Supported platinum catalyst for cathode of fuel cell and method for producing the same, cathode of fuel cell and fuel cell
By loading platinum particles on a carbon support and optimizing their structure, the problem of insufficient diffraction peak intensity and oxidation resistance of the platinum catalyst Pt(220) in the prior art is solved, and efficient manufacturing of platinum supported catalysts is achieved, which improves fuel cells activity and properties.
Patent Information
- Application Number
- CN202080040791.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-06-03
- Filing Date
- 2020-06-03
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-06-03
AI Technical Summary
The prior art has shortcomings in improving the diffraction peak intensity ratio and oxidation resistance of the Pt(220) plane in the platinum catalyst. Especially when polymers are not used, the method of manufacturing high-efficiency supported platinum catalysts is relatively complicated.
By loading platinum microparticles on a specific carbon support using a specific reducing agent, the diffraction peak intensity ratio of the Pt (220) surface of the platinum microparticles is increased, and by controlling the structural and process parameters of the carbon support, such as the oxidation consumption temperature and pore structure, are carried out. , improve its oxidation resistance.
It is achieved to improve the diffraction peak intensity ratio and oxidation resistance of the Pt(220) surface of the platinum catalyst without using polymers, providing a simple manufacturing method and improving the ORR activity and overall performance of the fuel cell.
Smart Images

Figure CN113924670B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a supported platinum catalyst for a cathode of a fuel cell, a cathode of a fuel cell, a fuel cell, and a method for producing the supported platinum catalyst. Background Art
[0002] In recent years, fuel cells have been expected to be used as power sources for mobile vehicles such as automobiles, and their practical use has also begun. Such fuel cells generally use expensive noble metal catalysts represented by platinum (Pt) or alloys containing platinum. In order to achieve high performance of fuel cells, it is important to improve the performance of noble metal catalysts.
[0003] As one of the properties of precious metal catalysts, the activity of oxygen reduction reaction (ORR) is known. A study report using single crystals of platinum reported that the sequence of ORR activity of each single crystal surface of platinum is Pt(100)<Pt(111)<Pt(110). So far, in order to increase the proportion of Pt(110) with high ORR activity, a method of using polymers for structural control is known (for example, non-patent document 1). Furthermore, Pt(110) represents the plane direction, and in X-ray diffraction, it is detected as a peak of the Pt(220) surface, so increasing the proportion of Pt(110) with high ORR activity is the same as increasing the proportion of the diffraction peak intensity of the Pt(220) surface.
[0004] [Prior art literature]
[0005] [Non-patent literature]
[0006] Non-patent document 1: "Surface Science" (Vol.32, No.11, pp.698-703, 2011) Summary of the invention
[0007] [Problems to be solved by the invention]
[0008] The present inventors believe that in the technology such as the above-mentioned non-patent document 1, in order to increase the ratio of the diffraction peak intensity of the Pt(220) plane in platinum, it is necessary to use a polymer to control the crystal plane, and there is room for further improvement in terms of performance and manufacturing.
[0009] Furthermore, the present inventors have found that it is also important to improve the oxidation resistance of the supported platinum catalyst in order to extend the life of the noble metal catalyst.
[0010] The present invention is made in view of the above-mentioned problems, and its object is to provide a supported platinum catalyst having a high ratio of diffraction peak intensity of the Pt (220) plane and excellent oxidation resistance, which can be produced by a simple method without using a polymer, and a technology for utilizing the same.
[0011] [Technical means to solve the problem]
[0012] The inventors found that by using a specific reducing agent to load platinum particles on a specific carbon carrier, the ratio of the diffraction peak intensity of the Pt (220) surface of the platinum particles increased and the oxidation resistance was also excellent, thus completing the present invention. That is, the present invention includes the following inventions.
[0013] <1> A supported platinum catalyst comprising a carbon carrier and platinum microparticles supported on the carbon carrier, wherein the ratio of the diffraction peak intensity of the (220) plane to the total of the diffraction peak intensities of the (111) plane, (200) plane and (220) plane obtained by X-ray diffraction is greater than 0.128, and the oxidation consumption temperature of the carbon carrier is greater than 620°C.
[0014] <2> A supported platinum catalyst comprising a carbon support and platinum microparticles supported on the carbon support, wherein the ratio of the diffraction peak intensity of the (220) plane to the total of the diffraction peak intensities of the (111) plane, (200) plane and (220) plane obtained by X-ray diffraction is greater than 0.150.
[0015] <3> The supported platinum catalyst according to <2>, wherein the oxidation consumption temperature of the carbon support is 640° C. or higher.
[0016] <4> The supported platinum catalyst according to <2> or <3>, wherein the resistivity of the carbon support is 0.1 Ω·cm or less.
[0017] <5> The supported platinum catalyst according to any one of <1> to <4>, wherein the carbon support has interconnecting pores.
[0018] <6> The supported platinum catalyst according to any one of <1> to <5>, wherein the Brunauer-Emmett-Teller (BET) specific surface area of the carbon support is 600 m 2 / g~2000m 2 / g.
[0019] <7> A supported platinum catalyst according to any one of <1> to <6>, wherein in an analysis based on the Barrett-Joyner-Halenda (BJH) method, in a pore distribution with the horizontal axis being the pore diameter and the vertical axis being the logarithmic differential pore volume, the carbon support has the highest peak in the pore diameter range of 3 nm to 50 nm.
[0020] <8> A cathode for a fuel cell, comprising the supported platinum catalyst according to any one of <1> to <7>.
[0021] <9> A fuel cell comprising the fuel cell cathode according to <8>.
[0022] <10>A method for manufacturing a supported platinum catalyst, which is a method for manufacturing a supported platinum catalyst comprising a carbon carrier and platinum microparticles supported on the carbon carrier, wherein in the platinum microparticles, the ratio of the diffraction peak intensity of the (220) plane to the total of the diffraction peak intensities of the (111) plane, (200) plane and (220) plane obtained by X-ray diffraction is greater than 0.128, and the manufacturing method comprises: using a reducing agent having a reduction potential of platinum of -0.6 V (vs. Saturated Calomel Electrode, vs. SCE) or more at pH 7 and 25°C to reduce a precursor of the platinum microparticles, thereby loading the platinum microparticles on the carbon carrier.
[0023] <11> According to the manufacturing method described in <10>, in the platinum microparticles, the ratio of the diffraction peak intensity of the (220) plane to the total of the diffraction peak intensities of the (111) plane, (200) plane and (220) plane obtained by X-ray diffraction is greater than 0.150.
[0024] [Effects of the Invention]
[0025] According to one aspect of the present invention, a supported platinum catalyst having a high ratio of diffraction peak intensity of the Pt (220) plane and excellent oxidation resistance can be provided by a simple production method without using a polymer, and a technology for utilizing the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a graph showing the results of measuring the pore distribution of the carbon support used in Example 1 by a gas adsorption method and analyzing it by a BJH method.
[0027] Figure 2 This is the X-ray diffraction pattern (XRD (X-ray diffraction) pattern) of the supported platinum catalyst obtained in Example 1.
[0028] Figure 3 This is the X-ray diffraction pattern (XRD pattern) of the supported platinum catalyst obtained in Example 2.
[0029] Figure 4 This is the X-ray diffraction pattern (XRD pattern) of the supported platinum catalyst obtained in Comparative Example 1.
[0030] Figure 5 This is a graph showing the relationship between the mass of the carbon support and the temperature for the carbon supports used in Examples 1 and 2 and Comparative Examples 1 and 2. DETAILED DESCRIPTION
[0031] An embodiment of the present invention is described below, but the present invention is not limited thereto. The present invention is not limited to the structures described below, and various changes can be made within the scope shown in the claims. The embodiments or embodiments obtained by appropriately combining the technical means disclosed in different embodiments or embodiments are also included in the technical scope of the present invention. In addition, in this specification, "A to B" indicating a numerical range means "above A and below B" unless otherwise specified.
[0032] 〔Supported platinum catalyst〕
[0033] A supported platinum catalyst according to one embodiment of the present invention includes a carbon support and platinum fine particles supported on the carbon support.
[0034] Hereinafter, each component constituting the supported platinum catalyst will be described.
[0035] 〔Carbon Support〕
[0036] In one embodiment of the present invention, the carbon carrier is a porous carbon including mesopores. In this specification, pores with a pore diameter less than 2 nm are referred to as micropores, pores with a pore diameter of 2 nm to 50 nm are referred to as mesopores, and pores with a pore diameter exceeding 50 nm are referred to as macropores, and these pores are collectively referred to as fine pores.
[0037] It is desirable that the mesopores are open pores, and at least a portion of the mesopores become connected pores whose pore portions are connected to each other. The mesopores are open pores and have connected pores, so that the water produced by the catalytic reaction can be discharged to the outside of the pores without being retained in the pores of the carbon carrier, so that the reaction can proceed smoothly. In addition, since oxygen can pass through the connected pores, not only the platinum particles loaded on the outside of the pores can fully contribute to the catalytic reaction, but also the platinum particles loaded on the inside of the pores can fully contribute to the catalytic reaction, and a high catalyst utilization rate can be achieved. Therefore, it is also possible to reduce the amount of the platinum particles required for achieving the desired catalytic activity.
[0038] In addition, the carbon carrier is porous carbon including mesopores and micropores, and the micropores are preferably formed at positions facing the mesopores on carbonaceous walls constituting the outer shells of the mesopores.
[0039] By including micropores, platinum particles can be more stably held on the carbon support. Furthermore, by forming micropores at positions facing the mesopores, fuel gas supplied and discharged to the communicating holes of the mesopores can more easily react with the platinum particles.
[0040] The pore size of the mesopore is preferably 3nm to 50nm, more preferably 3nm to 10nm. By the pore size of the mesopore being within the range, the platinum particles can be enclosed in the mesopores, and the platinum particles can be prevented from agglomerating with each other or falling off the carbon carrier. Therefore, there is an advantage that the life of the supported platinum catalyst can be extended.
[0041] The BET specific surface area of the carbon support is preferably 600 m 2 / g~2000m 2 / g, more preferably 600m 2 / g~1500m 2 / g. In addition, the total pore volume determined by the BET method is preferably 0.2 ml / g to 3.0 ml / g, and more preferably 0.5 ml / g to 2.6 ml / g. By setting the BET specific surface area and the total pore volume in the above range, a sufficient amount of pores can be formed, and the structure of the interconnected pores formed by the carbonaceous material can be well maintained.
[0042] The oxidation consumption temperature of the carbon support is preferably 620° C. or higher, more preferably 630° C. or higher. When the oxidation consumption temperature is within the above range, the oxidation resistance is excellent, and the consumption of the supported platinum catalyst accompanying the progress of the reaction can be suppressed. In addition, the higher the oxidation consumption temperature, the more preferred, and there is no particular upper limit, and for example, it can be 700° C. or lower.
[0043] In this specification, the pore diameter, BET specific surface area, total pore volume, and oxidation consumption temperature are values measured according to the method described in the examples described later.
[0044] The carbon support may also have a random pore structure in which the mesopores are arranged irregularly. The so-called "random pore structure" means that the pores are not arranged in an orderly manner, and the pore structure of the carbon powder is different from the structure in which the pores are arranged in an orderly manner.
[0045] (Carbon support having a carbonaceous wall forming a three-dimensional network structure)
[0046] In a further embodiment of the present invention, in the carbon carrier, the carbonaceous wall constituting the outer contour of the mesopore may form a three-dimensional mesh structure. In addition, the carbon carrier may also have a random pore structure formed by irregularly arranging the mesopores. The carbonaceous wall of the carbon carrier forms a three-dimensional mesh structure and has a random pore structure, thereby becoming a carbon carrier with higher strength. The other structures of the carbon carrier having a carbonaceous wall forming a three-dimensional mesh structure are the same as those of the carbon carrier, so their description is omitted.
[0047] (Carbon support having a carbonaceous wall forming a layered structure)
[0048] In a further aspect of the present invention, the carbon carrier may further include a portion forming a layered structure in the carbonaceous wall constituting the outer shell of the mesopore.
[0049] The portion of the carbonaceous wall that forms the layered structure may be formed by the development of crystallinity. Furthermore, it is not necessary for all portions of the carbonaceous wall to form a layered structure containing crystallinity, and an amorphous structure may exist in a portion of the carbonaceous wall.
[0050] The presence of a portion forming a layered structure in the carbonaceous wall of the carbon carrier can further increase the oxidation consumption temperature of the carbon carrier. Specifically, the oxidation consumption temperature of the carbon carrier having a carbonaceous wall forming a layered structure is preferably 640°C or higher, and can more preferably be 650°C or higher. In the above case, the higher the oxidation consumption temperature, the more preferred, and there is no particular upper limit, and for example, it can be exemplified as 700°C or lower.
[0051] In addition, by the presence of a portion forming a layered structure in the carbonaceous wall of the carbon carrier, the resistivity of the carbon carrier can be reduced. Specifically, the resistivity of the carbon carrier having a carbonaceous wall forming a layered structure is preferably 0.1Ω·cm or less, and can also be more preferably set to 0.05Ω·cm or less. By having a resistivity of 0.1Ω·cm or less, when used as a fuel cell cathode for a fuel cell, a high power generation efficiency can be achieved.
[0052] In this specification, the resistivity is a value measured by the method described in the examples described below. The lower the resistivity, the better, and there is no particular lower limit, but for example, it can be 0.004 Ω·cm or more.
[0053] The other structures of the carbon support having carbonaceous walls forming a layered structure are the same as those of the above-mentioned carbon support, and thus description thereof is omitted.
[0054] Furthermore, the carbon support preferably contains substantially only carbon. For example, the carbon support preferably does not contain resin, in which case a certain amount of oxide (such as MgO) and / or sulfate (such as MgSO4) may also be present.
[0055] [Method for producing carbon support]
[0056] In one form of the present invention, a carbon carrier can be manufactured by a method for manufacturing a carbon carrier comprising the following steps: a calcination step, in which a mixture of a carbon source that serves as a constituent material of a carbonaceous wall and a mesoporous casting source, or a metal organic acid that serves as both a carbon source and a casting source is calcined to produce a calcined body; and a removal step, in which the casting source is removed from the obtained calcined body.
[0057] As a carbon source constituting the carbonaceous wall, a resin can be preferably used. Such resins include thermoplastic resins such as polyvinyl alcohol, aliphatic or aromatic polyester resins, polyolefin resins, acrylic resins, styrene resins, polyamide resins, polyacrylonitrile resins, synthetic resins such as elastomers based on polybutadiene and polyisoprene, natural rubber, and petroleum resins, and thermosetting resins such as phenolic resins, furan resins, epoxy resins, and alkyd resins.
[0058] As the mold source of the mesopores, oxides can be cited. As such oxides, from the viewpoint of ease of removal in the removal step described later, oxides of alkaline earth metals can be preferably used. As alkaline earth metals, magnesium, calcium, strontium, barium, etc. can be cited, among which magnesium and calcium are preferred, and magnesium is most preferred.
[0059] Examples of the metal organic acid include magnesium citrate, magnesium oxalate, calcium citrate, calcium oxalate, etc. The metal organic acid may be in the form of a hydrate or an anhydride.
[0060] The calcination process may be suitably performed so that mesopores are formed by carbonization of the carbon source and coating of the sintered mold source, and micropores may develop at positions facing the mesopores.
[0061] As one aspect of the present invention, the calcination process is preferably carried out in a non-oxidizing environment such as an argon atmosphere or a nitrogen atmosphere, or under a reduced pressure of 133 Pa (1 Torr) or less. In addition, the calcination temperature is preferably 500° C. or more, more preferably 500° C. to 1500° C. The calcination time can be appropriately determined according to the materials used, the mixing ratio, and other calcination conditions, for example, 0.5 hours to 3 hours, more preferably 1 hour to 3 hours.
[0062] The removal step may be performed by immersing the calcined body obtained in the calcining step in a solution for removing the mold source to dissolve and remove the mold source.
[0063] As the mold source removal solution, common inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, acetic acid, and hot water can be used. In order to prevent the properties of the carbon support from changing, it is more preferable to use the inorganic acid as a dilute acid of 4 mol / l or less, or to use hot water of 80° C. or more. By using an inorganic acid, there is an advantage that the removal speed becomes faster.
[0064] By appropriately selecting the type of resin that becomes the carbon source, the type and particle size of the mold source, the mixing ratio of the carbon source and the mold source, the type of metal organic acid, the calcination conditions, the mold removal conditions, etc., the various physical properties of the carbon carrier can be controlled within the desired range. Furthermore, the carbon carrier manufactured by the method is a porous carbon including mesopores in a single particle, and does not have an organizational structure (a cohesive structure formed by welding multiple particles), so uniform slurry dispersion is desired when making an electrode.
[0065] The above-described production method can produce porous carbon in which a decrease in specific surface area due to carbon shrinkage is suppressed and desired physical properties are maintained.
[0066] (Method for producing a carbon support having a carbonaceous wall forming a layered structure)
[0067] The carbon support having a carbonaceous wall forming a layered structure can be produced by further performing a heat treatment step of heat-treating the calcined body having pores formed therein after the calcination step and the removal step in the above-mentioned method for producing the carbon support.
[0068] The heat treatment process is preferably carried out in a non-oxidizing environment such as an argon environment or a nitrogen environment, or under a reduced pressure of less than 133Pa (1Torr). In addition, there is no problem if the heat treatment temperature is above the temperature at which amorphous carbon is crystallized, but in order to smoothly and in a short time form a layered structure (crystallization), it is preferably above 1000°C, more preferably 1500°C to 2200°C. In addition, the heat treatment time can be appropriately determined according to the materials used, the mixing ratio, and other heat treatment conditions, for example, 1 hour to 3 hours, more preferably 1 hour to 2 hours.
[0069] By heat-treating the calcined body having pores formed therein, a carbon support having a layered structure formed entirely or partially in the carbonaceous wall can be produced without causing a decrease in the specific surface area.
[0070] 〔Platinum particles〕
[0071] (Diffraction peak intensity obtained by X-ray diffraction)
[0072] For example, by supporting platinum fine particles on the carbon support according to the method for producing a supported platinum catalyst described below, the ratio of the diffraction peak intensity of the Pt (220) plane of the platinum fine particles can be increased.
[0073] In one form of the platinum microparticles of the present invention, in the platinum microparticles loaded on the carbon carrier, the ratio of the diffraction peak intensity of the (220) plane to the total of the diffraction peak intensities of the (111) plane, (200) plane and (220) plane obtained by X-ray diffraction is greater than 0.128, and more preferably greater than 0.129.
[0074] In one form of the platinum microparticles of the present invention, by using a carbon carrier having a carbonaceous wall forming the layered structure as a carbon carrier, the ratio of the diffraction peak intensity of the Pt (220) surface of the platinum microparticles can also be further increased. More specifically, in the platinum microparticles supported on the carbon carrier having a carbonaceous wall forming the layered structure, the ratio of the diffraction peak intensity of the (220) surface to the total of the diffraction peak intensities of the (111) surface, (200) surface and (220) surface obtained by X-ray diffraction is 0.128 or more, more preferably 0.150 or more, and even more preferably 0.155 or more.
[0075] The ratio of the diffraction peak intensity of the Pt(220) surface of the platinum microparticles is 0.128 or more, and the supported platinum catalyst can show high ORR activity. Furthermore, the higher the ratio of the diffraction peak intensity of the Pt(220) surface of the platinum microparticles, the more preferred it is, and there is no particular upper limit, for example, it can be exemplified as 0.5 or less.
[0076] The diffraction peak intensities of the (111) plane, (200) plane, and (220) plane obtained by X-ray diffraction are values measured according to the method described in Examples described later.
[0077] (Particle size and platinum loading of platinum particles)
[0078] The particle size of the platinum microparticles supported on the carbon carrier is preferably less than 10 nm. By setting it to the above range, the supported platinum catalyst can be evenly coated when making the electrode. Furthermore, the particle size of the platinum microparticles is the average value of the major diameters of more than 20 particles measured using a transmission electron microscope (TEM).
[0079] The amount of platinum supported on the carbon support is not particularly limited and can be appropriately set according to the ORR activity of the platinum fine particles, application, and the like.
[0080] The particle size of the platinum fine particles and the amount of platinum supported can be controlled by appropriately selecting various conditions such as the type of precursor of the platinum fine particles used in the production of the supported platinum catalyst and the mass ratio to the carbon support.
[0081] [Method for producing supported platinum catalyst]
[0082] The supported platinum catalyst can be produced by a production method including the step of reducing a precursor of platinum fine particles using a specific reducing agent to support the platinum fine particles on the carbon support.
[0083] The process can be preferably carried out by a conventional method of bringing the carbon support into contact with the platinum particles for loading. Specifically, the platinum particles can be loaded on the carbon support by immersing the carbon support in a platinum solution containing a precursor of the platinum particles and a solvent, and adding a reducing agent to the obtained mixture for a reduction reaction.
[0084] Precursors of platinum particles include platinum powder, platinum (II) chloride, platinum (IV) chloride, chloroplatinic acid (IV), platinum (IV) oxide, dinitrosodiammine platinum (II), dichlorotetrammine platinum (II), hexahydroxyplatinic acid (IV), potassium tetrachloroplatinate (II), potassium tetrachloroplatinate (IV), and other platinum-containing compounds. These platinum-containing compounds may be used alone or in combination of two or more.
[0085] As the reducing agent, a reducing agent having a reducing power of -0.6 V (vs. SCE) or more, more preferably -0.55 V (vs. SCE) or more at pH 7 and 25° C. can be used. When the reduction potential of the reducing agent is within the above range, the ratio of the diffraction peak intensity of the Pt (220) surface of the platinum microparticles can be increased.
[0086] Specific examples of the reducing agent preferably used in the present invention include formaldehyde and sodium hypophosphite.
[0087] In the present invention, the reducing agent refers to a reducing agent in a solid or liquid state.
[0088] Examples of the solvent include water. The solvent may contain a pH adjuster such as sodium carbonate as needed.
[0089] The amount of the solvent added to the platinum solution can be appropriately determined by a person skilled in the art within a range in which the precursor of the platinum fine particles can be dissolved and a stable platinum complex can be formed.
[0090] In addition, in the mixture, the amount of the reducing agent added is preferably 1.0- to 1.1-fold the molar amount of the precursor of the platinum fine particles.
[0091] The impregnation temperature and time can be appropriately set according to the type and concentration of the precursors of the carbon carrier and platinum particles. For example, the impregnation temperature is 60°C to 90°C, more preferably 70°C to 85°C, and the impregnation time is 0.5 hour to 3 hours, more preferably 1 hour to 2 hours.
[0092] The reaction temperature and reaction time of the reduction reaction can be appropriately set according to the type and addition amount of the reducing agent. For example, the reaction temperature is 60°C to 90°C, more preferably 70°C to 85°C, and the reaction time is 1 hour to 5 hours, more preferably 3 hours to 4 hours.
[0093] After the reduction reaction, filtration, washing, drying, etc. may be performed as needed to obtain the supported platinum catalyst according to one embodiment of the present invention.
[0094] Furthermore, the carbon support in the obtained supported platinum catalyst preferably has the characteristics of the above-mentioned carbon support.
[0095] [Preferred Use]
[0096] The supported platinum catalyst according to one embodiment of the present invention exhibits excellent ORR activity and oxidation resistance under the operating environment of a fuel cell. Therefore, the supported platinum catalyst according to one embodiment of the present invention can be preferably used in a cathode for a fuel cell.
[0097] The cathode for a fuel cell can be applied to various fuel cells. Examples of such fuel cells include solid polymer fuel cells (polymer electrolyte fuel cells (PEFC)).
[0098] [Example]
[0099] In the following examples, various physical properties of the carbon support were measured by the following methods.
[0100] (pore size of the carbon support)
[0101] The pore size of the mesopores of the carbon support is measured using the Barrett-Joyner-Halenda (BJH) method. Specifically, in the pore distribution obtained based on the BJH method (the horizontal axis is the pore size, the vertical axis is the logarithmic differential pore volume (dV p / dlogd p )), the pore size at which the highest peak exists is defined as the pore size of the mesopore.
[0102] (BET specific surface area and total pore volume of carbon carrier)
[0103] Using nitrogen as the adsorption gas, the measurement was performed at 77K (-196°C) to obtain the nitrogen adsorption isotherm. In the measurement, the automatic gas / vapor adsorption measurement device BELSORP-MAX manufactured by Bayer (BEL) Co., Ltd. of Japan was used. The BET specific surface area was calculated based on the measurement points in the range of relative pressure (P / P0) = 0.05 to 0.20. The total pore volume was obtained based on the adsorption amount at the relative pressure (P / P0) = 0.95.
[0104] (Micropore capacity and mesopore capacity of carbon carrier)
[0105] The micropore volume was calculated using the Dubinin-Astakhov (DA) method, and the mesopore volume was obtained by subtracting the micropore volume from the total pore volume.
[0106] [Example 1]
[0107] First, prepare trimagnesium anhydride dicitrate [Mg3(C6H5O7)2] which serves as both a carbon source and a mold source, and heat treat it at 900°C for 1 hour in a nitrogen environment. Thus, a calcined product including magnesium oxide and carbonaceous walls as mold particles is obtained. Then, the calcined product obtained is washed with a 30wt% sulfuric acid solution to completely dissolve the magnesium oxide, thereby obtaining a porous carbon having a plurality of mesopores, and the carbonaceous walls constituting the outer contour of the mesopores form a three-dimensional mesh structure and an irregular pore structure. Thereafter, the obtained porous carbon is crushed using a planetary bead mill for 1.5 hours at a rotation speed of 120 rpm, and adjusted to a median diameter of 2μm to 4μm, to produce a carbon carrier that essentially contains only carbon. Furthermore, alumina beads of φ5mm are used as beads.
[0108] Figure 1 The carbon support thus obtained was subjected to pore distribution measurement using a gas adsorption method and analyzed using the BJH method. Figure 1 It can be confirmed that the obtained carbon support is analyzed based on the BJH method, with the horizontal axis being the pore diameter and the vertical axis being the logarithmic differential pore volume (dV p / dlogd p ) has the highest peak at a pore diameter of 4 nm.
[0109] The carbon carrier 0.225g, 0.12g of chloroplatinic acid (IV) and 0.13g of sodium carbonate were mixed in 100mL of ultrapure water and stirred for 1 hour while being heated to 80°C. Then, 20mL of 0.07mol / L formaldehyde (pH 7, platinum reduction potential at 25°C is -0.52) aqueous solution was added dropwise at a certain speed for 5 minutes while stirring, and then stirred for 4 hours while maintaining a temperature of 80°C. The obtained stirred solution was filtered, the solid component was vacuum dried, and then heated at 120°C under a nitrogen environment to obtain a black powder as a supported platinum catalyst. Furthermore, the carbon carrier in the supported platinum catalyst obtained has a plurality of mesopores, and the carbonaceous wall constituting the outer shell of the mesopore forms a three-dimensional mesh structure and has an irregular pore structure, and the carbon carrier substantially contains only carbon.
[0110] [Example 2]
[0111] The porous carbon prepared in the same manner as in Example 1 was further heat treated at 1800°C for 1 hour in a nitrogen environment. The obtained porous carbon had a plurality of mesopores, and the carbonaceous walls constituting the outer contours of the mesopores formed a three-dimensional mesh structure and had a random pore structure, and a portion forming a layered structure existed in the carbonaceous walls. The obtained porous carbon was pulverized using a planetary bead mill in the same manner as in Example 1 to obtain a carbon carrier having a carbonaceous wall forming a layered structure and substantially containing only carbon.
[0112] Using the obtained carbon support, a black powder was obtained as a supported platinum catalyst in the same manner as in Example 1. Furthermore, the carbon support in the supported platinum catalyst obtained has a plurality of mesopores, and the carbonaceous walls constituting the outer contours of the mesopores form a three-dimensional mesh structure and have a random pore structure, and further, there is a portion forming a layered structure in the carbonaceous walls, and the carbon support substantially contains only carbon.
[0113] [Comparative Example 1]
[0114] Vulcan (registered trademark) XC-72 (manufactured by CABOT, having no interconnecting pores and having a separate tissue structure) was subjected to ultrasonic dispersion treatment at room temperature for 10 minutes to produce a carbon support.
[0115] Using the carbon support obtained above, a black powder was obtained as a supported platinum catalyst in the same manner as in Example 1.
[0116] [Comparative Example 2]
[0117] Ketjen Black EC300J (manufactured by Lion Specialty Chemicals Co., Ltd., having no interconnecting pores and having a tissue structure) was subjected to ultrasonic dispersion treatment at room temperature for 10 minutes to prepare a carbon support.
[0118] Using the carbon support obtained above, a black powder was obtained as a supported platinum catalyst in the same manner as in Example 1.
[0119] [Comparative Example 3]
[0120] As a carbon support, the carbon support used in Example 2 was prepared.
[0121] The carbon support is dispersed in ultrapure water to obtain a dispersion. On the other hand, potassium tetrachloroplatinate (II) is dissolved in ultrapure water to obtain a platinum solution. The platinum solution is added to the dispersion and mixed, and a 0.1M sodium hydroxide aqueous solution is added to the obtained mixture to adjust the pH value to 8, and stirred at 70°C for 1 hour, thereby precipitating the hydroxide of platinum on the carbon support. The obtained stirred liquid is filtered, the solid component is vacuum dried, and then heat-treated at 300°C for 3 hours in an environment of 50% H2 and 50% argon to obtain a supported platinum catalyst. The amount of platinum loaded is 30wt% relative to the carbon support. Furthermore, in the platinum growth method, no reducing agent is used.
[0122] [Comparative Example 4]
[0123] A supported platinum catalyst was obtained in the same manner as in Comparative Example 3 except that the supported amount of platinum was 40 wt % based on the carbon support.
[0124] [Comparative Example 5]
[0125] A supported platinum catalyst was obtained in the same manner as in Comparative Example 3 except that the supported amount of platinum was 50 wt % based on the carbon support.
[0126] The physical properties of each carbon support used in Examples 1 and 2 and Comparative Examples 1 to 5 are summarized in Table 1 below.
[0127] [Table 1]
[0128]
[0129] 〔Confirmation of supported platinum catalyst〕
[0130] The black powders obtained in Examples 1 to 2 and Comparative Examples 1 to 5 were respectively dissolved in aqua regia, and platinum was quantified using inductively coupled plasma-atomic emission spectroscopy (ICP-AES) analysis. The platinum loading of the black powder was calculated based on the concentration.
[0131] In addition, each black powder was observed using a transmission electron microscope (TEM, manufactured by JEOL Ltd., JEM-2100) at an observation magnification of 500,000 times, and it was confirmed that platinum fine particles (diameter 1 nm to 5 nm) were dispersed and supported on the carbon support in all black powders.
[0132] [Measurement of the ratio of the diffraction peak intensity of the Pt (220) surface]
[0133] For the supported platinum catalysts obtained in Examples 1 to 2 and Comparative Examples 1 and 3 to 5, the diffraction peak intensities obtained by X-ray diffraction were measured according to the following procedure, and the ratio of each diffraction peak intensity to the total of the diffraction peak intensities of the (111) plane, (200) plane and (220) plane was calculated.
[0134] The peak separation of the diffraction peaks was performed using Multipeakfitting 2 attached to Igor Pro 6.36J. The baseline was analyzed using the Cubic formula, and the separation of each peak was analyzed using the Voigt formula. The diffraction peak intensity of each peak was calculated based on the height of each peak.
[0135] Figure 2 to Figure 4 It is the X-ray diffraction pattern (XRD pattern) of the supported platinum catalyst obtained in Example 1-Example 2 and Comparative Example 1.
[0136] 〔Evaluation of oxidation resistance〕
[0137] The oxidation consumption temperature of the carbon supports used in Examples 1 and 2 and Comparative Examples 1 to 5 was measured in the following manner.
[0138] The carbon carrier was heated from room temperature to 900°C at a rate of 5°C / min in an atmospheric environment to investigate the relationship between the mass of the carbon carrier and the temperature. Based on the obtained graph (the horizontal axis is the temperature, and the vertical axis is the mass of the carbon carrier), the temperature was calculated at the intersection of an imaginary extension line of a portion where the mass has hardly changed (a portion roughly parallel to the horizontal axis) and an imaginary extension line of a portion where the mass has changed significantly.
[0139] Figure 5This is a graph showing the relationship between the mass of the carbon support and the temperature for the carbon supports used in Examples 1 and 2 and Comparative Examples 1 and 2.
[0140] 〔Measurement of resistivity〕
[0141] The carbon supports used in Examples 1 to 2 and Comparative Examples 2 to 5 were pressurized to 40 MPa using a powder resistance system MCP-51 (manufactured by Mitsubishi Chemical Analytech Co., Ltd.), and then measured using a resistivity meter Loresta GP and a four-probe method using a constant current.
[0142] [Evaluation of ORR activity]
[0143] (Electrode Preparation)
[0144] Using the supported platinum catalysts obtained in Examples 1 to 2 and Comparative Examples 1 to 5, electrodes were prepared according to the method described in Taro Emoto and Hirohisa Yamada, Electrochemistry and Industrial Physical Chemistry (Vol. 79 (2), pp. 116-121 (2011)) in the following manner.
[0145] The prescribed amount of loaded platinum catalyst (1.5 μg in terms of platinum mass) estimated from the amount of platinum loading, 0.625 mL of ultrapure water, and 5.625 mg of ethanol were mixed, and an ultrasonic cleaner was used to perform a dispersion treatment for 30 minutes while cooling in an ice bath. 10.0 μL of the dispersion was applied to a disk electrode (5 mm in diameter) made of glassy carbon using a micropipette, and dried at 60° C. for 10 minutes using an air-supplied dryer. Subsequently, 0.10 mL of a 5% Nafion (registered trademark) dispersion (manufactured by Sigma-Aldrich) was mixed with 4.90 mL of 2-propanol, and 3.69 μL of the mixed solution was applied to the disk electrode using a micropipette, and dried at 60° C. for 1 minute using an air-supplied dryer to obtain an electrode.
[0146] (Calculation of platinum mass activity (ORR activity))
[0147] For the supported platinum catalysts obtained in Examples 1 to 2 and Comparative Examples 1 to 5, the platinum mass activity (ORR activity) under the operating environment of the fuel cell was calculated according to the calculation method described in Taro Itomoto and Hirohisa Yamada, "Electrochemistry and Industrial Physical Chemistry" (Vol. 79 (2), pp. 116-121 (2011)) according to the following procedures.
[0148] A half cell was prepared in which the obtained electrode was used as a working electrode, a platinum mesh was used as a counter electrode, a reversible hydrogen electrode was used as a reference electrode, and a nitrogen-saturated 0.1M perchloric acid aqueous solution was used as an electrolyte. The electrolyte was bubbled with nitrogen for 1 hour. Cyclic voltammetry was performed on the half cell for 100 cycles under the conditions of 25°C, 0.05V to 1.20V, and 0.05V / s.
[0149] The reduction current value at 0.40 V was used as the reference, and the reduction current value in the range of 0.05 V to 0.40 V in the current value during the cathode scan of the 100th cycle was integrated to obtain the hydrogen adsorption quantity (unit: C). The hydrogen adsorption quantity was divided by the theoretical area conversion quantity of hydrogen adsorption relative to platinum (2.10 C / m 2 ), and thus estimate the platinum surface area (unit: m 2 ).
[0150] In addition, for the electrode (working electrode), in order to obtain the ORR activity, a half-cell was made in which a platinum mesh was set as a counter electrode, a reversible hydrogen electrode was set as a reference electrode, and an oxygen-saturated 0.1M perchloric acid aqueous solution was set as an electrolyte. The electrolyte was bubbled with oxygen for 3 hours. In addition, while the working electrode was rotated at 400rpm, 625rpm, 900rpm, 1225rpm, and 1600rpm, the half-cell was scanned at a speed of 0.01V / S from the negative direction to the positive direction in the range of 25°C and 0.05V to 0.1V. Using the current value at 0.9V of the current-potential curve obtained at each rotation speed, the activation dominating current was obtained according to the Koutecky-Levich plot. Based on the estimated platinum surface area and the activation dominating current, the specific activity was calculated, and the platinum mass activity (A / g) was calculated by conversion per unit mass of the platinum catalyst.
[0151] The obtained results are shown in Table 2 below.
[0152] [Table 2]
[0153]
[0154] As shown in Table 2, when Examples 1 to 2 are compared with Comparative Examples 1 to 2, it is found that Examples 1 to 2 have high oxidation consumption temperatures and excellent oxidation resistance. In addition, when Examples 1 to 2 are compared with Comparative Examples 3 to 5, in Examples 1 to 2, which are reduced using a reducing agent having a platinum reduction potential of -0.6 V (vs. SCE) or more at pH 7 and 25°C, the ratio of the diffraction peak intensity of the (220) plane of the platinum microparticles (pt (220)) is 0.128 or more, indicating high ORR activity.
[0155] In addition, generally, porous carbon without a structure has a higher resistivity than a carbon carrier with a structure. However, as shown in Table 2, although the carbon carrier used in Example 2 has no structure, the resistivity is comparable to that of the carbon carrier of Comparative Example 2 having a structure.
[0156] [Industrial Applicability]
[0157] The supported platinum catalyst according to one embodiment of the present invention can be preferably used for a cathode for a fuel cell.
Claims
1. A supported platinum catalyst for a cathode of a fuel cell, comprising a carbon carrier and platinum particles supported on the carbon carrier, In the platinum fine particles, a ratio of the diffraction peak intensity of the (220) plane to the total diffraction peak intensities of the (111) plane, the (200) plane, and the (220) plane obtained by X-ray diffraction is 0.128 or more. The oxidation consumption temperature of the carbon carrier is above 620°C. The carbon support has the highest peak top in a pore diameter of 3 nm to 50 nm in a pore distribution in which the horizontal axis is the pore diameter and the vertical axis is the logarithmic differential pore volume in an analysis based on the Barrett-Joyner-Harend method.
2. A supported platinum catalyst for a cathode of a fuel cell, comprising a carbon support and platinum particles supported on the carbon support, In the platinum fine particles, a ratio of the diffraction peak intensity of the (220) plane to the total diffraction peak intensities of the (111) plane, (200) plane, and (220) plane obtained by X-ray diffraction is 0.155 or more. 3 . The supported platinum catalyst for a cathode for a fuel cell according to claim 2 , wherein the oxidation consumption temperature of the carbon support is 620° C. or higher.
4. The supported platinum catalyst for a cathode for a fuel cell according to claim 1 or 2, wherein the oxidation consumption temperature of the carbon support is 640°C or higher. 5 . The supported platinum catalyst for a cathode for a fuel cell according to claim 1 , wherein the resistivity of the carbon support is 0.1 Ω·cm or less.
6. The supported platinum catalyst for a cathode for a fuel cell according to claim 1 or 2, wherein the carbon support has interconnecting pores.
7. The supported platinum catalyst for a cathode of a fuel cell according to claim 1 or 2, wherein the Buerter specific surface area of the carbon support is 600 m 2 / g~2000m 2 / g.
8. A supported platinum catalyst for a cathode for a fuel cell according to claim 2, wherein in an analysis based on the Barrett-Joyner-Harend method, in a pore distribution with the horizontal axis being the pore diameter and the vertical axis being the logarithmic differential pore volume, the carbon support has the highest peak in the pore diameter range of 3 nm to 50 nm.
9. A supported platinum catalyst for a cathode for a fuel cell according to claim 1, wherein in an analysis based on the Barrett-Joyner-Harend method, in a pore distribution with the horizontal axis being the pore diameter and the vertical axis being the logarithmic differential pore volume, the carbon support has the highest peak in the pore diameter range of 3 nm to 10 nm. 10 . A cathode for a fuel cell, comprising the supported platinum catalyst for a cathode for a fuel cell according to claim 1 .
11. A fuel cell comprising the cathode for a fuel cell according to claim 10.
12. A method for producing a supported platinum catalyst for a cathode of a fuel cell, comprising a carbon carrier and platinum particles supported on the carbon carrier, wherein: In the platinum fine particles, a ratio of the diffraction peak intensity of the (220) plane to the total diffraction peak intensities of the (111) plane, the (200) plane, and the (220) plane obtained by X-ray diffraction is 0.128 or more. The carbon support has a highest peak in a pore size of 3 nm to 50 nm in a pore distribution in which the horizontal axis is the pore size and the vertical axis is the logarithmic differential pore volume in an analysis based on the Barrett-Joyner-Harend method. The method for producing a supported platinum catalyst for a fuel cell cathode includes: reducing a precursor of the platinum particles using a reducing agent having a pH value of 7 and a reduction potential of platinum of greater than -0.6 V relative to a saturated calomel electrode at 25°C, and loading the platinum particles on the carbon carrier.
13. A method for producing a supported platinum catalyst for a cathode for a fuel cell, comprising: a carbon support and platinum particles supported on the carbon support; wherein in the platinum fine particles, a ratio of the diffraction peak intensity of the (220) plane to the total diffraction peak intensities of the (111) plane, the (200) plane, and the (220) plane obtained by X-ray diffraction is 0.155 or more, The method for producing a supported platinum catalyst for a cathode of a fuel cell comprises: A step of reducing a precursor of the platinum fine particles using a reducing agent having a pH of 7 and a reduction potential of platinum at 25° C. of −0.6 V or more relative to a saturated calomel electrode, to support the platinum fine particles on the carbon support.