An electromagnetically driven Fabry-Perot filter chip and its wafer-level manufacturing process

Through the electromagnetic driven Fabric filter chip and its wafer-level manufacturing process, the problems of limited tuning range and slow response speed of the MEMS Fabric filter chip are solved, and the efficient and fidelity production of large aperture chips is achieved, which is suitable for spectral imaging. and infrared monitoring and other fields.

CN114019673BActive Publication Date: 2024-10-11NINGBO INST OF NORTHWESTERN POLYTECHNICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111226876.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-21
Publication Date
2024-10-11
Estimated Expiration
2041-10-21

AI Technical Summary

Technical Problem

Existing MEMS Fabric filter chips have problems such as limited tuning range, slow response speed and low processing efficiency, which makes it especially difficult to achieve large-aperture and high-efficiency mass production.

Method used

Adopting electromagnetic driven Fapper filter chips and their wafer-level manufacturing process, bidirectional wide-width linear modulation is achieved through the interaction of electromagnetic drive coils and permanent magnets, and efficient integrated batch preparation of large-aperture chips is carried out through MEMS volume processing technology. .

Benefits of technology

It achieves bidirectional wide-width linear modulation with a large tuning range and fast response speed, overcomes the shortcomings of traditional driving methods, and improves processing efficiency and product fidelity. It is suitable for the production of high-quality large-aperture MEMS Fabric filter chips. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114019673B_ABST
    Figure CN114019673B_ABST
Patent Text Reader

Abstract

The present invention discloses an electromagnetically driven Fabry-Perot filter chip and its wafer-level manufacturing process, which belongs to the field of intelligent optoelectronic chips and semiconductors, and mainly involves technologies such as micro-electromechanical systems, micro-nano optics, and electromagnetic drive. The main structure of the chip includes a movable mirror body 1, a fixed mirror body 2, a movable reflector 3, a fixed reflector 4, a supporting film 5, a bonding layer 6, a permanent magnet 7, a spacer layer 8, a PCB drive / control circuit 9, and a packaging shell 10. The electromagnetically driven Fabry-Perot filter chip proposed in the present invention can realize bidirectional wide-band linear modulation, increase the tuning range of the Fabry-Perot filter chip, and overcome the shortcomings of other drive-type Fabry-Perot filter chips, such as limited modulation range, nonlinear drive, and slow response speed. The MEMS wafer-level body processing technology adopted can realize low-cost, high-fidelity, and high-efficiency processing of large-aperture Fabry-Perot filter chips. The electromagnetically driven Fabry-Perot filter chip and its wafer-level processing technology proposed in the present invention will promote the development and promotion of related practical application systems.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of intelligent optoelectronic chips, and in particular to an electromagnetically driven Fabry-Perot filter chip and a wafer-level manufacturing process thereof. Background Art

[0002] The Fabry-Perot filter is an optical device that uses the principle of multi-beam interference for interference filtering. It was first proposed by French physicists C.Fabry and A.Perot in 1897. Its basic structure consists of two flat plates with semi-transparent and semi-reflective mirrors, and a Fabry-Perot interference cavity of a specific length is formed between the two mirrors. When the incident light enters the Fabry-Perot cavity, if the length of the Fabry-Perot cavity is equal to an integer multiple of half the wavelength of the incident light, a stable resonance can be formed in the Fabry-Perot cavity, generating multi-beam interference and transmitting with higher energy, while the light waves of the remaining wavelengths gradually disappear in the Fabry-Perot cavity. By adjusting the length of the Fabry-Perot cavity, an adjustable filtering function can be achieved.

[0003] Traditional Perot etalons are difficult to achieve tunable filtering. The development of micro-electro-mechanical systems (MEMS) technology provides technical support for the realization of tunable Perot filters and their miniaturization, integration and chipization. MEMS Perot filter chips have broad application prospects in the fields of weapon guidance, wireless communication and remote sensing and telemetry. In 1987, Mallinson et al. first used MEMS technology to produce MEMS Perot filter chips for wavelength division multiplexing (Electronics Letters, vol.9, pp.1041-1043, 1987). The electrostatic drive method used is the most commonly used drive method for existing Perot filter chips. The electrostatic force between the two driving electrodes drives the movable mirror to move, thereby changing the length of the Perot cavity to achieve tunable filtering function. Electrostatically driven MEMS Perot filter chips can achieve fast response, but large-range adjustment requires a large voltage, so its driving range is limited, and there are disadvantages such as nonlinear response, "pull-down" effect and easy breakdown. In 1997, J.Peerlings et al. reported a heat-driven MEMS perturbation filter chip (IEEE Photon. Technol. Lett, vol.9, pp.1235-1237, 1997), which drives the movable mirror to move through the electrothermal effect of the thermal resistor. When the voltage is stopped, the heat gradually dissipates and the perturbation cavity is reset. The heat-driven MEMS perturbation filter chip requires a long time for heating and heat dissipation, so the response speed is slow and the power consumption is large. In 2013, the Finnish National Technical Research Center developed a MEMS perturbation filter chip using piezoelectric drive technology (Proc. SPIE, vol.8870, 887002, 2013). Its principle is to use the inverse piezoelectric effect of piezoelectric materials, apply voltage to the piezoelectric material to cause deformation, and change the length of the perturbation cavity to achieve spectral control. However, piezoelectric materials are difficult to process using MEMS processing technology, which affects the mass production and high-efficiency production of filter chips. With the development of spectral imaging, infrared monitoring and medical diagnosis, the requirements for imaging quality and spectral big data are getting higher and higher. Therefore, wide-amplitude modulation MEMS Fabry-Perot filter chips with large apertures have become a hot topic of research. At the same time, the rationality of the design of the MEMS processing method used will greatly affect the optical performance of the filter chip and the imaging performance of the system. Therefore, a rationally designed processing flow is crucial to obtain high-quality large-aperture MEMS Fabry-Perot filter chips.

[0004] The two commonly used processing technologies for existing MEMS Fabry-Perot filter chips are body processing technology and surface processing technology. Both technologies show different advantages and disadvantages in the processing process. Body processing technology usually uses two or more substrates to construct MEMS Fabry-Perot filter chips, and makes movable structures and optical structures respectively by etching and deposition, and uses bonding technology to form Fabry-Perot interference cavity. Body processing technology has high flexibility and is suitable for the production of large-aperture wide-band modulation MEMS Fabry-Perot filter chips. However, the quality of the movable structure of the MEMS Fabry-Perot filter chip produced by this technology cannot be ignored, so the acceleration sensitivity is high and it is easily disturbed by external forces. In 2003, NASA reported an electrostatically driven Fabry-Perot filter chip for infrared astronomical imaging produced by MEMS body processing technology (Proc. SPIE, vol. 4841, pp. 578-585, 2003). Its 11mm clear aperture is the largest among MEMS Fabry-Perot filters to date, but its use of monolithic bonding leads to low processing efficiency. Similarly, Infortech of Germany used MEMS bulk processing technology to produce an electrostatically driven Perot filter chip with a light aperture of 5 mm for the visible light band (Proc. SPIE, vol. 10931, 109310Q, 2019). The six-inch wafer-level processing technology it used greatly improved the processing efficiency, but the SU-8 bonding method it used resulted in a large initial Perot cavity length and multiple levels of interference filtering peaks in the working band. On the other hand, surface processing technology usually uses thin film deposition, photolithography, etching and sacrificial layer processes on a monolithic substrate to produce MEMS Perot filter chips. Compared with bulk processing technology, MEMS Perot filter chips made using surface technology have the advantages of low device acceleration sensitivity and high processing quality, but due to the presence of film stress, this process makes it difficult to process large-aperture MEMS Perot filter chips, and because the film will bend when a large driving force is applied, large-range modulation cannot be achieved. The Finnish National Technical Research Center reported a Fabry-Perot filter chip made by MEMS surface technology (Proc. SPIE, vol. 10545, 105450U, 2018). It uses a layer-by-layer thin film deposition method and corresponding sacrificial layer technology to obtain a single-order interference Fabry-Perot filter chip with good processing quality, but is subject to the influence of the surface technology itself, and its maximum aperture is only 4mm. In view of the problems existing in the above existing MEMS Fabry-Perot filter chips, the present invention proposes a wafer-level manufacturing process of a MEMS tunable Fabry-Perot filter chip using electromagnetic drive to achieve high-fidelity, high-efficiency and customizable preparation of the chip. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide an electromagnetically driven Fabry-Perot filter chip which can realize bidirectional wide-band linear modulation filtering and has a large tuning range and a fast response speed.

[0006] The technical solution adopted by the present invention is an electromagnetically driven Fabry-Perot filter chip, comprising a Fabry-Perot filter chip body, the Fabry-Perot filter chip body comprising a bare chip, the bare chip comprising a movable mirror body, a supporting film located on the movable mirror body, a movable reflector located on the supporting film, a fixed mirror body bonded to the movable mirror body through a bonding layer, and a fixed reflector arranged on the fixed mirror body and opposite to the movable reflector, a Fabry-Perot interference cavity is formed between the movable reflector and the fixed reflector, the Fabry-Perot filter chip body also comprises a spacing layer connected to the bare chip, a PCB drive / control circuit board and a packaging shell, the bare chip and the spacing layer are packaged on the PCB drive / control circuit board, the PCB drive / control circuit board comprises a control circuit and an electromagnetic drive coil, the movable mirror body comprises a cantilever beam, a permanent magnet slot opening toward the electromagnetic drive coil and a light through hole, and the bare chip also comprises a permanent magnet embedded in the permanent magnet slot.

[0007] The beneficial effects of the present invention are: the above-mentioned electromagnetically driven Fabry-Perot filter chip can realize bidirectional wide-band linear modulation and increase the tuning range of the Fabry-Perot filter chip, overcoming the shortcomings of the Fabry-Perot filter chip with other driving modes in the prior art, such as limited modulation range, nonlinear driving and slow response speed.

[0008] Preferably, the movable mirror body is made of materials using wafer-level MEMS body processing technology, and the cantilever beam, permanent magnet slot and light-through hole are made using an etching process.

[0009] Preferably, when the operating band of the Fabry-Perot filter chip body is ultraviolet, visible light and near-infrared, the fixed mirror body is made of glass or quartz; when the operating band of the Fabry-Perot filter chip body is infrared, the fixed mirror body is made of silicon, zinc sulfide, sapphire or gallium arsenide.

[0010] Preferably, the movable reflector and the fixed reflector are metal reflectors, or dielectric multilayer film reflectors, or photonic crystal reflectors with periodic micro-nano structures, all of which are manufactured using MEMS technology, and their reflectivity is customized according to the film thickness, or the number of layers or the characteristic size of the micro-nano structure.

[0011] Preferably, when the operating band of the Fabry-Perot filter chip body is the ultraviolet, visible light and near-infrared bands, the supporting film is a Si3N4 film, or a SiO2 film, or a combination of a Si3N4 film and a SiO2 film; when the operating band of the Fabry-Perot filter chip body is the infrared band, the supporting film is a ZnS film.

[0012] Preferably, the bonding layer is made of the first bonding layer and the second bonding layer through polymer bonding, or gold-silicon bonding, or gold-gold-bonding or silicon-glass bonding, and the thickness after bonding is d4, and satisfies the relationship: d4 = mλ m / 2+d1+d2+d3, where d1 is the thickness of the movable reflector, d2 is the thickness of the fixed reflector, d3 is the thickness of the supporting film, and λ m is the central wavelength of the Fabry-Perot filter chip, and m is the interference level.

[0013] Preferably, the permanent magnet is made of a magnetic material with uniform residual magnetic flux distribution.

[0014] A wafer-level manufacturing process for an electromagnetically driven Fabry-Perot filter chip, the process comprising the following steps:

[0015] Step 1: Select the first substrate as the movable mirror body, and clean and dry it;

[0016] Step 2: Make a supporting film on the upper surface of the movable mirror body, and the thickness of the supporting film is d3;

[0017] Step 3, making a movable reflector on the upper surface of the supporting film, the thickness of which is d1;

[0018] Step 4: making a first bonding layer on the upper surface of the movable mirror body;

[0019] Step 5: Etching is performed on the back of the movable mirror body to make a permanent magnet groove, and the etching depth is less than the thickness of the substrate;

[0020] Step 6: Make a cantilever beam and a light hole by carving from the back of the movable mirror body;

[0021] Step 7, selecting the second substrate as the fixed mirror body, and cleaning and drying it;

[0022] Step 8, making a fixed reflector on the fixed mirror body, the thickness of which is d2;

[0023] Step 9, making a second bonding layer on the fixed mirror body;

[0024] Step 10: Use polymer bonding, gold-silicon bonding, gold-gold bonding or silicon-glass bonding to bond the movable mirror body and the fixed mirror body through the first bonding layer and the second bonding layer. The thickness of the bonding layer after bonding is d4, and satisfies the relationship: d4 = mλ m / 2+d1+d2+d3, where d1 is the thickness of the movable reflector, d2 is the thickness of the fixed reflector, d3 is the thickness of the supporting film, and λ m is the central wavelength of the Fabry-Perot filter chip, and m is the interference level;

[0025] Step 11, dicing the bonded wafer-level movable mirror body and fixed mirror body to separate a plurality of individual chips;

[0026] Step 12: embedding permanent magnets into the permanent magnet slots of each individual chip to form a plurality of bare chips;

[0027] Step 13, aligning and packaging the bare chip and the spacer layer onto the PCB drive / control circuit board;

[0028] Step 14: Install the package shell on the PCB drive / control circuit board and put it on the outside of the bare chip and the spacer layer to complete the wafer-level production of the Fabry-Perot filter chip.

[0029] The above process uses MEMS bulk processing technology to carry out wafer-level integrated batch preparation of large-aperture electromagnetically driven Fabry-Perot filter chips, achieving low-cost, high-fidelity and high-efficiency processing of large-aperture Fabry-Perot filter chips.

[0030] The electromagnetically driven Fabry-Perot filter chip and wafer-level manufacturing process thereof proposed in the present invention will promote the development and promotion of relevant practical application systems. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 It is a structural schematic diagram of an electromagnetically driven Fabry-Perot filter chip of the present invention;

[0032] Figure 2 The diagram is a working principle diagram of an electromagnetically driven Fabry-Perot filter chip of the present invention; wherein, (b.2) is a state diagram of the movable mirror body in (a.2) after being driven by electromagnetic force;

[0033] Figure 3The flowchart of the wafer-level manufacturing process of an electromagnetically driven Fabry-Perot filter chip of the present invention; wherein (a) is a schematic diagram of the structure in which the first substrate is selected as the movable mirror body; (b) is a schematic diagram of the structure in which a supporting film is manufactured on the movable mirror body; (c) is a schematic diagram of the structure of making a movable reflector on a supporting film; (d) is a schematic diagram of the structure of making a first bonding layer on a movable mirror body; (e) is a schematic diagram of the structure of etching the back of the movable mirror body to make a permanent magnet groove; (f) is a schematic diagram of the structure of etching through the back of the movable mirror body to make a cantilever beam and a light hole; (g) is a schematic diagram of the structure of selecting a second substrate as a fixed mirror body; (h) is a schematic diagram of the structure of making a fixed reflector on a fixed mirror body; (i) is a schematic diagram of the structure of making a second bonding layer on a fixed mirror body; (j) is a schematic diagram of the structure after the movable mirror body and the fixed mirror body are bonded through the first bonding layer and the second bonding layer; (k) is a schematic diagram of the structure of embedding a permanent magnet into a permanent magnet groove to form a bare chip; (l) is a schematic diagram of the structure of aligning the bare chip and the spacer layer and packaging them on a PCB drive / control circuit board; (m) is a schematic diagram of the structure of installing the packaging shell on the bare chip.

[0034] As shown in the figure: 1. Movable mirror body; 2. Fixed mirror body; 3. Movable reflector; 4. Fixed reflector; 5. Support film; 6. Bonding layer; 7. Permanent magnet; 8. Spacer layer; 9. PCB drive / control circuit board; 10. Package shell; 101. Cantilever beam; 102. Permanent magnet slot; 103. Light hole; 601. First bonding layer; 602. Second bonding layer; 901. Control circuit; 902. Electromagnetic drive coil. DETAILED DESCRIPTION

[0035] The invention will be further described below with reference to the accompanying drawings and in combination with specific implementations, so that those skilled in the art can implement the invention with reference to the description. The protection scope of the invention is not limited to the specific implementations.

[0036] Those skilled in the art should understand that, in the disclosure of the present invention, the orientation or positional relationship indicated by terms such as "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" are based on the orientation or positional relationship shown in the accompanying drawings, which are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, the above terms should not be understood as limiting the present invention.

[0037] The existing MEMS Fabry-Perot filter chips have shortcomings such as nonlinear modulation, limited tuning range and small aperture. The present invention proposes a MEMS Fabry-Perot filter chip driven by electromagnetic force, which realizes bidirectional wide-band linear modulation filtering of the filter chip by adjusting the direction and size of the electromagnetic field. At the same time, in view of the shortcomings of the existing MEMS Fabry-Perot filter chip processing technology, such as poor processing quality, low efficiency and inability to adapt to large-aperture chip manufacturing, the present invention proposes a wafer-level process flow based on body processing technology to achieve high-fidelity, high-efficiency and customizable preparation of filter chips.

[0038] The present invention relates to an electromagnetically driven Fabry-Perot filter chip, comprising a Fabry-Perot filter chip body, the Fabry-Perot filter chip body comprising a bare chip, the bare chip comprising a movable mirror body 1, a supporting film 5 located on the movable mirror body 1, a movable reflector 3 located on the supporting film 5, a fixed mirror body 2 bonded to the movable mirror body 1 through a bonding layer 6, and a fixed reflector 4 arranged on the fixed mirror body 2 and opposite to the movable reflector 3, a Fabry-Perot interference cavity is formed between the movable reflector 3 and the fixed reflector 4, the Fabry-Perot filter chip body further comprises a spacing layer 8 connected to the bare chip, a PCB drive / control circuit board 9 and a packaging shell 10, the bare chip and the spacing layer 8 are packaged on the PCB drive / control circuit board 9, the PCB drive / control circuit board 9 comprises a control circuit 901 and an electromagnetic drive coil 902, the movable mirror body 1 comprises a cantilever beam 101, a permanent magnet slot 102 opening toward the electromagnetic drive coil 902 and a light through hole 103, and the bare chip further comprises a permanent magnet 7 embedded in the permanent magnet slot 102.

[0039] The working principle of the large-aperture electromagnetically driven Fabry-Perot filter chip proposed in the present invention is as follows: Figure 2 As shown, current is passed through the control circuit 901 in the PCB drive / control circuit board 9, and the electromagnetic drive coil 902 generates a magnetic field, which interacts with the magnetic field of the permanent magnet 7 to generate an electromagnetic force, thereby driving the movable mirror body 1 to move; by controlling the direction of the input current, the direction of the magnetic field generated by the electromagnetic drive coil 902 can be changed, and the electromagnetic drive coil 902 generates magnetic fields in different directions, which attract or repel the fixed magnetic field of the permanent magnet 7, thereby realizing bidirectional wide-band modulation of the Fabry-Perot filter chip; by linearly adjusting the magnitude of the drive current, according to the relationship that the magnitude of the Lorentz force is proportional to the magnitude of the current, a linear change of the electromagnetic force can be realized, and the driving range of the electromagnetic force can be controlled, thereby realizing precise and controllable linear modulation filtering of the Fabry-Perot filter chip; compared with other driving methods such as electrostatics and piezoelectrics, the advantage of electromagnetic drive is that it can be adjusted in both directions, and there is no electrostatic "pull-down" (electrostatic attraction), and its modulation range is large, so it is a wide-band modulation.

[0040] The electromagnetically driven Fabry-Perot filter chip of the present invention has the advantage of fast response speed. The fast response speed here is relative to piezoelectric drive and thermal drive. The piezoelectric drive changes the FP cavity length through the inverse piezoelectric effect of the material, which requires a certain response time; the thermal drive method uses heating and heat dissipation to change the FP cavity length, which requires a longer response time; and the electromagnetic drive generates an electromagnetic field through an energized coil, which instantly interacts with the magnetic field of the permanent magnet to generate an electromagnetic force to drive the Fabry-Perot filter chip, so the response speed is fast.

[0041] The movable mirror body 1 is made of materials using wafer-level MEMS body processing technology, which can be a silicon wafer or a glass wafer, etc. The cantilever beam 101, the permanent magnet slot 102 and the light hole 103 are made using an etching process, wherein the size of the light hole 103 determines the diameter of the light hole 103 of the Fabry-Perot filter chip body.

[0042] Figure 1 In the figure, the light hole 103 is mainly used to transmit light. After the incident light is filtered by the Fabry-Perot interference cavity, it is transmitted through the light hole 103. Assuming that the initial cavity length of the Fabry-Perot interference cavity is d0, the wavelength of the output light that can pass through the Fabry-Perot interference cavity is λ0, and the relationship satisfied by the two is: , where m is the interference level (m is a positive integer, m = 1, 2, 3 ...), and m = 1 used in the present invention, that is, the so-called first-level interference, then the relationship is obtained: We apply a certain current through electromagnetic drive to deform the cantilever beam 101 of the movable mirror body 1, change the length of the Fabry-Perot interference cavity, and change the wavelength of the transmitted light accordingly, thus achieving adjustable filtering.

[0043] The material of the fixed mirror body 2 has a high transmittance to light waves within the working band of the Fabry-Perot filter chip body. When the working band of the Fabry-Perot filter chip body is the ultraviolet, visible light and near-infrared bands, the fixed mirror body 2 is made of glass or quartz; when the working band of the Fabry-Perot filter chip body is the infrared band, the fixed mirror body 2 is made of silicon, zinc sulfide, sapphire, or gallium arsenide.

[0044] The movable reflector 3 and the fixed reflector 4 are metal reflectors, or dielectric multilayer film reflectors, or photonic crystal reflectors with periodic micro-nano structures, which are all made by MEMS technology, and their reflectivity is customized according to the film thickness, or the number of layers or the characteristic size of the micro-nano structure; by customizing the appropriate mirror reflectivity, the chip filtering performance can be customized.

[0045] The supporting film 5 is a single-layer or multi-layer dielectric film, and has a high transmittance to light waves within the working band of the Fabry-Perot filter chip in the present invention. When the working band of the Fabry-Perot filter chip body is the ultraviolet, visible light and near-infrared bands, the supporting film 5 is a Si3N4 film, or a SiO2 film, or a combination of Si3N4 film and SiO2 film; when the working band of the Fabry-Perot filter chip body is the infrared band, the supporting film 5 is a ZnS film; the supporting film 5 is prepared on the movable mirror body 11 by MEMS technology, and mainly plays the role of supporting the movable reflecting mirror 33.

[0046] The bonding layer 6 is made of the first bonding layer 601 and the second bonding layer 602 by polymer bonding, or gold-silicon bonding, or gold-gold bonding, or silicon-glass bonding, and the thickness after bonding is d4, and satisfies the relationship: d4 = mλ m / 2+d1+d2+d3, wherein d1 is the thickness of the movable reflector 3, d2 is the thickness of the fixed reflector 4, d3 is the thickness of the supporting film 5, λm is the central wavelength of the Fabry-Perot filter chip body, and m is the interference level.

[0047] The permanent magnet 7 is made of a magnetic material with uniform residual magnetic flux distribution, and its inner and outer diameters are the same as those of the permanent magnet slot 102 . The permanent magnet 7 is assembled into the permanent magnet slot 102 in an embedded manner.

[0048] The spacing layer 8 is a high-precision gasket, which is encapsulated between the movable mirror body 1 and the PCB drive / control circuit board 9 and is mainly used to accurately control the distance between the permanent magnet 7 and the PCB drive / control circuit board 9.

[0049] The PCB drive / control circuit board 9 is manufactured using printed circuit board technology, and contains a control circuit 901 therein for applying current or voltage to the electromagnetic drive coil 902 ; the electromagnetic drive coil 902 contained therein is used to generate an electromagnetic field to drive the permanent magnet 7 to move.

[0050] The packaging shell 10 is mainly used to protect and fix the chip, and can be made of polymer or metal material.

[0051] In order to realize the high-fidelity, high-efficiency and customizable preparation of the proposed electromagnetically driven Fabry-Perot filter chip, the present invention also proposes a wafer-level manufacturing process of the electromagnetically driven Fabry-Perot filter chip, which includes the following steps:

[0052] Step 1: Figure 3 (a) Selecting a first substrate with high flatness, which may be a silicon wafer or a glass wafer, for making the movable mirror body 1, and cleaning and drying the first substrate;

[0053] Step 2: Figure 3(b) A supporting film 5 is made on the surface of the movable mirror body 1, and its thickness is d3. Its material needs to have a high transmittance to the light waves in the working band of the Fabry filter chip in the present invention. When the working band of the filter chip is the ultraviolet, visible light and near infrared bands, Si3N4 film, SiO2 film or a combination of the two is used; when the working band of the filter chip is the infrared band, ZnS film is used; it is prepared on the movable mirror body 1 by MEMS technology, and mainly plays the role of supporting the movable reflector 3;

[0054] Step 3: Figure 3 (c) A movable reflector 3 is fabricated on the supporting film 5, which may be a metal reflector, a dielectric multilayer reflector, or a photonic crystal reflector with a periodic micro-nano structure, and has a thickness of d1. The reflector is fabricated by MEMS technology, and its reflectivity can be customized according to the film thickness, the number of layers, or the characteristic size of the micro-nano structure;

[0055] Step 4: Figure 3 (d) forming a first bonding layer 601 on the movable mirror body 1, wherein the material of the first bonding layer 601 is a patternable polymer, a gold film, a silicon film, a SiO2 film, etc.;

[0056] Step 5: Figure 3 (e) etching the corresponding area on the back of the movable mirror body 1 to form the permanent magnet slot 102, wherein the etching depth is less than the thickness of the substrate. The corresponding area here refers to the area where the structure needs to be etched. Before etching, the size and shape of the etching area are limited by patterning by photolithography;

[0057] Step 6: Figure 3 (f) Carve through the corresponding area of ​​the movable mirror body 1 from the back of the movable mirror body 1 to make the cantilever beam 101 and the light-through hole 103, and complete the production of the movable mirror body 1. The corresponding area here refers to the area that needs to be carved through;

[0058] Step 7: Figure 3 (g) Selecting a second substrate with high flatness for making the fixed mirror body 2, the material of which needs to have high transmittance to light waves within the working band of the filter chip. When the working band of the filter chip is the ultraviolet, visible and near-infrared bands, the substrate can be glass or quartz; when the working band of the filter chip is the infrared band, the substrate can be silicon, zinc sulfide, sapphire, gallium arsenide and the like. Cleaning and drying the fixed mirror body 2;

[0059] Step 8: Figure 3 (h) A fixed reflector 4 is manufactured on the fixed mirror body 2, and the thickness of the fixed reflector 4 is d2. The fixed reflector 4 may be a metal reflector, a dielectric multilayer reflector, or a photonic crystal reflector with a periodic micro-nano structure, and the reflectivity of the fixed reflector may be customized according to the thickness of the film layer, the number of layers, or the characteristic size of the micro-nano structure.

[0060] Step 9: Figure 3 (i) A second bonding layer 602 is fabricated on the fixed mirror body 2. The material of the second bonding layer 602 may be a patternable polymer, a gold film, a silicon film or a SiO2 film. The second bonding layer 602 is bonded to the first bonding layer 601 to complete the fabrication of the fixed mirror body 2.

[0061] Step 10: Figure 3 (j) The movable mirror body 1 and the fixed mirror body 2 are bonded through the first bonding layer 601 and the second bonding layer 602 by using polymer bonding, gold-silicon bonding, gold-gold bonding or silicon-glass bonding technology. The thickness of the bonding layer after bonding is d4. The thickness d4 after bonding mainly depends on the central wavelength λm and interference level m of the Fabry-Perot filter chip, the thickness d1 of the movable reflector 3, the thickness d2 of the fixed reflector 4 and the thickness d3 of the supporting film 5, and satisfies the relationship: d4=mλ m / 2+d1+d2+d3;

[0062] Step 11, dicing the bonded wafer-level movable mirror body 1 and fixed mirror body 2 to separate a plurality of individual chips;

[0063] Step 12: Figure 3 (k) The permanent magnets 7 are respectively embedded into the permanent magnet slots 102 of each individual chip to form a plurality of bare chips. Figure 3 (k) shows a schematic diagram of the structure of a bare chip;

[0064] Step 13: Figure 3 (1) Encapsulating the bare chip and the spacer layer 8 on the PCB drive / control circuit board 9 in an aligned manner;

[0065] Step 14: Figure 3 (m) The packaging shell 10 is installed on the PCB drive / control circuit board 9 and is sleeved on the outside of the bare chip and the spacer layer 8 to complete the wafer-level production of the Fabry-Perot filter chip.

[0066] The above process uses MEMS bulk processing technology to carry out wafer-level integrated batch preparation of large-aperture electromagnetically driven Fabry-Perot filter chips, achieving low-cost, high-fidelity and high-efficiency processing of large-aperture Fabry-Perot filter chips.

[0067] The above-mentioned processing technology flow has high compatibility, and the processing step sequence and process steps can be adjusted according to the actual processing conditions. Adjusting the process sequence and adding process steps based on the chip processing technology flow of the present invention are all within the protection scope of the present invention.

[0068] Embodiment 1:

[0069] The present invention relates to an electromagnetically driven Fabry-Perot filter chip, comprising a Fabry-Perot filter chip body, the Fabry-Perot filter chip body comprising a bare chip, the bare chip comprising a movable mirror body 1, a supporting film 5 located on the movable mirror body 1, a movable reflector 3 located on the supporting film 5, a fixed mirror body 2 bonded to the movable mirror body 1 through a bonding layer 6, and a fixed reflector 4 arranged on the fixed mirror body 2 and opposite to the movable reflector 3, a Fabry-Perot interference cavity is formed between the movable reflector 3 and the fixed reflector 4, the Fabry-Perot filter chip body further comprises a spacing layer 8 connected to the bare chip, a PCB drive / control circuit board 9 and a packaging shell 10, the bare chip The sheet and the spacer layer 8 are packaged on a PCB drive / control circuit board 9, the PCB drive / control circuit board 9 includes a control circuit 901 and an electromagnetic drive coil 902, the movable mirror body 1 includes a cantilever beam 101, a permanent magnet slot 102 with an opening toward the electromagnetic drive coil 902, and a light hole 103, the bare chip also includes a permanent magnet 7 embedded in the permanent magnet slot 102, the working band of the Fabry-Perot filter chip body adopts the visible light band, the diameter of the light hole 103 is 6mm, the central wavelength λm of the working band is designed to be 600nm, and the first-order interference filter peak (m=1) is adopted, so the initial Fabry-Perot cavity length is designed to be 300nm;

[0070] The movable mirror body 1 is made of a 500μm thick four-inch double-polished silicon wafer. The cantilever beam 101, the permanent magnet slot 102 and the through hole 103 are made by deep reactive ion etching. The etching depth of the permanent magnet slot 102 is 300μm. The inner diameter and outer diameter of the permanent magnet slot 102 are 7mm and 9mm respectively. The diameter of the through hole 103103 is 6mm.

[0071] The fixed mirror body 2 is made of 4-inch double-polished BF33 glass with a thickness of 500 μm, and its transmittance to visible light can reach more than 90%;

[0072] The movable reflector 3 and the fixed reflector 4 are made of silver reflectors with the same thickness, that is, the thickness d1 = d2 = 40 nm, and are made by electron beam evaporation;

[0073] The supporting film 5 is made of Si3N4 film with a thickness of d3 = 600nm, which is produced by chemical vapor deposition and mainly plays the role of supporting the movable reflector 3;

[0074] The bonding layer is made of silicon-glass bonding, wherein the first bonding layer 601 is a SiO2 thin film, which is made by electron beam evaporation combined with photolithography and etching processes; the second bonding layer 602 is a silicon thin film, which is made by electron beam evaporation combined with photolithography and etching processes; according to the design of the Fabry filter chip, the central wavelength λm=600nm, the working level is the first level (m=1), the thickness of the movable reflector 3 and the fixed reflector 4 are both 40nm, and the thickness d3 of the supporting film 5 is 600nm, and finally the final thickness d4 of the bonding layer after bonding is calculated to be 980nm;

[0075] The permanent magnet 7 is made of sintered NdFeB material, with a grade of N45, and has the following dimensions: inner diameter × outer diameter × thickness = 7 mm × 9 mm × 0.5 mm, and is assembled into the permanent magnet slot 102 in an embedded manner;

[0076] The spacer layer 8 is a gasket with a thickness of 1 mm, made of ABS, produced by 3D printing, and encapsulated between the movable mirror body 1 and the PCB drive / control circuit board 9, and is mainly used to accurately control the distance between the permanent magnet 7 and the PCB drive / control circuit board 9;

[0077] The PCB driving / controlling circuit board 9 is an 8-layer printed circuit board with an internal copper line width of 0.25 mm, which contains a control circuit for applying current and precise linear control to the electromagnetic driving coil 902, thereby generating an electromagnetic field to drive the permanent magnet 7 to move;

[0078] The packaging shell 10 is a 3D printed shell made of ABS and is mainly used to protect and fix the chip.

[0079] In this embodiment, according to the design parameters and working requirements of the above chip, the wafer-level MEMS body processing process flow of the wafer-level electromagnetic driven Fabry-Perot filter chip is customized as follows: Figure 3 As shown in , it mainly includes the following steps:

[0080] Step 1: Figure 3 In (a), a four-inch double-polished silicon wafer with a thickness of 500 μm and high flatness is selected for processing the movable mirror body 1, and the silicon wafer is cleaned with deionized water, a hydrofluoric acid solution is used to remove the oxide layer on the surface of the silicon wafer, and then it is blown dry with nitrogen;

[0081] Step 2: Figure 3 In (b), a Si3N4 film with a thickness of d3 = 600 nm is formed on the surface of a silicon wafer by low pressure chemical vapor deposition, the Si3N4 film is photolithographically etched, and the Si3N4 film is etched by HF wet etching process to form a supporting film 5 for supporting the movable reflector 3;

[0082] Step 3: Figure 3In (c), photolithography is performed on the silicon wafer on which the Si3N4 support film 5 is made, and a silver film with a thickness of d1=40 nm is evaporated on the support film 5 by electron beam evaporation, and then the photoresist is dissolved and stripped in an acetone solution to complete the production of the movable reflector 3;

[0083] Step 4: Figure 3 In (d), a 500 nm thick SiO2 film is deposited on the silicon wafer on which the support film 5 and the movable reflector 3 are made by electron beam evaporation, and the SiO2 film is photoetched and patterned by plasma etching to complete the production of the first bonding layer 601;

[0084] Step 5: Figure 3 In (e), photolithography is performed on the back of the silicon wafer, and a deep reactive ion etching method is used to etch 300 μm to produce a permanent magnet slot 102 with an outer diameter of 9 mm and an inner diameter of 7 mm;

[0085] Step 6: Figure 3 In (f), a photoresist with a thickness of more than 10 μm is sprayed on the back of the silicon wafer, and photolithography is performed. The silicon wafer is etched through by deep reactive ion etching to produce the cantilever beam 101 and the light-through hole 103, thereby completing the production of the movable mirror body 1;

[0086] Step 7: Figure 3 In (g), a four-inch BF33 glass substrate with a thickness of 500 μm and high flatness is selected to make the fixed mirror body 2, and the surface of the BF33 glass is cleaned with acetone and deionized water and dried;

[0087] Step 8: Figure 3 In (h), a silver film with a thickness of d2 = 40 nm is deposited by photolithography on a BF33 substrate using electron beam evaporation, and then melted and peeled off in an acetone solution to complete the production of a fixed reflector 4;

[0088] Step 9: Figure 3 (i) Depositing a 480 nm silicon film on a BF33 substrate by electron beam evaporation, photolithography on the silicon film, and then removing excess silicon film by deep reactive ion etching to complete the production of the second bonding layer 602 and the fixed mirror body 2;

[0089] Step 10: Figure 3 In (j), the finished movable mirror body 1 and the fixed mirror body 2 are bonded at the wafer level by using a silicon-glass bonding process, and the first bonding layer 601 and the second bonding layer 602 form a bonding layer under the action of an electric field and heat pressure, and the final thickness d4=980nm;

[0090] Step 11: Use a dicing machine to diced the bonded movable mirror body 1 and the fixed mirror body 2 to separate individual chips;

[0091] Step 12: Figure 3 In (k), the permanent magnet 7 is embedded in the permanent magnet slot 102 by bonding to form a single bare chip;

[0092] Step 13: Figure 3 In (l), the bare chip and the spacer layer 8 are packaged on the PCB drive / control circuit board 9 in a centering manner, and the final distance between the permanent magnet 7 and the PCB drive / control circuit board 9 is 0.8 mm;

[0093] Step 14: Figure 3 In (m), the package shell 10 is bonded and mounted on the bare chip to protect the chip.

[0094] The above process uses MEMS bulk processing technology to carry out wafer-level integrated batch preparation of large-aperture electromagnetically driven Fabry-Perot filter chips, achieving low-cost, high-fidelity and high-efficiency processing of large-aperture Fabry-Perot filter chips.

[0095] The above-mentioned processing technology flow has high compatibility, and the processing step sequence and process steps can be adjusted according to the actual processing conditions. Adjusting the process sequence and adding process steps based on the chip processing technology flow of the present invention are all within the protection scope of the present invention.

[0096] Embodiment 2:

[0097] The present invention relates to an electromagnetically driven Fabry-Perot filter chip, comprising a Fabry-Perot filter chip body, the Fabry-Perot filter chip body comprising a bare chip, the bare chip comprising a movable mirror body 1, a supporting film 5 located on the movable mirror body 1, a movable reflector 3 located on the supporting film 5, a fixed mirror body 2 bonded to the movable mirror body 1 through a bonding layer 6, and a fixed reflector 4 arranged on the fixed mirror body 2 and opposite to the movable reflector 3, a Fabry-Perot interference cavity is formed between the movable reflector 3 and the fixed reflector 4, the Fabry-Perot filter chip body further comprises a spacing layer 8 connected to the bare chip, a PCB drive / control circuit board 9 and a packaging shell 10, the bare chip and the spacing layer 8 is packaged on a PCB drive / control circuit board 9, wherein the PCB drive / control circuit board 9 includes a control circuit 901 and an electromagnetic drive coil 902, the movable mirror body 1 includes a cantilever beam 101, a permanent magnet slot 102 with an opening toward the electromagnetic drive coil 902, and a light hole 103, the bare chip also includes a permanent magnet 7 embedded in the permanent magnet slot 102, the working band of the Fabry-Perot filter chip body adopts a long infrared band of 8 to 12 μm, the diameter of the light hole 103 is 10 mm, the central wavelength λm of the working band is designed to be 10 μm, and the first-order interference filter peak value (m=1) is adopted, so the cavity length of the initial Fabry-Perot interference cavity is designed to be 5 μm.

[0098] The movable mirror body 1 is made of a 500μm thick four-inch double-polished zone melting silicon wafer substrate. The cantilever beam 101, the permanent magnet slot 102 and the through hole 103 are made by deep reactive ion etching. The etching depth of the permanent magnet slot 102 is 300μm, the inner diameter and outer diameter of the slot are 11mm and 13mm respectively, and the diameter of the through hole 103 is 10mm.

[0099] The fixed mirror body 2 is made of a four-inch double-polished zinc sulfide substrate with a thickness of 1000 μm, and its transmittance in the long infrared band of 8 to 12 μm can reach about 75%;

[0100] The movable reflector 3 and the fixed reflector 4 are 5-layer Ge / ZnS film distributed Bragg reflectors, which are made by electron beam evaporation, with a refractive index ratio of Ge:ZnS=4:2.2, a single layer of Ge thickness of 625nm, and a single layer of ZnS thickness of 1136nm. Therefore, the thickness of the movable reflector 3 and the fixed reflector 4 is d1=d2=4.147μm;

[0101] The supporting film 5 is a ZnS film with a thickness of 1136 nm, which is made by thermal evaporation and mainly plays the role of supporting the movable reflector 3;

[0102] The bonding layer is made by gold-silicon bonding, the first bonding layer 601 is a gold film, and the second bonding layer 602 is a silicon film, both of which are made by photolithography process; according to the filter chip design center wavelength λm=10μm, working level m=1, the thickness of the movable reflector 3 and the fixed reflector 4 is d1=d2=4.147μm, and the thickness of the supporting film 5 is d3=1136nm, and finally the final thickness of the bonding layer after bonding is calculated to be d4=14.43μm;

[0103] The permanent magnet 7 is made of sintered NdFeB material, with a grade of N45, and has the following dimensions: inner diameter × outer diameter × thickness = 11 mm × 13 mm × 0.5 mm. It is assembled into the permanent magnet slot 102 in an embedded manner, and the matching relationship with the permanent magnet slot 102 is a clearance fit.

[0104] The spacer layer 8 is a gasket with a thickness of 1 mm, made of ABS, produced by 3D printing, and encapsulated between the movable mirror body 1 and the PCB drive / control circuit board 9, and is mainly used to accurately control the distance between the permanent magnet 7 and the PCB drive / control circuit board 9;

[0105] The PCB drive / control circuit board 9 is a 16-layer printed circuit board with an internal copper line width of 0.3 mm. It contains a control circuit for applying current and precise linear control to the electromagnetic drive coil 902, thereby generating an electromagnetic field to drive the permanent magnet 7 to move;

[0106] The packaging shell 10 is a 3D printed shell made of ABS and is mainly used to protect and fix the chip.

[0107] In this embodiment, according to the design parameters and working requirements of the above chip, the wafer-level MEMS body processing process flow of the wafer-level electromagnetic driven Fabry-Perot filter chip is customized as follows: Figure 3 As shown in , it mainly includes the following steps:

[0108] Step 1: Figure 3 In (a), a four-inch double-polished zone melting silicon wafer with a thickness of 500 μm and high flatness is selected for processing the movable mirror body 1. The silicon wafer is cleaned with deionized water, the surface oxide layer of the silicon wafer is removed with a hydrofluoric acid solution, and then dried with nitrogen gas;

[0109] Step 2: Figure 3 In (b), a ZnS film with a thickness of d3 = 1136 nm is formed on the surface of the silicon wafer by photolithography on a zone melting silicon substrate and electron beam evaporation is used. The silicon substrate with the ZnS film deposited is immersed in acetone for 24 hours for dissolution and peeling to form a supporting film 5 for supporting the movable reflector 3;

[0110] Step 3: Figure 3 In (c), five layers of distributed Bragg reflectors with a thickness of Ge / ZnS / Ge / ZnS / Ge=625nm / 1136nm / 625nm / 1136nm / 625nm are sequentially deposited by photolithography on the silicon wafer with the ZnS support film 5 by electron beam evaporation, and then the photoresist is melted and stripped off in an acetone solution to complete the production of the movable reflector 3, with a total thickness of d1=4.147μm;

[0111] Step 4: Figure 3 In (d), electron beam evaporation is used to perform photolithography on the substrate on which the support film 5 and the movable reflector 3 are made, and then a gold film with a thickness of 2.5 μm is deposited by magnetron sputtering, and then immersed in an acetone solution for 24 hours for dissolution and stripping, thereby completing the production of the first bonding layer 601;

[0112] Step 5: Figure 3 In (e), photolithography is performed on the back of the silicon wafer, and a deep reactive ion etching method is used to etch 300 μm to produce a permanent magnet slot 102 with an outer diameter of 13 mm and an inner diameter of 11 mm;

[0113] Step 6: Figure 3 In (f), a photoresist with a thickness of more than 10 μm is sprayed on the back of the silicon wafer, and the silicon wafer is etched through by deep reactive ion etching to produce the cantilever beam 101 and the light-through holes 103103, thereby completing the production of the movable mirror body 1;

[0114] Step 7: Figure 3In (g), a four-inch zinc sulfide substrate with a thickness of 500 μm and high flatness is selected to fix the mirror body 2, and the surface of the zinc sulfide substrate is cleaned with acetone and deionized water and dried;

[0115] Step 8: Figure 3 In (h), five layers of distributed Bragg reflectors with thicknesses of Ge / ZnS / Ge / ZnS / Ge=625nm / 1136nm / 625nm / 1136nm / 625nm are sequentially deposited by photolithography on a zinc sulfide substrate using electron beam evaporation, and then placed in an acetone solution to melt and strip the photoresist, thereby completing the manufacture of a fixed reflector 4 with a total thickness of d2=4.147μm;

[0116] Step 9: Figure 3 In (i), a silicon film with a thickness of 14 μm is deposited on a ZnS substrate by plasma chemical vapor deposition, and photolithography is performed on the silicon film. The excess silicon film is removed by deep reactive ion etching to complete the production of the second bonding layer 602 and the fixed mirror body 2;

[0117] Step 10: Figure 3 In (j), the finished movable mirror body 1 and the fixed mirror body 2 are bonded at the wafer level by using a gold-silicon bonding process, and the first bonding layer 601 and the second bonding layer 602 are formed into a bonding layer 6 under the action of hot pressing, and the final thickness d4=14.43 μm;

[0118] Step 11: Use a dicing machine to diced the bonded movable mirror body 1 and the fixed mirror body 2 to separate individual chips;

[0119] Step 12: Figure 3 In (k), the permanent magnet 7 is embedded in the permanent magnet slot 102 to obtain a bare chip;

[0120] Step 13: Figure 3 In (l), the bare chip and the spacer layer 8 are packaged on the PCB drive / control circuit board 9 in a centering manner, and the final distance between the permanent magnet 7 and the PCB drive / control circuit board 9 is 0.8 mm;

[0121] Step 14: Figure 3 In (m), the package shell 10 is bonded and mounted on the chip to protect the chip.

[0122] The above process uses MEMS bulk processing technology to carry out wafer-level integrated batch preparation of large-aperture electromagnetically driven Fabry-Perot filter chips, achieving low-cost, high-fidelity and high-efficiency processing of large-aperture Fabry-Perot filter chips.

[0123] The above-mentioned processing technology flow has high compatibility, and the processing step sequence and process steps can be adjusted according to the actual processing conditions. Adjusting the process sequence and adding process steps based on the chip processing technology flow of the present invention are all within the protection scope of the present invention.

Claims

1. An electromagnetically driven Fabry-Perot filter chip, comprising a Fabry-Perot filter chip body, characterized in that: The Fabry-Perot filter chip body comprises a bare chip, the bare chip comprises a movable mirror body (1), a supporting film (5) located on the movable mirror body (1), a movable reflector (3) located on the supporting film (5), a fixed mirror body (2) bonded to the movable mirror body (1) via a bonding layer (6), and a fixed reflector (4) arranged on the fixed mirror body (2) and opposite to the movable reflector (3), a Fabry-Perot interference cavity is formed between the movable reflector (3) and the fixed reflector (4), the Fabry-Perot filter chip body also comprises a spacer layer (8) connected to the bare chip, a PCB drive / control circuit board (9) and a packaging shell (10), the bare chip and the spacer layer (8) are packaged on the PCB drive / control circuit board (9), the spacing layer is a gasket, which is packaged between the movable mirror body and the control circuit board; the PCB drive / control circuit board (9) includes a control circuit (901) and an electromagnetic drive coil (902), the movable mirror body (1) includes a cantilever beam (101), a permanent magnet slot (102) opening toward the electromagnetic drive coil (902) and a light hole (103), and the bare chip also includes a permanent magnet (7) embedded in the permanent magnet slot (102); the bonding layer (6) is made of a first bonding layer (601) and a second bonding layer (602) through polymer bonding, or gold-silicon bonding, or gold-gold bonding or silicon-glass bonding, and its thickness after bonding is d4, and satisfies the relationship: d4=mλ m / 2+d1+d2+d3, wherein d1 is the thickness of the movable reflector (3), d2 is the thickness of the fixed reflector, d3 is the thickness of the supporting film (5), λm is the central wavelength of the Fabry-Perot filter chip body, and m is the interference level.

2. The electromagnetic driven Fabry-Perot filter chip according to claim 1, characterized in that: The movable mirror body (1) is made of materials using wafer-level MEMS body processing technology, and the cantilever beam (101), the permanent magnet slot (102) and the light-through hole (103) are made using an etching process.

3. The electromagnetic driven Fabry-Perot filter chip according to claim 1, characterized in that: When the working band of the Fabry-Perot filter chip body is the ultraviolet, visible light and near-infrared bands, the fixed mirror body (2) is made of glass or quartz; when the working band of the Fabry-Perot filter chip body is the infrared band, the fixed mirror body (2) is made of silicon, zinc sulfide, sapphire or gallium arsenide.

4. The electromagnetic driven Fabry-Perot filter chip according to claim 1, 2 or 3, characterized in that: The movable reflector (3) and the fixed reflector (4) are both made of metal reflectors, or dielectric multilayer film reflectors, or photonic crystal reflectors with periodic micro-nano structures, which are all manufactured through MEMS technology. The reflectivities of the movable reflector (3) and the fixed reflector (4) are customized according to the film thickness, or the number of layers, or the characteristic size of the micro-nano structure.

5. The electromagnetic driven Fabry-Perot filter chip according to claim 1, characterized in that: When the operating band of the Fabry-Perot filter chip body is the ultraviolet, visible and near infrared bands, the supporting film (5) is a Si3N4 film, or a SiO2 film, or a combination of a Si3N4 film and a SiO2 film; when the operating band of the Fabry-Perot filter chip body is the infrared band, the supporting film (5) is a ZnS film.

6. The electromagnetic driven Fabry-Perot filter chip according to claim 1, characterized in that: The permanent magnet (7) is made of a magnetic material with uniform residual magnetic flux distribution.

7. A wafer-level manufacturing process for manufacturing the electromagnetically driven Fabry-Perot filter chip as described in any one of claims 1 to 6, the process comprising the following steps: Step 1, selecting a first substrate as a movable mirror body (1), and cleaning and drying the substrate; Step 2: Making a supporting film (5) on the upper surface of the movable mirror body (1), the thickness of which is d3; Step 3, making a movable reflector (3) on the upper surface of the supporting film (5), the thickness of which is d1; Step 4: making a first bonding layer (601) on the upper surface of the movable mirror body (1); Step 5, etching is performed on the back of the movable mirror body (1) to form a permanent magnet groove (102), wherein the etching depth is less than the thickness of the substrate; Step 6: Making a cantilever beam (101) and a light hole (103) by engraving from the back of the movable mirror body (1); Step 7, selecting a second substrate as the fixed mirror body (2), and cleaning and drying the second substrate; Step 8, making a fixed reflector (4) on the fixed mirror body (2), the thickness of which is d2; Step 9, making a second bonding layer (602) on the fixed mirror body (2); Step 10: Using polymer bonding, gold-silicon bonding, gold-gold bonding or silicon-glass bonding technology, the movable mirror body (1) and the fixed mirror body (2) are bonded through the first bonding layer (601) and the second bonding layer (602). After bonding, the thickness of the bonding layer (6) is d4, and the relationship is satisfied: d4 = mλ m / 2+d1+d2+d3, wherein d1 is the thickness of the movable reflector (3), d2 is the thickness of the fixed reflector, d3 is the thickness of the supporting film (5), λm is the central wavelength of the Fabry-Perot filter chip body, and m is the interference level; Step 11, dicing the bonded wafer-level movable mirror body (1) and the fixed mirror body (2) to separate a plurality of individual chips; Step 12: embedding the permanent magnets (7) into the permanent magnet slots (102) of each individual chip to form a plurality of bare chips; Step 13, aligning and packaging the bare chip and the spacer layer (8) onto a PCB drive / control circuit board (9); Step 14: Install the packaging shell (10) on the PCB drive / control circuit board (9), and cover the outside of the bare chip and the spacer layer (8), so as to complete the wafer-level production of the Fabry-Perot filter chip.