A quantum dot light-emitting diode with an upright structure and its fabrication method

By arranging a free radical spacer layer in the quantum dot light-emitting diode that can oxidize primary or secondary alcohols into stable free radicals of carbonyl compounds, the problem of poor stability of the quantum dot light-emitting diode is solved, the lifespan is extended and the efficiency is improved, achieving Better photothermal stability and overall stability.

CN113972334BActive Publication Date: 2024-10-29TCL TECHNOLOGY GROUP CORPORATION
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202010712640.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-07-22
Publication Date
2024-10-29
Estimated Expiration
2040-07-22

AI Technical Summary

Technical Problem

The poor stability of existing quantum dot light-emitting diodes makes it impossible to balance efficiency and lifespan, making it difficult to achieve mass production.

Method used

Using a quantum dot light-emitting diode with an upright structure, an electron transport layer and a free radical spacer layer are provided between the quantum dot light-emitting layer and the cathode. The free radical spacer layer material is a stable state that can oxidize primary or secondary alcohols into carbonyl compounds. Free radicals play the role of photothermal stabilization and quenching of oxygen molecules, protecting the functional layer and improving overall stability.

Benefits of technology

It effectively extends the life of the quantum dot light-emitting diode, improves its overall stability and efficiency, avoids oxidation of the functional layer, and enhances the photothermal stability of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN113972334B_ABST
    Figure CN113972334B_ABST
Patent Text Reader

Abstract

The present invention discloses a quantum dot light-emitting diode with an upright structure and a preparation method thereof, comprising: an anode, a quantum dot light-emitting layer, an electron transport layer, a free radical spacer layer and a cathode, wherein the quantum dot light-emitting layer is located between the anode and the cathode, and the electron transport layer is located between the quantum dot light-emitting layer and the cathode; the free radical spacer layer is located between the electron transport layer and the cathode, and the free radical spacer layer material is a stable free radical capable of oxidizing a primary alcohol or a secondary alcohol into a carbonyl compound. The above-mentioned stable free radicals used in the present invention have a photothermal stabilizing effect; a free radical spacer layer is provided between the cathode and the electron transport layer of a QLED with an upright structure using the free radical spacer layer as a material, thereby increasing the photothermal stability of the QLED; and the oxidizing stable free radicals can capture and quench singlet oxygen, effectively preventing the functional layer of the QLED from being oxidized, thereby improving the overall stability and service life of the QLED.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of quantum dot light emitting diodes, and in particular to a quantum dot light emitting diode with an upright structure and a preparation method thereof. Background Art

[0002] Quantum dot light emitting diodes (QLED), as a new type of solid-state lighting source, have the advantages of low cost, light weight, fast response speed, high color saturation, etc. It has broad development prospects and has become one of the important research directions of the new generation of light-emitting diode lighting.

[0003] The existing QLED mainly includes a cathode, an anode, a hole / electron transport layer and a quantum dot light-emitting layer, but its stability is not ideal, resulting in the QLED not being able to have both efficiency and lifespan. This is the main reason why QLED is difficult to mass-produce.

[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, an object of the present invention is to provide a quantum dot light emitting diode with an upright structure and a preparation method thereof, aiming to solve the problem of poor stability of existing quantum dot light emitting diodes.

[0006] The technical solution of the present invention is as follows:

[0007] A quantum dot light-emitting diode with an upright structure, comprising: an anode, a quantum dot light-emitting layer, an electron transport layer, a free radical spacer layer and a cathode, wherein the quantum dot light-emitting layer is located between the anode and the cathode, the electron transport layer and the free radical spacer layer are located between the quantum dot light-emitting layer and the cathode; the free radical spacer layer is located between the electron transport layer and the cathode, and the free radical spacer layer material is a stable free radical capable of oxidizing a primary alcohol or a secondary alcohol into a carbonyl compound.

[0008] A method for preparing a quantum dot light-emitting diode with an upright structure, comprising the steps of:

[0009] providing an anode;

[0010] forming a quantum dot light-emitting layer on the anode;

[0011] An electron transport layer and a free radical spacer layer are sequentially formed on the quantum dot light-emitting layer, wherein the free radical spacer layer material is a stable free radical capable of oxidizing a primary alcohol or a secondary alcohol into a carbonyl compound;

[0012] A cathode is formed on the free radical spacer layer to obtain the quantum dot light emitting diode.

[0013] Beneficial effects: The present invention utilizes stable free radicals that can oxidize primary alcohols or secondary alcohols into carbonyl compounds to achieve photothermal stability; using the material to set a free radical spacer between the cathode and the electron transport layer of the QLED in an upright structure can effectively reduce the quenching of the electron transport layer and quantum dot light-emitting layer materials of the QLED device by high-intensity ultraviolet (such as contact during packaging) or high temperature (such as during device post-processing) during the preparation process, thereby enhancing the photothermal stability of the QLED device, thereby extending the life of the QLED device; in addition, utilizing the function of capturing and quenching singlet oxygen by the oxidizing stable free radical, the free radical spacer can quench the excited oxygen molecules through intermolecular energy transfer, converting them into fluorescence or phosphorescence, and causing radiation loss to return to the state of ground state oxygen, which can effectively prevent the functional layer of the QLED device from being oxidized, protect the functional layer of the QLED device, and thereby improve the overall stability of the QLED device. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 A schematic structural diagram of a quantum dot light emitting diode with an upright structure provided in an embodiment of the present invention.

[0015] Figure 2 A schematic flow chart of a method for preparing a quantum dot light-emitting diode with an upright structure provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0016] The present invention provides a quantum dot light emitting diode with an upright structure and a method for preparing the same. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0017] An embodiment of the present invention provides a quantum dot light-emitting diode with an upright structure, which includes: an anode, a quantum dot light-emitting layer, an electron transport layer, a free radical spacer layer and a cathode, wherein the quantum dot light-emitting layer is located between the anode and the cathode, and the electron transport layer is located between the quantum dot light-emitting layer and the cathode; the free radical spacer layer is located between the electron transport layer and the cathode, and the free radical spacer layer material is a stable free radical that can oxidize a primary alcohol or a secondary alcohol into a carbonyl compound.

[0018] In this embodiment, the use of stable free radicals that can oxidize primary alcohols or secondary alcohols into carbonyl compounds can play a role in photothermal stability; using the material to set a free radical spacer between the cathode and the electron transport layer of the QLED in an upright structure can effectively reduce the quenching of the electron transport layer and quantum dot light-emitting layer materials of the QLED device by high-intensity ultraviolet (such as contact during packaging) or high temperature (such as during device post-processing) during the preparation process, which plays a role in enhancing the photothermal stability of the QLED device, thereby extending the life of the QLED device; in addition, the oxidizing stable free radical has the function of capturing and quenching singlet oxygen. The free radical spacer can quench the excited oxygen molecules through intermolecular energy transfer, converting them into fluorescence or phosphorescence, and radiating them back to the state of ground state oxygen, which can effectively prevent the functional layer of the QLED device from being oxidized, protect the functional layer of the QLED device, and thus improve the overall stability of the QLED device.

[0019] In one embodiment, the stable free radical is 2,2,6,6-tetramethylpiperidinyl oxide. The stable free radical 2,2,6,6-tetramethylpiperidinyl oxide (TEMPO, structure is ) Due to the steric effect of four methyl groups, it has strong photothermal stability. At the same time, it has strong performance in capturing and quenching singlet oxygen. The positive QLED obtained by setting a free radical spacer between the cathode and the electron transport layer has better photothermal stability, which can further improve the overall stability and service life of the QLED. And the LUMO of TEMPO is around 3.57eV, so it is also a good transition layer material for the electron transport layer and the cathode.

[0020] In one embodiment, the free radical spacer layer is anchored on the electron transport layer through a carbonyl compound; the carbonyl compound may be an oxide of a primary alcohol or a secondary alcohol, and the carbonyl compound is distributed between the free radical spacer layer and the electron transport layer. In other words, the carbonyl compound may be an aldehyde compound or a ketone compound obtained by oxidation of a primary alcohol or a secondary alcohol by the stable free radical; preferably, the carbonyl compound is a C1-C6 aldehyde compound or a ketone compound, such as formaldehyde, acetaldehyde, propionaldehyde, butyraldehyde, valeraldehyde, hexanal, acetone, butanone, 2-pentanone, 3-pentanone, hexanone, etc.

[0021] Furthermore, the electron transport layer material often selects metal oxides or doped metal oxides (such as ZnO, TiO2, BaTiO3, aluminum-doped zinc oxide, lithium-doped zinc oxide, magnesium-doped zinc oxide, etc.), and the surface of the electron transport layer often contains hydroxyl groups. At this time, the carbonyl group in the carbonyl compound will have non-covalent interactions (non-covalent interactions, a force similar to hydrogen bonds) with the hydrogen on the hydroxyl group, so that part of the free radical spacer layer material penetrates into the electron transport layer where the film is not uniform (i.e., the crystal gap), and adheres thereto due to non-covalent interactions, playing the role of filling and paving the electron transport layer. In other words, anchoring refers to the non-covalent interaction between the carbonyl group of the carbonyl compound and the hydrogen on the surface hydroxyl group of the electron transport layer. The free radical spacer layer is anchored on the electron transport layer by the carbonyl compound, which can reduce the crystal gap of the electron transport layer, increase the compactness of the electron transport layer, and facilitate the transmission of carriers (electrons), thereby improving the efficiency of the QLED device.

[0022] In one embodiment, the thickness of the free radical spacer layer does not exceed 5 nm. For example, the thickness of the free radical spacer layer may be 1 nm, 2 nm, 3 nm, 4 nm, 5 nm, etc.

[0023] In one embodiment, the anode is a transparent anode. As an example, the anode material can be selected from but not limited to one or more of tin-doped indium oxide (ITO), aluminum-doped zinc oxide (AZO), antimony-doped tin oxide (ATO) and fluorine-doped tin oxide (FTO). Further, the anode material is tin-doped indium oxide (ITO).

[0024] In one embodiment, the thickness of the quantum dot light-emitting layer is 30 to 50 nm; the quantum dot light-emitting layer material is selected from one or more of II-VI group quantum dots and core-shell quantum dots, and the core material and shell material of the II-VI group quantum dots and core-shell quantum dots are independently selected from one of CdSe, CdS, ZnSe, CdS, PbS and PbSe.

[0025] In one embodiment, the thickness of the electron transport layer is 20 to 50 nm; the electron transport layer material may include one or more of ZnO, TiO2, BaTiO3, aluminum-doped zinc oxide (AZO), lithium-doped zinc oxide (LZO), and magnesium-doped zinc oxide (MZO). The surface of the electron transport layer formed by the above metal oxides or doped metal oxides often contains hydroxyl groups, which can react with the carbonyl group of the carbonyl compound to anchor the free radical spacer layer on the electron transport layer.

[0026] In one embodiment, a hole transport layer and / or a hole injection layer may be provided between the anode and the quantum dot light-emitting layer. When both a hole transport layer and a hole injection layer are provided between the anode and the quantum dot light-emitting layer, the hole injection layer is provided close to the anode, and the hole transport layer is provided close to the quantum dot light-emitting layer.

[0027] In this embodiment, the quantum dot light emitting diode with a positive structure will mainly be as follows Figure 1 Specifically, Figure 1 As shown, the upright structure quantum dot light-emitting diode includes an anode 10, a hole injection layer 11, a hole transport layer 12, a quantum dot light-emitting layer 13, an electron transport layer 14, a free radical spacer layer 15 and a cathode 16 arranged in sequence from bottom to top, and the material of the free radical spacer layer 15 is a stable free radical that can oxidize primary alcohols or secondary alcohols into carbonyl compounds.

[0028] In one embodiment, the thickness of the hole transport layer is 15 to 30 nm; the hole transport layer material can be selected from but not limited to poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(p-butylphenyl))diphenylamine)] (TFB, structure ), poly(9-vinylcarbazole) (PVK, structure ), poly[bis(4-phenyl)(4-butylphenyl)amine] (Poly-TPD, structure is ) and N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine (NPB, structure ) one or more; and / or,

[0029] The thickness of the hole injection layer is 20 to 35 nm; the hole injection layer material can be selected from but is not limited to one of poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonic acid) (PEDOT:PSS) and poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonic acid) doped with s-MoO3 (PEDOT:PSS:s-MoO3).

[0030] In one embodiment, the cathode material may be selected from but not limited to one or more of Al, Ag, Au and Cu. Further, the cathode material is Al or Ag. The thickness of the cathode is 15-150 nm; when the cathode material is Al, the thickness of the cathode is 60-90 nm; when the cathode material is Ag, the thickness of the cathode is 100-120 nm.

[0031] See also Figure 2The embodiment of the present invention further provides a method for preparing a quantum dot light-emitting diode with an upright structure, which comprises the steps of:

[0032] S10, providing an anode;

[0033] S20, forming a quantum dot light-emitting layer on the anode;

[0034] S30, forming an electron transport layer and a free radical spacer layer on the quantum dot light-emitting layer, wherein the free radical spacer layer is located on the electron transport layer, and the free radical spacer layer material is a stable free radical that can oxidize a primary alcohol or a secondary alcohol into a carbonyl compound;

[0035] S40, forming a cathode on the free radical spacer layer to obtain the quantum dot light emitting diode.

[0036] In this embodiment, a free radical spacer layer is formed between the cathode and the electron transport layer using a stable free radical that can oxidize a primary alcohol or a secondary alcohol into a carbonyl compound, which can play a role in photothermal stability, and can effectively reduce the quenching effect of the electron transport layer and the quantum dot light-emitting layer materials being subjected to high-intensity ultraviolet (contact during packaging) or high temperature (possibly performed during device post-processing) during the preparation process, thereby strengthening the photothermal stability of the device and directly improving the life of the device. In addition, the stable free radical with the above-mentioned oxidizing property has the function of capturing and quenching singlet oxygen, that is, through intermolecular energy transfer, the excited oxygen molecules are quenched, converted into fluorescence or phosphorescence, and radiation is lost to return to the state of ground state oxygen, which can effectively protect the functional layer of the device from oxidation and improve the overall stability of the device.

[0037] In one embodiment, the stable free radical is 2,2,6,6-tetramethylpiperidinyl oxide. TEMPO has strong photothermal stability and the ability to capture and quench singlet oxygen. The positive QLED obtained by setting a free radical spacer between the cathode and the electron transport layer using it as a material has better photothermal stability, which can further improve the overall stability and service life of the QLED. And the LUMO of TEMPO is around 3.57eV, so it is also a good transition layer material for the electron transport layer and the cathode.

[0038] In one embodiment, the quantum dot light-emitting diode may also be prepared with: at least one of a hole injection layer and a hole transport layer. That is, the QLED device of this embodiment may be prepared with other functional layers: the hole injection layer and the hole transport layer are located between the anode and the quantum dot light-emitting layer. When the two exist at the same time, the hole injection layer is prepared close to the anode, and the hole transport layer is prepared close to the quantum dot light-emitting layer. The material selection and thickness of the above functional layers are the same as those described above, and will not be repeated here.

[0039] In one embodiment, in order to obtain a high-quality hole injection layer, the anode needs to undergo a pretreatment process, wherein the pretreatment process specifically includes: cleaning the anode, and then treating the clean anode with ultraviolet-ozone or oxygen plasma to further remove organic matter attached to the surface of the anode and improve the work function of the anode.

[0040] In one embodiment, a substrate containing an anode is placed on a coating machine, and a prepared solution of hole injection material is spin-coated to form a film; the film thickness is controlled by adjusting the concentration of the solution, the spin-coating speed (2000-6000 rpm) and the spin-coating time, and then thermally annealed at an appropriate temperature; for example, annealing can be performed at 140-160° C. for 10-30 minutes (e.g., 15 minutes). Of course, the hole injection layer can also be prepared by printing.

[0041] In one embodiment, a substrate on which a hole injection layer has been spin-coated is placed on a coating machine, and a solution of a hole transport material prepared at a certain concentration is spin-coated to form a film, and the thickness of the hole transport layer is controlled by adjusting the concentration of the solution (5-10 mg / mL), the spin coating speed (2000-4000 rpm) and the spin coating time, and then thermally annealed at an appropriate temperature; for example, annealing can be performed at 130-150° C. for 15-30 minutes. The hole transport layer can also be prepared by printing, and the concentration of the hole transport ink used for printing is 1-5 mg / mL.

[0042] In one embodiment, a substrate with a hole transport layer prepared is placed on a coating machine, a quantum dot solution of a certain concentration is prepared and spin-coated to form a film, the thickness of the quantum dot light-emitting layer is controlled by adjusting the concentration of the solution (20-30 mg / mL), the spin-coating speed (2000-4000 rpm) and the spin-coating time, and the film is dried at an appropriate temperature. The quantum dot light-emitting layer can also be prepared by printing, and the concentration of the quantum dot ink used for printing is 3-10 mg / mL.

[0043] In one embodiment, in step S30, forming an electron transport layer and a free radical spacer layer on the quantum dot light-emitting layer comprises: depositing an electron transport layer material dispersed in a primary alcohol or a secondary alcohol and a free radical spacer layer material dispersed in an alcohol solvent or water on the quantum dot light-emitting layer in sequence, and then performing a first annealing treatment to form the electron transport layer and the free radical spacer layer;

[0044] or,

[0045] After depositing an electron transport layer material dispersed in an alcohol solvent on the quantum dot light-emitting layer, a second annealing treatment is performed to form the electron transport layer. After depositing a free radical spacer layer material dispersed in water on the electron transport layer, a third annealing treatment is performed in a primary alcohol or secondary alcohol atmosphere to form the free radical spacer layer.

[0046] Specifically, the surface of the electron transport layer often contains hydroxyl groups. The carbonyl groups generated by the free radical spacer layer after oxidation with primary alcohol or secondary alcohol will undergo non-covalent interactions with the hydrogen on the hydroxyl group, causing part of the free radical spacer layer material to penetrate into the areas where the electron transport layer is not uniformly formed (i.e., the crystal gaps) and adhere there due to non-covalent interactions, thereby filling and covering the electron transport layer.

[0047] In one embodiment, the temperature of the first annealing treatment and the second annealing treatment are both 70-120°C, and the time is 15-30 minutes; the temperature of the third annealing treatment is 70-120°C, and the time is 5-10 minutes. Further, the temperature of the second annealing treatment is less than or equal to the temperature of the third annealing treatment; this is because TEMPO has the effect of oxidizing primary alcohols or secondary alcohols into carbonyl compounds, and solvent annealing can reduce polarity, but the high-boiling point alcohol is directly spin-coated on the electron transport layer, resulting in the film not necessarily being completely spread out, and the oxidation that occurs makes the crystal gap of the film smaller, and the film formation is more uniform.

[0048] In one embodiment, the alcohol solvent may be selected from, but not limited to, one or more of methanol, ethanol and isopropanol.

[0049] In one embodiment, the primary alcohol may be selected from but not limited to C1-C6 primary alcohols; the secondary alcohol may be selected from but not limited to C1-C6 secondary alcohols. If the main chain of the primary alcohol or secondary alcohol is too long, it will cause problems such as incomplete annealing and insufficient volatilization due to its high boiling point.

[0050] In a preferred embodiment, the forming of the electron transport layer and the free radical spacer layer on the quantum dot light-emitting layer comprises: sequentially depositing an electron transport layer material dispersed in a primary alcohol or a secondary alcohol and a free radical spacer layer material dispersed in an alcohol solvent or water on the quantum dot light-emitting layer, and then performing a first annealing treatment to form the electron transport layer and the free radical spacer layer. First, the free radical spacer layer material and the electron transport layer material are deposited in sequence, and both the free radical spacer layer material and the electron transport layer material are in a wetting state. The primary alcohol or secondary alcohol is more evenly distributed between the free radical spacer layer and the electron transport layer in a wetting state by diffusion. Then, the primary alcohol or secondary alcohol is oxidized by the free radical spacer layer material to obtain a carbonyl compound, which is more evenly distributed between the free radical spacer layer and the electron transport layer in a wetting state. When uniformly annealed, the formed free radical spacer layer can be more evenly anchored on the electron transport layer through the evenly distributed carbonyl compound, so that the free radical barrier layer can more effectively prevent the functional layer of the QLED device from being oxidized, and protect the functional layer of the QLED device, thereby further improving the overall stability of the QLED device; in addition, the free radical barrier layer uniformly anchored on the electron transport layer can reduce the crystal gap of the electron transport layer, increase the density of the electron transport layer, and is beneficial to the transmission of carriers (electrons), thereby improving the efficiency of the QLED device.

[0051] In one embodiment, the obtained quantum dot light-emitting diode is packaged. The packaging process can be performed by a common machine packaging or manual packaging. Preferably, the oxygen content and water content in the packaging process environment are both less than 0.1 ppm to ensure the stability of the device.

[0052] In this embodiment, the preparation method of each layer can be a chemical method or a physical method, wherein the chemical method includes but is not limited to one or more of chemical vapor deposition, continuous ion layer adsorption and reaction, anodization, electrolytic deposition, and co-precipitation; the physical method includes but is not limited to one or more of solution method (such as spin coating, printing, scraping, dip pulling, immersion, spraying, roll coating, casting, slit coating or strip coating, etc.), evaporation method (such as thermal evaporation, electron beam evaporation, magnetron sputtering or multi-arc ion plating, etc.), deposition method (such as physical vapor deposition, atomic layer deposition, pulsed laser deposition, etc.).

[0053] The present invention is described in detail below through detailed embodiments.

[0054] Example 1 Preparation of a QLED device with an upright structure, whose structure is ITO (anode) / PEDOT:PSS:s-MoO3 (hole injection layer) / PVK (hole transport layer) / CdSe@ZnS (quantum dot light-emitting layer) / MZO (electron transport layer) / TEMPO (free radical spacer layer) / Al (cathode), comprising the following steps:

[0055] (1) A 30 nm hole injection layer (PEDOT:PSS:s-MoO3) was spin-coated on the ITO substrate and annealed at 150 °C in air for 15 min;

[0056] (2) In a nitrogen atmosphere, a 25 nm hole transport layer (made of PVK) was spin-coated on the hole injection layer and annealed at 150°C for 20 min;

[0057] (3) Spin-coat a 35nm quantum dot light-emitting layer (material: CdSe@ZnS) on the hole transport layer;

[0058] (4) spin coating a 40 nm magnesium-doped zinc oxide (MZO) electron transport layer dissolved in secondary amyl alcohol on the quantum dot light-emitting layer;

[0059] (5) Spin-coat a 5 nm thick TEMPO radical spacer layer dissolved in ethanol on the electron transport layer and anneal at 100 °C for 30 min;

[0060] (6) evaporating a 75 nm Al electrode on the free radical spacer layer;

[0061] (7) After packaging, an upright structure QLED device is obtained.

[0062] Example 2 Preparation of a QLED device with an upright structure, whose structure is ITO (anode) / PEDOT:PSS (hole injection layer) / NPB (hole transport layer) / CdSe@ZnS (quantum dot light-emitting layer) / ZnO (electron transport layer) / TEMPO (free radical spacer layer) / Ag (cathode), comprising the following steps:

[0063] (1) A 28 nm hole injection layer (PEDOT:PSS) was spin-coated on the ITO substrate and annealed at 140 °C in air for 15 min;

[0064] (2) In a nitrogen atmosphere, a 20 nm thick hole transport layer (made of NPB) was spin-coated on the hole injection layer and annealed at 135°C for 25 min.

[0065] (3) Spin-coat a 40 nm quantum dot light-emitting layer (material: CdSe@ZnS) on the hole transport layer;

[0066] (4) Spin-coat a 30 nm layer of ZnO dissolved in ethanol on the quantum dot light-emitting layer and anneal at 100 °C for 15 min to form an electron transport layer;

[0067] (5) Spin-coat a layer of about 3 nm of TEMPO dissolved in water on the electron transport layer, drop n-butanol in a culture dish, and quickly invert it on a hot plate with a device, and perform solvent annealing at 90°C for 5 min to form a free radical spacer layer;

[0068] (6) evaporating a 120 nm Ag electrode on the free radical spacer layer;

[0069] (7) After packaging, an upright structure QLED device is obtained.

[0070] Comparative Example 1 Preparation of a QLED device with an upright structure, whose structure is ITO (anode) / PEDOT:PSS (hole injection layer) / PVK (hole transport layer) / CdSe@ZnS (quantum dot light-emitting layer) / ZnO (electron transport layer) / Al (cathode), includes the following steps:

[0071] (1) A 29 nm hole injection layer (PEDOT:PSS) was spin-coated on the ITO substrate and annealed at 140 °C in air for 15 min;

[0072] (2) In a nitrogen atmosphere, a 20 nm thick hole transport layer (made of NPB) was spin-coated on the hole injection layer and annealed at 135°C for 25 min.

[0073] (3) Spin-coat a 40 nm quantum dot light-emitting layer (material: CdSe@ZnS) on the hole transport layer;

[0074] (4) Spin-coat a 30 nm layer of ZnO dissolved in ethanol on the quantum dot light-emitting layer and anneal at 100 °C for 15 min to form an electron transport layer;

[0075] (5) 120 nm Ag electrode was evaporated on the ZnO electron transport layer;

[0076] (6) After packaging, an upright structure QLED device is obtained.

[0077] Example 3 Evaluation of the performance of the QLED devices prepared in Examples 1, 2 and Comparative Example 1

[0078] According to the process mentioned in Examples 1, 2 and Comparative Example 1, a QLED device was prepared. Four devices were placed on the same substrate to obtain the average value of EQE (external quantum efficiency). On the first day (T1), the third day (T3), and the eighth day (T8) after the QLED device was prepared, the current voltage brightness (JVL) test was performed to obtain its external quantum efficiency. After the JVL test on the eighth day, the life span was tested. The life span test was carried out under the 1mA constant current mode. When the brightness dropped to 80% of the highest brightness during the test time, the corresponding value of the life span LT80 was obtained, and the brightness was finally converted to the life span under 1000nit. The performance test results of the QLED devices prepared in Examples 1, 2 and Comparative Example 1 are shown in Table 1. It can be seen that compared with the QLED device with an upright structure without a free radical spacer layer prepared in Comparative Example 1, the QLED device with an upright structure with a free radical spacer layer prepared in Examples 1 and 2 has better stability and a longer service life without a significant decrease in efficiency. The EQE of the QLED prepared in Example 1 measured within the predetermined test time is lower than that of the QLED prepared in Example 2, but this is only because the process window of the QLED prepared in Example 1 has not yet been reached. Through a suitable device post-processing process, the EQE of the QLED prepared in Example 1 can be improved; the EQE of the QLED prepared in Example 2 increases because water and oxygen have some positive aging effects on electron transmission and the interface of the electrode, which can improve the EQE but will cause the life of the device to decay. Therefore, the life and overall performance of the QLED prepared in Example 1 are better.

[0079] Table 1 Performance test results of QLED devices prepared in Examples 1, 2 and Comparative Example 1

[0080]

[0081] In summary, the present invention provides a quantum dot light-emitting diode with an upright structure and a preparation method thereof, wherein a stable free radical capable of oxidizing a primary alcohol or a secondary alcohol into a carbonyl compound can be used to achieve photothermal stability; a free radical spacer is provided between the cathode and the electron transport layer of the QLED with an upright structure using the free radical spacer as a material, which can effectively reduce the quenching of the electron transport layer and the quantum dot light-emitting layer materials of the QLED device by high-intensity ultraviolet light (such as contact during packaging) or high temperature (such as during device post-processing) during the preparation process, thereby enhancing the photothermal stability of the QLED device, thereby extending the life of the QLED device; at the same time, the stable oxidizing free radical has the function of capturing and quenching singlet oxygen, and the free radical spacer can quench the excited oxygen molecules through intermolecular energy transfer, converting them into fluorescence or phosphorescence, and causing radiation loss to return to the state of ground state oxygen, which can effectively prevent the functional layer of the QLED device from being oxidized, and protect the functional layer of the QLED device, thereby improving the overall stability of the QLED device. In addition, the oxidizing stable free radical can oxidize the primary alcohol or secondary alcohol into a carbonyl compound, and the formation of the carbonyl group enables the free radical spacer layer material to be anchored on the electron transport layer, thereby reducing the crystal gap of the electron transport layer and making the film denser, which is beneficial to the transmission of carriers (electrons) and plays a role in improving the efficiency of the device.

[0082] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. A quantum dot light emitting diode with an upright structure, characterized in that: include: An anode, a quantum dot light-emitting layer, an electron transport layer, a free radical spacer layer and a cathode, wherein the quantum dot light-emitting layer is located between the anode and the cathode, and the electron transport layer is located between the quantum dot light-emitting layer and the cathode; the free radical spacer layer is located between the electron transport layer and the cathode, and the free radical spacer layer material is a stable free radical capable of oxidizing a primary alcohol or a secondary alcohol into a carbonyl compound; The radical spacer layer is anchored on the electron transport layer via a carbonyl compound.

2. The quantum dot light emitting diode of the upright structure according to claim 1, characterized in that: The stable free radical is 2,2,6,6-tetramethylpiperidinyl oxide.

3. The quantum dot light emitting diode of the upright structure according to claim 1, characterized in that: The carbonyl compound is an oxide of a primary alcohol or a secondary alcohol, and the carbonyl compound is distributed between the free radical spacer layer and the electron transport layer.

4. The quantum dot light emitting diode of the upright structure according to claim 1, characterized in that: The anchoring refers to a non-covalent interaction between the carbonyl group of the carbonyl compound and the hydrogen on the surface hydroxyl group of the electron transport layer.

5. The quantum dot light emitting diode of the upright structure according to claim 1, characterized in that: The thickness of the free radical spacer layer does not exceed 5 nm.

6. The quantum dot light emitting diode of the upright structure according to claim 1, characterized in that: The anode is a transparent anode.

7. The quantum dot light emitting diode of the upright structure according to claim 1, characterized in that: The quantum dot light-emitting layer material is selected from one or more of II-VI group compounds and core-shell quantum dots, and the core material and shell material of the II-VI group compounds and core-shell quantum dots are independently selected from one of CdSe, CdS, ZnSe, CdS, PbS and PbSe.

8. The quantum dot light emitting diode of the upright structure according to claim 1, characterized in that: The electron transport layer material includes one or more of ZnO, TiO2, BaTiO3, aluminum-doped zinc oxide, lithium-doped zinc oxide, and magnesium-doped zinc oxide.

9. The quantum dot light emitting diode of the upright structure according to claim 1, characterized in that: A hole transport layer and / or a hole injection layer is arranged between the anode and the quantum dot light-emitting layer.

10. The quantum dot light emitting diode of the upright structure according to claim 9, characterized in that: The hole transport layer material is selected from one or more of poly[(9,9-dioctylfluorenyl-2,7-diyl)-co-(4,4'-(N-(p-butylphenyl))diphenylamine)], poly(9-vinylcarbazole), poly[bis(4-phenyl)(4-butylphenyl)amine] and N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine; and / or, The hole injection layer material is selected from one of poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonic acid) and poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonic acid) doped with s-MoO3.

11. A method for preparing a quantum dot light-emitting diode with an upright structure, characterized in that: Includes steps: providing an anode; forming a quantum dot light-emitting layer on the anode; An electron transport layer and a free radical spacer layer are formed on the quantum dot light-emitting layer, wherein the free radical spacer layer material is a stable free radical capable of oxidizing a primary alcohol or a secondary alcohol into a carbonyl compound; and the free radical spacer layer is anchored on the electron transport layer through the carbonyl compound; A cathode is formed on the free radical spacer layer to obtain the quantum dot light emitting diode.

12. The method for preparing a quantum dot light-emitting diode with an upright structure according to claim 11, characterized in that: The stable free radical is 2,2,6,6-tetramethylpiperidinyl oxide.

13. The method for preparing a quantum dot light-emitting diode with an upright structure according to claim 11, characterized in that: The forming of the electron transport layer and the free radical spacer layer on the quantum dot light-emitting layer comprises: depositing an electron transport layer material dispersed in a primary alcohol or a secondary alcohol and a free radical spacer layer material dispersed in an alcohol solvent or water on the quantum dot light-emitting layer in sequence, and then performing a first annealing treatment to form the electron transport layer and the free radical spacer layer; or, After depositing an electron transport layer material dispersed in an alcohol solvent on the quantum dot light-emitting layer, a second annealing treatment is performed to form the electron transport layer. After depositing a free radical spacer layer material dispersed in water on the electron transport layer, a third annealing treatment is performed in a primary alcohol or secondary alcohol atmosphere to form the free radical spacer layer.

14. The method for preparing a quantum dot light-emitting diode with an upright structure according to claim 13, characterized in that: The temperature of the second annealing treatment is less than or equal to the temperature of the third annealing treatment.

Citation Information

Patent Citations

  • Electroluminescent device including stable organic radical compounds

    CN105226184A

  • Quantum dot light emitting diode and preparation method thereof

    CN110739404A