Preparation method of copper-based catalyst and method for preparing bio-based cyclopentanone through furfural hydrogenation rearrangement

The copper-based catalyst prepared by co-precipitation method is used for furfural hydrogenation rearrangement, which solves the problems of pollution of existing cyclopentanone preparation methods and scarce resources of precious metal catalysts, and realizes efficient and low-cost cyclopentanone preparation, which is suitable for industrial applications. .

CN118949983APending Publication Date: 2024-11-15ZHEJIANG UNIV

Patent Information

Application Number
CN202411042906.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing cyclopentanone preparation method relies on petroleum-based raw materials, and the production process is seriously polluted, and precious metal catalyst resources are scarce and the cost is high, which limits industrial applications.

Method used

Co-precipitation method is used to prepare cheap copper-based catalysts, including active component Cu and additive components Cr, Al, Zn, Mg, Zr, for furfural hydrogenation rearrangement reaction, and cyclopentanone and Cyclopentanol.

Benefits of technology

It has achieved high selectivity and high yield preparation of cyclopentanone, high thermal stability of the catalyst, mild reaction conditions, suitable for industrial applications, and has significant economic and environmental benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949983A_ABST
    Figure CN118949983A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a copper-based catalyst and a method for preparing bio-based cyclopentanone through furfural hydrogenation rearrangement, the copper-based catalyst is prepared by adopting a coprecipitation method, active metal components and auxiliary agent components of the copper-based catalyst are from corresponding salt solutions, a precipitator is from sodium carbonate and the like, the mixed solution is heated for several hours under a water bath condition, and then the copper-based catalyst is obtained. After uniform precipitation, the catalyst is washed with deionized water, dried and reduced, and then the catalyst is applied to a reaction for preparing cyclopentanone through furfural hydrogenation rearrangement. The catalyst is simple and convenient in preparation method, low in price and good in cycling stability, a catalytic reaction system is green and environment-friendly, a reaction substrate is renewable, reaction conditions are mild, the comprehensive yield of cyclopentanone under experimental conditions is larger than 90%, and the catalyst is low in input production cost and has wide market application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of metal catalyst preparation and green functional materials, and in particular to a method for preparing a copper-based catalyst and a method for preparing cyclopentanone by hydrogenating and rearranging furfural. Background Art

[0002] With the gradual deepening of the concept of sustainable development, in order to avoid the many problems caused by excessive consumption of fossil fuels, to achieve the "dual carbon target" as soon as possible, the development and utilization of renewable resources to replace fossil energy is one of the feasible methods. Biomass resources are a kind of renewable non-fossil resources, which are widely regarded as excellent substitutes for fossil energy because of their renewability and abundant reserves. Among them, furfural is an important biomass platform compound, and a variety of high value-added downstream products can be developed through chemical reactions, such as: cyclopentanone, cyclopentanol, furfuryl alcohol, tetrahydrofurfural, 2-methylfuran, pentanediol, etc. In these downstream products, cyclopentanone and cyclopentanol are important fine chemical intermediates, which are important raw materials for spices and pharmaceutical chemicals, and can prepare a variety of anti-inflammatory and anticancer drugs, and can also be used in the production of electronics industry, pesticides and herbicides and the synthesis of rubber (Scognamiglio J,. Food Chem Toxicol, 2012, 50 Suppl 3: S608-12).

[0003] At present, the preparation method of cyclopentanone is mainly based on the method of adipic acid pyrolysis decarboxylation and cyclopentene oxidation of petroleum-based. Wherein, the adipic acid pyrolysis method raw material comes from petroleum-based, and requires a higher reaction temperature, and the production process will produce larger pollution (Renz M.European Journal of Organic Chemistry, 2005, 2005 (6): 979-88); the cyclopentene oxidation method is to use cyclopentene as raw material, and this method is more harsh to reaction conditions, so that it does not have a large range of applications in industry (Van de Vyver S, Catal Sci Technol, 2013, 3 (6): 1465-79). In contrast, furfural has a wide range of sources and has renewable characteristics, so furfural hydrogenation rearrangement to prepare cyclopentanone and cyclopentanol is an important upgrading strategy, which meets the development requirements of green chemical industry.

[0004] In the early stage of research, precious metal catalysts have attracted widespread attention in the catalytic conversion of biomass-based platform compounds to prepare cyclopentanone and cyclopentanol due to their advantages of high hydrogenation activity (Hronec M, Catalysis Communications, 2012, 24: 100-4; Hronec M, Applied Catalysis B: Environmental, 2016, 181: 210-9; Fang RQ, Green Chemistry, 2015, 17 (8): 4183-8), and have made certain progress. Wang Chuan et al. published a loaded catalyst prepared by co-loading precious metal Pt with transition metal (CN114605246A), which was applied to the furfural hydrogenation rearrangement system to obtain 100% furfural conversion rate and 89% cyclopentanone selectivity; Yang Hengdong et al. published a Ru-based precious metal catalyst (CN108067253A), under the reaction conditions, the cyclopentanone yield was as high as 98.9%. However, the scarcity of precious metal resources and high prices limit their widespread application in industry. At the same time, non-precious metal catalytic systems have the advantages of being cheap, easy to obtain, and simple to prepare. Therefore, the development of a cheap and stable non-precious metal catalyst is an important measure to bring the technology of furfural hydrogenation rearrangement to prepare cyclopentanone and cyclopentanol to the market. Summary of the invention

[0005] In view of the above background, the present invention proposes a non-precious metal copper-based catalyst prepared by a coprecipitation method, and applies it to the reaction of furfural hydrogenation rearrangement to prepare cyclopentanone and cyclopentanol. The system is green and environmentally friendly. The catalyst is mainly composed of non-precious metal oxides. Compared with precious metal catalysts, it has the advantages of being cheap and having a simple preparation method, and can meet the needs of industrialization. The purpose of the present invention is to improve the selectivity and yield of furfural hydrogenation rearrangement to prepare cyclopentanone, and to provide a method for preparing an efficient, low-cost and environmentally friendly copper-based catalyst and a method for preparing cyclopentanone and cyclopentanol by furfural hydrogenation rearrangement.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] One of the technical solutions of the present invention:

[0008] A copper-based catalyst, characterized in that it comprises an active component and an auxiliary component;

[0009] The active component is Cu, and the auxiliary component is at least one of Cr, Al, Zn, Mg, Zr, and Si.

[0010] When the auxiliary agent component is Si, the copper-based catalyst is a Cu / SiO2 catalyst;

[0011] When the auxiliary component is at least one of Cr, Al, Zn, Mg and Zr, the copper-based catalyst is a composite catalyst, and the active components and auxiliary components of the composite catalyst are respectively derived from corresponding metal salt solutions.

[0012] The second technical solution of the present invention:

[0013] A method for preparing a copper-based catalyst comprises the following steps:

[0014] The preparation steps are as follows:

[0015] Adding an aqueous solution of a precipitant dropwise to an aqueous solution of a metal salt to obtain a mixture after sufficient reaction, and then filtering, washing, drying, calcining and reducing to obtain the composite catalyst; or,

[0016] SiO2 is added to the aqueous solution of the metal salt, and then the aqueous solution of the precipitant is added dropwise, and a mixture is obtained after sufficient reaction, and then filtered, washed, dried, calcined and reduced to obtain the Cu / SiO2 catalyst.

[0017] Furthermore, the molar ratio of the auxiliary component to copper in the composite catalyst is: (0.1-1.5):1, preferably 0.5-1.0:1.

[0018] Furthermore, the copper source is Cu(NO3)2·3H20, and the other metal salts are nitrates, chlorides or sulfates of Cr, Al, Zn, Mg and Zr.

[0019] Furthermore, the precipitant is one or more of sodium carbonate, potassium carbonate, sodium hydroxide, potassium hydroxide, ammonia water, and urea.

[0020] Furthermore, the heating temperature of the water bath is 30-90°C.

[0021] Furthermore, the hydrogen reduction heat treatment temperature is 400°C to 800°C.

[0022] The third technical solution of the present invention: the composite catalyst catalyzes the hydrogenation and rearrangement of furfural to prepare cyclopentanone and cyclopentanol.

[0023] The fourth technical solution of the present invention: the preparation of cyclopentanone by rearrangement of furfural in aqueous phase by hydrogenation. The specific steps are: weigh a certain mass of furfural, a certain volume of deionized water and a composite catalyst and put them into a reactor. Replace the air in the reactor with hydrogen three to four times, then fill it with hydrogen to the initial target pressure, and start the stirring device. After heating to the target temperature and reacting for a period of time, cool it down, separate the product by suction filtration, and use gas chromatography (7890B, Agilent) for quantitative analysis.

[0024] Furthermore, the reaction hydrogen pressure is 1-6Mpa, preferably 2-4Mpa; the concentration of the furfural aqueous solution is 10-100g / L, preferably 0.3mol / L; the mass volume ratio of the hydrogenation catalyst to the furfural aqueous solution is (5-25)mg:1ml, preferably 10mg:1ml; the heating temperature is 140-220°C, preferably 160-180°C; the reaction time is 2-6h, preferably 4h.

[0025] Compared with the prior art, the advantages and beneficial effects of the present invention are:

[0026] The catalyst synthesis process prepared by the present invention is simple, efficient and environmentally friendly. It can be seen from the results of the examples that the hydrogenation catalyst provided by the present invention has higher cyclopentanone selectivity, high thermal stability and mild catalytic reaction conditions compared with precious metal catalysts, and can be carried out at low temperature and low pressure to prepare cyclopentanone; at the same time, the yield of cyclopentanone is high, and a new process for preparing cyclopentanone by catalyzing furfural under green and mild conditions using a cheap, stable and non-toxic catalyst is realized. The process has mild reaction conditions, a green and environmentally friendly route, a safe and easy-to-control process, is easy to implement in industrialization, and has significant economic and environmental benefits. DETAILED DESCRIPTION

[0027] Figure 1 is the XRD pattern of the catalyst obtained in Example 1;

[0028] Figure 2 This is the TEM image of the catalyst obtained in Example 5. DETAILED DESCRIPTION

[0030] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Embodiment 1:

[0032] A method for preparing a copper-based catalyst specifically comprises the following steps:

[0033] 1) Add copper nitrate and zinc nitrate (molar ratio 1:0.6) into 100 ml of water to prepare a metal salt solution with a total concentration of 0.05 M, and dissolve by ultrasonication for 20 min to obtain solution A.

[0034] 2) Take a certain amount of sodium hydroxide and dissolve it in water to prepare a 0.1M sodium hydroxide aqueous solution. Stir and dissolve for 15 minutes to obtain solution B.

[0035] 3) Solution B was added dropwise to solution A (the volume ratio of solution A to solution B was 1:1.3), and the mixed solution was stirred at room temperature for 12 h to obtain a turbid solution.

[0036] 4) The obtained turbid liquid was dried at 80° C. for 10 h, calcined at 400° C. for 3 h, and then reduced at 500° C. for 6 h in a hydrogen atmosphere to obtain a bimetallic CuZn catalyst.

[0037] The synthesized CuZn catalyst was characterized by XRD. Figure 1 The successful synthesis and good dispersion of copper oxide in the catalyst were demonstrated. 0 It is the main active center of the catalyst and plays a role in the adsorption and dissociation of hydrogen, which is one of the reasons why the catalyst has a significant effect.

[0038] Embodiment 2:

[0039] A method for preparing a copper-based catalyst specifically comprises the following steps:

[0040] 1) Add copper sulfate and chromium chloride (molar ratio 1:0.6) to 100 ml of water to prepare a metal salt solution with a total concentration of 0.05 M, and dissolve by ultrasonic for 20 minutes to obtain solution A.

[0041] 2) Take a certain amount of potassium hydroxide and dissolve it in water to prepare a 0.1M potassium hydroxide aqueous solution. Stir and dissolve for 15 minutes to obtain solution B.

[0042] 3) Solution B was added dropwise to solution A (the volume ratio of solution A to solution B was 1:1.3), and the mixed solution was stirred at room temperature for 12 h to obtain a turbid solution.

[0043] 4) The obtained turbid liquid was dried at 80° C. for 10 h, calcined at 600° C. for 3 h, and then reduced at 600° C. for 8 h in a hydrogen atmosphere to obtain a bimetallic CuCr catalyst.

[0044] Embodiment 3:

[0045] A method for preparing a copper-based catalyst specifically comprises the following steps:

[0046] 1) Add copper nitrate, zinc nitrate and aluminum nitrate (molar ratio 1:0.6:0.4) into 100 ml of water to prepare a metal salt solution with a total concentration of 0.05 M, and dissolve by ultrasonic for 20 minutes to obtain solution A.

[0047] 2) Take a certain amount of urea and dissolve it in water to prepare a 0.1M urea aqueous solution. Stir and dissolve for 15 minutes to obtain solution B.

[0048] 3) Solution B was added dropwise to solution A (the volume ratio of solution A to solution B was 1:1.5), and the mixed solution was stirred at room temperature for 6 h to obtain a turbid solution.

[0049] 4) The obtained turbid liquid was dried at 80° C. for 10 h, calcined at 400° C. for 3 h, and then reduced at 600° C. for 8 h in a hydrogen atmosphere to obtain a trimetallic CuZnAl catalyst.

[0050] Embodiment 4:

[0051] A method for preparing a copper-based catalyst specifically comprises the following steps:

[0052] 1) A certain amount of copper nitrate is added into water to prepare a metal salt solution with a concentration of 0.05 M, and ultrasonically dissolves the solution for 20 min to obtain a copper nitrate aqueous solution.

[0053] 2) A certain mass of SiO2 is added to a copper nitrate aqueous solution to obtain a mixture A.

[0054] 3) Take a certain amount of potassium carbonate and dissolve it in water to prepare a 0.1M potassium carbonate aqueous solution. Stir and dissolve for 15 minutes to obtain solution B.

[0055] 3) Solution B was added dropwise to mixture A (the volume ratio of solution A to solution B was 1:0.7), and the mixture was stirred at room temperature for 6 h to obtain a turbid solution.

[0056] 4) The obtained turbid liquid was dried at 80°C for 10 h, calcined at 400°C for 3 h, and then reduced at 600°C in a hydrogen atmosphere for 8 h to obtain a supported Cu / SiO2 catalyst.

[0057] Embodiment 5:

[0058] A method for preparing a copper-based catalyst specifically comprises the following steps:

[0059] 1) Add copper nitrate, zinc nitrate and zirconium oxynitrate (molar ratio 1:0.5:0.5) into 100 ml of water to prepare a metal salt solution with a total concentration of 0.05 M, and dissolve by ultrasonic for 20 minutes to obtain solution A.

[0060] 2) Take a certain amount of sodium carbonate and dissolve it in water to prepare a 0.1M sodium carbonate aqueous solution. Stir and dissolve for 15 minutes to obtain solution B.

[0061] 3) Solution B was added dropwise to solution A (the volume ratio of solution A to solution B was 1:0.7), and the mixed solution was stirred at room temperature for 6 h to obtain a turbid solution.

[0062] 4) The obtained turbid liquid was dried at 80° C. for 10 h, calcined at 400° C. for 3 h, and then reduced at 450° C. for 4 h in a hydrogen atmosphere to obtain a trimetallic CuZnZr catalyst.

[0063] The morphology and structure of the synthesized catalysts were characterized by TEM. Figure 2 As shown, the catalyst is mainly composed of uniformly dispersed spherical nanoparticles, and the dispersion is good, and the particle size is about 11.4nm.

[0064] Application Example 1:

[0065] A method for preparing cyclopentanone by catalyzing the hydrogenation and rearrangement of furfural using the catalyst of Example 1, comprising the following steps:

[0066] Take 0.5 g of the CuZn hydrogenation catalyst obtained in Example 1, 1 g of furfural, and 40 mL of water, mix them evenly, then transfer them to a reactor and react them at 160° C. and 4 MPa hydrogen pressure for 4 h. After the reaction is completed, cool and filter, and the obtained liquid product is analyzed by chromatography.

[0067] The furfural conversion rate and the yield of cyclopentanone were calculated, and the calculation results are shown in Table 1. It can be concluded from the table that the catalyst prepared in Example 1 can achieve a cyclopentanone yield of 85% under the conditions of 160° C., 4 MPa, and 4 h, showing its high selectivity.

[0068] Application Example 2:

[0069] A method for preparing cyclopentanone by catalyzing the hydrogenation and rearrangement of furfural using the catalyst of Example 2, comprising the following steps:

[0070] Take 0.2 g of the CuCr hydrogenation catalyst obtained in Example 2, 1 g of furfural, and 40 mL of water, mix them evenly, then transfer them to a reactor and react them at 140° C. and 3 MPa hydrogen pressure for 6 h. After the reaction is completed, cool and filter, and the obtained liquid product is analyzed by chromatography.

[0071] The furfural conversion rate and the yield of cyclopentanone were calculated, and the calculation results are shown in Table 1. It can be concluded from the table that the catalyst prepared in Example 2 can achieve a cyclopentanone yield of 93% under the conditions of 140° C., 3 MPa, and 6 h.

[0072] Application Example 3:

[0073] A method for preparing cyclopentanone by catalyzing the hydrogenation and rearrangement of furfural using the catalyst of Example 3, comprising the following steps:

[0074] Take 0.5 g of the CuZnAl hydrogenation catalyst obtained in Example 3, 2 g of furfural, and 40 mL of water, mix them evenly, then transfer them to a reactor and react them at 140° C. and 4 MPa hydrogen pressure for 4 h. After the reaction is completed, cool and filter, and the obtained liquid product is analyzed by chromatography.

[0075] The furfural conversion rate and the yield of cyclopentanone were calculated, and the calculation results are shown in Table 1. It can be concluded from the table that the catalyst prepared in Example 3 can achieve a cyclopentanone yield of 90% under the conditions of 140° C., 4 MPa, and 4 h.

[0076] Application example 4:

[0077] A method for preparing cyclopentanone by catalyzing the hydrogenation and rearrangement of furfural using the catalyst of Example 4, comprising the following steps:

[0078] Take 0.5 g of the supported Cu / SiO2 hydrogenation catalyst obtained in Example 4, 2 g of furfural, and 40 mL of water, mix them evenly, then transfer them to a reactor and react them at 120° C. and 3 MPa hydrogen pressure for 4 h. After the reaction is completed, cool and filter, and the obtained liquid product is analyzed by chromatography.

[0079] The furfural conversion rate and the yield of cyclopentanone were calculated, and the calculation results are shown in Table 1. It can be concluded from the table that the catalyst prepared in Example 4 can achieve a cyclopentanone yield of 90% under the conditions of 120° C., 3 MPa, and 4 h.

[0080] Application Example 5:

[0081] A method for preparing cyclopentanone by catalyzing the hydrogenation and rearrangement of furfural using the catalyst of Example 5, comprising the following steps:

[0082] Take 0.2 g of the CuZnZr hydrogenation catalyst obtained in Example 5, 0.5 g of furfural, 32 g of water and 8 g of isopropanol, mix them evenly, then transfer them to a reactor and react them at 200° C. and 3 MPa of hydrogen pressure for 2 h. After the reaction is completed, cool and filter, and the obtained liquid product is analyzed by chromatography.

[0083] The furfural conversion rate and the yield of cyclopentanone were calculated, and the calculation results are shown in Table 1. It can be concluded from the table that the catalyst prepared in Example 5 can achieve a cyclopentanone yield of 97% under the conditions of 200° C., 3 MPa, and 2 h.

[0084] Table 1 Experimental conditions and results of application examples 1-5

[0085]

[0086] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A copper-based catalyst, characterized in that It includes active ingredients and auxiliary ingredients; The active component is Cu, and the auxiliary component is at least one of Cr, Al, Zn, Mg, Zr, and Si.

2. The copper-based catalyst according to claim 1, characterized in that When the auxiliary agent component is Si, the copper-based catalyst is a Cu / SiO2 catalyst; When the auxiliary component is at least one of Cr, Al, Zn, Mg and Zr, the copper-based catalyst is a composite catalyst, and the active components and auxiliary components of the composite catalyst are respectively derived from corresponding metal salt solutions.

3. A method for preparing a copper-based catalyst as claimed in claim 1 or 2, characterized in that: The following steps are involved: Adding an aqueous solution of a precipitant dropwise to an aqueous solution of a metal salt to obtain a mixture after sufficient reaction, and then filtering, washing, drying, calcining and reducing to obtain the composite catalyst; or, SiO2 is added to the aqueous solution of the metal salt, and then the aqueous solution of the precipitant is added dropwise, and a mixture is obtained after sufficient reaction, and then filtered, washed, dried, calcined and reduced to obtain the Cu / SiO2 catalyst.

4. The preparation method according to claim 3, characterized in that: The metal salt of the active component of the catalyst is one or more of Cu(NO3)2·3H2O, CuCl2·2H2O, CuSO4·5H2O, preferably Cu(NO3)2·3H2O; The metal salt of the auxiliary component is one or more of Zn(NO3)2·6H2O, ZnSO4·H2O, Zn(CH3COO)2·2H2O; ZrO(NO3)2·xH2O, ZrOCl2·xH2O; Cr(NO3)2·9H20, CrCl2·6H20; Al(NO3)3·6H20, AlCl3·6H20; Mg(NO3)2·6H20, MgCl2·6H20, preferably Zn(NO3)2·6H2O and ZrO(NO3)2·xH2O.

5. The preparation method according to claim 3, characterized in that: The molar ratio of the auxiliary component to copper in the composite catalyst is: (0.1-1.5):1, preferably 0.5-1.0:1; The precipitant is one or more of sodium carbonate, potassium carbonate, sodium hydroxide, potassium hydroxide, ammonia water, and urea; In terms of molar amount, the precipitant: (active component + auxiliary component) is 1.1 to 3.0:1, preferably 1.4 to 2:

1.

6. The preparation method according to claim 5, characterized in that: The reaction temperature after adding the precipitant is 30-90°C, preferably 60°C; the reaction time is 3-9h, preferably 6h; The drying is performed at 85-95°C for 8-12 hours; the calcination is performed at 300-600°C for 2-6 hours; The reduction is carried out under the condition of 5-15% H2 / Ar at 300-600°C for 2-6 hours, preferably under the condition of 5-15% H2 / Ar at 450°C for 4 hours.

7. Use of the copper-based catalyst as claimed in any one of claims 1 to 6 in the hydrogenation reaction of furfural and furfuryl alcohol as substrates.

8. A method for preparing cyclopentanone by catalytic hydrogenation and rearrangement of furfural, characterized in that: The method comprises the following steps: adding furfural, a solvent and the copper-based catalyst according to any one of claims 1 to 6 into a high-pressure reaction device, and carrying out a catalytic selective hydrogenation reaction in hydrogen under stirring to obtain the product cyclopentanone.

9. The method according to claim 8, characterized in that The amount of the copper-based catalyst is 1 / 10 to 1, preferably 1 / 2, of the mass of furfural, the initial hydrogen pressure is 2-6MPa, the reaction temperature is 140-220°C, preferably 160-180°C, the reaction time is 1-4h, preferably 2-5h; the solvent is a mixed solvent of deionized water and low-carbon alcohol.

10. The method according to claim 9, characterized in that The low-carbon alcohol in the mixed solvent is one or more of methanol, ethanol, isopropanol, n-propanol, and tert-butanol, preferably isopropanol; The mass ratio of water to alcohol in the mixed solvent is 1-10:1.

Citation Information

Patent Citations

  • Method for preparing cyclopentanone and / or cyclopentanol by furfural or furfuryl alcohol

    CN102807483A

  • Method for preparing cyclopentanone by using furaldehyde as raw material

    CN103159606A

  • Catalyst for preparation of furfuryl alcohol by furfural liquid phase hydrogenation and preparation method

    CN105498788A

  • Method for continuously synthesizing cyclopentanone

    CN115894196A

  • IN1661DE2005A

Cited By

  • Nickel-based catalyst for catalyzing 5-hydroxymethylfurfural to prepare 5-hydroxymethyl-2-furfurylamine as well as preparation method and application of nickel-based catalyst

    CN119680548A

  • Preparation method and application of palladium / amphoteric chelate resin hydrogenation catalyst

    CN120054642A

  • Preparation method and application of palladium / amphoteric chelate resin hydrogenation catalyst

    CN120054642B

  • Electrocatalytic synthesis method of tetramethylpyrazine

    CN120924990A