Core block, laminated core and rotating motor
By controlling the bonding area ratio and designing non-bonded areas in the laminated core, combined with room temperature curing adhesives, the problems of improving the magnetic properties and iron loss control of the existing cores are solved, achieving more efficient magnetic properties and Bond strength.
Patent Information
- Application Number
- CN202080044985.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-06-26
- Filing Date
- 2020-06-22
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-06-22
AI Technical Summary
There is room for improvement in the magnetic properties of existing laminated iron cores, especially in terms of strain suppression and iron loss control in the bonded parts.
By setting a bonding portion between adjacent electromagnetic steel sheets in the stacking direction, the bonding area ratio is controlled between 1% and 60%. Combined with the design of the arc-shaped core back and teeth, a non-bonded In order to suppress strain and iron loss, a room-temperature curing acrylic adhesive is used, and the thickness and tensile elastic modulus of the adhesive part are adjusted to ensure magnetic properties.
It effectively improves the magnetic properties of the laminated iron core, suppresses the strain of the bonding part, reduces the iron loss, and ensures the overall bonding strength and magnetic property stability of the core block.
Smart Images

Figure CN114008891B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a core block, a laminated core, and a rotating electric machine.
[0002] This application claims priority based on Japanese Patent Application No. 2019-118337 filed in Japan on June 26, 2019, the contents of which are incorporated herein by reference. Background Art
[0003] Conventionally, there is known a laminated iron core as described in the following Patent Document 1. In this laminated iron core, electromagnetic steel sheets adjacent to each other in the lamination direction are bonded together.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 2011-023523 Summary of the Invention
[0007] Technical problem to be solved by the invention
[0008] In the above-mentioned conventional laminated core, there is room for improvement in terms of improving magnetic properties.
[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to improve the magnetic properties of a laminated iron core.
[0010] Technical means for solving technical problems
[0011] In order to solve the above technical problems, the present invention proposes the following means.
[0012] (1) A first embodiment of the present invention is an iron core block that forms a laminated iron core by connecting a plurality of iron core blocks in an annular shape, comprising: a plurality of electromagnetic steel sheets stacked on each other; and a bonding portion that is provided between the electromagnetic steel sheets adjacent to each other in the stacking direction and bonds the electromagnetic steel sheets to each other, wherein the bonding area ratio of the bonding portion to the electromagnetic steel sheets is not less than 1% and not more than 60%.
[0013] If adjacent electromagnetic steel sheets in the stacking direction are not fixed by any means, they will shift relative to each other. On the other hand, if adjacent electromagnetic steel sheets in the stacking direction are fixed by, for example, rivets, plastic strain will be applied to a portion of the electromagnetic steel sheets, degrading the magnetic properties of the core blocks.
[0014] In the core block structured as described above, adjacent electromagnetic steel sheets in the stacking direction are bonded together by bonding sections. Therefore, relative displacement of adjacent electromagnetic steel sheets in the stacking direction can be suppressed across the entirety of the plurality of electromagnetic steel sheets. Since the bonding sections provided on the electromagnetic steel sheets have a bonding area ratio of 1% or greater, the bonding sections reliably adhere the electromagnetic steel sheets to each other, effectively limiting relative displacement of adjacent electromagnetic steel sheets in the stacking direction even during winding. Furthermore, since the electromagnetic steel sheets are secured together by bonding, rather than riveting as described above, strain in the electromagnetic steel sheets can be suppressed. Consequently, the magnetic properties of the core block can be maintained.
[0015] However, as the adhesive portion solidifies, compressive stress is generated in the electromagnetic steel sheet. Therefore, even with the adhesive portion, strain may occur in the electromagnetic steel sheet. In the core block having the above-described structure, the adhesive portion has a bonding area ratio of 60% or less to the electromagnetic steel sheet. Therefore, strain in the electromagnetic steel sheet caused by the adhesive portion can be suppressed to a low level. Consequently, the magnetic properties of the core block can be further maintained.
[0016] (2) In the core block described in (1) above, the bonding area ratio may be greater than or equal to 1% and less than or equal to 20%.
[0017] According to this configuration, the strain generated in the electromagnetic steel sheet due to the bonding portion can be suppressed to a lower level.
[0018] (3) In the core block described in (1) or (2), it can also be constructed to have an arc-shaped core back and a tooth portion protruding from the core back to one side of the radial direction of the core back, and the bonding portion has: a pair of first parts extending along the circumference of both sides of the tooth portion; a second part extending along the circumference of the front end of the tooth portion and connecting the front ends of a pair of the first parts to each other; a pair of third parts extending from the base end of the first part along the circumference of one side of the radial direction of the core back to both sides of the circumference; a fourth part 45b extending circumferentially along the circumference of the other side of the radial direction of the core back; and a pair of fifth parts extending along the circumference of both sides of the circumference of the core back and connecting the third part and the fourth part respectively.
[0019] (4) In the core block described in (3), the widths of the second portion and the fifth portion may be narrower than the width of the fourth portion.
[0020] (5) In the core block described in any one of (1) to (4), the bonding portion may be provided on at least a portion of the peripheral edge of the electromagnetic steel sheet.
[0021] By arranging the bonding portion on the periphery of the electromagnetic steel sheet, for example, curling of the electromagnetic steel sheet can be suppressed. This facilitates the winding process and further ensures the magnetic properties of the laminated core.
[0022] (6) In the iron core block described in any one of (1) to (4), a non-bonding area of the electromagnetic steel sheet where the bonding portion is not provided is formed between the bonding area of the electromagnetic steel sheet where the bonding portion is provided and the peripheral edge of the electromagnetic steel sheet.
[0023] The electromagnetic steel sheets that form the core blocks are manufactured by punching out the base material, which is an electromagnetic steel sheet. During the punching process, strain is imparted from the periphery of the electromagnetic steel sheet toward the inside, over a width equivalent to the thickness of the electromagnetic steel sheet. This strain hardens the periphery of the electromagnetic steel sheet, making it less likely to deform, such as causing the periphery of the electromagnetic steel sheet to curl up locally. Therefore, even if the periphery of the electromagnetic steel sheet is not joined, deformation of the electromagnetic steel sheet is less likely to occur. Therefore, even if a non-bonded area is formed at the periphery of the electromagnetic steel sheet, deformation of the electromagnetic steel sheet can be suppressed. Furthermore, by forming this non-bonded area, the application of excess strain to the electromagnetic steel sheet can be suppressed. Consequently, the magnetic properties of the core blocks can be further maintained.
[0024] (7) In the core block described in (6), the width of the non-bonded region may be greater than or equal to 1 time and less than or equal to 10 times the thickness of the electromagnetic steel sheet.
[0025] (8) In the core block described in (1) or (2), it can also be constructed to have an arc-shaped core back and a tooth portion radially protruding from the core back toward the core back, and in the electromagnetic steel sheet, a non-bonding area of the electromagnetic steel sheet where the bonding portion is not provided is formed at the front end of the tooth portion and the circumferential ends of the core back.
[0026] In the core block, the magnetic flux spreads and extends from the front end of the tooth portion to both circumferential sides. Therefore, the magnetic flux tends to concentrate at the front end of the tooth portion. In addition, the magnetic flux invades the adjacent core block from both circumferential ends of the core back. Therefore, the magnetic flux tends to concentrate at both circumferential ends of the core back. If a bonding area is provided in the area where the magnetic flux is concentrated, the increase in iron loss tends to become significant. Therefore, if the bonding area is provided at the front end of the tooth portion and both circumferential ends of the core back, the iron loss tends to increase. According to the above-mentioned structure, since the non-bonding area without the bonding area is located at the front end of the tooth portion and both circumferential ends of the core back, the bonding area can be arranged away from the area with high magnetic flux density, and the increase in iron loss can be suppressed.
[0027] (9) In the core block described in (1) or (2), it can also be constructed to have an arc-shaped core back and a tooth portion radially protruding from the core back toward the core back, and the bonding area of the bonding portion to the core back is greater than the bonding area of the bonding portion to the tooth portion.
[0028] When the width of the teeth (circumferential dimension) is narrower than the width of the core back (radial dimension), magnetic flux tends to concentrate in the teeth, increasing the magnetic flux density there. Therefore, when strain is applied to the electromagnetic steel sheet through the bonding area, the magnetic properties of the teeth are more significantly affected than those of the core back, for the same amount of strain.
[0029] The bonding area of the bonding portion to the core back is greater than the bonding area of the bonding portion to the teeth. This suppresses the effects of strain in the bonding portion that degrades the magnetic properties of the teeth, while maintaining the overall bonding strength of the laminated core in the core back.
[0030] (10) In the laminated iron core described in any one of (1) to (9), the average thickness of the bonding portion may be 1.0 μm to 3.0 μm.
[0031] (11) In the laminated iron core described in any one of (1) to (10), the average tensile modulus E of the bonding portion may be 1500 MPa to 4500 MPa.
[0032] (12) In the laminated iron core described in any one of (1) to (11), the adhesive portion may be a room temperature adhesive type acrylic adhesive comprising SGA composed of an acrylic adhesive containing an elastomer.
[0033] (13) A second aspect of the present invention is a laminated core formed by annularly connecting a plurality of core blocks described in any one of (1) to (12).
[0034] (14) A second aspect of the present invention is a rotating electrical machine including the laminated iron core described in (13).
[0035] Effects of the Invention
[0036] According to the present invention, the magnetic characteristics of the laminated core can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 It is a plan view of a rotating electrical machine according to one embodiment of the present invention.
[0038] Figure 2 yes Figure 1 A side view of a core block included in the rotating electrical machine shown.
[0039] Figure 3 yes Figure 1 A top view of a core block included in the rotating electrical machine shown.
[0040] Figure 4 This is a top view of the core block of Modification 1.
[0041] Figure 5 This is a top view of a core block according to Modification 2.
[0042] Figure 6 This is a top view of a core block according to Modification 3.
[0043] Figure 7 This is a plan view of a stator used as a simulation object for iron loss in a verification test, and is a plan view showing a state where the bonding area ratio is 100%.
[0044] Figure 8 This is a plan view of a stator used as a simulation object for iron loss in a verification test, and shows a state where the bonding area ratio is 90%.
[0045] Figure 9 This is a plan view of a stator used as a simulation object for iron loss in a verification test, and is a plan view showing a state where the bonding area ratio is 85%.
[0046] Figure 10 This is a plan view of a stator used as a simulation object for iron loss in a verification test, and is a plan view showing a state where the bonding area ratio is 70%.
[0047] Figure 11 This is a plan view of a stator used as a simulation object for iron loss in a verification test, and is a plan view showing a state where the bonding area ratio is 60%.
[0048] Figure 12 This is a plan view of a stator used as a simulation object for iron loss in a verification test, and is a plan view showing a state where the bonding area ratio is 50%.
[0049] Figure 13 This is a plan view of a stator used as a simulation object for iron loss in a verification test, and shows a state where the bonding area ratio is 40%.
[0050] Figure 14 This is a plan view of a stator used as a simulation object for iron loss in a verification test, and is a plan view showing a state where the bonding area ratio is 30%.
[0051] Figure 15 This is a plan view of a stator used as a simulation object for iron loss in a verification test, and is a plan view showing a state where the bonding area ratio is 20%.
[0052] Figure 16 This is a plan view of a stator used as a simulation object for iron loss in a verification test, and is a plan view showing a state where the bonding area ratio is 15%.
[0053] Figure 17 This is a plan view of a stator used as a simulation object for iron loss in a verification test, and shows a state where the bonding area ratio is 10%.
[0054] Figure 18 This is a plan view of a stator used as a simulation object for iron loss in a verification test, and is a plan view showing a state where the bonding area ratio is 0%.
[0055] Figure 19 This is a plan view of a comparative stator used as a simulation target for iron loss in a verification test, and is a plan view showing a state in which electromagnetic steel sheets are caulked and joined.
[0056] Figure 20 It is a graph showing the results of the verification test.
[0057] Figure 21 This is a top view of the stator used as the simulation object for iron loss in the verification test.
[0058] Figure 22 This is a top view of the stator used as the simulation object for iron loss in the verification test. DETAILED DESCRIPTION
[0059] A rotating electrical machine according to one embodiment of the present invention will be described below with reference to the accompanying drawings. In this embodiment, an electric motor is used as an example of a rotating electrical machine, specifically an AC motor, more specifically a synchronous motor, and even more specifically a permanent magnet excitation motor. This type of motor is suitable for use in, for example, electric vehicles.
[0060] like Figure 1 As shown, the rotary electric machine 10 includes a stator 20, a rotor 30, a housing 50, and a rotating shaft 60. The stator 20 and the rotor 30 are housed in the housing 50. The stator 20 is fixed to the housing 50.
[0061] In this embodiment, the rotating electrical machine 10 employs an inner rotor type in which the rotor 30 is located inside the stator 20. However, an outer rotor type in which the rotor 30 is located outside the stator 20 may also be employed. In this embodiment, the rotating electrical machine 10 is a 12-pole, 18-slot three-phase AC motor. However, for example, the number of poles, slots, and phases can be appropriately modified. Furthermore, the rotating electrical machine 10 can rotate at 1000 rpm by applying an excitation current of 10A effective value and 100 Hz frequency to each phase.
[0062] The stator 20 includes a stator core (laminated core) 21, a connecting ring 29, and windings (not shown). Hereinafter, the direction along the central axis O of the stator core 21 will be referred to as the axial direction, the direction passing through and perpendicular to the central axis O of the stator core 21 will be referred to as the radial direction, and the direction circumferentially around the central axis O of the stator core 21 will be referred to as the circumferential direction. In this specification, "radially inward" may be referred to as "one radial side."
[0063] The rotor 30 is arranged radially inward of the stator 20 (stator core 21 ) and includes a rotor core 31 and a plurality of permanent magnets 32 .
[0064] The rotor core 31 is formed in an annular shape (ring shape) and is arranged coaxially with the stator 20. The rotating shaft 60 is arranged in the rotor core 31. The rotating shaft 60 is fixed to the rotor core 31.
[0065] Multiple permanent magnets 32 are fixed to the rotor core 31. In this embodiment, a set of two permanent magnets 32 forms a single magnetic pole. Multiple sets of permanent magnets 32 are arranged at equal intervals in the circumferential direction. In this embodiment, 12 sets (24 permanent magnets in total) are arranged at 30-degree intervals around the central axis O.
[0066] In this embodiment, an embedded magnet type motor is used as a permanent magnet excitation type motor. A plurality of through holes 33 are formed on the rotor core 31, which penetrate the rotor core 31 in the axial direction. The plurality of through holes 33 are provided corresponding to the plurality of permanent magnets 32. Each permanent magnet 32 is fixed to the rotor core 31 while being arranged in the corresponding through hole 33. The fixation of each permanent magnet 32 relative to the rotor core 31 can be achieved, for example, by bonding the outer surface of the permanent magnet 32 to the inner surface of the through hole 33 with an adhesive. In addition, as a permanent magnet excitation type motor, a surface magnet type motor can also be used instead of an embedded magnet type motor.
[0067] The rotor core 31 is a laminated core. Specifically, the rotor core 31 is formed by laminating multiple electromagnetic steel sheets. The laminated thickness of the rotor core 31 is, for example, 50.0 mm. The outer diameter of the rotor core 31 is, for example, 163.0 mm. The inner diameter of the rotor core 31 is, for example, 30.0 mm.
[0068] In the present embodiment, the plurality of electromagnetic steel sheets forming the rotor core 31 are fixed to each other by caulking portions (pins) C. However, the plurality of electromagnetic steel sheets forming the rotor core 31 may be bonded to each other.
[0069] Next, the stator core 21 will be described in more detail.
[0070] The stacking thickness of the stator core 21 is, for example, 50.0 mm. The outer diameter of the stator core 21 is, for example, 250.0 mm. The inner diameter of the stator core 21 is, for example, 165.0 mm. The inner diameter of the stator core 21 is based on the tip of the teeth 23 in the stator core 21. The inner diameter of the stator core 21 is the diameter of an imaginary circle inscribed within the tip of all teeth 23.
[0071] The stator core 21 is a split core. Therefore, the stator core 21 includes multiple core blocks 24. The core blocks 24 are connected in a ring shape to form the stator core 21. Connecting rings 29 are arranged radially outside the core blocks 24. The core blocks 24 are fixed to each other by being fitted into the connecting rings 29.
[0072] Next, the core blocks 24 will be described.
[0073] The core block 24 has an arc-shaped core back 22 and a tooth portion 23 extending in the circumferential direction. Figure 1 The figure shows the boundary line 24BL between the core back 22 and the teeth 23. The core block 24 has a pair of corner portions 24c, which are located between the radially inward and circumferentially facing surfaces of the outer surface. Boundary line 24BL is an arc centered on the central axis O and passing through the pair of corner portions 24c.
[0074] The core back 22 is formed in an arc shape centered on the central axis O when the stator 20 is viewed from above in the axial direction.
[0075] The teeth 23 protrude radially inward from the core back 22 (radially toward the center axis O of the core back 22). The stator core 21 is constructed by arranging a plurality of core blocks 24 in a circular pattern in the circumferential direction, so that the teeth 23 are arranged at equal intervals in the circumferential direction. In the stator 20 of this embodiment, 18 teeth 23 are provided at 20-degree intervals around the center axis O. The teeth 23 are formed to have the same shape and size.
[0076] The winding is wound around the teeth 23. The winding can be concentratedly wound or distributedly wound.
[0077] The core blocks 24 are constructed by stacking multiple electromagnetic steel sheets 40 in the axial direction. These electromagnetic steel sheets 40 are formed by punching electromagnetic steel sheets. Specifically, the core blocks 24 include multiple electromagnetic steel sheets 40 stacked one on top of the other. Therefore, the stator core 21 is a laminated core. Each of the multiple electromagnetic steel sheets 40 has a T-shape when viewed axially.
[0078] Each electromagnetic steel sheet 40 forming the core block 24 is formed, for example, by punching an electromagnetic steel sheet serving as a base material. A known electromagnetic steel sheet can be used as the electromagnetic steel sheet 40. The chemical composition of the electromagnetic steel sheet 40 is not particularly limited. In this embodiment, a non-oriented electromagnetic steel sheet is used as the electromagnetic steel sheet 40. For example, a non-oriented electrical steel strip according to JIS C 2552:2014 can be used as the non-oriented electromagnetic steel sheet. However, a directional electromagnetic steel sheet can be used as the electromagnetic steel sheet 40 instead of the non-oriented electromagnetic steel sheet. For example, a directional electrical steel strip according to JIS C2553:2012 can be used as the directional electromagnetic steel sheet.
[0079] In order to improve the workability of the electromagnetic steel sheet 40 and the iron loss of the core block 24, an insulating film is provided on both sides of the electromagnetic steel sheet 40. As a material constituting the insulating film, for example, (1) an inorganic compound, (2) an organic resin, (3) a mixture of an inorganic compound and an organic resin, etc. can be used. Examples of the inorganic compound include (1) a complex of dichromate and boric acid, and (2) a complex of phosphate and silicon dioxide. Examples of the organic resin include epoxy resin, acrylic resin, acrylic styrene resin, polyester resin, silicone resin, fluorine resin, etc.
[0080] In order to ensure the insulation performance between the mutually stacked electromagnetic steel sheets 40 , the thickness of the insulating film (the thickness per single surface of the electromagnetic steel sheet 40 ) is preferably 0.1 μm or more.
[0081] On the other hand, as the insulation coating becomes thicker, the insulation effect saturates. Furthermore, as the insulation coating becomes thicker, the proportion of the insulation coating in the core block 24 increases, which degrades the magnetic properties of the core block 24 and reduces its performance as a laminated core. Therefore, it is best to keep the insulation coating thin while ensuring insulation performance. The thickness of the insulation coating (the thickness per single surface of the electromagnetic steel sheet 40) is preferably 0.1 μm to 5 μm, and more preferably 0.1 μm to 2 μm.
[0082] As the electromagnetic steel sheet 40 becomes thinner, the iron loss improvement effect gradually saturates. Furthermore, as the electromagnetic steel sheet 40 becomes thinner, the manufacturing cost of the electromagnetic steel sheet 40 increases. Therefore, considering the iron loss improvement effect and manufacturing cost, the thickness of the electromagnetic steel sheet 40 is preferably 0.10 mm or greater.
[0083] On the other hand, if the electromagnetic steel sheet 40 is too thick, it becomes difficult to punch the electromagnetic steel sheet 40. Therefore, considering the punching work of the electromagnetic steel sheet 40, the thickness of the electromagnetic steel sheet 40 is preferably 0.65 mm or less.
[0084] Furthermore, iron loss increases when the electromagnetic steel sheet 40 is thicker. Therefore, considering the iron loss characteristics of the electromagnetic steel sheet 40, the thickness of the electromagnetic steel sheet 40 is preferably 0.35 mm or less, and more preferably 0.20 mm or 0.25 mm.
[0085] Considering the above, the thickness of each electromagnetic steel sheet 40 is, for example, 0.10 mm to 0.65 mm, preferably 0.10 mm to 0.35 mm, and more preferably 0.20 mm or 0.25 mm. The thickness of the electromagnetic steel sheet 40 also includes the thickness of the insulation coating.
[0086] The plurality of electromagnetic steel sheets 40 forming the core block 24 are bonded together by bonding portions 41. The bonding portions 41 are provided between the electromagnetic steel sheets 40 adjacent to each other in the stacking direction and are adhesives that solidify without being separated. Among adhesives, for example, thermosetting adhesives based on polymerization bonding are used. As adhesive compositions, those containing (1) acrylic resins, (2) epoxy resins, (3) compositions containing acrylic resins and epoxy resins, etc. can be applied. As such adhesives, in addition to thermosetting adhesives, free radical polymerization adhesives can also be used. From the perspective of productivity, room temperature curing adhesives are preferably used. Room temperature curing adhesives cure at 20°C to 30°C. As room temperature curing adhesives, acrylic adhesives are preferred. Representative acrylic adhesives include SGA (Second Generation Acrylic Adhesive). Any of anaerobic adhesives, quick-drying adhesives, and acrylic adhesives containing elastomers can be used within the scope that does not impair the effects of the present invention. The adhesive mentioned here refers to the state before curing, and the adhesive becomes the adhesive portion 41 after curing.
[0087] The average tensile modulus E of the bonding portion 41 at room temperature (20°C to 30°C) is within the range of 1500 MPa to 4500 MPa. If the average tensile modulus E of the bonding portion 41 is less than 1500 MPa, the rigidity of the laminated core is reduced. Therefore, the lower limit of the average tensile modulus E of the bonding portion 41 is 1500 MPa, and more preferably 1800 MPa. On the other hand, if the average tensile modulus E of the bonding portion 41 exceeds 4500 MPa, the insulating coating formed on the surface of the electromagnetic steel sheet 40 is peeled off. Therefore, the upper limit of the average tensile modulus E of the bonding portion 41 is 4500 MPa, and more preferably 3650 MPa.
[0088] The average tensile modulus E is measured by a resonance method. Specifically, the tensile modulus E is measured in accordance with JIS R 1602:1995.
[0089] More specifically, a sample for measurement (not shown) is first prepared. This sample is obtained by bonding two electromagnetic steel sheets 40 with an adhesive to be measured and curing the adhesive to form a bonded portion 41. If the adhesive is thermosetting, this curing is achieved by applying heat and pressure under practical heating and pressurizing conditions. On the other hand, if the adhesive is room-temperature curing, this curing is achieved by applying pressure at room temperature.
[0090] The tensile modulus of the sample is then measured using the resonance method. The method for measuring the tensile modulus using the resonance method is performed in accordance with JIS R 1602:1995, as described above. The tensile modulus of the adhesive portion 41 alone is then calculated by removing the influence of the electromagnetic steel sheet 40 itself from the tensile modulus of the sample (measured value).
[0091] Since the tensile modulus obtained from the sample is equal to the average value for the entire laminated core, this value is considered the average tensile modulus E. The composition is set so that the average tensile modulus E remains substantially constant at any stacking position along the stacking direction or at any circumferential position around the central axis of the laminated core. Therefore, the average tensile modulus E can also be measured at the cured adhesive portion 41 at the upper end of the laminated core.
[0092] As a bonding method, for example, an adhesive may be applied to the electromagnetic steel sheet 40 and then bonded by heating, pressing, or both. Furthermore, various heating methods may be used, such as heating in a high-temperature tank or electric furnace, or directly applying electricity.
[0093] In order to obtain stable and sufficient adhesive strength, the thickness of the adhesive portion 41 is preferably 1 μm or more.
[0094] On the other hand, if the thickness of the adhesive portion 41 exceeds 100 μm, the adhesive force saturates. Furthermore, as the thickness of the adhesive portion 41 increases, the proportion of the adhesive portion in the core block 24 increases, and the magnetic properties of the core block 24, such as iron loss, deteriorate. Therefore, the thickness of the adhesive portion 41 is preferably 1 μm to 100 μm, and more preferably 1 μm to 10 μm.
[0095] In addition, in the above description, the thickness of the adhesive portion 41 refers to the average thickness of the adhesive portion 41 .
[0096] The average thickness of the adhesive portion 41 is more preferably 1.0 μm or greater and 3.0 μm or less. If the average thickness of the adhesive portion 41 is less than 1.0 μm, sufficient bonding strength cannot be ensured as described above. Therefore, the lower limit of the average thickness of the adhesive portion 41 is 1.0 μm, and more preferably 1.2 μm. Conversely, if the average thickness of the adhesive portion 41 increases to exceed 3.0 μm, undesirable effects may occur, such as a significant increase in the strain of the electromagnetic steel sheet 40 due to shrinkage during thermal curing. Therefore, the upper limit of the average thickness of the adhesive portion 41 is 3.0 μm, and more preferably 2.6 μm.
[0097] The average thickness of the adhesive portion 41 is the average value for the entire laminated core. The average thickness of the adhesive portion 41 is substantially constant at any position along the laminated direction or circumferentially around the central axis of the laminated core. Therefore, the average thickness of the adhesive portion 41 can be the average of values measured at the upper end of the laminated core at 10 or more locations in the circumferential direction.
[0098] The average thickness of the adhesive portion 41 can be adjusted, for example, by changing the amount of adhesive applied. Furthermore, the average tensile modulus E of the adhesive portion 41 can be adjusted, for example, by changing the heating and pressurizing conditions applied during bonding and the type of curing agent, or both, in the case of a thermosetting adhesive.
[0099] like Figure 2 As shown, in this embodiment, adjacent electromagnetic steel sheets 40 in the stacking direction are bonded together by bonding portions 41. In the illustrated example, adjacent electromagnetic steel sheets 40 in the stacking direction are fixed together only by bonding and are not fixed by other means (e.g., caulking, etc.).
[0100] exist Figure 3 In FIG. 4 , the bonding portion 41 is emphasized by a dot pattern. Figure 3 As shown, the electromagnetic steel sheets 40 adjacent to each other in the stacking direction are not bonded to each other over their entire surfaces. These electromagnetic steel sheets 40 are bonded to each other partially.
[0101] In this embodiment, adjacent electromagnetic steel sheets 40 in the stacking direction are bonded together by bonding portions 41 provided on the peripheries of the electromagnetic steel sheets 40. According to this embodiment, the bonding portions 41 are provided over the entire periphery of the electromagnetic steel sheets 40. However, the bonding portions 41 may be provided over at least a portion of the periphery of the electromagnetic steel sheets 40.
[0102] The adhesive portions 41 are each formed into a strip shape when viewed from above. Here, the term "strip shape" also includes shapes where the width of the strip varies along the strip. For example, a shape where a circular point is not broken but continues in one direction is also included in a strip shape extending in one direction. Furthermore, the term "along the periphery of the electromagnetic steel sheet 40" includes not only being completely parallel to the periphery but also being inclined within 5 degrees relative to the periphery, for example.
[0103] The bonding portion 41 includes a tooth portion 44 disposed on the tooth portion 23 and a core back portion 45 disposed on the core back 22. The tooth portion 44 of the bonding portion 41 includes a pair of first portions 44a and a second portion 44b. The core back portion 45 of the bonding portion 41 includes a pair of third portions 45a, a fourth portion 45b, and a pair of fifth portions 45c. In other words, the bonding portion 41 includes a pair of first portions 44a, a second portion 44b, a pair of third portions 45a, a fourth portion 45b, and a pair of fifth portions 45c.
[0104] A pair of first portions 44a extend along the circumferential edges of the tooth portion 23 on both sides. The pair of first portions 44a are arranged at intervals in the circumferential direction. The second portion 44b extends along the circumferential edge of the front end of the tooth portion 23 and connects the front ends of the pair of first portions 44a. A pair of third portions extend from the base ends of the first portions 44a along the circumferential edges of the radially inner side (one radial side) of the core back 22 to both sides in the circumferential direction. The fourth portion 45b extends circumferentially along the circumferential edge of the radially outer side (the other radial side) of the core back 22. A pair of fifth portions 45c extend along the circumferential edges of the core back 22 on both sides in the circumferential direction and connect the third portion 45a and the fourth portion 45b, respectively.
[0105] According to this embodiment, the first portion 44a, second portion 44b, third portion 45a, fourth portion 45b, and fifth portion 45c of the bonding portion 41 are formed to define the outer periphery of each of the electromagnetic steel sheets 40. Therefore, the stacked electromagnetic steel sheets 40 can be securely held near the periphery of the bonding portion 41. As a result, curling, which is likely to occur near the periphery of the electromagnetic steel sheets 40, can be effectively suppressed, reducing the bonding area ratio while achieving secure fixation between the electromagnetic steel sheets 40.
[0106] In addition, in this embodiment, the bonding portion 41 is provided without a gap from the periphery of the electromagnetic steel sheet 40 in a plan view of the electromagnetic steel sheet 40, but the present invention is not limited thereto. Figure 4As shown in the core block 124 of the first modification, the adhesive portion 141 may be provided with a gap relative to the peripheral edge of the electromagnetic steel sheet 40 in a plan view of the electromagnetic steel sheet 40. Specifically, a non-adhesive region 143 of the electromagnetic steel sheet 40 may be formed between the adhesive region 142 of the electromagnetic steel sheet 40 provided with the adhesive portion 141 and the peripheral edge of the electromagnetic steel sheet 40. The adhesive region 142 of the electromagnetic steel sheet 40 provided with the adhesive portion 141 refers to a region on the surface of the electromagnetic steel sheet 40 facing the stacking direction (hereinafter referred to as the first surface of the electromagnetic steel sheet 40) where the adhesive is not separated and solidified. The non-adhesive region 143 of the electromagnetic steel sheet 40 not provided with the adhesive portion 141 refers to a region on the first surface of the electromagnetic steel sheet 40 where the adhesive is not separated and solidified.
[0107] In addition, for example Figure 5 As shown in the core block 224 of the second modification, the bonding portion 241 may be configured without portions corresponding to the second portion 44b and the fifth portion 45c of the bonding portion 41 in the above-described embodiment. Specifically, the electromagnetic steel sheet 40 may include non-bonded regions 243 of the electromagnetic steel sheet 40 at the tips of the teeth 23 and at both circumferential ends of the core back 22, where the bonding portion 241 is not provided. Furthermore, in this modification, the bonding portion 241 includes a pair of first portions 244a circumferentially spaced apart on the teeth 23 and extending radially; a pair of third portions 245a extending along the radially inner edge of the core back 22; and a fourth portion 245b extending along the radially outer edge of the core back 22.
[0108] Furthermore, if Figure 6 As shown in the core block 324 of the third modification, the width dimensions of each portion of the bonding portion 341 may also be configured differently from those in the above-described embodiment. The bonding portion 341 of the third modification, like the above-described embodiment, includes a pair of first portions 344a, a second portion 344b, a pair of third portions 345a, a fourth portion 345b, and a pair of fifth portions 345c. In this modification, the widths of the first portion 344a, the second portion 344b, the third portion 345a, and the fifth portion 345c are approximately equal. On the other hand, the width of the fourth portion 345b is wider than the widths of the other portions of the bonding portion 341 (the first portion 344a, the second portion 344b, the third portion 345a, and the fifth portion 345c).
[0109] In this specification, the "width" of each portion of the adhesive portion 341 refers to the dimension in a direction perpendicular to the direction in which the portion extends. For example, the width of the second portion 344b, the third portion 345a, and the fourth portion 345b refers to the dimension along the radial direction of each portion. Furthermore, the width of the first portion 344a and the fifth portion 345c refers to the dimension along the circumferential direction of each portion.
[0110] In this specification, the width of each portion of the bonding portion 41 is 1.5% or more of the outer diameter of the stator core 21. By making the width of each portion of the bonding portion 41 1.5% or more of the outer diameter of the stator core 21, sufficient bonding strength between the electromagnetic steel sheets 40 can be ensured.
[0111] like Figure 2 As shown, in this embodiment, all bonding portions 41 provided between the electromagnetic steel sheets 40 have the same top-view shape. The top-view shape of the bonding portion 41 refers to the overall shape of the bonding portion 41 when viewed from the stacking direction. The top-view shape of all bonding portions 41 provided between the electromagnetic steel sheets 40 includes not only the case where all bonding portions 41 provided between the electromagnetic steel sheets 40 have exactly the same top-view shape, but also the case where all bonding portions 41 provided between the electromagnetic steel sheets 40 have substantially the same top-view shape, with 95% or more of the top-view shape being common.
[0112] Furthermore, in this embodiment, the bonding area ratio of the adhesive portion 41 to the electromagnetic steel sheet 40 is greater than 1% and less than 60%. In the illustrated example, the bonding area ratio is greater than 1% and less than 20%, specifically, 20%. Furthermore, the bonding area ratio of the adhesive portion 41 to the electromagnetic steel sheet 40 refers to the ratio of the area of the region (adhesive region 42) on the first surface where the adhesive portion 41 is provided, relative to the area of the first surface of the electromagnetic steel sheet 40. The region where the adhesive portion 41 is provided refers to the region (adhesive region 42) on the first surface of the electromagnetic steel sheet 40 where the adhesive is provided without being broken and solidified. The area of the region where the adhesive portion 41 is provided can be determined, for example, by photographing the first surface of the electromagnetic steel sheet 40 after peeling and performing image analysis on the photographed result.
[0113] In this embodiment, the bonding area ratio of the bonding portion 41 between the electromagnetic steel sheets 40 is 1% or more and 20% or less. For each of the two adjacent electromagnetic steel sheets 40 in the stacking direction, the bonding area ratio of the bonding portion 41 to the electromagnetic steel sheets 40 is 1% or more and 20% or less. When bonding portions 41 are provided on both sides of a single electromagnetic steel sheet 40 in the stacking direction, the bonding area ratio on both surfaces of the electromagnetic steel sheet 40 is 1% or more and 20% or less.
[0114] Furthermore, in this embodiment, the bonding area of the bonding portion 41 to the core back 22 (hereinafter referred to as the "first bonding area S1") is preferably greater than the bonding area of the bonding portion 41 to the teeth 23 (hereinafter referred to as the "second bonding area S2"). In other words, S1 ≥ S2.
[0115] Here, the first bonding area S1 is the area of the core back portion 45 on the first surface of the electromagnetic steel sheet 40, where the bonding portion 41 is provided. Similarly, the second bonding area S2 is the area of the tooth portion 44 on the first surface of the electromagnetic steel sheet 40, where the bonding portion 41 is provided. Furthermore, similar to the area of the area where the bonding portion 41 is provided, the first bonding area S1 and the second bonding area S2 can be obtained by, for example, imaging the first surface of the electromagnetic steel sheet 40 after peeling and performing image analysis on the imaging results.
[0116] In the core block 24, if adjacent electromagnetic steel sheets 40 in the stacking direction are not fixed by any means, they will displace relative to each other. On the other hand, if adjacent electromagnetic steel sheets 40 in the stacking direction are fixed by, for example, riveting, plastic strain is applied to portions of the electromagnetic steel sheets 40, degrading the magnetic properties of the core block 24. Riveting is a method of restricting relative displacement of the electromagnetic steel sheets 40 by plastically deforming portions of the electromagnetic steel sheets 40 and causing them to bite in the stacking thickness direction. Since the magnetic properties of the electromagnetic steel sheets 40 degrade when plastic strain is applied, using riveting to secure the electromagnetic steel sheets 40 degrades the magnetic properties of the core block 24 as a whole.
[0117] In contrast, in the core block 24 of this embodiment, adjacent electromagnetic steel sheets 40 in the stacking direction are bonded together by bonding portions 41. Consequently, relative displacement of adjacent electromagnetic steel sheets 40 in the stacking direction can be suppressed across the entire plurality of electromagnetic steel sheets 40. The bonding area ratio of the bonding portions 41 to the electromagnetic steel sheets 40 is 1% or greater. This ensures reliable bonding by the bonding portions 41, effectively limiting relative displacement of adjacent electromagnetic steel sheets 40 in the stacking direction, for example, even during winding of the teeth 23 of the core block 24. Furthermore, since the electromagnetic steel sheets 40 are secured by bonding rather than riveting as described above, strain in the electromagnetic steel sheets 40 can be suppressed. Consequently, the magnetic properties of the core block 24 can be maintained. Furthermore, to further enhance bonding strength and prevent separation of the electromagnetic steel sheets 40 even under impact, the bonding area ratio is preferably set to 10% or greater.
[0118] Furthermore, if adhesive is applied to the electromagnetic steel sheet 40 , compressive stress is generated in the electromagnetic steel sheet 40 as the adhesive cures. Therefore, when adhesive is applied to the electromagnetic steel sheet 40 to form the bonded portion 41 , strain may be generated in the electromagnetic steel sheet 40 .
[0119] However, in the core block 24 of this embodiment, the bonding area ratio of the bonding portion 41 to the electromagnetic steel sheet 40 is 60% or less. Therefore, the strain caused by the adhesive in the electromagnetic steel sheet 40 can be suppressed to a low level. Consequently, the magnetic properties of the core block 24 can be further maintained.
[0120] Furthermore, the bonding area ratio of the bonding portion 41 to the electromagnetic steel sheet 40 is 20% or less. Therefore, the strain generated in the electromagnetic steel sheet 40 due to the adhesive can be suppressed to a lower level.
[0121] The bonding portion 41 is provided in a bonding region 42 formed on at least a portion of the periphery of the electromagnetic steel sheet 40. This can prevent, for example, curling of adjacent electromagnetic steel sheets 40 in the stacking direction. This facilitates winding of the teeth 23 of the core blocks 24 and further ensures the magnetic properties of the core blocks 24. Consequently, the magnetic properties of the core blocks 24 can be further maintained.
[0122] When the width W1 (circumferential dimension) of the teeth 23 is narrower than the width W2 (radial dimension) of the core back 22, magnetic flux tends to concentrate in the teeth 23, increasing the magnetic flux density in the teeth 23. Therefore, when strain is applied to the steel sheet by the adhesive, the magnetic properties of the teeth 23 are more significantly affected than those of the core back 22, provided the strain is the same.
[0123] In this embodiment, the first bonding area S1 is preferably greater than the second bonding area S2. In this case, the influence of strain in the adhesive on the deterioration of the magnetic properties of the teeth 23 can be suppressed, while ensuring the bonding strength of the core blocks 24 as a whole in the core back 22.
[0124] Furthermore, the electromagnetic steel sheet 40 forming the core block 24 is manufactured by punching out the electromagnetic steel sheet serving as the base material. During the punching process, a strain caused by the punching process is applied to a width corresponding to the thickness of the electromagnetic steel sheet 40 from the periphery of the electromagnetic steel sheet 40 toward the inner side of the electromagnetic steel sheet 40. The periphery of the electromagnetic steel sheet 40 is work-hardened by the above-mentioned strain, so that deformation such as partial curling of the periphery of the electromagnetic steel sheet 40 is unlikely to occur. Therefore, even if the periphery of the electromagnetic steel sheet 40 is not bonded, deformation of the electromagnetic steel sheet 40 is unlikely to occur. Therefore, as Figure 4Even when the non-bonded region 143 is formed around the periphery of the electromagnetic steel sheet 40, as in the core block 124 of the first modification shown, deformation of the electromagnetic steel sheet 40 can be suppressed. Furthermore, by forming the non-bonded region 143 in this manner, excessive strain on the electromagnetic steel sheet 40 can be suppressed. Consequently, the magnetic properties of the core block 24 can be further maintained.
[0125] In addition, if Figure 4 As shown, by providing a non-contact region 143 between the periphery of the electromagnetic steel sheet 40 and the adhesive portion 141, it is possible to prevent uncured adhesive from being squeezed out of the periphery of the electromagnetic steel sheet 40 during lamination. If the adhesive were to solidify while being squeezed out from the tip of the teeth 23, it could interfere with the rotating rotor 30. Furthermore, if the adhesive were to solidify while being squeezed out from the side of the teeth 23, the cross-sectional area of the slots between the teeth 23 would be reduced, potentially reducing the space factor of the coil.
[0126] The width of the non-adhesive region 143 is preferably at least 1 times and no more than 10 times the thickness of the electromagnetic steel sheet 40. By setting the width of the non-adhesive region 143 to at least 1 times the thickness, squeeze-out of the adhesive can be effectively suppressed. Furthermore, by setting the width of the non-adhesive region 143 to no more than 10 times the thickness, curling of the electromagnetic steel sheet 40 due to work hardening at the peripheral edge of the electromagnetic steel sheet 40 can be suppressed.
[0127] In this specification, the "width" of the non-adhesive region 143 refers to the dimension in the direction perpendicular to the direction in which each portion of the non-adhesive region 143 extends. The width of the non-adhesive region 143 is preferably within the above range over the entire length of the non-adhesive region 143.
[0128] In the core block 24, the magnetic flux spreads and extends from the front end of the tooth portion 23 to both sides in the circumferential direction. Therefore, the magnetic flux at the front end of the tooth portion 23 is easily concentrated. In addition, the magnetic flux invades the adjacent core block 24 from both ends of the circumferential direction of the core back 22. Therefore, the magnetic flux is easily concentrated at both ends of the circumferential direction of the core back 22. If the bonding area 42 is provided in the area where the magnetic flux is concentrated, the increase in the iron loss is likely to become significant. Therefore, if Figure 5 As shown in the second modification, by providing non-bonding regions 243 at the front end of the tooth portion 23 and at both circumferential ends of the core back 22, the bonding regions 242 can be arranged away from regions with high magnetic flux density, thereby suppressing an increase in iron loss.
[0129] The magnetic flux B tends to flow through the shortest distance with the lowest magnetic resistance. Therefore, in the core back 22, the magnetic flux density decreases as it moves from the radial inner side (radial one side) connected to the tooth portion 23 to the radial outer side (radial other side) away from the tooth portion 23. On the other hand, as described above, the magnetic flux tends to concentrate at the front end of the tooth portion 23 and the circumferential ends of the core back 22. Figure 6 In Modification 3, the widths of the second portion 344b and the fifth portion 345c located at the tips of the teeth 23 and at both circumferential ends of the core back 22 are narrower than the width of the fourth portion 345b extending along the radially outer circumference of the core back 22. Specifically, Modification 3 reduces the widths of the second portion 344b and the fifth portion 345c, where the magnetic flux density tends to increase, thereby suppressing increases in iron loss. Furthermore, Modification 3 increases the width of the fourth portion 345b, where the magnetic flux density tends to decrease, thereby improving the bonding strength between the electromagnetic steel sheets 40 while reducing the effect of the bonding portion 341 on iron loss.
[0130] In addition, the protective scope of the present invention is not limited to the above-described embodiment, and various modifications can be added without departing from the spirit of the present invention.
[0131] The shape of the core block 24 is not limited to that shown in the above embodiment. The dimensions of each part of the core block 24, the thickness of the electromagnetic steel sheet 40, and the like can be arbitrarily designed according to the desired characteristics of the rotating electrical machine.
[0132] Alternatively, the core blocks may have a convex shape on one circumferential end face of the core back and a concave shape on the other circumferential end face. In this case, the convex shape can be inserted into the concave shape to suppress positional shifting when connecting the core blocks in the circumferential direction.
[0133] Furthermore, the core block may have two or more teeth for one core back. Furthermore, the core block may have separate core backs and teeth.
[0134] In the rotor of the embodiment described above, a set of two permanent magnets 32 forms one magnetic pole, but the present invention is not limited thereto. For example, one permanent magnet 32 may form one magnetic pole, or three or more permanent magnets 32 may form one magnetic pole.
[0135] In the above embodiment, a permanent magnet excitation type motor is described as an example of a rotating electrical machine. However, the structure of the rotating electrical machine is not limited to this as exemplified below, and various well-known structures not exemplified below may be employed.
[0136] In the above embodiment, a permanent magnet excitation type motor is described as an example of a synchronous motor, but the present invention is not limited thereto. For example, the rotating electrical machine may be a reluctance type motor or an electromagnetic excitation type motor (winding excitation type motor).
[0137] In the above embodiment, a synchronous motor is described as an example of an AC motor, but the present invention is not limited thereto. For example, the rotating electrical machine may be an induction motor.
[0138] In the above embodiment, an AC motor is described as an example of an electric motor, but the present invention is not limited thereto. For example, the rotating electrical machine may be a DC motor.
[0139] In the above embodiment, an electric motor is described as an example of a rotating electrical machine, but the present invention is not limited thereto. For example, the rotating electrical machine may be a generator.
[0140] In the above embodiment, the laminated iron core of the present invention is applied to a stator core, but it can also be applied to a rotor core. In addition, the laminated iron core of the present invention can also be applied to laminated iron cores other than rotating electrical machines such as transformers.
[0141] Furthermore, components in the above-described embodiments may be appropriately replaced with well-known components without departing from the spirit of the present invention, and the above-described modifications may be appropriately combined.
[0142] For example, the core block may also combine the structure of Modification 1 and the structure of Modification 2. Figure 4 As shown in the first modification, a non-contact region 143 is provided between the periphery of the electromagnetic steel sheet 40 and the bonding portion 141, and further as shown in the modification Figure 5 As in the second modified example shown, non-bonding regions 243 are provided at the front ends of the teeth 23 and at both ends in the circumferential direction of the core back 22 .
[0143] Similarly, the core block can also combine the structure of modification example 1 and the structure of modification example 3. That is, it can also be, Figure 4 As in the first modification shown in FIG. 1 , a non-contact region 143 is provided between the periphery of the electromagnetic steel sheet 40 and the bonding portion 141, and as shown in FIG. Figure 6 As in the third modified example shown, the widths of the second portion 344b and the fifth portion 345c of the adhesive portion 341 are configured to be narrower than the width of the fourth portion 345b.
[0144] Example
[0145] Next, verification tests (first to third verification tests) were conducted to verify the above-mentioned effects. The verification tests were conducted by simulation using software. As the software, JMAG, a finite element method electromagnetic field analysis software manufactured by JSOL Corporation, was used.
[0146] (First verification test)
[0147] Figures 7 to 18 The following are 12 types of stator cores 21A to 21L that were simulated in this verification test. Figure 3The stator core 21 of the illustrated embodiment has a basic structure with the following modifications. Each stator core 21A to 21L includes a plurality of core blocks 24A to 24L. Furthermore, the thickness of the electromagnetic steel sheet 40 is set to 0.25 mm. Furthermore, the bonding area ratio of the bonding portion 41 to each electromagnetic steel sheet 40 varies between 0% and 100%. More specifically, the bonding area ratio of the stator core 21A is 100%. The bonding area ratio of the stator core 21B is 90%. The bonding area ratio of the stator core 21C is 85%. The bonding area ratio of the stator core 21D is 70%. The bonding area ratio of the stator core 21E is 60%. The bonding area ratio of the stator core 21F is 50%. The bonding area ratio of the stator core 21G is 40%. The bonding area ratio of the stator core 21H is 30%. The bonding area ratio of the stator core 21I is 20%. The bonding area ratio of the stator core 21J is 15%, the bonding area ratio of the stator core 21K is 10%, and the bonding area ratio of the stator core 21L is 0%.
[0148] The iron losses of 12 types of stator cores 21A to 21L were obtained by the simulation. Figure 19 As shown, the iron loss of a comparative stator core 21X in which multiple electromagnetic steel sheets 40 are riveted throughout the entire layer is also calculated. The comparative stator core 21X includes multiple core blocks 24X. The thickness of the electromagnetic steel sheets 40 of the comparative stator core 21X is also 0.25 mm. The core blocks of the comparative stator core 21X are each provided with a first riveted portion C1 located on the core back 22 and two second riveted portions C2 located on the teeth 23. The first riveted portion C1 is located at the circumferential center of the core back 22. The two second riveted portions C2 are radially arranged at the circumferential center of the teeth 23. The area occupied by the riveted portions C1 and C2 on the first surface of the electromagnetic steel sheet 40 is approximately 3.2%.
[0149] The results are shown in Figure 20 . Figure 20 In the graph, the horizontal axis represents the bonding area ratio of the electromagnetic steel sheets 40 of the stator cores 21A to 21L. The vertical axis represents the iron loss suppression rate Rt, which is the value obtained by dividing the difference between the iron loss of each stator core 21A to 21L and the iron loss of the comparative stator core 21X by the iron loss of the comparative stator core 21X. That is, Figure 20 The iron loss suppression rate Rt on the vertical axis of the graph is expressed by the following equation (1) when the iron loss of each stator core 21A to 21L is represented by W and the iron loss of the comparative stator core 21X is represented by Worg.
[0150] [Formula 1]
[0151]
[0152] If the iron loss of the electromagnetic steel sheets 40 in each stator core 21A to 21L is equal to the iron loss in the comparative stator core 21X, the value on the vertical axis is 0%. A smaller iron loss suppression rate indicates a smaller iron loss, indicating better magnetic properties as a stator core.
[0153] according to Figure 20 The graph shown in FIG. 1 shows that by setting the bonding area ratio of the bonding portion 41 to the electromagnetic steel sheet 40 to 60% or less, the iron loss is reduced compared to the conventional comparative stator core 21X. Furthermore, by setting the bonding area ratio of the bonding portion 41 to the electromagnetic steel sheet 40 to 40% or less, the iron loss is improved by 3% or more compared to the conventional comparative stator core 21X. Furthermore, by setting the bonding area ratio of the bonding portion 41 to the electromagnetic steel sheet 40 to 20% or less, the iron loss is improved by 5% or more compared to the conventional comparative stator core 21X.
[0154] (Second verification test)
[0155] Next, the bonding strength of the electromagnetic steel sheets was verified when the bonding area ratio was changed.
[0156] First, core blocks were prepared, each consisting of a stack of electromagnetic steel sheets with a bonding area ratio of 0% (i.e., no bonding), a stack of electromagnetic steel sheets with a bonding area ratio of 0.5%, a stack of electromagnetic steel sheets with a bonding area ratio of 1%, and a stack of electromagnetic steel sheets with a bonding area ratio of 10%. Coils were then wound around the teeth of these core blocks to confirm successful winding. The results are shown in Table 1.
[0157] [Table 1]
[0158] Bonding area ratio Can winding be done 0% × 0.5% × 1% ○ 10% ○
[0159] In Table 1, "×" indicates that the core block collapsed due to the force applied to the core block during winding. Also, "○" indicates the end of winding. This verification confirmed that by setting the bonding area ratio of the electromagnetic steel sheet to 1% or more, the bonding strength required for winding can be ensured. Furthermore, the bonding strength of samples with bonding area ratios of 1% and 10% was confirmed, and the sample with a bonding area ratio of 10% was found to have higher strength. From the perspective of achieving sufficient bonding strength to prevent peeling of the bonded portion during dropping, it is preferable to set the bonding area ratio to 10% or more.
[0160] (3rd verification test)
[0161] This verification test is a verification test related to the width of each part of the adhesive portion. In addition, the simulation conditions and dimensional conditions are the same as those of the first verification test.
[0162] Figure 21 and Figure 22 The two types of stator cores 21M and 21N simulated in this verification test are shown. Figure 3 The stator core 21 of the illustrated embodiment has a basic structure.
[0163] Figure 21 The width of the second portion 44b and the fifth portion 45c of the bonding portion 41M of the stator core 21M shown is wider than the width of the other portions. Figure 22 The width of the fourth portion 45b of the bonding portion 41N of the stator core 21N shown is wider than the width of the other portions. Furthermore, the bonding portions 41N of the stator cores 21M and 21N have the same area. Therefore, the bonding strengths of the stator cores 21M and 21N are equal.
[0164] Simulations calculated the iron losses of stator cores 21M and 21N, revealing that the iron loss of stator core 21N is 98% of that of stator core 21M. This means that stator core 21N exhibits a 2% improvement in iron loss compared to stator core 21M. This is believed to be because the widths of second portion 44b and fifth portion 45c in stator core 21N are narrower than those of fourth portion 45b, allowing magnetic flux to flow more easily within stator core 21N.
[0165] Description of Reference Numerals
[0166] 10…Rotary motor
[0167] 21… stator core (laminated core)
[0168] 22…Core back
[0169] 23…teeth
[0170] 24, 124, 224, 324… iron core blocks
[0171] 40…Electromagnetic steel sheet
[0172] 41, 141, 241, 341…bonding part
[0173] 42, 142, 242…bonding area
[0174] 143, 243…non-adhesive area
[0175] 44a, 244a, 344a…Part 1
[0176] 44b, 344b…Part 2
[0177] 45a, 245a, 345a…Part 3
[0178] 45b, 245b, 345b…Part 4
[0179] 45c, 345c…Part 5
Claims
1. A core block is a core block formed by connecting a plurality of core blocks in a ring shape to form a laminated core, include: A plurality of electromagnetic steel sheets stacked on top of each other; as well as a bonding portion provided between the electromagnetic steel sheets adjacent to each other in the stacking direction and bonding the electromagnetic steel sheets to each other, The electromagnetic steel sheet has an arc-shaped core back and a tooth portion protruding from the core back toward one side in a radial direction of the core back. The bonding portion has: a pair of first portions extending along the peripheral edges of both sides of the tooth portion in the circumferential direction; a pair of third portions extending from a base end of the first portion to both sides in the circumferential direction along a peripheral edge of one side in the radial direction of the core back; and a fourth portion extending circumferentially along the peripheral edge of the other radial side of the core back, The bonding area ratio of the bonding portion to the electromagnetic steel sheet is 1% or more and 60% or less. A non-bonded region of the electromagnetic steel sheet where the bonding portion is not provided is formed between the bonding region of the electromagnetic steel sheet where the bonding portion is provided and the peripheral edge of the electromagnetic steel sheet.
2. The core block according to claim 1, in, The bonding area ratio is 1% or more and 20% or less.
3. The core block according to claim 1 or 2, in, The bonding portion has: a second portion extending along the periphery of the front end of the tooth portion and connecting the front ends of the pair of first portions; as well as A pair of fifth portions extending along the peripheral edges of both sides of the core back in the circumferential direction and respectively connecting the third portion and the fourth portion.
4. The core block according to claim 3, in, The widths of the second portion and the fifth portion are narrower than the width of the fourth portion.
5. The core block according to claim 1 or 2, in, The bonding portion is provided at least in a portion of a peripheral edge of the electromagnetic steel sheet.
6. The core block according to claim 1, in, The width of the non-bonded region is 1 to 10 times the thickness of the electromagnetic steel sheet.
7. The core block according to claim 1 or 2, in, In the electromagnetic steel sheet, non-bonding regions of the electromagnetic steel sheet where the bonding portion is not provided are formed at the front end of the tooth portion and at both ends in the circumferential direction of the core back.
8. The core block according to claim 1 or 2, in, An area where the bonding portion is bonded to the core back is larger than an area where the bonding portion is bonded to the teeth.
9. The core block according to claim 1 or 2, in, The average thickness of the adhesive portion is 1.0 μm to 3.0 μm.
10. The core block according to claim 1 or 2, in, The average tensile elastic modulus E of the bonding portion is 1500 MPa to 4500 MPa.
11. The core block according to claim 1 or 2, in, The adhesive portion is an acrylic adhesive of a room temperature adhesive type including SGA composed of an acrylic adhesive containing an elastomer. 12 . A laminated core, comprising a plurality of core blocks according to claim 1 connected in an annular shape.
13. A rotating electric machine comprising the laminated core according to claim 12.