A welding cold crack test and evaluation method
Through finite element analysis and simple test fixtures, a cold crack test model is established, which solves the problems of unstable cold crack testing and equipment dependence in the existing technology, achieves efficient and accurate welding cold crack evaluation, and improves the safety of welded structures. and quality.
Patent Information
- Application Number
- CN202111073127.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-09-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-09-14
AI Technical Summary
Existing welding cold crack testing methods have limitations. It is difficult to accurately evaluate the tendency of cold cracks under different stress states. The test results are unstable and require complex sample processing and special equipment.
The finite element analysis method is combined with a simple annular specimen and a combined test fixture. By calculating the transverse residual stress of the weld, a cold crack test model is established, and the size of the annular specimen is adjusted to change the restraint strength, achieving accurate evaluation without the need for special equipment.
It achieves accurate evaluation of the tendency of welding cold cracks, is easy to operate, and has good consistency in test results. It is suitable for testing under different restraint conditions and improves the safety and connection quality of welded structures.
Smart Images

Figure CN113959801B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of welding, and in particular relates to a welding cold crack test and evaluation method. Background Art
[0002] In high-strength steel welding, cold cracks are a common form of quality defects that can occur in any area of the welded joint, including the weld zone, fusion zone, and heat-affected zone. For high-strength steel welds, the presence of cold cracks will lead to a serious decrease in the bearing capacity of the connected structure. In addition, cold cracks in high-strength steel welded joints generally have the characteristics and tendency of delayed cracking, which will bring more uncertainty and greater difficulty to the safety assessment of the product connection structure, the design and development of the connection process, the accurate assessment of weldability, and the application of high-strength steel.
[0003] Before high-strength steel materials are used in product design, in addition to evaluating the basic properties of the materials themselves, their organizational state, weld strength, and the processability of the connecting structure, it is more important to evaluate the comprehensive weldability of the materials and structures, especially the tendency of cold cracks in the welded joints, in order to provide guidance for the subsequent optimization and improvement of welding methods and the precise design of the process.
[0004] At present, the existing test methods for welding cold cracks all have certain limitations. For the inclined Y groove butt crack test and the rigid fixed butt crack test, since the size of the sample is limited before the test, it is difficult to make a more accurate evaluation of the cold cracking tendency under different situations and stress states by using the above methods; at the same time, during the test, the above methods generally have the disadvantages of complex sample preparation process, difficult to ensure preparation consistency and unstable test results. Taking the inclined Y groove butt crack test as an example, since it is not specified that the test sample is fixed by a restrained weld around the four sides, it is difficult to ensure that the test sample does not warp and deform and the spacing between the two sides of the parent material is consistent when welding the restrained welds on both sides of the test weld, and then it is impossible to ensure that the restraint state at the test weld is basically consistent and the stability of the test results. If the tensile restrained crack test TRC or the rigid restrained crack test (RRC) is used to perform welding cold crack tests under variable restraint, it is also necessary to use special equipment to achieve it, which will bring various inconveniences to the evaluation of cold crack tendency under different welding process conditions in actual production.
[0005] The tendency of cold cracking is one of the test contents that must be carried out before the high-strength steel welding process is determined. It has very important practical significance for the safety of the entire subsequent welding structure and the guarantee of production quality. Up to now, there has not been a relatively systematic and simple test method with relatively stable test results and adjustable restraint state for the evaluation technology of the tendency of cold cracking of high-strength steel. Summary of the invention
[0006] In order to overcome the above problems, the present invention provides a welding cold crack test and evaluation method. This method does not require the use of special testing equipment or complicated sample processing and preparation. It only requires welding simulation analysis software, a simple annular specimen and a simple combined test fixture to accurately evaluate the tendency of welding cold cracks. The test is simple and has good operability.
[0007] A welding cold crack test and evaluation method, the specific steps are as follows:
[0008] Step 1, calculating the maximum value σ1 of the transverse residual stress of the target weld of the product based on the finite element analysis method, wherein the target weld is a butt weld;
[0009] Step 2: Establish a cold crack test model:
[0010] The cold crack test model 1 is composed of a circular sample 11, a ring sample 12 and a test weld 13, wherein the circular sample 11 is welded inside the ring sample 12 and is concentric with the ring sample 12, and the upper surfaces of the circular sample 11 and the ring sample 12 are ensured to be in the same plane; the test weld 13 is formed by welding at the longitudinal half position of the Y-shaped groove between the circular sample 11 and the ring sample 12;
[0011] Step 3: Determine the maximum transverse residual stress σ2 of the test weld and lock the size of the cold crack test model:
[0012] Based on the finite element analysis method, the maximum value σ2 of the weld transverse residual stress at the test weld 13 in the cold crack test model 1 is calculated;
[0013] Specifically, the maximum transverse residual stress σ2 of the test weld 13 is determined and the size of the cold crack test model 1 is locked by the following two methods:
[0014] Method 1: The inner diameter of the circular ring specimen 12 is fixed, and the outer diameter of the circular ring specimen 12 is adjusted to obtain the maximum transverse residual stress σ2 of the test weld 13 under different restraint strengths;
[0015] Method 2: fix the outer diameter of the circular ring specimen 12, and adjust the inner diameter of the circular ring specimen 12 to obtain the maximum transverse residual stress σ2 of the test weld under different restraint strengths;
[0016] When the value of σ2 is 1.2σ1≤σ2≤1.3σ1, the outer and inner diameter dimensions of the locking ring specimen 12;
[0017] Step 4, according to the size of the cold crack test model 1 locked in step 3, a circular sample 11 and a ring sample 12 are processed and manufactured;
[0018] Step 5: Make a cold crack test welding fixture:
[0019] The cold crack test welding fixture 2 comprises a cylindrical base 21 and a square fixing plate 22, wherein the cylindrical base 21 is welded at the bottom center of the square fixing plate 22;
[0020] Step 6: Prepare cold crack test samples:
[0021] The circular sample 11 and the annular sample 12 are fastened to the square fixing plate 22 of the cold crack test welding fixture 2, and the assembled sample and the fixture are clamped as a whole on the three-jaw chuck, and the test weld 13 is welded to form the test weld by the same welding process and working conditions as the target weld of the product, thereby completing the preparation of the cold crack test sample;
[0022] Step 7: Cold crack test sample test weld crack detection:
[0023] The test weld crack detection is carried out after the test weld is formed and left to stand for 24 hours. The crack generation conditions on the test weld surface and the test weld cross section are evaluated in turn, and the presence or absence of cracks is used as the evaluation basis;
[0024] Step 8: Comprehensive determination of cold cracking tendency:
[0025] When cold cracks are detected at any point on the test weld surface or in the test weld cross section, the entire welded structure has a greater tendency to cold crack, and the current welding process needs to be redesigned and optimized; if cold cracks are not detected on the test weld surface or in the test weld cross section, the entire welded structure has no obvious tendency to cold crack under the current welding process.
[0026] In the step 1, the maximum value σ1 of the transverse residual stress of the target weld of the product is calculated according to the following steps:
[0027] Step 1: Mesh division: Import the CATIA 3D model of the product into the Hypermesh software to complete the hexahedral mesh division of each component of the 3D model without changing the original assembly relationship;
[0028] Step 2: Import components: Open the Simufact.welding software, input the two environmental variables of ambient temperature and gravity acceleration, and input the ambient temperature as 20℃ and gravity acceleration as 9.8m / S. 2 , and then import the meshed file in step 1 into the Simufact.welding software;
[0029] Step 3, define materials: according to the material type requirements of each component, assign corresponding material properties to each component based on the material library data in the Simufact.welding software, including mechanical, thermal and electrical properties. The weld material properties are assigned the properties of the parent material of the component on the side with lower tensile strength;
[0030] Step 4: Define temperature objects: Set the initial temperature of each component to 20°C and the convection conductivity to 20W / m 2 .K; contact conductivity is set to 1000W / m 2 .K, the radiation heat exchange coefficient is set to 0.6;
[0031] Step 5. Define the fixture: Create the clamping fixture geometry based on the Simufact.welding software, and configure the corresponding properties, including shape, size, position, applied force value and direction, to simulate the actual welding clamping state to achieve the tightening and fixation of the component;
[0032] Step 6. Create welding trajectory: The design of welding trajectory and welding direction should be consistent with the actual welding of the product, and the relevant settings should be completed in Simufact.welding software;
[0033] Step 7, heat source selection and welding parameter input: arc welding heat source selects double ellipsoid heat source model, and welding parameters are input according to actual welding parameters, including corresponding welding speed, welding current, welding voltage and thermal efficiency value; laser wire welding selects conical heat source, and welding parameters are input according to actual welding parameters, including corresponding laser power, welding speed and thermal efficiency value;
[0034] Step 8, configure welding gun and weld: assign welding trajectory, welding parameters, welding gun rotation angle, and offset information to the welding gun according to welding process requirements, and configure the weld size according to weld cross-sectional size requirements;
[0035] Step 9, simulation configuration: select thermodynamic calculation for process definition, configure the number of domains and cores in the parallel option, enter the welding end time value in the time control option, select fixed automatic for welding time step, and select level 1 for global refinement level;
[0036] Step 10: Run the model: save the simulation analysis project and submit it for operation;
[0037] Step 11, result review: export the target product weld residual stress cloud map, extract and obtain the maximum value σ1 of the target product weld transverse residual stress in the cloud map.
[0038] In the step three, the maximum value σ2 of the transverse residual stress of the weld at the test weld 13 in the cold crack test model 1 is calculated based on the finite element analysis method. The specific method is the same as step one, except that the cold crack test model 1 is used instead of the actual product to calculate the transverse residual stress value of the weld, the welding trajectory and welding direction are set according to the actual size of the test weld 13, and the weld cross-sectional size does not need to be set. It is automatically formed in the cold crack test model 1 based on the actual welding parameters input in the Simufact.welding software.
[0039] The thickness dimension δ of the circular specimen 11 and the ring specimen 12 is the same, 6mm≤δ≤20mm; the welding groove between the circular specimen 11 and the ring specimen 12 is Y-shaped, the welding groove depth h=0.5δ, the welding groove angle α is 25°≤α≤75°, the welding groove surface angle β=0.5α, and the welding groove blunt edge gap b is 1.9mm≤b≤2.1mm.
[0040] The number n of the circular through holes 15 satisfies 3≤n≤6 and is evenly distributed on the circular ring sample 12 along the circumference. The minimum distance d between the inner circular surface of the circular through hole 15 and the outer circular surface of the circular ring sample 12 is 5mm≤d≤10mm. The manufacturing material and heat treatment state of the circular sample 11 and the circular ring sample 12 correspond to the manufacturing material and heat treatment state of the parent material on both sides of the target weld of the product.
[0041] The thickness of the square fixing plate 22 is H, δ+5mm≤H≤δ+15mm, the number and position of the annular specimen fixing threaded through holes 27 are the same as the number of the circular through holes 15 and the positions correspond, the positions of the circular specimen fixing threaded through holes 26 correspond to the positions of the central circular through holes 14, and the outer diameter of the cylindrical base 21 and the circular groove 25 are in a transitional fit.
[0042] The cooperation form between the central circular through hole 14 and the circular sample fixing bolt 23 is a clearance fit, and the cooperation clearance K satisfies 0.05mm≤K≤0.10mm. The cooperation form between the circular through hole 15 and the annular sample fixing bolt 24 is a clearance fit, and the cooperation clearance M satisfies 0.05mm≤M≤0.15mm.
[0043] During the static state of the test weld in step 7, the cold crack test sample is always fastened on the cold crack test welding fixture.
[0044] The interception direction of the test weld cross section should pass through the center of the test weld. The number of weld cross sections inspected in the entire test weld is m, 4≤m≤6, and they are evenly distributed on the circumference of the entire test weld.
[0045] In the step 1, the welding groove is opened on the outer cylindrical surface of the circular sample 11 and the inner cylindrical surface of the ring sample 12; a central circular through hole 14 is provided at the center of the circular sample 11, and a plurality of circular through holes 15 are provided on the outer edge of the ring sample 12.
[0046] In the step five, a circular groove 25 for mounting the cylindrical base 21 is processed at the center of the bottom of the square fixing plate 22, and the cylindrical base 21 is connected to the circular groove 25 by an annular fillet weld 29. A circular specimen fixing threaded through hole 26 is also provided at the center of the square fixing plate 22. The circular specimen fixing bolt 23 passes through the central circular through hole 14 and the circular specimen fixing threaded through hole 26 in sequence to fix the circular specimen 11 on the square fixing plate 22.
[0047] In the step five, the upper surface of the square fixing plate 22 is provided with annular sample fixing threaded through holes 27 corresponding one to one with the circular through holes 15 on the outer edge of the annular sample 12, and the annular sample fixing bolts 24 pass through the circular through holes 15 and the annular sample fixing threaded through holes 27 in sequence to fix the annular sample 12 on the square fixing plate 22.
[0048] A stepped blind hole 28 for accommodating the round sample fixing bolt 23 is formed on the upper portion of the cylindrical base 21 .
[0049] In step seven, surface cracks of the test weld are considered to have occurred if they can be seen visually or through a 5-20 times magnifying glass. Cross-sectional cracks of the test weld are evaluated by transversely cutting the weld to make metallographic samples. Cross-sectional cracks are also considered to have occurred if they can be seen visually or through a 5-20 times magnifying glass.
[0050] Beneficial effects of the present invention:
[0051] 1. No need for special testing equipment or complicated sample processing and preparation, only welding simulation analysis software, simple annular specimens and simple combined test fixtures are needed to accurately evaluate the tendency of welding cold cracks. The test is simple and easy to operate. Since the annular specimen is effectively fixed during welding and its matching gap is well controlled, the overall restraint state of the test weld is basically the same during the test, so the consistency of the test results is good; by adjusting the size of the single-sided annular specimen, the strength of the self-restraint of the test weld of the test specimen can be changed, so the tendency of welding cold cracks under different restraint conditions can also be tested.
[0052] 2. The application of this method can provide guidance for the optimization, improvement and process design of high-strength steel welding methods, and can greatly improve the safety and connection quality of the overall welded structure. BRIEF DESCRIPTION OF THE DRAWINGS
[0053] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings used in the description of the embodiments of the present invention. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the contents of the embodiments of the present invention and these drawings without creative work.
[0054] Figure 1 It is a schematic diagram of the cold crack test model structure of the present invention.
[0055] Figure 2 It is a schematic diagram of the cold crack test welding fixture structure of the present invention.
[0056] Figure 3 This is a half-section view of the cold crack test sample and welding fixture of the present invention.
[0057] Among them: 11. circular specimen; 12. ring specimen; 13. test weld; 14. central circular through hole; 15. circular through hole; 21. cylindrical base; 22. square fixing plate; 23. circular specimen fixing bolt; 24. ring specimen fixing bolt; 25. circular groove; 26. circular specimen fixing threaded through hole; 27. ring specimen fixing threaded through hole; 28. stepped blind hole; 29. ring fillet weld. DETAILED DESCRIPTION
[0058] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for ease of description, only parts related to the present invention, rather than all structures, are shown in the accompanying drawings.
[0059] In the description of the present invention, unless otherwise clearly specified and limited, the terms "connected", "connected", and "fixed" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0060] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.
[0061] In the description of this embodiment, the terms "upper", "lower", "left", "right" and other directions or positional relationships are based on the directions or positional relationships shown in the drawings, and are only for the convenience of description and simplification of operation, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operate in a specific direction, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used to distinguish in the description and have no special meaning.
[0062] A welding cold crack test and evaluation method, the specific steps are as follows:
[0063] Step 1, calculating the maximum value σ1 of the transverse residual stress of the target weld of the product based on the finite element analysis method, wherein the target weld is a butt weld;
[0064] Step 2: Establish a cold crack test model:
[0065] The cold crack test model 1 is composed of a circular sample 11, a ring sample 12 and a test weld 13, wherein the circular sample 11 is welded inside the ring sample 12 and is concentric with the ring sample 12, and the upper surfaces of the circular sample 11 and the ring sample 12 are ensured to be in the same plane; the test weld 13 is formed by welding at the longitudinal half position of the Y-shaped groove between the circular sample 11 and the ring sample 12;
[0066] Step 3: Determine the maximum transverse residual stress value σ2 of the test weld and lock the size of the cold crack test model:
[0067] Based on the finite element analysis method, the maximum value σ2 of the weld transverse residual stress at the test weld 13 in the cold crack test model 1 is numerically simulated and calculated;
[0068] Specifically, the maximum transverse residual stress σ2 of the test weld 13 is determined and the size of the cold crack test model 1 is locked by the following two methods:
[0069] Method 1: fix the inner diameter of the ring specimen 12, i.e., the diameter of the through hole inside the ring specimen 12 for welding the circular specimen 11, and adjust the outer diameter of the ring specimen 12 to obtain the maximum transverse residual stress σ2 of the test weld 13 under different restraint strengths;
[0070] Method 2: fix the outer diameter of the circular ring specimen 12, and adjust the inner diameter of the circular ring specimen 12 to obtain the maximum transverse residual stress σ2 of the test weld under different restraint strengths;
[0071] When the value of σ2 is 1.2σ1≤σ2≤1.3σ1, the outer and inner diameter dimensions of the locking ring specimen 12;
[0072] Step 4, according to the size of the cold crack test model 1 locked in step 3, a circular sample 11 and a ring sample 12 are processed and manufactured;
[0073] Step 5: Make a cold crack test welding fixture:
[0074] The cold crack test welding fixture 2 comprises a cylindrical base 21 and a square fixing plate 22, wherein the cylindrical base 21 is welded at the bottom center of the square fixing plate 22;
[0075] Step 6: Prepare cold crack test samples:
[0076] According to the positional assembly relationship in the cold crack test model 1, the circular sample 11 and the circular sample 12 are fastened to the square fixing plate 22 of the cold crack test welding fixture 2 by means of the circular sample fixing bolts 23 and the circular sample fixing bolts 24, and the assembled sample and the fixture are clamped as a whole on the three-jaw chuck, and the test weld 13 is welded to form the test weld by means of the same welding process and working conditions as the target weld of the product, thereby completing the preparation of the cold crack test sample;
[0077] Step 7: Cold crack test sample test weld crack detection:
[0078] The test weld crack detection is carried out after the test weld is formed and left to stand for 24 hours. The crack generation conditions on the test weld surface and the test weld cross section are evaluated in turn, and the presence or absence of cracks is used as the evaluation basis;
[0079] Step 8: Comprehensive determination of cold cracking tendency:
[0080] When cold cracks are detected at any point on the test weld surface or in the test weld cross section, the entire welded structure has a greater tendency to cold crack, and the current welding process needs to be redesigned and optimized; if cold cracks are not detected on the test weld surface or in the test weld cross section, the entire welded structure has no obvious tendency to cold crack under the current welding process.
[0081] In the step 1, the maximum value σ1 of the transverse residual stress of the target weld of the product is calculated according to the following steps:
[0082] Step 1: Mesh division: Import the CATIA 3D model of the product into the Hypermesh software to complete the hexahedral mesh division of each component of the 3D model without changing the original assembly relationship;
[0083] Step 2: Import components: Open the Simufact.welding software, input the two environmental variables of ambient temperature and gravity acceleration, and input the ambient temperature as 20℃ and gravity acceleration as 9.8m / S. 2 , and then import the meshed file in step 1 into the Simufact.welding software;
[0084] Step 3, define materials: according to the material type requirements of each component, assign corresponding material properties to each component based on the material library data in the Simufact.welding software, including mechanical, thermal and electrical properties. The weld material properties are assigned the properties of the parent material of the component on the side with lower tensile strength;
[0085] Step 4: Define temperature objects: Set the initial temperature of each component to 20°C and the convection conductivity to 20W / m 2 .K; contact conductivity is set to 1000W / m 2 .K, the radiation heat exchange coefficient is set to 0.6;
[0086] Step 5. Define the fixture: Create the clamping fixture geometry based on the Simufact.welding software, and configure the corresponding properties, including shape, size, position, applied force value and direction, to simulate the actual welding clamping state to achieve the tightening and fixation of the component;
[0087] Step 6. Create welding trajectory: The design of welding trajectory and welding direction should be consistent with the actual welding of the product, and the relevant settings should be completed in Simufact.welding software;
[0088] Step 7, heat source selection and welding parameter input: arc welding heat source selects double ellipsoid heat source model, and welding parameters are input according to actual welding parameters, including corresponding welding speed, welding current, welding voltage and thermal efficiency value; laser wire welding selects conical heat source, and welding parameters are input according to actual welding parameters, including corresponding laser power, welding speed and thermal efficiency value;
[0089] Step 8, configure welding gun and weld: assign welding trajectory, welding parameters, welding gun rotation angle, and offset information to the welding gun according to welding process requirements, and configure the weld size according to weld cross-sectional size requirements;
[0090] Step 9, simulation configuration: select thermodynamic calculation for process definition, configure the number of domains and cores in the parallel option, enter the welding end time value in the time control option, select fixed automatic for welding time step, and select level 1 for global refinement level;
[0091] Step 10: Run the model: save the simulation analysis project and submit it for operation;
[0092] Step 11, result review: export the target product weld residual stress cloud map, extract and obtain the maximum value σ1 of the target product weld transverse residual stress in the cloud map.
[0093] The mesh division principle of the product three-dimensional model in step 1 is that the size of the mesh unit gradually increases from the center of the weld to the two sides of the welded component, and the mesh unit size within 20 mm from the center of the weld is set to 0.5 mm×0.5 mm×0.5 mm.
[0094] In the step three, the transverse residual stress value σ2 of the weld at the test weld 13 in the cold crack test model 1 is calculated based on the finite element analysis method. The specific method is the same as step one, except that the cold crack test model 1 is used instead of the actual product to calculate the transverse residual stress value of the weld, the welding trajectory and welding direction are set according to the actual size of the test weld 13, and the weld cross-sectional size does not need to be set. The actual welding parameters input in the Simufact.welding software are automatically formed in the cold crack test model 1, and the remaining parameter settings are all the same as in step one.
[0095] The structure, size, material type and state of the actual product finite element model are the same as those of the actual product, and the welding method, process parameters and constraint state boundary conditions used in simulation calculation and analysis are consistent with actual welding conditions.
[0096] The thickness dimension δ of the circular specimen 11 and the ring specimen 12 is the same, 6mm≤δ≤20mm; the welding groove between the circular specimen 11 and the ring specimen 12 is Y-shaped, the welding groove depth h=0.5δ, the welding groove angle α is 25°≤α≤75°, the welding groove surface angle β=0.5α, and the welding groove blunt edge gap b is 1.9mm≤b≤2.1mm.
[0097] The number n of the circular through holes 15 satisfies 3≤n≤6 and is evenly distributed on the circular ring sample 12 along the circumference. The minimum distance d between the inner circular surface of the circular through hole 15 and the outer circular surface of the circular ring sample 12 is 5mm≤d≤10mm. The manufacturing material and heat treatment state of the circular sample 11 and the circular ring sample 12 correspond to the manufacturing material and heat treatment state of the parent material on both sides of the target weld of the product.
[0098] The thickness of the square fixing plate 22 is H, δ+5mm≤H≤δ+15mm, the number and position of the annular specimen fixing threaded through holes 27 are the same as the number of the circular through holes 15 and the positions correspond, the positions of the circular specimen fixing threaded through holes 26 correspond to the positions of the central circular through holes 14, and the outer diameter of the cylindrical base 21 and the circular groove 25 are in a transitional fit.
[0099] The cooperation form between the central circular through hole 14 and the circular sample fixing bolt 23 is a clearance fit, and the cooperation clearance K satisfies 0.05mm≤K≤0.10mm. The cooperation form between the circular through hole 15 and the annular sample fixing bolt 24 is a clearance fit, and the cooperation clearance M satisfies 0.05mm≤M≤0.15mm.
[0100] During the static state of the test weld in step 7, the cold crack test sample is always fastened on the cold crack test welding fixture.
[0101] The interception direction of the test weld cross section should pass through the center of the test weld. The number of weld cross sections inspected in the entire test weld is m, 4≤m≤6, and they are evenly distributed on the circumference of the entire test weld.
[0102] In the step 1, the welding groove is opened on the outer cylindrical surface of the circular sample 11 and the inner cylindrical surface of the ring sample 12; a central circular through hole 14 for fixing is provided at the center of the circular sample 11, and a plurality of circular through holes 15 for fixing are provided on the outer edge of the ring sample 12.
[0103] In the step five, a circular groove 25 for mounting the cylindrical base 21 is processed at the center of the bottom of the square fixing plate 22, and the cylindrical base 21 is connected to the circular groove 25 by an annular fillet weld 29. A circular specimen fixing threaded through hole 26 is also provided at the center of the square fixing plate 22. The circular specimen fixing bolt 23 passes through the central circular through hole 14 and the circular specimen fixing threaded through hole 26 in sequence to fix the circular specimen 11 on the square fixing plate 22.
[0104] In the step five, the upper surface of the square fixing plate 22 is provided with annular sample fixing threaded through holes 27 corresponding one to one with the circular through holes 15 on the outer edge of the annular sample 12, and the annular sample fixing bolts 24 pass through the circular through holes 15 and the annular sample fixing threaded through holes 27 in sequence to fix the annular sample 12 on the square fixing plate 22.
[0105] A stepped blind hole 28 for accommodating the round sample fixing bolt 23 is formed on the upper portion of the cylindrical base 21 .
[0106] In step seven, surface cracks of the test weld are considered to have occurred if they can be seen visually or through a 5-20 times magnifying glass. Cross-sectional cracks of the test weld are evaluated by transversely cutting the weld to make metallographic samples. Cross-sectional cracks are also considered to have occurred if they can be seen visually or through a 5-20 times magnifying glass.
[0107] Example 1
[0108] The cold crack tendency of the butt weld of the differential assembly of a rear drive unit of a certain vehicle was evaluated. The differential assembly is connected by the differential housing and the differential gear by MIG welding. The differential housing is made of 40Cr medium carbon tempered steel, and the differential gear is made of 20CrMnTiH steel.
[0109] Step 1: Obtain the maximum value of the transverse residual stress σ1 of the differential assembly weld
[0110] The finite element model of the differential assembly was established, and the MIG welds of the differential housing and differential gear were numerically simulated and calculated, and the maximum value of the transverse residual stress of the target weld of the product, σ1 = 353Mpa, was obtained. The structure, size, material type and state of the finite element model of the differential assembly are the same as those of the actual product, and the boundary conditions such as the welding method, heat source model, process parameters and restraint state used in the simulation calculation and analysis are consistent with the actual welding conditions.
[0111] Step 2: Establish a cold crack test model
[0112] The cold crack test model 1 consists of a circular specimen 11, a ring specimen 12 and a test weld 13. The circular specimen 11 and the ring specimen 12 are arranged concentrically and their upper surfaces are ensured to be in the same plane. The test weld 13 is located at the center of the welding groove of the circular specimen 11 and the ring specimen 12. The welding groove is opened on the outer cylindrical surface of the circular specimen 11 and the inner cylindrical surface of the ring specimen 12. A central circular through hole 14 for fixing is processed at the center of the circular specimen 11, and 4 circular through holes 15 for fixing are processed on the circumference of the ring specimen 12. The thickness dimension of the circular specimen 11 and the ring specimen 12 is δ=12mm; the welding groove between the circular specimen 11 and the ring specimen 12 is Y-type, the groove depth h=6mm, the groove surface angle β=30°, the groove angle α=60°, and the value of the groove blunt edge gap b is b=2.0mm; the number of circular through holes 15 is n=4, and they are evenly distributed on the ring specimen 12 along the circumference, and the minimum distance d between the inner circular surface of the circular through hole 15 and the outer circular surface of the ring specimen 12 is d=8mm; the manufacturing material and heat treatment state of the circular specimen 11 are set to 40Cr medium carbon tempered steel, and the manufacturing material and heat treatment state of the ring specimen 12 are set to 20CrMnTiH steel.
[0113] Step 3: Determine the maximum transverse residual stress σ2 of the test weld and lock the cold crack test model size
[0114] Through finite element analysis, numerical simulation and calculation are performed on the test weld 13 in the cold crack test model. The boundary conditions such as welding method, heat source model, process parameters, etc. are consistent with the actual welding conditions. This step uses the same finite element analysis software as step 1 for numerical simulation and calculation.
[0115] The inner diameter of the fixed ring sample 12 is 70 mm. By adjusting the outer diameter of the ring sample 12 to 168 mm, the cold crack test model size is locked when the maximum transverse residual stress of the test weld σ2=462 MPa is obtained.
[0116] Step 4: Processing and manufacturing sample parts based on the locked cold crack test model
[0117] Based on the locked cold crack test model, a circular specimen 11 and a ring specimen 12 are manufactured.
[0118] Step 5: Make a cold crack test welding fixture
[0119] The cold crack test welding fixture 2 consists of a cylindrical base 21, a square fixing plate 22, a circular sample fixing bolt 23 and an annular sample fixing bolt 24. A circular groove 25 for mounting the cylindrical base 21 and a circular sample fixing threaded through hole 26 are processed at the center of the square fixing plate 22, and an annular sample fixing threaded through hole 27 is also processed on its upper surface. A stepped blind hole 28 for avoiding the circular sample fixing bolt 23 is processed on the upper part of the cylindrical base 21. The thickness of the square fixing plate 22 is H=22mm, and the position of the annular sample fixing threaded through hole 27 corresponds to the position of the circular through hole 15, and the number is 4. The matching clearance K between the central circular through hole 14 and the circular sample fixing bolt 23 is 0.08mm, and the clearance matching M between the circular through hole 15 and the annular sample fixing bolt 24 is 0.10mm. The matching form between the outer diameter of the cylindrical base 21 and the circular groove 25 is a transition fit, and the connection is achieved through an annular fillet weld 29.
[0120] Step 6: Prepare cold crack test samples
[0121] According to the positional assembly relationship in the cold crack test model, the circular specimen 11 and the annular specimen 12 are fastened to the cold crack test welding fixture 2 by the circular specimen fixing bolts 23 and the annular specimen fixing bolts 24 respectively, and the assembled specimen and the fixture are clamped on the three-jaw chuck as a whole. Through the same welding process and working conditions as the target weld of the product, welding is performed at the position of the test weld 13 to form a test weld, and the production of the cold crack test sample is completed.
[0122] Step 7: Test weld crack detection of cold crack test specimens
[0123] The test weld crack detection should be carried out after the test weld 13 is formed and fastened on the fixture and left to stand for 24 hours. The crack generation situation on the weld surface and weld cross section should be evaluated in turn, and the presence or absence of cracks shall be used as the basis for evaluation.
[0124] The weld surface cracks were evaluated visually or with a 10x magnifying glass.
[0125] The weld cross section cracks are evaluated by cutting the weld cross section into metallographic samples. The cutting direction of the weld cross section should pass through the center of the test weld. The number of weld cross sections to be inspected in the entire test weld 13 is m = 5, and they are evenly distributed on the circumference of the entire test weld. The cross section cracks are also considered to have occurred if they can be seen visually or with a 10x magnifying glass.
[0126] Step 8: Comprehensive determination of cold cracking tendency
[0127] Through testing, it was found that no cold cracks were detected on the weld surface or in the weld cross section. It can be judged that when the current welding process is used to weld the differential assembly, the entire welded structure has no obvious cold crack tendency.
[0128] After multiple spot checks on the butt welds of the rear drive unit differential assembly of the vehicle, no cracks were detected on the weld surface or in the cross section.
[0129] Example 2
[0130] The cold crack tendency of the butt weld of the intermediate shaft assembly of an automobile auxiliary box was evaluated. The manufacturing material of the parts on both sides of the laser wire-filled weld of the intermediate shaft assembly of the auxiliary box was 16MnCr5H steel.
[0131] Step 1: Obtain the maximum value of the transverse residual stress σ1 of the auxiliary box intermediate shaft assembly weld
[0132] The finite element model of the auxiliary box intermediate shaft assembly was established, and the laser wire-filled welds on both sides of the auxiliary box intermediate shaft assembly were numerically simulated and calculated, and the maximum value of the transverse residual stress of the product target weld was obtained, σ1 = 589Mpa. The structure, size, material type and state of the finite element model of the auxiliary box intermediate shaft assembly are the same as those of the actual product, and the boundary conditions such as the welding method, heat source model, process parameters and constraint state used in the simulation calculation and analysis are consistent with the actual welding conditions.
[0133] Step 2: Establish a cold crack test model
[0134] The cold crack test model 1 consists of a circular specimen 11, a ring specimen 12 and a test weld 13. The circular specimen 11 and the ring specimen 12 are arranged concentrically and their upper surfaces are ensured to be in the same plane. The test weld 13 is located at the center of the welding groove of the circular specimen 11 and the ring specimen 12. The welding groove is opened on the outer cylindrical surface of the circular specimen 11 and the inner cylindrical surface of the ring specimen 12. A central circular through hole 14 for fixing is processed at the center of the circular specimen 11, and 5 circular through holes 15 for fixing are processed on the circumference of the ring specimen 12. The thickness dimension of the circular specimen 11 and the ring specimen 12 is δ=18mm; the welding groove between the circular specimen 11 and the ring specimen 12 is Y-type, the groove depth h=9mm, the groove surface angle β=15°, the groove angle α=30°, and the value of the groove blunt edge gap b is b=1.9mm; the number of circular through holes 15 is n=4, and they are evenly distributed on the ring specimen 12 along the circumference, and the minimum distance d between the inner circular surface of the circular through hole 15 and the outer circular surface of the ring specimen 12 is d=10mm; the manufacturing material and heat treatment state of the circular specimen 11 and the ring specimen 12 are set to 16MnCr5H steel.
[0135] Step 3: Determine the maximum transverse residual stress σ2 of the test weld and lock the cold crack test model size
[0136] Through finite element analysis, numerical simulation and calculation are performed on the test weld 13 in the cold crack test model. The boundary conditions such as welding method, heat source model, filling material, process parameters, etc. are consistent with the actual welding conditions. This step uses the same finite element analysis software as step 1 for numerical simulation and calculation.
[0137] The inner diameter of the fixed ring specimen 12 is 70 mm. By adjusting the outer diameter of the ring specimen 12 to 218 mm, the cold crack test model size is locked when the transverse residual stress value of the test weld σ2=744 MPa is obtained.
[0138] Step 4: Processing and manufacturing sample parts based on the locked cold crack test model
[0139] Based on the locked cold crack test model, a circular specimen 11 and a ring specimen 12 are manufactured.
[0140] Step 5: Make a cold crack test welding fixture
[0141] The cold crack test welding fixture 2 consists of a cylindrical base 21, a square fixing plate 22, a circular sample fixing bolt 23 and an annular sample fixing bolt 24. A circular groove 25 for mounting the cylindrical base 21 and a circular sample fixing threaded through hole 26 are processed at the center of the square fixing plate 22, and an annular sample fixing threaded through hole 27 is also processed on its upper surface. A stepped blind hole 28 for avoiding the circular sample fixing bolt 23 is processed on the upper part of the cylindrical base 21. The thickness of the square fixing plate 22 is H=26mm, and the position of the annular sample fixing threaded through hole 27 corresponds to the position of the circular through hole 15, and the number is 6. The matching clearance K between the central circular through hole 14 and the circular sample fixing bolt 23 is 0.06mm, and the clearance matching M between the circular through hole 15 and the annular sample fixing bolt 24 is 0.12mm. The matching form between the outer diameter of the cylindrical base 21 and the circular groove 25 is a transition fit, and the connection is achieved through an annular fillet weld 29.
[0142] Step 6: Prepare cold crack test samples
[0143] According to the positional assembly relationship in the cold crack test model, the circular specimen 11 and the annular specimen 12 are fastened to the cold crack test welding fixture 2 by the circular specimen fixing bolts 23 and the annular specimen fixing bolts 24 respectively, and the assembled specimen and the fixture are clamped on the three-jaw chuck as a whole. Through the same welding process and working conditions as the target weld of the product, welding is performed at the position of the test weld 13 to form a test weld, and the production of the cold crack test sample is completed.
[0144] Step 7: Test weld crack detection of cold crack test specimens
[0145] The test weld crack detection should be carried out after the test weld 13 is formed and fastened on the fixture and left to stand for 24 hours. The crack generation situation on the weld surface and weld cross section should be evaluated in turn, and the presence or absence of cracks shall be used as the basis for evaluation.
[0146] The weld surface cracks were evaluated visually or with a 15x magnifying glass.
[0147] The weld cross-section cracks are evaluated by cutting the weld cross-section into metallographic samples. The cutting direction of the weld cross-section should pass through the center of the test weld. The number of weld cross-sections tested in the entire test weld 13 is m = 6, and they are evenly distributed on the circumference of the entire test weld. Cross-section cracks are also considered to have occurred if they can be seen visually or with a 10x magnifying glass. Step 8: Comprehensive determination of the tendency of cold cracking
[0148] Through testing, it was found that no cracks were found on the weld surface, and cold cracks were detected in the cross sections of the two welds. It can be judged that when the current welding process is used to weld the automobile auxiliary box intermediate shaft assembly, the entire welding structure has a tendency to cold crack. The current welding process should be improved or replaced, or the current welding structure should be optimized.
[0149] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. However, the protection scope of the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention. These simple variations all belong to the protection scope of the present invention.
[0150] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0151] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A welding cold crack test and evaluation method, characterized in that The specific steps are as follows: Step 1, calculating the maximum value σ1 of the transverse residual stress of the target weld of the product based on the finite element analysis method, wherein the target weld is a butt weld; Step 2: Establish a cold crack test model: The cold crack test model (1) is composed of a circular sample (11), a circular ring sample (12), and a test weld (13), wherein the circular sample (11) is welded inside the circular ring sample (12) and is concentric with the circular ring sample (12), and the upper surfaces of the circular sample (11) and the circular ring sample (12) are ensured to be in the same plane; the test weld (13) is formed by welding at the longitudinal half position of the Y-shaped groove welded between the circular sample (11) and the circular ring sample (12); Step 3: Determine the maximum transverse residual stress σ2 of the test weld and lock the size of the cold crack test model: The maximum value σ2 of the weld transverse residual stress at the test weld (13) in the cold crack test model (1) is calculated based on the finite element analysis method; Specifically, the maximum transverse residual stress σ2 of the test weld (13) is determined and the size of the cold crack test model (1) is locked by the following two methods: Method 1: fixing the inner diameter of the circular ring specimen (12), and adjusting the outer diameter of the circular ring specimen (12) to obtain the maximum transverse residual stress σ2 of the test weld (13) under different restraint strengths; Method 2: fixing the outer diameter of the circular ring specimen (12), and adjusting the inner diameter of the circular ring specimen (12) to obtain the maximum transverse residual stress σ2 of the test weld under different restraint strengths; When the value of σ2 is 1.2σ1≤σ2≤1.3σ1, the outer and inner diameter dimensions of the locking ring specimen (12); Step 4, according to the size of the cold crack test model (1) locked in step 3, a circular specimen (11) and a ring specimen (12) are manufactured; Step 5: Make a cold crack test welding fixture: The cold crack test welding fixture (2) comprises a cylindrical base (21) and a square fixing plate (22), wherein the cylindrical base (21) is welded at the bottom center of the square fixing plate (22); Step 6: Prepare cold crack test samples: The circular specimen (11) and the annular specimen (12) are fastened to the square fixing plate (22) of the cold crack test welding fixture (2), and the assembled specimen and the fixture are clamped as a whole on a three-jaw chuck, and the test weld (13) is welded at the position of the test weld (13) by the same welding process and working conditions as the target weld of the product to complete the preparation of the cold crack test sample; Step 7: Cold crack test sample test weld crack detection: The test weld crack detection is carried out after the test weld is formed and left to stand for (24) hours. The crack generation conditions on the test weld surface and the test weld cross section are evaluated in turn, and the presence or absence of cracks is used as the evaluation basis; Step 8: Comprehensive determination of cold cracking tendency: When cold cracks are detected at any point on the test weld surface or in the test weld cross section, the entire welded structure has a greater tendency to cold crack, and the current welding process needs to be redesigned and optimized; if cold cracks are not detected on the test weld surface or in the test weld cross section, the entire welded structure has no obvious tendency to cold crack under the current welding process.
2. A welding cold crack test and evaluation method according to claim 1, characterized in that In the step 1, the maximum value σ1 of the transverse residual stress of the target weld of the product is calculated according to the following steps: Step 1: Mesh division: Import the CATIA 3D model of the product into the Hypermesh software to complete the hexahedral mesh division of each component of the 3D model without changing the original assembly relationship; Step 2: Import components: Open the Simufact.welding software, input the two environmental variables of ambient temperature and gravity acceleration, and input the ambient temperature as 20℃ and gravity acceleration as 9.8m / S. 2 , and then import the meshed file in step 1 into the Simufact.welding software; Step 3, define materials: according to the material type requirements of each component, assign corresponding material properties to each component based on the material library data in the Simufact.welding software, including mechanical, thermal and electrical properties. The weld material properties are assigned the properties of the parent material of the component on the side with lower tensile strength; Step 4: Define temperature objects: Set the initial temperature of each component to 20°C and the convection conductivity to 20W / m 2 .K; contact conductivity is set to 1000W / m 2 .K, the radiation heat exchange coefficient is set to 0.6; Step 5. Define the fixture: Create the clamping fixture geometry based on the Simufact.welding software, and configure the corresponding properties, including shape, size, position, applied force value and direction, to simulate the actual welding clamping state to achieve the tightening and fixation of the component; Step 6. Create welding trajectory: The design of welding trajectory and welding direction should be consistent with the actual welding of the product, and the relevant settings should be completed in Simufact.welding software; Step 7, heat source selection and welding parameter input: arc welding heat source selects double ellipsoid heat source model, and welding parameters are input according to actual welding parameters, including corresponding welding speed, welding current, welding voltage and thermal efficiency value; laser wire welding selects conical heat source, and welding parameters are input according to actual welding parameters, including corresponding laser power, welding speed and thermal efficiency value; Step 8, configure welding gun and weld: assign welding trajectory, welding parameters, welding gun rotation angle, and offset information to the welding gun according to welding process requirements, and configure the weld size according to weld cross-sectional size requirements; Step 9, simulation configuration: select thermodynamic calculation for process definition, configure the number of domains and cores in the parallel option, enter the welding end time value in the time control option, select fixed automatic for welding time step, and select level 1 for global refinement level; Step 10: Run the model: save the simulation analysis project and submit it for operation; Step 11, result review: export the target product weld residual stress cloud map, extract and obtain the maximum value σ1 of the target product weld transverse residual stress in the cloud map.
3. A welding cold crack test and evaluation method according to claim 2, characterized in that In the step three, the maximum value σ2 of the transverse residual stress of the weld at the test weld (13) in the cold crack test model (1) is calculated based on the finite element analysis method. The specific method is the same as step one, except that the cold crack test model (1) is used instead of the actual product to calculate the transverse residual stress value of the weld, the welding trajectory and welding direction are set according to the actual size of the test weld (13), and the weld cross-sectional size does not need to be set. The actual welding parameters input in the Simufact.welding software are automatically generated in the cold crack test model (1).
4. A welding cold crack test and evaluation method according to claim 3, characterized in that The thickness dimension δ of the circular specimen (11) and the ring specimen (12) is the same, 6mm≤δ≤20mm; the welding groove between the circular specimen (11) and the ring specimen (12) is in a Y-type form, the welding groove depth h=0.5δ, the welding groove angle α is 25°≤α≤75°, the welding groove surface angle β=0.5α, and the welding groove blunt edge gap b is 1.9mm≤b≤2.1mm.
5. A welding cold crack test and evaluation method according to claim 4, characterized in that During the static state of the test weld in step 7, the cold crack test sample is always fastened on the cold crack test welding fixture.
6. A welding cold crack test and evaluation method according to claim 5, characterized in that The interception direction of the test weld cross section should pass through the center of the test weld. The number of weld cross sections inspected in the entire test weld is m, 4≤m≤6, and they are evenly distributed on the circumference of the entire test weld.
7. A welding cold crack test and evaluation method according to claim 6, characterized in that In the step 1, the welding groove is opened on the outer cylindrical surface of the circular sample (11) and the inner cylindrical surface of the ring sample (12); a central circular through hole (14) is provided at the center of the circular sample (11), and a plurality of circular through holes (15) are provided on the outer edge of the ring sample (12).
8. A welding cold crack test and evaluation method according to claim 7, characterized in that In the step 5, a circular groove (25) for mounting the cylindrical base (21) is processed at the center of the bottom of the square fixing plate (22), the cylindrical base (21) and the circular groove (25) are connected by an annular fillet weld (29), and a circular sample fixing threaded through hole (26) is also provided at the center of the square fixing plate (22), and the circular sample fixing bolt (23) passes through the central circular through hole (14) and the circular sample fixing threaded through hole (26) in sequence to fix the circular sample (11) on the square fixing plate (22).
9. A welding cold crack test and evaluation method according to claim 8, characterized in that In the step 5, the upper surface of the square fixing plate (22) is provided with annular sample fixing threaded through holes (27) corresponding one to one with the circular through holes (15) on the outer edge of the annular sample (12), and the annular sample fixing bolts (24) are passed through the circular through holes (15) and the annular sample fixing threaded through holes (27) in sequence to fix the annular sample (12) on the square fixing plate (22).
10. A welding cold crack test and evaluation method according to claim 9, characterized in that The thickness of the square fixing plate (22) is H, δ+5mm≤H≤δ+15mm, the number and position of the annular specimen fixing threaded through holes (27) are the same as the number of the circular through holes (15) and the positions correspond to each other, the position of the circular specimen fixing threaded through holes (26) corresponds to the position of the central circular through hole (14), and the matching form between the outer diameter of the cylindrical base (21) and the circular groove (25) is a transition match.
11. A welding cold crack test and evaluation method according to claim 10, characterized in that The upper part of the cylindrical base (21) is processed with a stepped blind hole (28) for accommodating the circular sample fixing bolt (23).
12. A welding cold crack test and evaluation method according to claim 11, characterized in that In step seven, cracks on the test weld surface are considered to have occurred if they can be seen visually or through a 5-20 times magnifying glass. Cracks in the cross section of the test weld are evaluated by transversely cutting the weld to make a metallographic sample. Cracks in the cross section are considered to have occurred if they can also be seen visually or through a 5-20 times magnifying glass.