Preparation method of propane dehydrogenation catalyst

By loading manganese onto an alumina support and reducing it with C1-C3 alkanes and H2, the activity and selectivity of the propane dehydrogenation catalyst were improved, solving the problems of high cost and low activity of existing catalysts, and realizing a highly efficient propane dehydrogenation to propylene reaction.

CN113967472BActive Publication Date: 2024-11-12CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202010720215.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-24
Publication Date
2024-11-12
Estimated Expiration
2040-07-24

AI Technical Summary

Technical Problem

Existing propane dehydrogenation catalysts for propylene production suffer from high cost, low activity, poor stability, and pose environmental and health risks.

Method used

Using non-toxic, low-cost, and environmentally friendly manganese as the active component and alumina as the carrier, the oxidized catalyst is reduced by a mixture of C1-C3 alkanes and H2 at an appropriate temperature to increase the content of trivalent manganese in the catalyst, thereby enhancing the catalyst's propane dehydrogenation activity and propylene selectivity.

Benefits of technology

This improved the propane conversion rate and propylene selectivity of the catalyst, reduced the catalyst cost, and enabled a highly efficient propane dehydrogenation to propylene reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002599694420000081
    Figure BDA0002599694420000081
  • Figure BDA0002599694420000082
    Figure BDA0002599694420000082
  • Figure HDA0002599694430000011
    Figure HDA0002599694430000011
Patent Text Reader

Abstract

A method for preparing a propane dehydrogenation catalyst comprises reducing an oxidized propane dehydrogenation catalyst with a mixed gas of C1-C3 alkanes and H2 at 500-700°C, wherein the oxidized propane dehydrogenation catalyst comprises an alumina carrier and manganese in an amount of 0.5-10% by mass calculated on the basis of the carrier. The catalyst prepared by the method is used for the dehydrogenation of propane to produce propylene and has high activity and selectivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a catalyst for dehydrogenating low-carbon alkanes, in particular to a method for preparing a catalyst for dehydrogenating propane to produce propylene. Background Art

[0002] Propylene is the most consumed basic organic chemical raw material besides ethylene. Propylene products such as polypropylene, acrylonitrile, propylene oxide, and propylene ester are closely related to people's production and life. Propane dehydrogenation process is an important method for producing propylene.

[0003] The main industrialized technologies for catalytic dehydrogenation of propane to propylene are UOP's Oleflex technology and Lummus' Catofin technology. The Oleflex process uses a moving bed reactor with continuous catalyst regeneration and uses Pt-Sn / Al 2 O 3 As the catalyst, K or Li is added for modification. The catalyst has high activity and good stability, but the catalyst cost is high. The Catofin process uses a fixed bed reactor with Cr 2 O 3 / Al 2 O 3 The catalyst deactivates quickly and needs to be regenerated every 15 minutes, and there are environmental and health risks. Therefore, it is of great significance to develop a propane dehydrogenation catalyst with high activity, low cost and green environmental protection.

[0004] CN102451677B discloses a catalyst for isobutane dehydrogenation, wherein the catalyst is composed of MgO, P 2 O 5 、ZrO 2 、Al 2 O 3 or SiO 2 One or more oxides in are used as carriers, wherein the active component A contains one or more oxides selected from Ti, Nb, Ta, W, Re, In or Ga, the component C contains one or more oxides selected from Zn, Cr and Sn, and the component D is selected from alkali metal oxides or alkaline earth metal oxides. The isobutane dehydrogenation to olefins is carried out using a continuous reaction-regeneration device, and the isobutene yield can reach up to 41.60%, but the catalyst is easily deactivated, the reaction device is expensive, and the presence of sulfur causes great loss to the device.

[0005] CN103861619A discloses a sulfide catalyst for alkane dehydrogenation reaction, comprising an active component and a carrier, wherein the active component is one or more of Fe, Co, Ni, Cu, Zn, Mo, W and Mn elements, and the carrier is SiO 2 、Al2 O 3 、ZrO 2 ,La 2 O 3 、CeO 2 , CaO, P 2 O 5 , Nb 2 O 5 and MgO to form a mixed oxide or composite oxide, the active components on the surface of the alkane dehydrogenation sulfide catalyst exist in the form of sulfide. The catalyst preparation steps are complicated, and the oxidized catalyst obtained after calcination needs to be pre-sulfurized with hydrogen sulfide.

[0006] CN105582929A discloses a catalyst for the dehydrogenation reaction of low-carbon alkanes and its preparation method, which mainly solves the problem of low activity and poor stability of the dehydrogenation catalyst prepared by the prior art. It is prepared by impregnation precipitation method, including the following components: a) 0.1 to 5 parts of Pt or its oxide; b) 0.1 to 5 parts of Sn or its oxide; c) 0.1 to 5 parts of alkali metal or its oxide; d) 0.1 to 5 parts of Ga, In, Tl, Cr, Mn or its oxide; e) 0.1 to 10 parts of Ce-La-O solid solution; f) 80 to 99 parts of carrier Al 2 O 3 The catalyst has good performance, but due to the presence of a high content of Pt, the cost is high and issues such as regeneration of deactivated catalyst and Pt recovery are involved.

[0007] CN104936696A discloses a manganese-containing catalyst for dehydrogenation reaction, and its preparation method and use, comprising components (A)-(G), (A) is a catalyst matrix, (B) is platinum with a total content of 0.5-1.5wt%, (C) is at least one of germanium, tin, lead, gallium, indium and titanium, with a total content of 0.2-5wt%, (D) is phosphorus with a total content of 1-3wt%, (E) is at least one of magnesium, calcium, strontium, barium, radium and lanthanide elements, with a total content of 0.1-5wt%, (F) is chloride with a total content of 0.1-2wt%, and (G) is manganese. The catalyst is used for propane dehydrogenation to propylene reaction, the olefin selectivity decreases rapidly, and it also involves the problem of recovering high-content Pt. Summary of the invention

[0008] The purpose of the present invention is to provide a method for preparing a propane dehydrogenation catalyst. The catalyst prepared by the method is used for dehydrogenating propane to produce propylene and has high activity and selectivity.

[0009] The preparation method of the propane dehydrogenation catalyst provided by the present invention comprises the following steps: 1 ~C 3 Alkanes and H2 The mixed gas is subjected to reduction treatment at 500-700° C., and the oxidized propane dehydrogenation catalyst comprises an alumina carrier and manganese in an amount of 0.5-10 mass % calculated based on the carrier.

[0010] The method of the present invention is to use C 1 ~C 3 Alkanes and H 2 Reduction of the mixed gas can effectively improve the propane dehydrogenation activity and propylene selectivity of the catalyst. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 X-ray diffraction (XRD) patterns of catalyst A prepared in Example 1 of the present invention and catalyst J prepared in Comparative Example 1.

[0012] Figure 2 X-ray photoelectron spectroscopy (XPS) graphs of catalyst A prepared in Example 1 of the present invention and catalyst J prepared in Comparative Example 1. DETAILED DESCRIPTION

[0013] The method of the present invention uses non-toxic, low-cost and environmentally friendly manganese as an active component and uses aluminum oxide as a carrier to prepare an oxidized catalyst. 1 ~C 3 Alkanes and H 2 The mixed gas is reduced at an appropriate temperature to increase the content of highly active trivalent manganese in the reduced catalyst, thereby improving the propane dehydrogenation conversion rate and propylene selectivity of the catalyst.

[0014] The oxidized propane dehydrogenation catalyst of the present invention comprises an alumina carrier and an active component of manganese, wherein the manganese content calculated based on the carrier is preferably 1-5% by mass. The alumina is preferably γ-alumina or θ-alumina.

[0015] The specific surface area of ​​the alumina is preferably 110 to 230 m 2 / g, the pore volume is preferably 0.4 to 0.7 cm 3 When the alumina is γ-alumina, the specific surface area is preferably 190 to 220 m 2 / g, pore volume is preferably 0.4 to 0.6 cm 3 / g; when the alumina is θ-alumina, the specific surface area is preferably 115 to 120 m 2 / g, pore volume is preferably 0.5 to 0.7 cm 3 / g.

[0016] The γ-alumina carrier can be prepared by a sol-gel method, a coprecipitation method or a hydrothermal synthesis method, or can be directly prepared by using metal oxides. The θ-alumina can be prepared by using γ-alumina by calcining at a high temperature of 900 to 1100°C.

[0017] The shape of the alumina carrier of the present invention can be spherical, granular, sheet, strip or clover. For a moving bed reactor used in the reaction process and continuous catalyst regeneration, a spherical carrier is preferably used to facilitate the transportation of the catalyst during the reaction and regeneration process. The average diameter of the spherical alumina carrier is preferably 1.2 to 2.0 mm.

[0018] There are two methods for preparing the oxidized propane dehydrogenation catalyst of the present invention. The first method is to prepare it by an impregnation method; the second method is to prepare it by a drop ball method.

[0019] The first preparation method of the oxidized propane dehydrogenation catalyst of the present invention comprises impregnating an alumina carrier with a manganese compound solution, followed by drying and calcining.

[0020] The second preparation method of the oxidized propane dehydrogenation catalyst of the present invention comprises forming alumina sol droplets containing manganese compounds into spheres, followed by drying and calcining.

[0021] In the first preparation method, the alumina is preferably γ-alumina or θ-alumina. The alumina carrier used can be spherical, strip-shaped or clover-shaped. The temperature for impregnating the alumina with the manganese-containing compound solution is preferably 20 to 70°C, and the liquid / solid ratio of the impregnation is preferably 1.0 to 2.0 ml / g.

[0022] In the second preparation method, there are many methods for preparing alumina sol, such as reacting aluminum chloride and ammonia water at a temperature of 50 to 90°C, preferably 60 to 80°C, then filtering, washing with water, and adding an acid solution to the filter cake to prepare it. It can also be prepared by directly adding water to aluminum hydroxide powder to form a slurry, and then adding acid to the slurry to obtain a sol. The acid used for peptization is preferably nitric acid or hydrochloric acid, and an organic acid such as acetic acid or citric acid can also be added. The calcination temperature of the solid obtained after drop ball formation and drying is 450 to 1100°C to form γ-alumina or θ-alumina. When preparing γ-alumina, the calcination temperature is preferably 450 to 650°C, and when preparing θ-alumina, the calcination temperature is preferably 900 to 1100°C.

[0023] In the above method, the spherical carrier can be prepared by a drop ball molding method, such as oil-ammonia column or hot oil column drop ball molding. The strip or clover-shaped carrier can be prepared by a conventional extrusion molding method.

[0024] In the above catalyst preparation method, the manganese-containing compound is preferably manganese acetate, manganese chloride or manganese nitrate. The drying temperature is preferably 100-300°C, the drying time is preferably 1-20 hours, the calcination temperature is preferably 500-630°C, and the calcination time is preferably 1-20 hours.

[0025] The method of the present invention reduces the C in the mixed gas 1 ~C 3 Alkanes and H 2 The volume ratio of is preferably 0.1 to 0.9:1, more preferably 0.3 to 0.8:1, and the reduction treatment time is preferably 0.2 to 1 hour. The mass space velocity of the mixed gas for treating the oxidized propane dehydrogenation catalyst is preferably 4 to 6 hours. -1 .

[0026] The C 1 ~C 3 Alkanes and H 2 The temperature for reducing the oxidized propane dehydrogenation catalyst with the mixed gas is preferably 550-630°C.

[0027] The C 1 ~C 3 The alkane is methane, ethane or propane.

[0028] The catalyst prepared by the method of the present invention is suitable for the reaction of dehydrogenating propane to propylene. Propane and the catalyst of the present invention are contacted and reacted at 400-800°C, preferably 550-650°C, and 0.01-1.0 MPa, preferably 0.01-0.3 MPa (absolute pressure).

[0029] During the reaction, the appropriate mass space velocity of propane contacting the catalyst is 0.1 to 20 h -1 , more preferably 0.5 to 10 hours -1 .

[0030] The above dehydrogenation reaction can also use water vapor, argon, methane, ethane, carbon dioxide, nitrogen, etc. as diluents to mix with propane and pass into the reactor. The preferred diluent is hydrogen. When hydrogen is selected, the molar ratio of hydrogen to propane is preferably 0.03 to 0.5:1, more preferably 0.1 to 0.5:1.

[0031] The present invention is further described in detail below by examples, but the present invention is not limited thereto.

[0032] Example 1

[0033] Preparation of the propane dehydrogenation catalyst of the present invention.

[0034] (1) Take 0.28g of manganese acetate and dissolve it in 30ml of deionized water to make an impregnation solution. Take 20.0g of manganese acetate with a specific surface area of ​​210m 2 / g, pore volume is 0.5cm 3 / g γ-Al 2 O 3 The γ-Al 2 O 3 The pellet carrier was placed in the impregnation solution, stirred at 25°C for 0.5h, and allowed to stand for 4h for impregnation. The solid / liquid ratio of the impregnation was 1.5g / ml. It was then dried at 120°C for 12h and calcined at 550°C for 6h to obtain an oxidized catalyst.

[0035] (2) Take the above oxidized catalyst and introduce propane and H 2 The mixed gas with a volume ratio of 0.7:1 was subjected to reduction treatment at 580°C for 0.5h. The mass space velocity of the mixed gas passing through the oxidized catalyst was 4.2h -1 , and catalyst A was obtained. The Mn content in catalyst A calculated based on alumina was 0.5 mass %, and its composition was shown in Table 2, and its X-ray diffraction pattern was shown in Figure 1 , X-ray photoelectron spectroscopy Figure 2 , Figure 2 Medium Mn2p 3 / 2 The spectrum of the region can be fitted into three characteristic peaks at 640.6eV, 641.7eV, and 643.0eV, which are respectively attributed to Mn 2+ , Mn 3+ , Mn 4+ ions, and the three characteristic peak binding energies are added with 11.7 eV to obtain Mn2p 1 / 2 The characteristic peaks of three valence states of Mn are divided into Mn2p 3 / 2 Area and Mn2p 1 / 2 The characteristic peaks of the region were integrated, and the manganese contents in various valence states were obtained and are shown in Table 1.

[0036] Example 2

[0037] The catalyst was prepared according to the method of Example 1, except that 0.56 g of manganese acetate was used in the preparation of the impregnation solution in step (1), and the oxidized catalyst was reduced according to the method of step (2) to obtain Catalyst B. The Mn content in Catalyst B was 1.0 mass %, and its composition is shown in Table 2.

[0038] Example 3

[0039] The catalyst was prepared according to the method of Example 1, except that 1.13 g of manganese acetate was used in the preparation of the impregnation solution in step (1), and the oxidized catalyst was reduced according to the method of step (2) to obtain Catalyst C. The Mn content in Catalyst C was 2.0 mass %, and its composition is shown in Table 2.

[0040] Example 4

[0041] The catalyst was prepared according to the method of Example 1, except that 1.69 g of manganese acetate was used in the preparation of the impregnation solution in step (1), and the oxidized catalyst was reduced according to the method of step (2) to obtain Catalyst D. The Mn content in Catalyst D was 3.0 mass %, and its composition is shown in Table 2.

[0042] Example 5

[0043] The catalyst was prepared according to the method of Example 1, except that 2.26 g of manganese acetate was used in the preparation of the impregnation solution in step (1), and the oxidized catalyst was reduced according to the method of step (2) to obtain Catalyst E. The Mn content in Catalyst E was 4.0 mass %, and its composition is shown in Table 2.

[0044] Example 6

[0045] The catalyst was prepared according to the method of Example 1, except that 2.82 g of manganese acetate was used in the preparation of the impregnation solution in step (1), and the oxidized catalyst was reduced according to the method of step (2) to obtain Catalyst F. The Mn content in Catalyst F was 5.0 mass %, and its composition is shown in Table 2.

[0046] Example 7

[0047] (1) Take 26.32 g of aluminum hydroxide powder (produced by Sasol, Germany, brand SB, aluminum oxide content 76% by mass), add 20 ml of deionized water, stir for 1 hour to make it slurry, and then add 2 ml of nitric acid with a volume ratio of 1:1 to acidify it to obtain aluminum sol.

[0048] Add 10 ml of an aqueous solution containing 6 g of urea and 2.26 g of manganese acetate to the aluminum sol, so that the Mn content in the solution is 4.0% by mass of the dry basis aluminum oxide, stir for 1 hour, continue stirring and add 6 g of kerosene and 0.6 g of fatty alcohol polyoxyethylene ether dropwise thereto to obtain a sol for dropping balls. Drop the sol for dropping balls into an oil-ammonia column with an oil phase on the upper layer and an ammonia phase on the lower layer to form a drop ball. The oil phase is kerosene, and the concentration of ammonia in the ammonia phase is 8% by mass. The wet ball solidifies in the ammonia phase for 1 hour, is taken out and rinsed with deionized water, dried at 60°C for 6 hours, dried at 120°C for 10 hours, and calcined at 650°C in air for 4 hours to obtain Mn-containing γ-Al 2 O 3 The average diameter of the carrier is 1.6 mm.

[0049] (2) Take the above-mentioned γ-Al containing Mn 2 O 3 The carrier was subjected to reduction treatment according to the method of step (2) of Example 1 to obtain Catalyst G. The Mn content in Catalyst G was 4.0 mass %, and its composition is shown in Table 2.

[0050] Example 8

[0051] (1) Take 10.58g of aluminum flakes, add 240g of 18% by mass hydrochloric acid solution to dissolve the aluminum flakes, and obtain a solution with an aluminum chloride content of 21% by mass. Add 340g of 6% by mass ammonia water, mix at 60°C, and the pH value is 7.5-8.5. The generated aluminum hydroxide is filtered and washed, and 4ml of 1:1 volume ratio nitric acid is added to the filter cake to acidify and obtain a sol.

[0052] 16 ml of a solution containing 12 g of urea and a solution containing 2.26 g of manganese acetate were added to the sol under stirring to make the Mn content in the solution 4.0 mass % of dry aluminum oxide. The mixture was stirred for 1 hour, and 12 g of kerosene and 1.2 g of fatty alcohol polyoxyethylene ether were then added dropwise under stirring to obtain a sol for dropping balls.

[0053] The ball-dropping sol was formed into balls in an oil-ammonia column according to the method of step 7 (1) of Example 7, and then dried and calcined to obtain a γ-Al containing Mn. 2 O 3 The average diameter of the carrier is 1.6 mm.

[0054] (2) Take the above-mentioned γ-Al containing Mn 2 O 3 The carrier was subjected to reduction treatment according to the method of step (2) of Example 1 to obtain Catalyst H. The Mn content in Catalyst H was 4.0 mass %, and its composition is shown in Table 2.

[0055] Example 9

[0056] (1) Take the γ-Al described in Example 1 2 O 3 The pellet carrier was treated in air with a water vapor content of 5 vol% for 10 h, heated to 1000 °C and calcined for 4 h to obtain θ-Al 2 O 3 Support, the obtained θ-Al 2 O 3 The specific surface area of ​​the carrier is 118m 2 / g, pore volume 0.6cm 3 / g, the average diameter of the balls is 1.6mm.

[0057] Take 2.26g of manganese acetate and dissolve it in 30ml of deionized water to prepare an impregnation solution. Take 20.0g of the above θ-Al 2 O 3 The carrier was placed in the impregnation solution, stirred for 0.5 h, allowed to stand for 4 h for impregnation, then dried at 120 ° C for 12 h, and calcined at 550 ° C for 10 h to obtain the Mn-containing θ-Al 2 O 3 carrier.

[0058] (2) Take the above Mn-containing θ-Al 2 O 3The carrier was subjected to reduction treatment according to the method of step (2) of Example 1 to obtain Catalyst I. The Mn content in Catalyst I was 4.0 mass %, and its composition is shown in Table 2.

[0059] Example 10

[0060] The catalyst was prepared according to the method of Example 1, except that the manganese acetate used in the preparation of the impregnation solution in step (1) was 2.26 g, and the propane and H in the mixed gas used to reduce the oxidized catalyst in step (2) was 1.3 g. 2 The volume ratio of 0.3:1 was used to obtain Catalyst L. The Mn content in Catalyst L was 4.0 mass %, and its composition is shown in Table 2.

[0061] Comparative Example 1

[0062] The catalyst was prepared according to the method of Example 1, except that hydrogen was used for reduction treatment in step (2), to obtain catalyst J. The Mn content in catalyst J was 4 mass %, and its composition was shown in Table 2, and its X-ray diffraction pattern was shown in Figure 1 , X-ray photoelectron spectroscopy Figure 2 , Figure 2 Medium Mn2p 3 / 2 The spectrum of the region can be fitted into three characteristic peaks at 640.6eV, 641.7eV, and 643.0eV, which are respectively attributed to Mn 2+ , Mn 3+ , Mn 4+ ions, and the three characteristic peak binding energies are added with 11.7 eV to obtain Mn2p 1 / 2 The characteristic peaks of three valence states of Mn are divided into Mn2p 3 / 2 Area and Mn2p 1 / 2 The characteristic peaks of the region were integrated, and the manganese contents in various valence states were obtained and are shown in Table 1.

[0063] Comparative Example 2

[0064] Take 2.26g of manganese acetate and dissolve it in 30ml of deionized water to prepare an impregnation solution. Take 20.0g of the γ-Al 2 O 3 The γ-Al 2 O 3 The pellet carrier was placed in the impregnation liquid, stirred at 25°C for 0.5h, and allowed to stand for 4h for impregnation, the solid / liquid ratio of the impregnation was 1.5g / ml, and then dried at 120°C for 12h and calcined at 550°C for 6h to obtain the oxidized catalyst K. The Mn content in the catalyst K was 4.0% by mass, and its composition is shown in Table 2.

[0065] Example 11

[0066] In the microreactor, 2 ml of catalyst was loaded, and a mixture of hydrogen and propane was used as the raw material. The reaction temperature was 600 °C, 0.1 MPa (absolute pressure), and the propane feed mass space velocity was 9.0 h -1 The reaction was carried out for 10 hours at a molar ratio of hydrogen to propane of 0.1:1. Samples were collected every 0.5 hours for chromatographic analysis. The propane conversion and propylene selectivity were calculated. The reaction results of each catalyst are shown in Table 2.

[0067] Table 1

[0068]

[0069] Table 2

[0070]

[0071] Depend on Figure 1 It can be seen that the catalyst A prepared in Example 1 of the method of the present invention shows more characteristic peaks of manganese compared with the catalyst J in Comparative Example 1 which is reduced only with hydrogen.

[0072] Depend on Figure 2 As shown in Table 1, the catalyst A prepared in Example 1 of the present invention has more highly active trivalent manganese oxides than the catalyst J prepared in Comparative Example 1 which is reduced only with hydrogen.

[0073] As shown in Table 2, the catalyst prepared by the method of the present invention is better than that prepared by the comparative example 1 using only H 2 The reduced catalyst or the unreduced catalyst of comparative example 2 has higher propane conversion rate and propylene selectivity. This is because the catalyst reduced by the method of the present invention can generate more trivalent manganese oxides, which makes the catalyst more active in dehydrogenation, better in propylene selectivity, and significantly improves the propylene yield.

Claims

1. A method for preparing a propane dehydrogenation catalyst, comprising reducing an oxidized propane dehydrogenation catalyst with a mixed gas of C1-C3 alkanes and H2 at 500-700°C, wherein the oxidized propane dehydrogenation catalyst comprises an alumina carrier and manganese in an amount of 3-4 mass % calculated based on the carrier; The volume ratio of C1-C3 alkanes to H2 in the mixed gas is 0.1-0.9:1, and the reduction treatment time is 0.2-1 hour; The preparation method of the oxidized propane dehydrogenation catalyst comprises the steps of impregnating an alumina carrier with a manganese compound solution, followed by drying and calcining.

2. The catalyst according to claim 1, characterized in that The aluminum oxide is γ-aluminum oxide or θ-aluminum oxide.

3. The method according to claim 1, characterized in that The mass space velocity of the mixed gas for treating the oxidized propane dehydrogenation catalyst is 4 to 6 hours -1 .

4. The method according to claim 1, characterized in that The temperature for reducing the oxidized propane dehydrogenation catalyst with a mixed gas of C1-C3 alkanes and H2 is 550-630°C.

5. The method according to claim 1, characterized in that The calcination temperature is 450-1100°C.

6. The method according to claim 1, characterized in that The calcination time is 0.5 to 4 hours.

7. The method according to claim 1, characterized in that The manganese-containing compound is manganese acetate, manganese chloride or manganese nitrate.

8. The method according to claim 1, characterized in that The C1-C3 alkane is methane, ethane or propane.

Citation Information

Patent Citations

  • Catalyst for alkane dehydrogenation and device

    CN102451677B

  • Alkane dehydrogenation sulfide catalyst and alkane dehydrogenation method

    CN103861619A

  • Dehydrogenation manganese-containing catalyst, its use and method of preparation

    CN104936696A

  • Light alkane dehydrogenation catalyst, and preparation method and application thereof

    CN105582929A

  • Low carbon alkane dehydrogenation catalyst and its preparation method and application

    CN103769079A