristor device of the present invention under bidirectional voltage stimulation of 0 to 1V and current limiting of 500μA. The SET voltage of the device is about 0.55V, and the device exhibits obvious resistance switching characteristics. At 0 to 0.55V, the current of the device rises slowly. When the device reaches the SET voltage, the conductive filaments of the device are formed under the stimulation of the voltage, and the current of the device undergoes a sudden change and quickly reaches the current limit. When the device is stimulated by a voltage of 1 to 0V, the current decreases slowly in proportion. Under the current limiting of 500μA, the resistance value of the device can be maintained for a short time.
[0063] Figure 6 This is a typical IV curve of the memristor device of the present invention under bidirectional voltage stimulation of -1.5V to 1.5V and 1mA current limit. The SET voltage of the device is 0.8V, the RESET voltage is -0.65V, and the device exhibits typical positive on and negative off characteristics. Under the stimulation of 0 to 0.8V, the current of the device rises slowly. When the SET voltage is reached, the conductive filaments of the device are formed under the stimulation of the voltage, the current of the device undergoes a sudden change, and the current limit is reached. When the device is stimulated by a voltage of 0.55 to -0.65V, the voltage and current decrease proportionally and slowly, the resistance of the device can be maintained, and the device exhibits non-volatile characteristics. When the RESET voltage is reached, the current of the device undergoes a sudden change, the resistance increases, and gradually returns to the original high resistance state. Under the stimulation of -1.25V to 0V, the high resistance of the device can be maintained, which is beneficial to our next cycle of SET / RESET operation. The device can realize the cycle process of positive writing and negative erasing at a large current limit, indicating that the sericin-based memristor device has the potential to realize binary storage computing.
[0064] In summary, the sericin memristor based on two-dimensional MXene material regulation and its preparation method provided by the present invention can switch from volatile to non-volatile state by adjusting the stimulation voltage and test current limit. The insertion of the MXene dielectric layer enhances the stability of the conductive filaments, improves the device performance, enhances the cyclability of the device, and reduces power consumption. This work shows that the sericin memristor based on two-dimensional MXene material regulation has laid a foundation for the application of MXene materials in protein-based memristors and promoted the development of memristors in brain-like computing systems.
[0065] It is worth noting that the present invention uses the two-dimensional vanadium-based MXene material V2C to regulate the performance of the sericin memristor device, which is only used to explain the present invention but not to limit the present invention. If other two-dimensional vanadium-based MXenes are used to prepare memristor devices, they should all fall within the scope of protection of the claims attached to the present invention.
[0066] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them. Although the present invention has been described in detail with reference to the above embodiments, it should be understood by those skilled in the art that the technical solutions described in the above embodiments can still be modified, or some of the technical features can be replaced by equivalents, and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the present invention.
Claims
1. A vanadium-based MXene-based sericin memristor, the memristor comprising an upper electrode, a resistive switching layer, a lower electrode and a substrate from top to bottom, characterized in that: The resistive switching layer is composed of a sericin dielectric layer and a two-dimensional MXene film spin-coated thereon, and the MXene material is a two-dimensional vanadium-based MXene; The method for preparing the sericin memristor based on vanadium-based MXene comprises the following steps: S1. Fit the first mask tightly on the substrate, then fix the substrate on the target table of the sputtering system, evacuate the sputtering chamber, take out the electrode material and put it into the target gun as the sputtering source, and deposit the lower electrode flatly on the substrate through the magnetron sputtering instrument; S2, subjecting the lower electrode deposited in step S1 to ultraviolet irradiation; S3, mixing sericin powder and deionized water in an amount of required concentration, placing in a centrifuge tube for mixing, and then ultrasonically oscillating for 20 min to 40 min to prepare a sericin aqueous solution; S4, taking the prepared sericin aqueous solution, dropping it on the center of the lower electrode obtained in step S2, spin coating for a certain period of time, and naturally drying the spin-coated film to obtain a uniform and flat sericin dielectric layer on the upper side of the lower electrode; S5, mixing the two-dimensional vanadium-based MXene material and deionized water in the required concentration and placing them in a centrifuge tube, and then ultrasonically oscillating for 50 min to 80 min to prepare a vanadium-based MXene suspension; S6. Take the prepared vanadium-based MXene suspension, drop it on the obtained sericin medium layer, and then spin-coat it to obtain a uniform thin film. After natural drying, the preparation of the vanadium-based MXene film is completed; S7, closely attaching a second mask plate on the top of the vanadium-based MXene film, and then fixing it on the target stage of the sputtering system, evacuating the sputtering chamber, taking the upper electrode material and putting it into the target gun as a sputtering source, and depositing the upper electrode on the vanadium-based MXene film by a magnetron sputtering instrument, thereby preparing the sericin memristor; The sericin powder and deionized water in step S3 are mixed at a concentration of 20 mg / ml, and the ultrasonic oscillation duration is 30 min; the spin coating speed in step S4 is first set to 1000 r / min, and the spin coating is carried out at this speed for 40 s; after the spin coating speed is completed, the spin coating speed is set to 2000 r / min, and the spin coating is carried out at this speed for 2 min; In the step S5, the two-dimensional vanadium-based MXene material is selected as V2C, and the two-dimensional vanadium-based MXene material V2C and deionized water are mixed at a concentration ratio of 10 mg / ml, and the ultrasonic oscillation time is 1 hour; in the step S6, the vanadium-based MXene suspension is firstly dropped onto the sericin medium layer and allowed to stand for 30 seconds; then the spin coating speed is set to 1500 / min, and the spin coating is performed at this speed for 2 minutes.
2. The vanadium-based MXene-based sericin memristor according to claim 1, characterized in that: The vanadium-based MXene is V2C.
3. The vanadium-based MXene-based sericin memristor according to claim 1, characterized in that: The upper electrode is any one of aluminum, molybdenum, niobium, copper, gold, palladium, platinum, ruthenium, ruthenium oxide, silver, tantalum nitride, titanium nitride, tungsten and tungsten nitride, and the thickness of the upper electrode is 80 nm.
4. The vanadium-based MXene-based sericin memristor according to claim 1, characterized in that: The lower electrode is any one of aluminum, molybdenum, niobium, copper, gold, palladium, platinum, ruthenium, ruthenium oxide, silver, tantalum nitride, titanium nitride, tungsten and tungsten nitride, and the thickness of the lower electrode is 80 nm.
5. The vanadium-based MXene-based sericin memristor according to claim 1, characterized in that: In the preparation method of the vanadium-based MXene-based sericin memristor, tungsten is selected as the sputtering source in step S1, the magnetron sputtering power is 30 W, and the sputtering is heated at 100° C. The sputtering time of the entire deposited lower electrode is 40 minutes.
6. The vanadium-based MXene-based sericin memristor according to claim 1, characterized in that: In the method for preparing the vanadium-based MXene-based sericin memristor, in step S2, the deposited lower electrode is subjected to ultraviolet irradiation for 30 minutes.
7. The vanadium-based MXene-based sericin memristor according to claim 1, characterized in that: In the method for preparing the vanadium-based MXene-based sericin memristor, Ag is selected as the sputtering source in step S7, the power of the magnetron sputtering instrument is set to 100 W, the sputtering process does not require heating, and the sputtering time of the entire deposited upper electrode is 3 min 29 s.
Citation Information
Patent Citations
Metal nano-cluster doped memristor and method for preparing same
CN109326711A
Memristor based on two-dimensional MXene material and preparation method of memristor
CN109920909A
Ferroelectric memristor based on two-dimensional material and manfuacturing method of ferroelectric memristor
CN111129299A
Memristor based on two-dimensional V2C material and preparation method thereof
CN112271253A
Silicon oxide-based memristor based on solution method, and preparation method and application thereof
WO2021003683A1