An extrusion coating device for manganese dioxide coated with carbon material and its application

By using extrusion and cladding equipment inlaid carbon materials in the positive electrode material of lithium manganese battery, the problem of intimate combination of manganese dioxide and carbon materials is solved, the pulse discharge performance and production efficiency of the battery are improved, and more uniform cladding is achieved Effect.

CN114005951BActive Publication Date: 2024-11-29FUJIAN NANPING NANFU BATTERY
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202111463550.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-03
Publication Date
2024-11-29
Estimated Expiration
2041-12-03

AI Technical Summary

Technical Problem

The combination of manganese dioxide and carbon material in the positive electrode materials of existing lithium manganese batteries is not tight enough, resulting in insufficient conductivity and affecting the pulse discharge performance of the battery.

Method used

The extrusion and coating equipment using manganese dioxide outer coated carbon material is embedded in the surface of manganese dioxide through mechanical extrusion, improving its bonding strength and conductivity, and reducing battery impedance.

Benefits of technology

The close contact and combination between manganese dioxide and carbon materials is achieved, the pulse discharge performance of lithium manganese batteries is improved, and the production efficiency is greatly improved. Compared with the traditional ball mill method, the coating time is shortened to achieve uniform packaging within 60 minutes. cover.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114005951B_ABST
    Figure CN114005951B_ABST
Patent Text Reader

Abstract

The present invention provides an extrusion coating device for coating carbon material on the outside of manganese dioxide and its application. The device includes a central axis, a cylinder coaxially mounted on the central axis, and at least one extrusion unit installed on the outer peripheral wall of the central axis. Each extrusion unit contains a scraper and two stripper plates. All stripper plates and all scrapers are radially distributed on the outer peripheral wall of the central axis with the central axis as the center. A gap is left between each scraper and the inner peripheral wall of the cylinder to form a material extrusion channel. A wavy convex structure is arranged on the edge of each stripper plate facing the inner peripheral wall of the cylinder, and the front end of the convex structure conflicts with the inner peripheral wall of the cylinder. The crest of the convex structure of one stripper plate and the trough of the convex structure of the other stripper plate in the two stripper plates in each extrusion unit are always located on the same circumferential line. The use of the present invention can improve the bonding strength between manganese dioxide and carbon materials, which is beneficial to improving the pulse discharge performance of batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of battery manufacturing, and in particular to an extrusion coating device for coating manganese dioxide with carbon material and a production process for positive electrode materials of lithium manganese batteries using the device. Background Art

[0002] Lithium-manganese battery was first successfully developed in Japan in 1975 and has developed into the most widely used and largest-produced lithium battery in the market. It is the lowest-priced and safest battery type among lithium-ion primary batteries.

[0003] The positive active material of lithium manganese battery is manganese dioxide, but manganese dioxide itself has poor conductivity. Usually, when making the positive electrode material of lithium manganese battery, manganese dioxide needs to be mixed with conductive carbon material to enhance its conductivity. The positive electrode material of existing lithium manganese battery is generally prepared by mixing sintered manganese dioxide with carbon material and adhesive at one time or after ball milling. The carbon material is a mixture of acetylene black, graphite, carbon nanotubes and graphene, wherein acetylene black is a granular material with a particle size of 50 to 100 nanometers, graphite is a flaky material with a particle size of 1 to 10 microns, carbon nanotubes are tubular materials with a length of 0.5 to 2 microns, and graphene is a corrugated sheet material with a particle size of 300 nanometers to 500 nanometers. Manganese dioxide is usually a granular material with a particle size of 28 to 30 microns. The carbon material is mixed with manganese dioxide to form a composite conductive network between manganese dioxide.

[0004] When manganese dioxide and carbon materials are mixed and stirred in ordinary ways, the bonding between manganese dioxide and carbon materials is not tight enough, and even part of the manganese dioxide cannot conduct electrons due to lack of contact with the carbon material, resulting in loss of battery capacity. Therefore, it is particularly important to improve the effective contact and bonding tightness between manganese dioxide and carbon materials. Summary of the invention

[0005] One of the purposes of the present invention is to provide an extrusion coating device for coating carbon material on the outside of manganese dioxide. The device can embed the carbon material on the surface of manganese dioxide by physical extrusion to achieve the purpose of coating, which not only ensures good contact between manganese dioxide and the carbon material, but also improves the bonding strength between manganese dioxide and the carbon material, thereby reducing the impedance of the battery and helping to improve the pulse discharge performance of the lithium manganese battery.

[0006] An extrusion coating device for coating manganese dioxide with carbon material, comprising a horizontally arranged central shaft and a cylinder coaxially mounted on the central shaft, the two ends of the cylinder are closed, and a central shaft driving device is arranged on the outer side of either end of the cylinder, the central shaft driving device is in transmission connection with the central shaft and drives the central shaft to rotate;

[0007] At least one set of extrusion units is sequentially arranged on the outer peripheral wall of the central axis in the cylindrical body, each set of the extrusion units comprises a scraper and two material-diverting plates, and all the material-diverting plates and all the scrapers in all the extrusion units are radially distributed on the outer peripheral wall of the central axis with the central axis as the center;

[0008] A gap is left between each scraper and the inner peripheral wall of the cylinder to form a material extrusion channel;

[0009] A wave-shaped protrusion structure is arranged on the edge of each of the stripping plates facing the inner peripheral wall of the cylinder, and the front end of the protrusion structure contacts the inner peripheral wall of the cylinder;

[0010] The wave crest of the convex structure of one of the two stripper plates in each extrusion unit and the wave trough of the convex structure of the other stripper plate are always located on the same circumferential line;

[0011] A feed inlet and a discharge outlet are also provided on the outer wall of the cylinder.

[0012] The extrusion coating equipment for coating the manganese dioxide with carbon material of the present invention can coat a layer of carbon material on the surface of manganese dioxide by mechanical extrusion coating, so that the carbon material can be embedded in the surface of manganese dioxide to achieve the purpose of improving the tightness of the combination of manganese dioxide and carbon material, thereby reducing the impedance of the battery and facilitating the improvement of the pulse discharge performance of the lithium manganese battery.

[0013] Preferably, the number of the extrusion units is two, and the extrusion units are symmetrically distributed around the central axis. In this case, the central axis can rotate more smoothly and is not easily eccentric. At the same time, the mixture of manganese dioxide and carbon material can be more fully mixed between two mechanical extrusions.

[0014] Preferably, the scraper has a thickness of 0.2 to 1 cm, and the front end surface of the scraper is a smooth curved surface.

[0015] The second object of the present invention is to provide a production process for positive electrode materials for lithium manganese batteries, comprising the following steps: (1) firstly putting manganese dioxide and carbon material A into the extrusion coating equipment of the above-mentioned manganese dioxide outer-coated carbon material in a ratio of 80-95wt%:5-20wt%, and setting the rotation speed of the extrusion coating equipment to 50-1000 rpm for mixing, wherein the average particle size of the carbon material A is smaller than the average particle size of the manganese dioxide, and the carbon material A is any one of acetylene black and graphite or a combination of two; (2) adjusting the rotation speed to 3000-6000 rpm for mechanical fusion for more than 30 minutes, coating the surface of manganese dioxide with a layer of carbon material A, and collecting the mechanically fused mixed material; (3) finally taking out the mechanically fused mixed material obtained in step (2) from the extrusion coating equipment of the manganese dioxide outer-coated carbon material, and fully mixing it with other types of raw material mixers of existing lithium manganese battery positive electrode materials, and the rotation speed of the mixer is ≤1000 rpm to obtain the lithium manganese battery positive electrode material.

[0016] The existing ball mills on the market have a large load. In order to avoid the central rotating shaft from deflecting when running at high speed, the rotation speed can generally only reach 1000 rpm at most. If the existing ball mill is used for extrusion coating, it takes more than 10 hours to embed the carbon material on the surface of manganese dioxide, which is inefficient; and the powder is pressed on the cylinder wall by centrifugal force, which is also easy to cause agglomeration, resulting in insufficient ball milling, and the carbon material coated on the surface of manganese dioxide is difficult to be evenly distributed. The extrusion coating machine of the present invention has no grinding balls, so the overall weight is lighter, and the central rotating shaft is not easily affected by the weight of the grinding balls and deflected. Therefore, the extrusion coating machine of the present invention can achieve a rotation speed of 5000 rpm. The fast rotation speed can make the extrusion force acting on the coating material (i.e., the mixture of manganese dioxide and carbon material A) and the cylinder larger, so that the coating material and the cylinder are more tightly combined. The high rotation speed combined with the stirring and mixing again after each extrusion can achieve the purpose of uniform coating within 60 minutes. Compared with the mechanical coating using a ball mill, the production efficiency can be greatly improved.

[0017] When other types of raw materials (including carbon nanotubes, graphene, adhesives, etc.) of the existing lithium manganese battery positive electrode materials, carbon material A, and manganese dioxide are put into the above-mentioned extrusion coating equipment for manganese dioxide outer carbon material for extrusion coating at one time, under the mechanical extrusion force, nano-scale acetylene black will be coated on the tubular carbon nanotubes. At the same time, the carbon nanotubes themselves are easy to aggregate into agglomerates. Under the mechanical extrusion force, the carbon nanotubes are aggregated and mechanically extruded and compacted, resulting in that acetylene black or graphite cannot contact with manganese dioxide and cannot be coated on the surface of manganese dioxide, so that the carbon material cannot form a uniform and stable conductive network. Therefore, the lithium manganese battery positive electrode material of the present invention is produced. The production process adopts the feeding method of "first extruding and coating manganese dioxide and carbon material A, and then mixing the extruded and coated materials with other types of raw materials of lithium manganese battery positive electrode materials", which can not only achieve full coating of carbon material A on the surface of manganese dioxide to reduce battery impedance, but also avoid the adhesion of nano-scale acetylene black on the micron-scale flaky graphite surface to reduce the utilization efficiency of carbon materials; in addition, the extrusion coating equipment of the present invention can stir and mix carbon material A and manganese dioxide before each mechanical extrusion, so that the distribution of carbon material A and manganese dioxide is more uniform, avoiding aggregation between carbon material A, and ensuring that a layer of carbon material A can be quickly and evenly formed on the surface of manganese dioxide.

[0018] Preferably, when the carbon material A is only acetylene black, the particle size of the acetylene black is 50 to 100 nanometers, and the particle size of the manganese dioxide is 1 to 15 micrometers. After mechanical coating for 30 minutes, the nano-scale acetylene black can have a good coating effect on the manganese dioxide particles of 1 to 15 micrometers, and can form a fluffy coating layer on the surface of the manganese dioxide to enhance the conductivity of the manganese dioxide.

[0019] Preferably, when the carbon material A contains graphite, the particle size of the graphite particles is 1 to 10 microns, and the particle size of the manganese dioxide is 5 to 10 microns. Graphite particles are usually flaky, and the mechanical coating is performed for 30 minutes, and the manganese dioxide of about 5 to 10 microns can be closely attached to its surface to form a coating layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic diagram of the longitudinal cross-sectional structure of the extrusion coating equipment of the manganese dioxide coated carbon material of the present invention;

[0021] Figure 2 The extrusion coating equipment of the manganese dioxide outer coating carbon material of the present invention is Figure 1 Schematic diagram of the cross-sectional structure along the CC line;

[0022] Figure 3 The extrusion coating equipment of the manganese dioxide outer coating carbon material of the present invention is Figure 1Schematic diagram of the expanded cross-section structure after sectioning along the AA line;

[0023] Figure 4 is a SEM image of the extrusion-coated material of Example 1;

[0024] Figure 5 is a SEM image of the extrusion-coated material of Example 2;

[0025] Figure 6 This is a SEM image of the extrusion coated material of Example 4. DETAILED DESCRIPTION

[0026] The following is a detailed description of the extrusion coating equipment of the manganese dioxide coated carbon material and the specific implementation methods of its application in conjunction with the accompanying drawings:

[0027] Combination Figures 1 to 3 , an extrusion coating device for coating carbon material on the outside of manganese dioxide, comprising a horizontally arranged central shaft 10 and a cylindrical body 20 coaxially sleeved on the central shaft 10, wherein both ends of the cylindrical body 20 are closed, and a central shaft driving device 30 is arranged on the outer side of either end of the cylindrical body 20, wherein the central shaft driving device 30 is transmission-connected to the central shaft 10 and drives the central shaft 10 to rotate;

[0028] Two sets of extrusion units are sequentially arranged on the outer peripheral wall of the central axis 10 in the cylindrical body 20, each set of the extrusion units comprises a scraper 40 and two material-diverting plates 50, and all the material-diverting plates 50 and all the scrapers 40 in all the extrusion units are symmetrically distributed in a radially radial shape on the outer peripheral wall of the central axis 10 with the central axis as the center;

[0029] A gap is left between each scraper 40 and the inner peripheral wall 21 of the cylinder to form a material extrusion channel 60;

[0030] A wave-shaped protrusion structure 51 is provided on the edge of each of the stripping plates 50 facing the inner peripheral wall 21 of the cylinder, and the front end of the protrusion structure 51 abuts against the inner peripheral wall 21 of the cylinder;

[0031] The wave crest of the protruding structure 51 of one of the two stripping plates 50 in each extrusion unit and the wave trough of the protruding structure 51 of the other stripping plate 50 are always located on the same circumferential line;

[0032] The outer wall of the cylindrical body 20 is also provided with a feed inlet and a discharge outlet.

[0033] During operation, manganese dioxide and carbon material are put into the cylindrical body 20 from the feed port, and the central shaft 10 drives all scrapers 40 and all stripper plates 50 to rotate. Under the action of the stripper plates 50, manganese dioxide and carbon material are evenly mixed; and under the action of the scraper 40, manganese dioxide and carbon material are squeezed and rubbed in the material extrusion channel 60 between the scraper 40 and the inner circumferential wall 21 of the cylindrical body 20. Since manganese dioxide has a porous structure and the particle size of manganese dioxide is larger than that of carbon material, smaller carbon material is mechanically squeezed and partially embedded in the pores of manganese dioxide; and the manganese dioxide and carbon material after mechanical extrusion can be stirred evenly again under the action of the stripper plates 50, and the next round of mechanical extrusion is performed again, and the above mixing and mechanical extrusion are cyclically performed until a layer of carbon material is evenly coated on the surface of manganese dioxide.

[0034] The production process of positive electrode materials for lithium manganese battery using the extrusion coating equipment of the above-mentioned manganese dioxide outer-coated carbon material of the present invention comprises the following steps: (1) firstly, manganese dioxide and carbon material A are put into the above-mentioned extrusion coating equipment of the manganese dioxide outer-coated carbon material in a ratio of 80-95wt%:5-20wt%, and the speed of the extrusion coating equipment is set at 50-1000 rpm for mixing, wherein the average particle size of the carbon material A is smaller than the average particle size of the manganese dioxide, and the carbon material A is any one of acetylene black, graphite, etc. (2) adjusting the rotation speed to 3000-6000 rpm for mechanical fusion for more than 30 minutes, coating the surface of manganese dioxide with a layer of carbon material A, and collecting the mechanically fused mixture; (3) finally taking out the mechanically fused mixture obtained in step (2) from the extrusion coating equipment for coating the manganese dioxide with carbon material, and fully mixing it with other types of raw material mixers for lithium manganese battery positive electrode materials, wherein the rotation speed of the mixer is ≤1000 rpm, to obtain lithium manganese battery positive electrode materials.

[0035] For the production process of the positive electrode material of lithium manganese battery of the present invention, the inventors list the feeding ratio and particle size of manganese dioxide and carbon material A in 5 groups of embodiments and 4 groups of comparative examples, and the rotation speed of mechanical fusion in the following table 1. At the same time, the coating time corresponding to these 5 groups of embodiments and 4 groups of comparative examples is recorded, and the prepared positive electrode material of lithium manganese battery is prepared into positive electrode sheet by wet mixing, tableting, granulation, tableting, drying and other processes, with metal lithium as negative electrode, glass fiber diaphragm, 1 mol / L lithium perchlorate (LiClO4) / propylene carbonate (PC) + ethylene glycol dimethyl ether (DME) (volume ratio 1:1) as electrolyte, and assembled into CR2032 lithium manganese battery in a drying room with a dew point as low as -30 degrees, and the large current discharge performance data of CR2032 lithium manganese battery is measured. The experimental data are shown in the following table 2. In addition, the inventors have also tried to use a ball mill to replace the extrusion coating equipment of the present invention to produce lithium manganese battery positive electrode materials (Comparative Example 3) and ordinary stirring and mixing equipment to replace the extrusion coating equipment of the present invention to produce lithium manganese battery positive electrode materials (Comparative Example 4).

[0036] Table 1

[0037]

[0038] Table 2

[0039]

[0040] It can be seen from the experimental data in Table 1 and Table 2 that the lithium manganese battery positive electrode material production process using the above-mentioned manganese dioxide outer carbon material extrusion coating equipment of the present invention is used to prepare the lithium manganese battery positive electrode material, and the prepared CR2032 lithium manganese battery has good large current discharge performance. In addition, the material after extrusion coating in Example 1 of the present invention is characterized by SEM (such as Figure 4 As shown in Figure 2 and Mapping, it can be seen that the surface of manganese dioxide is covered with a flaky coating layer, and Mapping shows that the coating layer is a signal of carbon. At the same time, the material after extrusion coating in Example 2 of the present invention was characterized by SEM (as shown in Figure 2). Figure 5 The SEM characterization of the material after extrusion coating in Example 4 of the present invention (as shown) and Mapping characterization shows that the surface of manganese dioxide is covered with a granular coating layer, and Mapping shows that it is a carbon signal. Figure 6As shown) and Mapping characterization, it can be seen that: a large number of flaky and granular carbon materials are embedded on the surface of manganese dioxide, proving that this method can also obtain a relatively good coating effect, but there are still a large number of carbon materials that are not coated with manganese dioxide. In addition, in Example 5 of the present invention, when manganese dioxide is manganese dioxide of a general particle size (28 to 30 microns), even if the coating time is increased to 60 minutes, its coating effect will still deviate from that of Examples 1 to 4, but it is better than the coating effect of ball milling coating (Comparative Example 3) and the coating effect of ordinary stirring and mixing equipment (Comparative Example 4). The production process of the positive electrode material of the lithium manganese battery of the present invention can achieve the effect of improving the conductivity of the positive electrode, thereby improving the large current discharge performance of the battery, while the coating time is controlled within 1 hour, the energy consumption is controlled at a low level, and a high coating efficiency is maintained.

[0041] It should be noted that the extrusion coating equipment of the manganese dioxide coated carbon material of the present invention may include but is not limited to two sets of extrusion units, it may also include only one set of extrusion units, or it may include three or more sets of extrusion units.

[0042] The extrusion coating equipment of the manganese dioxide coated carbon material of the present invention is made of superhard stainless steel, and the extrusion coating equipment can be improved as follows: the thickness of the scraper 40 is 0.2 to 1 cm, and the front end surface 41 of the scraper 40 is a smooth arc surface (such as Figure 1 as shown).

[0043] In the specific implementation process, one end of the cylinder 20 is closed by setting a fixed sealing plate, and the other end is closed during operation by setting an openable end cover 22. At this time, the end of the cylinder 20 provided with the end cover serves as both the feed port and the discharge port. Of course, the feed port and the discharge port of the cylinder can also be set separately, or can be set on the peripheral wall of the cylinder, as long as the feed port and the discharge port can realize convenient feeding and taking of materials, and can be closed during operation.

[0044] For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. An extrusion coating device for coating manganese dioxide with carbon material, characterized in that: It comprises a horizontally arranged central shaft and a cylinder coaxially sleeved on the central shaft, the two ends of the cylinder are closed, and a central shaft driving device is arranged on the outer side of either end of the cylinder, the central shaft driving device is in transmission connection with the central shaft and drives the central shaft to rotate; At least one set of extrusion units is sequentially arranged on the outer peripheral wall of the central axis in the cylindrical body, each set of the extrusion units comprises a scraper and two material-diverting plates, and all the material-diverting plates and all the scrapers in all the extrusion units are radially distributed on the outer peripheral wall of the central axis with the central axis as the center; A gap is left between each scraper and the inner peripheral wall of the cylinder to form a material extrusion channel; A wave-shaped protrusion structure is arranged on the edge of each of the stripping plates facing the inner peripheral wall of the cylinder, and the front end of the protrusion structure contacts the inner peripheral wall of the cylinder; The wave crest of the convex structure of one of the two stripper plates in each extrusion unit and the wave trough of the convex structure of the other stripper plate are always located on the same circumferential line; A feed inlet and a discharge outlet are also provided on the outer wall of the cylinder.

2. The extrusion coating equipment of manganese dioxide coated with carbon material according to claim 1, characterized in that: The number of the extrusion units is two, and the extrusion units are symmetrically distributed around the central axis.

3. The extrusion coating equipment of manganese dioxide coated with carbon material according to claim 1, characterized in that: The thickness of the scraper is 0.2-1 cm, and the front end surface of the scraper is a smooth curved surface.

4. A lithium manganese battery positive electrode material production process, comprising the following steps: (1) First, manganese dioxide and carbon material A are put into an extrusion coating device for manganese dioxide coated carbon material according to any one of claims 1 to 3 in a ratio of 80 to 95wt%: 5 to 20wt%, and the rotation speed of the extrusion coating device is set to 50 to 1000 rpm for mixing, wherein the average particle size of the carbon material A is smaller than the average particle size of the manganese dioxide, and the carbon material A is any one of acetylene black and graphite or a combination of two; (2) the rotation speed is adjusted to 3000 to 6000 rpm for mechanical fusion for more than 30 minutes, a layer of carbon material A is coated on the surface of manganese dioxide, and the mechanically fused mixture is collected; (3) finally, the mechanically fused mixture obtained in step (2) is taken out from the extrusion coating device, and is fully mixed with other types of raw material mixers of existing lithium manganese battery positive electrode materials, and the rotation speed of the mixer is ≤1000 rpm to obtain lithium manganese battery positive electrode materials.

5. The process for producing a positive electrode material for a lithium-manganese battery according to claim 4, characterized in that: When the carbon material A is only acetylene black, the particle size of the acetylene black is 50-100 nanometers, and the particle size of the manganese dioxide is 1-15 micrometers.

6. The process for producing a positive electrode material for a lithium-manganese battery according to claim 4, characterized in that: When the carbon material A contains graphite, the particle size of the graphite is 1 to 10 microns, and the particle size of the manganese dioxide is 5 to 10 microns.

Citation Information

Patent Citations

  • Extrusion coating equipment for coating manganese dioxide with carbon material

    CN216354295U