A presulfurization method for heavy oil hydrogenation catalyst and heavy oil hydrogenation presulfurization catalyst
By pressurizing sulfurization in an inert atmosphere and using gaseous olefins and CO for passivation treatment, the problem of long sulfurization time and catalyst stability in the presulfurization of heavy oil hydrogenation catalysts is solved, and highly active and safe catalyst preparation is achieved. It meets the needs of the refinery for quick start-up and safe transportation.
Patent Information
- Application Number
- CN202010656980.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-07-09
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2040-07-09
AI Technical Summary
The existing pre-sulfidation technology of heavy oil hydrogenation catalysts has problems such as long sulfurization time, low sulfur rate on the catalyst, uneven sulfurization, complex passivation operation, and transportation safety problems. Especially when the content of sulfur, nitrogen, and heavy metal impurities in heavy oil is high, the catalyst must be presulfurized. Hydrogen performance requirements are high and difficult to meet.
Use an oxidized catalyst to increase pressure and vulcanize in an inert atmosphere, and then pass in passivation gas for passivation treatment. The vulcanization temperature and time are 170~400°C, 2~30 hours, and the passivation gas consists of 2~15wt% gaseous olefins and The balance is composed of CO, the passivation time is 0.5-5 hours, and the catalyst carrier used includes alumina, silica-alumina and molecular sieves.
It achieves high activity and safe storage and transportation of the catalyst, shortens the start-up time of the refinery, simplifies the steps of starting the device, and improves the stability and application safety of the catalyst.
Smart Images

Figure CN113908888B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a presulfurization method for a heavy oil hydrogenation catalyst, and in particular to a presulfurization method for a heavy oil hydrogenation catalyst used for the conversion and modification of heavy oil products such as wax oil, deasphalted oil, and residual oil, and a heavy oil hydrogenation presulfurization catalyst prepared by the presulfurization method. Background Art
[0002] Heavy oil hydroprocessing mainly refers to the hydrodemetallization, hydrodesulfurization, hydrodenitrogenation, aromatic saturation, olefin saturation and hydrocracking reactions of residue oil and other fractions. Most of the metals in crude oil exist in the residue oil. Although the content of metals (mainly Ni, V, Fe, etc.) in the residue oil is only in the order of parts per million, it is easy to permanently poison and deactivate the residue oil hydrodesulfurization catalyst, hydrodenitrogenation catalyst and catalytic cracking catalyst. Therefore, it is necessary to remove the trace metals in the residue oil raw material. The residue oil hydrodemetallization reaction is an important chemical reaction that occurs during the residue oil hydroprocessing process. Under the action of the catalyst, the metal compound reacts with hydrogen sulfide to form metal sulfide, and then the generated metal sulfide is deposited on the catalyst, thereby being removed. In order to ensure the performance of the catalyst loaded in the subsequent reactor, the best way is to force the metal to deposit on the hydrodemetallization catalyst of the protective reactor to prevent the catalyst from being deactivated prematurely in the subsequent reactor, because the pores of the catalyst in the subsequent reactor are very small, and the hydroprocessing and conversion reactions are mostly carried out in the subsequent reactor; the hydrodesulfurization reaction of residual oil is the most important chemical reaction that occurs during the hydroprocessing of residual oil. In the presence of catalysts and hydrogen, various sulfur-containing compounds are converted into sulfur-free hydrocarbons and hydrogen sulfide through the hydrodesulfurization reaction. Hydrocarbons remain in the product, while hydrogen sulfide is removed from the reactants; most of the nitrogen in crude oil is also present in the residual oil, and the nitrides in the residual oil can be divided into two categories: alkaline and non-alkaline. During the hydrogenation of residual oil, various nitrogen compounds generate ammonia and hydrocarbons under the action of catalysts. Ammonia is removed from the reactants, while hydrocarbons remain in the products. The hydrogenation saturation reaction of residual oil aromatics is mainly the hydrogenation of polycyclic aromatics. This type of reaction is the most difficult reaction among all hydrogenation reactions in the residual oil hydroprocessing process. Monocyclic aromatics are difficult to hydrogenate and saturate, while polycyclic aromatics are hydrogenated and saturated ring by ring, and the difficulty of hydrogenation increases ring by ring. The hydrogenation reaction of each ring of polycyclic aromatics is a reversible reaction and is in a state of equilibrium. The depth of hydrogenation is often limited by chemical equilibrium. If there are substituents on the benzene ring, the hydrogenation saturation of aromatics will be more difficult. The temperature of the residue hydrodenitrogenation catalyst should not be too high, and a relatively high hydrogen partial pressure should be maintained to facilitate the occurrence of aromatic hydrogenation saturation reaction; the olefin saturation reaction has a relatively fast reaction rate among all residue hydrotreating reactions, second only to the hydrodemetallization reaction, and at the hydrodesulfurization reaction temperature, the olefin hydrogenation reaction basically reaches complete saturation; the hydrocracking reaction is a reaction in which larger hydrocarbon molecules in the feed are converted into small molecules under the presence of hydrogen and a catalyst, and it occurs almost throughout the entire reaction process.
[0003] The goal of the residue oil hydrogenation unit is to provide high-quality raw materials for its downstream heavy oil catalytic cracking unit. For reactions such as residue oil hydrodemetallization, hydrodesulfurization, hydrodenitrogenation, aromatic saturation, olefin saturation and hydrocracking, the fixed-bed residue oil hydrogenation process generally includes multiple reactors (mostly four or five reactors in series), and the reactors need to be loaded with catalysts with different functions. When the unit is started, the catalyst needs to be pre-sulfurized in order to react the loaded oxidized metal with sulfur-containing compounds to convert it into sulfided metal to stimulate the catalyst activity.
[0004] The sulfidation process is mainly divided into two types: in-vessel sulfidation and ex-vessel sulfidation. In-vessel sulfidation refers to the in-situ sulfidation after the catalyst is loaded into the reactor. In-vessel sulfidation can be carried out in two ways: dry sulfidation and wet sulfidation. Dry sulfidation refers to mixing the sulfiding agent and hydrogen in a certain proportion and directly passing them into the catalyst bed, while wet sulfidation refers to sulfiding the catalyst with the sulfiding agent carried by oil products. The purpose of converting the oxidized metal into the sulfided metal is achieved by controlling the flow rate of the sulfide and adjusting the temperature and pressure of the bed. For the residual oil hydrogenation process, dimethyl disulfide is usually used as the sulfiding agent, and diesel and wax oil are used as solvents to perform the sulfidation operation on the catalyst. During the start-up sulfidation process of the residual oil unit, the temperature control is extremely strict. Because in the oxidized state, the residual oil hydrogenation catalyst contacts with pure hot H2 (without hydrogen sulfide), which will cause the active metal of the catalyst to undergo a reduction reaction, resulting in permanent deactivation of the catalyst. Generally, if the hydrogen temperature exceeds 260°C, the deactivation of the catalyst can occur within a few hours, so the hot H2 temperature must be controlled. And during the sulfidation process, before hydrogen sulfide is detected in the circulating hydrogen, it is also necessary to control the maximum temperature of the catalyst bed to prevent the reduction reaction from occurring. At present, the typical method of pre-sulfidation of hydrogenation catalyst in the reactor is: the reactor is heated to about 180°C under a hydrogen atmosphere, and the sulfided oil containing a sulfiding agent is introduced, and the temperature is continued to be raised to about 230°C and maintained at a constant temperature for a period of time, and then the temperature is raised to 360-380°C and maintained at a constant temperature, and then the required reaction temperature is adjusted to switch the raw oil for normal reaction. There are certain disadvantages of in-vessel sulfidation. First, in order to ensure the degree of sulfidation, several reactors need to reach the optimal sulfidation temperature, and the sulfidation time is very long, resulting in a long start-up time of the industrial unit, affecting the production progress of the refinery. Secondly, it is easy to produce a high temperature of the catalyst bed, resulting in temporary or permanent loss of catalyst activity, and in-vessel sulfidation is prone to incomplete catalyst sulfidation, affecting its activity. In addition, the in-vessel vulcanization method requires special equipment, and the vulcanizing agent is generally toxic. Especially under high temperature conditions, the vulcanizing agent will react with hydrogen to produce hydrogen sulfide and methane. Once leaked, it will pollute the environment and cause harm to the operators.
[0005] Ex-situ sulfurization is usually divided into two types: sulfur-carrying type and sulfurization type. The former mostly uses elemental sulfur or organic sulfides with different decomposition temperatures to load on the catalyst by impregnation technology, and changes the active metal on the catalyst from an oxidized state to an oxysulfided state. The prepared presulfided catalyst is relatively stable in the air. When starting the sulfurization, hydrogen needs to be introduced to complete the whole process of catalyst presulfidation. Its activation time and temperature are basically equivalent to or slightly shorter than the online in-situ sulfurization time. For the activation of sulfur-carrying catalysts, there are generally two possible reaction pathways: the catalyst contacts hydrogen at a certain temperature, and the active components are directly converted from an oxidized state or an oxysulfided state to a sulfided state; or the catalyst generates hydrogen sulfide under hydrogen conditions, and hydrogen sulfide converts the oxidized or oxysulfided catalyst into a sulfided catalyst. The metal components used in the sulfurized catalyst are completely in a sulfided state. When starting, the temperature is directly increased and the oil is added, without the need for sulfurization or activation. The start-up time is very short and pollution-free. Refineries are willing to use this type of hydrogenation catalyst that does not require on-site activation, but this catalyst also has problems such as the sulfided catalyst being prone to spontaneous combustion when exposed to air and being unable to be stored and transported for a long time, which affects the application of this technology. Therefore, the catalyst usually needs to be passivated.
[0006] The currently disclosed passivation technologies are roughly divided into two types: gas phase passivation and liquid phase passivation. Gas phase passivation mainly uses an oxidizing gas to form an oxide film on the surface of the sulfided catalyst at an appropriate temperature to protect the sulfided catalyst. For gas phase passivation, the sulfided catalyst formed after the oxidized catalyst is completely sulfided is passivated by trace oxygen, and part of the sulfur in the microcrystals of the active metal sulfide is replaced by oxygen to form metal oxysulfide. This compound is easily activated under hydrogen conditions and provides acidic active sites in addition to metal sites, so the acidic active sites of the catalyst passivated by oxygen are more than the acidic sites of the sulfided catalyst, which also explains why the activity of the gas phase passivated catalyst increases after reactivation. Liquid phase passivation mainly uses methods such as spraying and dipping to load organic oxygen-containing hydrocarbons onto the surface of the sulfided catalyst to form a protective film. Liquid phase passivation can evenly spray the liquefied protective liquid on the surface of the solid catalyst at a temperature lower than the condensation point of the protective liquid, and the protective liquid can crystallize to form a solid protective film; heavy hydrocarbons (such as vacuum distillate oil) can also be used to spray hot hydrocarbons on the surface of low-temperature catalysts, so that the viscosity of the hydrocarbons increases and the diffusion rate to the center of the particles is slowed down to achieve the effect of wrapping the catalyst surface and isolating the air; the above-mentioned passivating substances can also be diluted or emulsified in a solvent to form a mixed solution, and the mixed solution can be sprayed on the catalyst surface under the condition that the temperature is higher than the boiling point of the solvent. The solvent evaporates quickly, and the passivating substance forms a protective film on the catalyst surface. When liquid passivation is used, the spraying amount of the protective liquid needs to be strictly controlled. If there are too many protective substances, it is not easy to remove at the beginning of the reaction, which will affect the activity of the catalyst. On the contrary, too little protective substance cannot play the role of isolating oxygen from invading the catalyst surface and pores. There are currently two main explanations for the mechanism of liquid phase passivation: one is that the passivating substance (such as organic hydrocarbons) does not change the physical and chemical properties of the catalyst, but is just a simple physical protection process. During the reaction, the protective film is removed by heating or solvent dissolution and carrying. One is that certain hydrocarbons contained in the passivation react with the sulfide of the catalyst, and the new substances generated can prevent oxygen from invading and play a role in protecting the catalyst.
[0007] After the presulfurized catalyst is passivated, it can improve the stability of the catalyst, facilitate storage and transportation, and reduce equipment investment and start-up costs during the start-up period of the refinery. Based on the refinery's requirements for rapid start-up of the device, its preparation technology and means have been rapidly developed.
[0008] CN102041045B, CN1129609A and US2002000394A1 belong to sulfur-carrying type off-site presulfurization methods. The selected sulfurizing agent is elemental sulfur or sulfur-containing compounds, and the organic solvent loaded on the catalyst together with the sulfurizing agent is an organic solvent containing unsaturated bonds. The method is simple in process and saves costs, but the method uses a large amount of organic solvents in the production process, which are not easy to obtain in refineries and are not conducive to safety and environmental protection.
[0009] CN102284299A discloses a method for presulfiding an oxidized hydrogenation catalyst outside a hydrogenation reactor. In addition to presulfidation and passivation, the method has the added step of reactivation, i.e., the process of reactivating the passivated catalyst loaded in the hydrogenation reactor in an atmosphere containing a sulfiding agent. The presulfidation process of the method only involves the use of sulfiding gas (sulfur content 0.5-3%), does not require the sulfidation pressure, and the catalyst active metal is Mo and / or Ni.
[0010] US6294498B1 discloses a method for protecting active catalysts by spraying on the outer surface. The method sprays an inert material on the outer surface of the catalyst to obtain a protective film to protect the core and internal pores of the catalyst particles. The concentration of the protective material decreases gradually from the outer surface to the core, and the protective film disappears automatically under the reaction conditions. After passivation, the mechanical properties and wear resistance of the catalyst are effectively improved, but the operation method of spraying the inert protective film disclosed in this method is slightly complicated.
[0011] CN105233867B discloses a presulfurized sulfur-resistant shift catalyst and a preparation method. The surface of the sulfurized catalyst is coated with a surface layer formed by a polymer compound to prevent the active component from contacting with oxygen. The external coating compound is two or more of polyacrylamide, polystyrene acrylonitrile, polyamide, melamine or naphthalene, the mixing ratio is 1:1, and the compound can be gasified at 250-350°C. The preparation method of the presulfurized sulfur-resistant shift catalyst is to pass the gasified coating compound through the sulfurized catalyst bed under vacuum conditions (0.2-1psi), and obtain a stable catalyst after cooling. The polymer compound film will not react chemically with the active center of the catalyst and will not affect the activity of the catalyst. At the same time, in the initial stage of activation in the catalyst device, the polymer compound film is gasified at a certain temperature, discharged from the catalyst pore in a gaseous form, and has a secondary adjustment effect on the catalyst pore structure. The catalyst prepared by this method has high activity and good stability, but it is difficult to evacuate in industrial applications.
[0012] In summary, the existing problems of the public off-site presulfurization technology are: long sulfurization time, low sulfur rate on catalyst, uneven sulfurization, complicated catalyst passivation operation, and catalyst transportation safety. In addition, the heavy oil raw material has high content of sulfur, nitrogen, and heavy metal impurities and is rich in polycyclic aromatic hydrocarbons, which puts higher requirements on the hydrogenation performance of the catalyst. Heavy oil hydrogenation catalysts often have high metal content, and there are certain difficulties in passivation using existing technologies. Summary of the invention
[0013] In view of the above problems in the prior art, the present invention aims to provide a presulfurization method for a heavy oil hydrogenation catalyst and a catalyst prepared by the presulfurization method. The catalyst prepared by the presulfurization method has high activity, safe and reliable storage and transportation, and can meet the requirements of safe and rapid start-up of refineries.
[0014] To this end, the present invention provides a method for presulfiding a heavy oil hydrogenation catalyst, comprising the following steps:
[0015] (1) adding an oxidized catalyst or a calcination-free catalyst into a sulfidation reactor, and increasing the pressure to 0.5-20 MPa under an inert atmosphere;
[0016] (2) introducing a sulfurization raw material into the sulfurization reactor for sulfurization;
[0017] (3) After the vulcanization is completed, the passivation gas is introduced for passivation.
[0018] The presulfiding method of the heavy oil hydrogenation catalyst of the present invention is preferably that the sulfiding conditions are: 170-400° C., constant temperature sulfiding for 2-30 hours.
[0019] In the presulfurization method of the heavy oil hydrogenation catalyst of the present invention, it is preferred that the passivation gas consists of 2 to 15 wt % of gaseous olefins and the balance of CO.
[0020] In the presulfurization method of the heavy oil hydrogenation catalyst of the present invention, preferably, the passivation time is 0.5-5 hours.
[0021] In the method for presulfiding a heavy oil hydrogenation catalyst of the present invention, it is preferred that the active metal supported by the oxidized catalyst or the calcination-free catalyst is selected from at least one of Group VIB metals and Group VIII metals.
[0022] In the presulfurization method of the heavy oil hydrogenation catalyst of the present invention, it is preferred that the VIB group metal is molybdenum and / or tungsten, and the VIII group metal is cobalt and / or nickel.
[0023] In the presulfurization method of the heavy oil hydrogenation catalyst of the present invention, it is preferred that the carrier of the oxidized catalyst or the calcination-free catalyst is a hydrogenation catalyst carrier. The hydrogenation catalyst carrier can be a conventional hydrogenation catalyst carrier, including but not limited to alumina, silica-alumina, molecular sieve or a combination thereof.
[0024] In the method for presulfiding a heavy oil hydrogenation catalyst of the present invention, it is preferred that the hydrogenation catalyst carrier comprises at least one of alumina, silica-alumina, molecular sieves and magnesium oxide.
[0025] The presulfurization method of the heavy oil hydrogenation catalyst of the present invention is preferably that the sulfiding raw material is a mixed gas composed of hydrogen sulfide, hydrogen and inert gas, and the hydrogen sulfide content is 3-25%, the hydrogen content is 15-77%, and the inert gas content is 20-60% by volume.
[0026] In the method for presulfiding a heavy oil hydrogenation catalyst of the present invention, it is preferred that the inert gas comprises at least one of nitrogen, argon, xenon, helium, neon, krypton and carbon dioxide.
[0027] In the method for presulfurization of a heavy oil hydrogenation catalyst of the present invention, it is preferred that the gaseous olefin is selected from at least one of monoolefins and diolefins.
[0028] To this end, the present invention also provides a heavy oil hydrogenation presulfurization catalyst, which is prepared by the above-mentioned presulfurization method, and the specific surface area of the catalyst is greater than 10m 2 .g -1 , pore volume greater than 0.1cm 3 .g -1 .
[0029] The heavy oil hydrogenation presulfurization catalyst of the present invention preferably has a specific surface area of 11-500m 2 .g -1 , pore volume is 0.2-3cm 3 .g -1 .
[0030] The heavy oil hydrogenation presulfurization catalyst of the present invention is preferably such that, in the catalyst, the Group VIII metal sulfide is Ni3S2, and its content is 1.0-10.0wt%; the Group VIB metal sulfide is MoS2, and its content is 3.0-35.0wt%.
[0031] The presulfurization method of the heavy oil hydrogenation catalyst provided by the present invention is applicable to a series of heavy oil hydrogenation catalysts, including a hydrodemetallization agent, a hydrodesulfurization agent, and a hydrodenitrogenation agent. The presulfurization method includes three steps: drying, sulfurization, and passivation. The specific process is as follows:
[0032] (1) Catalyst drying: The oxidized catalyst or the catalyst that has been impregnated and dried but not calcined is loaded into a sulfidation reactor and purged with inert gas and dried at 100-150°C for 2-6 hours.
[0033] (2) Catalyst sulfurization: Raise the pressure to 0.5-20 MPa, introduce sulfurization raw materials for sulfurization, the sulfurization temperature is 170-400°C, and keep the temperature constant for 2-10 hours.
[0034] (3) Catalyst passivation: A mixed gas consisting of 2 to 30 wt% of gaseous olefins and the remainder of CO is introduced for passivation. The passivation time is 0.5 to 5 hours.
[0035] The passivation gas used in the present invention is composed of gaseous olefins and CO, which can ensure uniform passivation, effectively avoid spontaneous combustion of the catalyst, and simplify the start-up steps of the device. The gaseous olefin can be a monoolefin, a diolefin, or a mixture of several thereof.
[0036] The presulfurization method provided by the present invention can shorten the start-up time of the refinery, and the catalyst passivation process is simple, the passivation is uniform, the catalyst activity is good, it can exist stably in the air, and it is convenient to store and transport. The catalyst prepared by the present invention has good economic benefits and broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 A process flow chart of an evaluation device for a heavy oil hydrogenation presulfurization catalyst obtained by the presulfurization method of the present invention.
[0038] in,
[0039] 1- Buffer tank,
[0040] 2- the first hydrogenation reactor,
[0041] 3- The second hydrogenation reactor,
[0042] 4- the third hydrogenation reactor,
[0043] 5-Gas-liquid separator combination (including high-pressure separator and low-pressure separator). DETAILED DESCRIPTION
[0044] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.
[0045] Example 1
[0046] Presulfidation of Residue Hydrodemetallization Catalyst
[0047] The residue hydrodemetallization catalyst was prepared by the method described in Example 1 of CN101928593A. The properties of the oxidized catalyst are shown in Table 1.
[0048] The above-mentioned oxidized catalyst is added to the sulfurization reactor and sealed, and purged with nitrogen. It is dried for 4 hours at a catalyst bed temperature of 130°C. After the catalyst bed is heated to 180°C at a rate of 10°C / h, a mixed gas consisting of 6v% hydrogen sulfide, 30v% argon and 64v% hydrogen is introduced as the sulfide gas, and the sulfide gas pressure is ensured to be 1MPa during the entire sulfurization process. After the bed is heated to 280°C, the temperature is kept constant for 5 hours; a mixed gas consisting of 5v% olefins (C3 and C4 mixed olefins, the ratio of the two is 50 / 50) and the remainder CO is introduced as the passivation gas, and the temperature is kept constant for 1.5 hours. The device is cooled and depressurized, and the catalyst is sealed in a barrel.
[0049] Example 2
[0050] Presulfidation of Residue Hydrodesulfurization Catalyst
[0051] The residue hydrodesulfurization catalyst was prepared by the method described in Example 1 of CN101928593A. The properties of the oxidized catalyst are shown in Table 1.
[0052] The above-mentioned oxidized catalyst is added to the sulfurization reactor and sealed, and purged with nitrogen. It is dried for 4 hours at a catalyst bed temperature of 130°C. After the catalyst bed is heated to 170°C at 10°C / h, a mixed gas consisting of 10v% hydrogen sulfide, 40v% argon and 50v% hydrogen is introduced as the sulfide gas, and the sulfide gas pressure is ensured to be 8MPa during the entire sulfurization process. After the bed is heated to 290°C, the temperature is kept constant for 4 hours; a mixed gas consisting of 5v% olefins (C2 and C3 mixed olefins, the ratio of the two is 30 / 70) and the remainder CO is introduced as the passivation gas, and the temperature is kept constant for 2 hours. After the device is cooled and depressurized, the catalyst is sealed in a barrel.
[0053] Example 3
[0054] (1) Preparation of residue hydrodenitrogenation catalyst
[0055] Take 500g (dry basis) of silicon-containing pseudo-boehmite dry rubber powder (SiO2 content is 39%), add 15g of sesbania powder, and mix well. Add 395g of acetic acid solution with a concentration of 3.5wt% to the above materials, knead for 40 minutes, and then extrude into a cylindrical shape with a diameter of 2.0mm on a single screw extruder. Dry in a 120℃ oven for 3 hours, then place in a roasting furnace, heat to 780℃ at a heating rate of 100-150℃ / h, and roast for 3 hours.
[0056] Weigh 150g of the above carrier with a water absorption rate of 1.10ml / g, and spray it with a measured ammonia solution of ammonium molybdate (containing 82.0wt% MoO3) and nickel nitrate (containing 25.2wt% NiO) according to the amount of saturated absorption solution. Homogenize in a spraying device for 5 minutes, dry at 60℃ for 2 hours, then heat to 120℃ and dry for 3 hours to obtain a nickel-molybdenum-containing, non-calcined hydrodenitrification catalyst.
[0057] To facilitate the characterization of the catalyst, the prepared nickel-molybdenum-containing calcination-free hydrodenitrogenation catalyst was calcined in air at 500°C for 3 hours. After cooling, the catalyst properties were analyzed. The results are shown in Table 1.
[0058] (2) Presulfurization of residue hydrodenitrogenation agent
[0059] The calcination-free hydrodenitrogenation catalyst is added to the sulfidation reactor and sealed, and purged with nitrogen. It is dried for 4 hours at a catalyst bed temperature of 130°C. After the catalyst bed is heated to 200°C at 10°C / h, a mixed gas consisting of 3v% hydrogen sulfide, 50v% neon and 47v% hydrogen is introduced as sulfiding gas, and the sulfiding gas pressure is ensured to be 15MPa during the entire sulfidation process. After the bed is heated to 320°C, the temperature is kept constant for 3 hours; a mixed gas consisting of 5% olefins (C2, C3, C4, C5 mixed olefins, the ratio of the four is 15 / 40 / 10 / 35) and the remainder CO is introduced as a passivation gas, and the temperature is continued to rise to 360°C and kept constant for 3 hours, and the sulfidation is completed. After the device is cooled and depressurized, the catalyst is sealed in a barrel.
[0060] Example 4
[0061] This example uses the presulfurized catalyst prepared by the present invention to test its performance. The hydrodemetallization presulfurized catalyst, hydrodesulfurization presulfurized catalyst, and hydrodenitrogenation presulfurized catalyst prepared in the above examples 1-3 are added in order. Figure 1 The reaction device (3×300ml small test evaluation device) was added with weight contents of 40wt%, 40wt%, and 20wt%, respectively, and hydrogen and evaluation oil were directly passed for evaluation. The properties of the evaluated raw oil are shown in Table 2. The process conditions and 2000 hours reaction results are shown in Table 3.
[0062] See also Figure 1 As shown, the evaluation process of the present invention is as follows: the feedstock oil and hydrogen for hydrogenation evaluation are mixed in the buffer tank 1, and then sequentially enter the first hydrogenation reactor 2, the second hydrogenation reactor 3, and the third hydrogenation reactor 4 for reaction, and then pass through the gas-liquid separator 5 (pass through the high-pressure separator and the low-pressure separator successively), and finally obtain gas and hydrogenated full-fraction oil. The first hydrogenation reactor 2, the second hydrogenation reactor 3, and the third hydrogenation reactor 4 are arranged in series, and the reaction conditions are consistent.
[0063] Comparative Example 1
[0064] This comparative example adopts conventional in-situ sulfurization to carry out sulfurization and conduct performance comparison evaluation. The unpresulfurized oxidized hydrodemetallization catalyst, unpresulfurized oxidized hydrodesulfurization catalyst, and unpresulfurized calcined hydrodenitrogenation catalyst prepared in Examples 1-3 are added in order. Figure 1 The reaction device shown in the figure has the addition ratios of 40wt%, 40wt% and 20wt% respectively. The in-vessel vulcanization adopts wet vulcanization, the vulcanization pressure is 10MPa, the vulcanizing agent uses carbon disulfide, the addition amount is 2.0wt%, the vulcanization is carried out for 10 hours at 240℃ using vulcanized diesel oil, and the vulcanization is carried out for 6 hours at 300℃ using vulcanized wax oil. The evaluation raw oil and process conditions are the same as those in Example 4, and the reaction results of 2000 hours are shown in Table 3.
[0065] Table 1 Catalyst properties
[0066]
[0067] Table 2 Evaluation of crude oil properties
[0068] project Crude oil <![CDATA[Density at 20 °C (g / cm -3 )]]> 0.9733 Carbon residue (w%) 9.2 S(w%) 1.47 N(w%) 0.33 Ni+V(wppm) 65.19
[0069] Table 3 2000 hours evaluation results
[0070]
[0071]
[0072] As shown in Table 3, the performance of the presulfurized catalyst of the present invention is comparable to that of the catalyst using conventional in-situ sulfurization in the comparative example. This indicates that the performance of the heavy oil hydrogenation presulfurized catalyst prepared using the presulfurization method meets the use requirements, does not require reactivation during use, and can effectively reduce the start-up time of the device (2-4 days).
[0073] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.
Claims
1. A method for presulfiding a heavy oil hydrogenation catalyst, characterized in that: The following steps are involved: (1) Add the oxidized catalyst or the calcination-free catalyst into the sulfidation reactor and increase the pressure to 0.5-20 MPa under an inert atmosphere; (2) introducing a sulfurization raw material into the sulfurization reactor for sulfurization; (3) After the vulcanization is completed, the passivation gas is introduced for passivation; The passivation gas is composed of 2 to 15 wt% of gaseous olefins and the balance of CO; The sulfiding raw material is a mixed gas consisting of hydrogen sulfide, hydrogen and inert gas; The gaseous olefin is selected from at least one of monoolefin and diolefin.
2. The method for presulfiding a heavy oil hydrogenation catalyst according to claim 1, characterized in that: The vulcanization conditions are: 170-400° C., constant temperature vulcanization for 2-30 hours.
3. The presulfurization method of the heavy oil hydrogenation catalyst according to claim 1, characterized in that: The passivation time is 0.5-5 hours.
4. The method for presulfiding a heavy oil hydrogenation catalyst according to claim 1, characterized in that: The active metal supported by the oxidized catalyst or the calcination-free catalyst is selected from at least one of Group VIB and Group VIII.
5. The method for presulfiding a heavy oil hydrogenation catalyst according to claim 1, characterized in that: The carrier of the oxidized catalyst or the calcination-free catalyst is a hydrogenation catalyst carrier.
6. The method for presulfiding a heavy oil hydrogenation catalyst according to claim 5, characterized in that: The hydrogenation catalyst carrier includes at least one of aluminum oxide, silicon aluminum oxide, molecular sieve, and magnesium oxide.
7. The method for presulfiding a heavy oil hydrogenation catalyst according to claim 1, characterized in that: The sulfiding raw material has a hydrogen sulfide content of 3-25%, a hydrogen content of 15-77%, and an inert gas content of 20-60% by volume.
8. The method for presulfiding a heavy oil hydrogenation catalyst according to claim 1, characterized in that: The inert gas includes at least one of nitrogen, argon, xenon, helium, neon, krypton and carbon dioxide.
9. A heavy oil hydrogenation presulfurization catalyst, which is prepared by the presulfurization method according to any one of claims 1 to 8, characterized in that: The specific surface area of the catalyst is greater than 10 m 2 .g -1 , pore volume greater than 0.1 cm 3 .g -1 .
10. The heavy oil hydrogenation presulfurization catalyst according to claim 9, characterized in that The specific surface area of the catalyst is 11-500 m 2 .g -1 , pore volume is 0.2-3 cm 3 .g -1 .
11. The heavy oil hydrogenation presulfurization catalyst according to claim 9, characterized in that: In the catalyst, the Group VIII metal sulfide is Ni3S2, and its content is 1.0-10.0 wt%; the Group VIB metal sulfide is MoS2, and its content is 3.0-35.0 wt%.