Methacrylic acid melt extrusion molded product
By using high-content methyl methacrylate units and multi-layer polymer structures in methacrylic melt extruded molded bodies, combined with spherical or columnar phase distribution of block copolymers, the cracking and excellent performance of molded bodies are solved. The problems of both considerations have been taken into account, and multiple excellent properties such as transparency, smoothness and bending resistance are achieved.
Patent Information
- Application Number
- CN202080045961.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-25
- Filing Date
- 2020-07-22
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2040-07-22
AI Technical Summary
The prior art is difficult to suppress the cracking of the methacrylic resin molded body while maintaining a high surface hardness, and achieve film properties with excellent transparency, surface smoothness, bending resistance and pencil hardness.
Methacrylic melt extrusion molded body, which contains more than 80% of methyl methacrylate units, acrylic multilayer polymer has rubber component layers and thermoplastic resin component layers, and controls the structure of block copolymer and The particle size is distributed to form spherical or columnar phases to improve the transparency and stress-resistant whitening properties of the molded body.
It achieves excellent performances of transparency, surface smoothness, bending resistance and pencil hardness, and is suitable for decoration and building materials.
Smart Images

Figure CN114026171B_ABST
Abstract
Description
Technical Field
[0001] [Cross-reference to related applications]
[0002] This application claims priority based on Japanese Patent Application No. 2019-137232 filed on July 25, 2019, and Japanese Patent Application No. 2019-173842 filed on September 25, 2019 (these disclosures are incorporated herein by reference in their entirety).
[0003] The present invention relates to a methacrylic acid melt-extruded molded product. More specifically, the present invention relates to a methacrylic acid melt-extruded molded product which is excellent in transparency, surface smoothness, resistance to whitening on bending, pencil hardness, bendability, moldability and appearance after molding and is suitable for decorative purposes and building material applications. Background Art
[0004] Methacrylic resin molded bodies have excellent optical properties such as transparency and weather resistance, and the molded bodies have beautiful appearances, etc., and therefore are gradually used in decorative applications such as automotive interior and exterior decoration and building materials. For the purpose of protecting decorative layers such as printed layers and imparting design features such as a sense of luxury and depth, methacrylic resin films with excellent weather resistance, transparency, pencil hardness and surface smoothness have been used as surface protective films. In recent years, their application in components molded into three-dimensional shapes has also been increasing. As problems during three-dimensional molding, there are stress whitening during molding, increased surface haze, cracking, etc. For the surface protective layer, stress whitening resistance, surface smoothness, flexibility, and bending resistance are also required on the basis of the above characteristics.
[0005] As a resin molded body with excellent whitening property during molding, a method using cross-linked rubber polymer particles with a particle size of 0.1 μm or less has been proposed (Patent Document 1). However, in the case of cross-linked polymer particles or block copolymers with only small particle sizes, it is difficult to suppress cracking during molding while maintaining high surface hardness.
[0006] As a film having excellent pencil hardness and stress whitening resistance, a method using rubber polymer particles having a particle size of 0.07 μm or less (Patent Document 1) and a method using block copolymers as rubber particles (Patent Document 2) are disclosed. However, in the case of polymer particles having only small particle sizes, it is difficult to suppress cracking during molding while maintaining high surface hardness.
[0007] As a film having excellent pencil hardness, stress whitening resistance, and cracking resistance, a method using two types of elastomer particles with different particle sizes, namely, crosslinked elastomer particles with a large particle size of 0.2 to 0.4 μm and crosslinked elastomer particles with a small particle size of 0.18 μm or less, is disclosed (Patent Documents 3 and 4). However, it is known that even when a small amount of elastomer particles with a large particle size of 0.2 μm or more are added, the surface smoothness is impaired and the haze of the film is deteriorated, and film performance having excellent transparency, surface smoothness, pencil hardness, stress whitening resistance, and cracking resistance has not yet been achieved.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2001-316557
[0011] Patent Document 2: WO2016 / 157908
[0012] Patent Document 3: Japanese Patent Application Publication No. 2003-183471
[0013] Patent document 4: WO2013 / 051239 Summary of the invention
[0014] Problems to be solved by the invention
[0015] An object of the present invention is to provide a methacrylic melt-extruded molded product suitable for decorative purposes, which is excellent in transparency, surface smoothness, resistance to whitening on bending, pencil hardness, bendability, moldability and appearance after molding.
[0016] Methods used to solve problems
[0017] As a result of conducting studies to solve the above-mentioned problems, the present invention including the following aspects has been completed.
[0018] [1]
[0019] A methacrylic acid melt extrusion molded body, comprising:
[0020] A methacrylic resin (A) comprising 80% by mass or more of methyl methacrylate units and having a weight average molecular weight of 50,000 or more and 500,000 or less;
[0021] An acrylic multilayer polymer (B) having at least one rubber component layer (b1) inside and at least one thermoplastic resin component layer (b2), the outermost being the thermoplastic resin component layer (b2), and the average particle size of the rubber component layer (b1) being in the range of 0.05 to 0.15 μm; and
[0022] an acrylic block copolymer (C) comprising a methacrylate polymer block (c1) and an acrylate polymer block (c2),
[0023] The methacrylic acid melt extrusion molded product is characterized in that
[0024] The acetone insoluble component of the molded body is 1 to 60% by mass. In the cross section of the molded body parallel to the extrusion direction, the acrylic ester polymer block (c2) forms a spherical or columnar phase, the diameter of the spherical phase or the short axis of the columnar phase is greater than 1 nm and less than 100 nm, and the long axis of the columnar phase is greater than 10 nm and less than 500 nm.
[0025] [2]
[0026] The methacrylic acid melt-extruded molded product according to [1], characterized in that
[0027] In the acrylic multilayer polymer (B),
[0028] The rubber component layer (b1) contains a copolymer composed of 50 to 98.99 mass % of acrylic acid ester monomer units, 1 to 44.99 mass % of other monofunctional monomer units and 0.01 to 10 mass % of multifunctional monomer units, and the thermoplastic resin component layer (b2) contains a copolymer composed of 40 to 100 mass % of methacrylic acid ester monomer units and 60 to 0 mass % of other monomer units.
[0029] 〔3〕
[0030] The methacrylic acid melt-extruded molded product according to [1], characterized in that
[0031] The acrylic block copolymer (C) comprises at least one methacrylate polymer block (c1) and at least one acrylate polymer block (c2), wherein the acrylic block copolymer (C) has 30 to 60% by mass of the methacrylate polymer block (c1) and 40 to 70% by mass of the acrylate polymer block (c2), and the content of the acrylic block copolymer (C) in the methacrylic melt-extrusion molded product is 1 to 15% by mass.
[0032] [4] The methacrylic acid melt-extruded molded product according to [1], wherein the methacrylic acid melt-extruded molded product is a film having a thickness of 20 to 200 μm.
[0033] 〔5〕
[0034] The methacrylic acid-based melt-extruded molded product according to any one of [1] to [4], further comprising a matting agent.
[0035] [6]
[0036] The methacrylic acid-based melt-extruded molded product according to any one of [1] to [5], further comprising a functional layer.
[0037] 〔7〕
[0038] The methacrylic acid melt-extruded molded product according to any one of [1] to [6], wherein the methacrylic acid melt-extruded molded product is a film, and the film is laminated with another thermoplastic resin film.
[0039] 〔8〕
[0040] The methacrylic acid melt-extruded molded product according to any one of [1] to [7], which is used for decoration.
[0041] 〔9〕
[0042] The methacrylic acid melt-extruded molded product according to any one of [1] to [7], which is used for building materials.
[0043] 〔10〕
[0044] A method for producing a methacrylic melt-extrusion molded product, comprising the step of melt-extruding a methacrylic resin composition using a T-die, wherein the method is characterized in that:
[0045] The methacrylic resin composition comprises: a methacrylic resin (A) containing 80% by mass or more of methyl methacrylate units and having a weight average molecular weight of 50,000 or more and 500,000 or less; an acrylic multilayer polymer (B) having at least one rubber component layer (b1) inside and at least one thermoplastic resin component layer (b2), with the outermost layer being the thermoplastic resin component layer (b2); and an acrylic block copolymer (C) containing a methacrylate polymer block (c1) and an acrylate polymer block (c2),
[0046] In the melt extrusion step, the shear rate applied during extrusion from the die is in the range of 200 to 650 / s.
[0047] Effects of the Invention
[0048] The methacrylic acid melt-extruded molded product of the present invention is excellent in transparency, surface smoothness, resistance to whitening on bending, pencil hardness and bendability, and is suitable for decorative purposes and building material applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1This is a schematic diagram of a cross-sectional slice of a methacrylic acid melt extrusion molded product of the present invention obtained in an example, taken along a plane parallel to the extrusion direction. The acrylic ester polymer blocks (c2) of the acrylic block copolymer (C) are spherically dispersed. (I): acrylic multilayer polymer, (II): acrylic block copolymer.
[0050] Figure 2 Schematic diagram of a cross-sectional slice of a methacrylic melt extruded product of the present invention obtained in Example, taken along a plane parallel to the extrusion direction. The acrylic ester polymer blocks (c2) of the acrylic block copolymer (C) are dispersed in a columnar shape. (I): acrylic multilayer polymer, (II): acrylic block copolymer. DETAILED DESCRIPTION
[0051] "Methacrylic acid melt extrusion molded product"
[0052] The methacrylic melt extrusion molded product of the present invention comprises: a methacrylic resin (A) containing 80% by mass or more of methyl methacrylate units and having a weight average molecular weight of 50,000 to 500,000; an acrylic multilayer polymer (B) comprising an outermost layer composed of a thermoplastic resin component and at least one rubber component layer in contact with and covered by the outermost layer; and an acrylic block copolymer (C) containing a methacrylate polymer block (c1) and an acrylate polymer block (c2), wherein the acetone-insoluble component of the molded product is 1 to 60% by mass, and in a cross section of the molded product parallel to the extrusion direction, the acrylate polymer block (c2) forms a spherical or columnar phase, the diameter of the spherical phase or the short axis of the columnar phase is 1 nm to 100 nm, and the long axis of the columnar phase is 10 nm to 500 nm.
[0053] In a preferred embodiment of the present invention, the molded article of the present invention is a molded article in which a methacrylic resin (A) forms a matrix and a rubbery elastic body including an acrylic multilayer polymer (B) and an acrylic block copolymer (C) is dispersed.
[0054] The acetone-insoluble content of the methacrylic acid melt-extruded molded product of the present invention is preferably 1 to 60% by mass, more preferably 1 to 50% by mass, further preferably 5 to 45% by mass, particularly preferably 10 to 40% by mass, and most preferably 20 to 40% by mass. The molded product is preferably cut into pieces before measurement of the acetone-insoluble content.
[0055] The methacrylic acid melt-extrusion molded product of the present invention preferably has an acetone-soluble content of 99 to 40% by mass, more preferably 99 to 50% by mass, further preferably 95 to 55% by mass, particularly preferably 90 to 60% by mass, and most preferably 80 to 60% by mass.
[0056] The acetone-insoluble content can be determined by using 25 mL of acetone per 1 g of the molded product, stirring at room temperature for 24 hours, centrifuging, separating the precipitate as the acetone-insoluble content, and measuring the mass after drying. The acetone-insoluble content can be determined according to the following formula.
[0057] Acetone insoluble content (%) = [(mass of precipitate) / (mass before separation)] × 100
[0058] The methacrylic melt extrusion molded product contains a methacrylic resin (A), an acrylic multilayer polymer (B) and an acrylic block copolymer (C) in the following ratio:
[0059] ·Methacrylic resin (A) content
[0060] Preferably it is 10-89.9 mass %, More preferably, it is 20-79 mass %
[0061] ·Content of acrylic multilayer polymer (B)
[0062] Preferably it is 10-89.9 mass %, More preferably, it is 20-79 mass %
[0063] ·Content of acrylic block copolymer (C)
[0064] It is preferably 0.1 to 15 mass %, more preferably 1 to 10 mass %.
[0065] (Methacrylic resin (A))
[0066] In the methacrylic resin (A) used in the present invention, the proportion of structural units derived from methyl methacrylate is 80% by mass or more, preferably 90% by mass or more. In addition, in the methacrylic resin (A), the proportion of structural units derived from monomers other than methyl methacrylate is 20% by mass or less, preferably 10% by mass or less.
[0067] Examples of monomers other than methyl methacrylate include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, amyl acrylate, isoamyl acrylate, n-hexyl acrylate, 2-ethylhexyl acrylate, pentadecyl acrylate, and dodecyl acrylate; phenyl acrylate, benzyl acrylate, phenoxyethyl acrylate, 2-hydroxyethyl acrylate, 2-ethoxyethyl acrylate, glycidyl acrylate, and allyl acrylate; acrylic acid esters such as cyclohexyl acrylate, norbornyl acrylate, and isobornyl acrylate; ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, amyl methacrylate, isoamyl methacrylate, n-hexyl methacrylate, 2-ethoxyethyl methacrylate, glycidyl acrylate, and allyl acrylate; acrylic acid esters such as cyclohexyl acrylate, norbornyl acrylate, and isobornyl acrylate; 2-Hydroxyhexyl methacrylate, pentadecyl methacrylate, dodecyl methacrylate; phenyl methacrylate, benzyl methacrylate, phenoxyethyl methacrylate, 2-hydroxyethyl methacrylate, 2-ethoxyethyl methacrylate, glycidyl methacrylate, allyl methacrylate; methacrylates other than methyl methacrylate such as cyclohexyl methacrylate, norbornyl methacrylate and isobornyl methacrylate; unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic anhydride, maleic acid and itaconic acid; olefins such as ethylene, propylene, 1-butene, isobutylene and 1-octene; conjugated dienes such as butadiene, isoprene and myrcene; aromatic vinyl compounds such as styrene, α-methylstyrene, p-methylstyrene and m-methylstyrene; acrylamide, methacrylamide, acrylonitrile, methacrylonitrile, vinyl acetate, vinylpyridine, vinyl ketone, vinyl chloride, vinylidene chloride and vinylidene fluoride.
[0068] The stereoregularity of the methacrylic resin (A) is not particularly limited, and for example, a methacrylic resin having stereoregularity such as isotactic, heterotactic, or syndiotactic can be used.
[0069] The weight average molecular weight (hereinafter referred to as Mw(A)) of the methacrylic resin (A) is preferably 50,000 or more and 500,000 or less, and more preferably 60,000 or more and 200,000 or less. If Mw(A) is too small, the impact resistance and toughness of the obtained molded product tend to decrease. If Mw(A) is too large, the fluidity of the methacrylic resin composition used for melt extrusion tends to decrease, and the molding processability tends to decrease.
[0070] The ratio Mw(A) / Mn(A) of the weight average molecular weight Mw(A) to the number average molecular weight Mn(A) of the methacrylic resin (A) (hereinafter, the ratio of the weight average molecular weight to the number average molecular weight (weight average molecular weight / number average molecular weight) may be referred to as "molecular weight distribution") is preferably 1.03 or more and 2.6 or less, more preferably 1.05 or more and 2.3 or less, and particularly preferably 1.2 or more and 2.0 or less. If the molecular weight distribution is too small, the molding processability of the methacrylic resin composition tends to decrease. If the molecular weight distribution is too large, the impact resistance of the obtained molded body tends to decrease and become brittle.
[0071] In addition, Mw(A) and Mn(A) are standard polystyrene conversion values measured by GPC (gel permeation chromatography).
[0072] The molecular weight and molecular weight distribution of the methacrylic resin can be controlled by adjusting the type and amount of the polymerization initiator and the chain transfer agent.
[0073] The methacrylic resin (A) can be obtained by polymerizing a monomer or a monomer mixture containing 80% by mass or more of methyl methacrylate.
[0074] As the methacrylic resin (A), commercially available products may be used. Examples of the commercially available methacrylic resin include "Parapet H1000B" (MFR: 22 g / 10 min (230° C., 37.3 N)), "Parapet GF" (MFR: 15 g / 10 min (230° C., 37.3 N)), "Parapet EH" (MFR: 1.3 g / 10 min (230° C., 37.3 N)), "Parapet HRL" (MFR: 2.0 g / 10 min (230° C., 37.3 N)), and "Parapet G" (MFR: 8.0 g / 10 min (230° C., 37.3 N)) [all trade names, manufactured by Kuraray Co., Ltd.].
[0075] (Acrylic multilayer polymer (B))
[0076] The acrylic multilayer polymer (B) is a particle of a core-shell structure having at least one rubber component layer (b1) (hereinafter sometimes simply referred to as "(b1)") inside and at least one thermoplastic resin component layer (b2) (hereinafter sometimes simply referred to as "(b2)"), with the outermost layer being the thermoplastic resin component layer (b2). It should be noted that the core of the acrylic multilayer polymer (B) is regarded as a "layer". The number of layers of the acrylic multilayer polymer (B) may be two or more, and may be three or four or more layers. Examples of the layer structure include: a two-layer structure of (b1)-(b2) from the center; a three-layer structure of (b1)-(b1)-(b2), (b1)-(b2)-(b2) or (b2)-(b1)-(b2) from the center; a four-layer structure of (b1)-(b2)-(b1)-(b2) from the center, etc. Among them, from the viewpoint of handling properties, a two-layer structure of (b1)-(b2), a three-layer structure of (b1)-(b1)-(b2) or (b2)-(b1)-(b2) is preferred, and a three-layer structure of (b2)-(b1)-(b2) is more preferred.
[0077] The mass ratio ((b1) / (b2)) of the total amount of the rubber component layer (b1) to the total amount of the thermoplastic resin component layer (b2) is 30 / 70 to 90 / 10. When the ratio of (b1) is less than the above range, there is a concern that the impact strength of the molded body may become insufficient. When the ratio of (b1) exceeds the above range, the formation of the particle structure becomes difficult, and the melt fluidity decreases, and there is a concern that mixing with other components and molding of the resin composition may become difficult. The mass ratio ((b1) / (b2)) is preferably 30 / 70 to 80 / 20, and more preferably 40 / 60 to 70 / 30. When the resin composition has two or more rubber component layers (b1), the mass ratio is calculated based on their total amount, and when the resin composition has two or more thermoplastic resin component layers (b2), the mass ratio is calculated based on their total amount.
[0078] (b1) preferably comprises a copolymer containing 50 to 98.99% by mass of an acrylate monomer unit, 44.99 to 1% by mass of other monofunctional monomer units, and 0.01 to 10% by mass of a multifunctional monomer unit. The content of the acrylate monomer unit is more preferably 55 to 89.9% by mass, the content of the monofunctional monomer unit is more preferably 44.9 to 10% by mass, and the content of the multifunctional monomer unit is more preferably 0.1 to 5% by mass.
[0079] When the content of the acrylic acid ester monomer unit is less than 50% by mass, the rubber elasticity of the acrylic multilayer polymer (B) becomes insufficient, and there is a concern that the impact strength of the molded article becomes insufficient. When it exceeds 98.99% by mass, there is a concern that the formation of the particle structure becomes difficult. When the content of other monofunctional monomer units is less than 1% by mass, there is a concern that the optical properties of the multilayer structure polymer particles become insufficient. When it exceeds 44.99% by mass, there is a concern that the weather resistance of the acrylic multilayer polymer (B) becomes insufficient. When the content of the multifunctional monomer unit exceeds 10% by mass, the rubber elasticity of the acrylic multilayer polymer (B) becomes insufficient, and there is a concern that the impact strength of the molded article becomes insufficient. When it is less than 0.01% by mass, there is a concern that the formation of the particle structure becomes difficult.
[0080] Next, the raw material monomers of the rubber component layer (b1) are described.
[0081] Examples of the acrylic acid ester include acrylic acid and saturated aliphatic alcohols (preferably C 2-4-hydroxy-2-propene) such as methyl acrylate (MA), ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate (BA), isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, amyl acrylate, hexyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, dodecyl acrylate, and octadecyl acrylate. 1 ~C 18 esters of saturated aliphatic alcohols); cyclohexyl acrylate and other acrylic acid and C 5 or C 6 esters of alicyclic alcohols; esters of acrylic acid and phenols such as phenyl acrylate; esters of acrylic acid and aromatic alcohols such as benzyl acrylate, etc. The acrylic acid esters can be used alone or in combination of two or more.
[0082] Examples of other monofunctional monomers include methyl methacrylate (MMA), ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, amyl methacrylate, hexyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, dodecyl methacrylate, myristyl methacrylate, palmityl methacrylate, stearyl methacrylate, behenyl methacrylate, and methacrylic acid and saturated aliphatic alcohols (preferably C 1 ~C 22 esters of saturated aliphatic alcohols); methacrylic acid and C 5 or C 6Esters of alicyclic alcohols; methacrylates such as esters of methacrylic acid and phenols such as phenyl methacrylate, esters of methacrylic acid and aromatic alcohols such as benzyl methacrylate; aromatic vinyl monomers such as styrene (St), α-methylstyrene, 1-vinylnaphthalene, 3-methylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene and halogenated styrene; cyanide vinyl monomers such as acrylonitrile and methacrylonitrile, etc. Among them, styrene is preferred. Other monofunctional monomers can be used alone or in combination.
[0083] A multifunctional monomer is a monomer having two or more carbon-carbon double bonds in the molecule. Examples of multifunctional monomers include: esters of unsaturated monocarboxylic acids such as acrylic acid, methacrylic acid, and cinnamic acid with unsaturated alcohols such as allyl alcohol and methallyl alcohol; diesters of the above-mentioned unsaturated monocarboxylic acids with glycols such as ethylene glycol, butanediol, and hexanediol; esters of dicarboxylic acids such as phthalic acid, terephthalic acid, isophthalic acid, and maleic acid with the above-mentioned unsaturated alcohols, etc. Specifically, examples include allyl acrylate, methallyl acrylate, allyl methacrylate, methallyl methacrylate, allyl cinnamate, methallyl cinnamate, diallyl maleate, diallyl phthalate, diallyl terephthalate, diallyl isophthalate, divinylbenzene, ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, and hexanediol di(meth)acrylate. Among them, allyl methacrylate (ALMA) is preferred. The polyfunctional monomer may be used alone or in combination of two or more.
[0084] Layer (b2) preferably comprises a copolymer composed of 40 to 100% by mass of methacrylate monomer units and 60 to 0% by mass of other monomer units. The content of the methacrylate monomer units is more preferably 50 to 99% by mass, further preferably 60 to 99% by mass, and particularly preferably 80 to 99% by mass, and the content of the other monomer units is more preferably 50 to 1% by mass, further preferably 40 to 1% by mass, and further preferably 20 to 1% by mass. When the content of the methacrylate monomer units is less than 50% by mass, there is a concern that the weather resistance of the acrylic multilayer polymer (B) becomes insufficient.
[0085] Next, the raw material monomers of the thermoplastic resin component layer (b2) are described.
[0086] Examples of the methacrylate include methyl methacrylate (MMA), ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, amyl methacrylate, hexyl methacrylate, octyl methacrylate, 2-ethylhexyl methacrylate, cyclohexyl methacrylate, dodecyl methacrylate, myristyl methacrylate, palmityl methacrylate, stearyl methacrylate, behenyl methacrylate, octadecyl methacrylate, phenyl methacrylate, and benzyl methacrylate. Among them, methyl methacrylate (MMA) is preferred.
[0087] Examples of other monomers include acrylic acid and saturated aliphatic alcohols (preferably C 2- 4- 4- acrylate), such as methyl acrylate (MA), ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate (BA), isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, amyl acrylate, hexyl acrylate, octyl acrylate, 2-ethylhexyl acrylate, dodecyl acrylate, and octadecyl acrylate. 1 ~C 18 esters of saturated aliphatic alcohols); cyclohexyl acrylate and other acrylic acid and C 5 or C 6 Esters of alicyclic alcohols; aromatic vinyl monomers such as styrene (St), α-methylstyrene, 1-vinylnaphthalene, 3-methylstyrene, 4-propylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene and halogenated styrene; vinyl cyanide monomers such as acrylonitrile and methacrylonitrile; maleimide monomers such as maleimide, N-methylmaleimide, N-ethylmaleimide, N-propylmaleimide, N-isopropylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, N-(p-bromophenyl)maleimide and N-(chlorophenyl)maleimide; and polyfunctional monomers exemplified in layer (b1). Among them, preferred are alkyl acrylates such as methyl acrylate (MA), ethyl acrylate and n-butyl acrylate (BA).
[0088] In the acrylic multilayer polymer (B), the weight average molecular weight (Mw) of the copolymer constituting the outermost layer (b2) measured by the GPC method is preferably in the range of 20,000 to 100,000, more preferably in the range of 30,000 to 90,000, and particularly preferably in the range of 40,000 to 80,000. When Mw is less than 20,000, the rubber elasticity of the acrylic multilayer polymer (B) becomes insufficient, and there is a concern that molding of the resin composition becomes difficult. When Mw exceeds 100,000, there is a concern that the impact strength of the molded body decreases.
[0089] The average particle size (de) of the rubber component layer (b1) of the acrylic multilayer polymer (B) closest to the outermost layer (preferably in contact with the outermost layer) is in the range of 0.05 to 0.15 μm. When the average particle size (de) is less than 0.05 μm, stress concentration on the acrylic multilayer polymer (B) becomes insufficient, and there is a concern that the impact strength of the molded body will decrease. When the average particle size (de) exceeds 0.15 μm, voids are generated inside the acrylic multilayer polymer (B), and whitening occurs. In addition, when the rubber content in the resin composition remains constant, if the particle size increases to a certain level, the number of particles decreases, so there is a tendency for the surface distance between the particles to increase, and the probability of cracks in the continuous phase increases, and there is a concern that the impact strength of the molded body will decrease. The voids referred to here refer to damage that occurs only inside the particles, and the amount of energy absorbed is very small, so it does not contribute much to the performance of impact resistance.
[0090] From the viewpoint of stress concentration on the acrylic multilayer polymer (B), the average particle diameter (de) is preferably 0.05 to 0.15 μm, more preferably 0.07 to 0.12 μm.
[0091] It should be noted that the average particle size (de) of the rubber component layer (b1) of the acrylic multilayer polymer (B) can be obtained by measuring a section of a molded body using an electron microscope or by measuring a latex using a light scattering method. In the method using an electron microscope, it is the average value of the major axis diameter and the minor axis diameter of the outermost layer in the rubber component layer (b1) of the stained acrylic multilayer polymer (B) observed by a transmission electron microscope when the section of the molded body is electron stained with ruthenium tetroxide. In the method using the light scattering method, the latex polymerized to the rubber component layer can be sampled when the multilayer structure polymer particles are polymerized and measured using a laser diffraction / scattering particle size distribution measuring device LA-950V2 manufactured by Horiba, Ltd.
[0092] In a preferred embodiment of the present invention, the method for producing the acrylic multilayer polymer (B) is not particularly limited as long as it is a method that can obtain an acrylic multilayer polymer (B) having the rubber component layer (b1) / thermoplastic resin component layer (b2) as described above. The preferred method for producing the acrylic multilayer polymer (B) having a three-layer structure (core-middle layer-outermost layer) includes the following steps: emulsion polymerization of monomers for obtaining a polymer constituting the central core to obtain seed particles (i), seed emulsion polymerization of monomers for obtaining a polymer constituting the middle layer in the presence of seed particles (i) to obtain seed particles (ii), and seed emulsion polymerization of monomers for obtaining a polymer constituting the outermost layer in the presence of seed particles (ii) to obtain seed particles (iii). A person skilled in the art can easily produce an acrylic multilayer polymer (B) having a two-layer structure or a layer structure of more than four layers by referring to the above-mentioned production method of the acrylic multilayer polymer (B) having a three-layer structure. Emulsion polymerization or seed emulsion polymerization is a conventional method for obtaining multilayer structure polymer particles, and is a well-known technique in the technical field, so a detailed description can be referred to other documents. In the above-mentioned preferred examples, the seed particle (i) is a single-layer particle consisting of a thermoplastic resin component layer (b2, core), the seed particle (ii) is a two-layer particle consisting of a thermoplastic resin component layer (b2, core) + a rubber component layer (b1, middle layer), and the seed particle (iii) is a three-layer particle consisting of a thermoplastic resin component layer (b2, core) + a rubber component layer (b1, middle layer) + a thermoplastic resin component layer (b2, outermost layer).
[0093] In the polymerization reaction step, the polymerization conditions are adjusted so that at least the Mw of the copolymer constituting the outermost thermoplastic resin component layer (b2) reaches 20,000 to 100,000. The adjustment of the polymerization conditions is mainly carried out by adjusting the amount of a molecular weight modifier such as alkyl mercaptan. The polymerization conditions of the entire polymerization reaction step are adjusted so that the average particle size of the acrylic multilayer polymer (B) to the outermost thermoplastic resin component layer (b2) obtained in the end is in the range of 0.05 to 0.15 μm.
[0094] It should be noted that the average particle size of the acrylic multilayer polymer particles (B) up to the outermost thermoplastic resin component layer (b2) can be measured as follows: when the multilayer structure polymer particles are polymerized, the polymerized latex is sampled and measured by a light scattering method using a laser diffraction / scattering particle size distribution measuring device LA-950V2 manufactured by Horiba, Ltd.
[0095] (Acrylic block copolymer (C))
[0096] The acrylic block copolymer (C) used in the present invention has a methacrylate polymer block (c1) and an acrylate polymer block (c2). The acrylic block copolymer (C) may have only one methacrylate polymer block (c1) or may have two or more methacrylate polymer blocks (c1). In addition, the acrylic block copolymer (C) may have only one acrylate polymer block (c2) or may have two or more acrylate polymer blocks (c2). The acrylic block copolymer (C) has good compatibility with the methacrylic resin (A) and the acrylic multilayer polymer (B).
[0097] From the viewpoint of the above compatibility, the acrylic block copolymer (C) preferably comprises 10 to 80% by mass of a polymer block (c1) having a methacrylate monomer unit and 90 to 20% by mass of a polymer block (c2) mainly having an acrylate monomer unit (wherein the total amount of the polymer block (c1) and the polymer block (c2) is 100% by mass). In the acrylic block copolymer (C), the content of the polymer block (c1) is more preferably 20 to 70% by mass, and further preferably 30 to 60% by mass, and the content of the polymer block (c2) is more preferably 80 to 30% by mass, and further preferably 70 to 40% by mass.
[0098] The number of polymer blocks (c1) in one molecule may be a single number or two or more. When the number of polymer blocks (c1) in one molecule is two or more, the composition and molecular weight of the structural units of the two or more polymer blocks (c1) may be the same or different. Similarly, the number of polymer blocks (c2) in one molecule may be a single number or two or more. When the number of polymer blocks (c2) in one molecule is two or more, the composition and molecular weight of the structural units of the two or more polymer blocks (c2) may be the same or different.
[0099] The polymer block (c1) mainly comprises methacrylate monomer units. The content of methacrylate monomer units in the polymer block (c1) is preferably 80% by mass or more, more preferably 90% by mass or more, particularly preferably 95% by mass or more, and most preferably 98% by mass or more, and may be composed only of methacrylate monomer units.
[0100] The raw material monomers of the methacrylic polymer block (c1) are described below.
[0101] As methacrylate, methyl methacrylate (MMA), ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, tert-butyl methacrylate, amyl methacrylate, isoamyl methacrylate, n-hexyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl methacrylate, pentadecyl methacrylate, dodecyl methacrylate, isobornyl methacrylate, phenyl methacrylate, benzyl methacrylate, phenoxyethyl methacrylate, 2-hydroxyethyl methacrylate, 2-methoxyethyl methacrylate, glycidyl methacrylate, and allyl methacrylate (ALMA) are listed. Among them, from the viewpoint of improving transparency and heat resistance, methyl methacrylate (MMA), ethyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, tert-butyl methacrylate, cyclohexyl methacrylate, and isobornyl methacrylate are preferred, and methyl methacrylate (MMA) is particularly preferred. One or more of the methacrylates can be used.
[0102] The lower limit of the weight average molecular weight (Mw(c1)) of the methacrylic polymer block (c1) is preferably 5000, more preferably 8000, further preferably 12000, particularly preferably 15000, and most preferably 20000, and the upper limit is preferably 150000, more preferably 120000, and particularly preferably 100000. When the acrylic block copolymer (C) has two or more polymer blocks (c1), the weight average molecular weight (Mw(c1)) is the total amount of Mw of the two or more polymer blocks (c1).
[0103] In a preferred embodiment of the present invention, the weight average molecular weight Mw(c1) of the methacrylic polymer block (c1) of the acrylic block copolymer (C) and the weight average molecular weight Mw(A) of the methacrylic resin (A) satisfy the following formula (Y).
[0104] 0.5≤Mw(A) / Mw(c1)≤2.5(Y)
[0105] The ratio of the weight average molecular weight Mw(A) of the methacrylic resin (A) to Mw(c1), i.e., Mw(A) / Mw(c1), is 0.5 or more and 2.5 or less, preferably 0.6 or more and 2.3 or less, and more preferably 0.7 or more and 2.2 or less. When Mw(A) / Mw(c1) deviates from the above range, the dispersed particle size of the acrylic block copolymer (C) in the methacrylic resin (A) becomes larger, and whitening occurs when stress is applied. When Mw(A) / Mw(c1) is within the above range, the dispersed particle size of the acrylic block copolymer (C) in the methacrylic resin (A) becomes smaller, so the stress whitening resistance is excellent.
[0106] From the viewpoint of transparency, softness, flexibility, bending resistance, impact resistance, moldability and surface smoothness of the molded article of the present invention, the content of the methacrylic polymer block (c1) in the acrylic block copolymer (C) is preferably 10 to 80% by mass, and more preferably 20 to 70% by mass. When the acrylic block copolymer (C) has two or more polymer blocks (c1), the content of the polymer block (c1) is the total content of the two or more polymer blocks (c1).
[0107] In a preferred embodiment of the present invention, the acrylic polymer block (c2) mainly comprises acrylic acid ester monomer units. The content of acrylic acid ester monomer units in the acrylic polymer block (c2) is preferably 45% by mass or more, more preferably 50% by mass or more, further preferably 60% by mass or more, and particularly preferably 90% by mass or more.
[0108] The raw material monomers of the acrylic polymer block (c2) are described below.
[0109] Examples of the acrylic acid ester include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate (BA), isobutyl acrylate, sec-butyl acrylate, tert-butyl acrylate, amyl acrylate, isoamyl acrylate, n-hexyl acrylate, cyclohexyl acrylate, 2-ethylhexyl acrylate, pentadecyl acrylate, dodecyl acrylate, isobornyl acrylate, phenyl acrylate, benzyl acrylate, phenoxyethyl acrylate, 2-hydroxyethyl acrylate, 2-methoxyethyl acrylate, glycidyl acrylate, and allyl acrylate. One or more of the acrylic acid esters may be used.
[0110] In another preferred embodiment of the present invention, from the viewpoint of transparency, the acrylic polymer block (c2) is preferably a polymer block (c2-p) containing an alkyl acrylate monomer unit and a (meth) acrylate aromatic hydrocarbon ester monomer unit. Here, the content of the alkyl acrylate monomer unit in the polymer block (c2) is preferably 50 to 90% by mass, more preferably 60 to 80% by mass, and the content of the (meth) acrylate aromatic hydrocarbon ester monomer unit is preferably 50 to 10% by mass, more preferably 40 to 20% by mass.
[0111] In a preferred embodiment of the present invention, the weight average molecular weight Mw(c2) of the acrylic polymer block (c2) satisfies the following formula (Z), and more preferably satisfies the following formula (Z1).
[0112] 5000≤Mw(c2)≤120000(Z)
[0113] 40000≤Mw(c2)≤120000(Z1)
[0114] The lower limit of the weight average molecular weight Mw(c2) of the acrylic polymer block (c2) is preferably 5000, more preferably 15000, further preferably 20000, particularly preferably 30000, and most preferably 40000, and the upper limit is preferably 120000, more preferably 110000, and particularly preferably 100000. It should be noted that when Mw(c2) is too small, there is a concern that the impact resistance of the molded body decreases. On the other hand, when Mw(c2) is too large, there is a concern that the surface smoothness of the molded body decreases. When the acrylic block copolymer (C) has two or more polymer blocks (c2), the weight average molecular weight Mw(c2) is the total amount of the Mw of the two or more polymer blocks (c2).
[0115] From the viewpoint of transparency, softness, flexibility, bending resistance, impact resistance, moldability and surface smoothness of the molded product, the content of the acrylic polymer block (c2) in the acrylic block copolymer (C) is preferably 10 to 90% by mass, and more preferably 20 to 80% by mass. When the acrylic block copolymer (C) has two or more polymer blocks (c2), the content of the polymer block (c2) is the total content of the two or more acrylic polymer blocks (c2).
[0116] In the melt extrusion molded article, the dispersed phase of the acrylic polymer block (c2) in the cross section parallel to the extrusion direction of the methacrylic resin (A) is preferably a spherical or columnar phase. When the dispersed phase is a lamellar phase, the extruded article becomes turbid and whitens when stress is applied.
[0117] In the case of a spherical phase, the particle size of the dispersed phase of the acrylic polymer block (c2) is preferably 1 nm to 200 nm, more preferably 10 nm to 100 nm. When the particle size is less than 1 nm, stress concentration around the acrylic polymer block is small and bending resistance is not exhibited. When the particle size exceeds 200 nm, whitening occurs when stress is applied.
[0118] In the case of a columnar phase, the short diameter of the columnar phase is 1 nm to 200 nm, and the long diameter of the columnar phase is preferably 1 nm to 500 nm, and more preferably 10 nm to 400 nm. When the long diameter is less than 10 nm, stress concentration around the acrylic polymer block is small and bending resistance is not exhibited. When it exceeds 500 nm, whitening occurs when stress is applied.
[0119] There is no particular restriction on the bonding method of the methacrylic polymer block (c1) and the acrylic polymer block (c2) in the acrylic block copolymer (C). Examples of the acrylic block copolymer (C) include: a diblock copolymer having a (c1)-(c2) structure in which one end of the polymer block (c1) is connected to one end of the polymer block (c2); a triblock copolymer having a (c2)-(c1)-(c2) structure in which one end of the polymer block (c2) is connected to each of the two ends of the polymer block (c1); and a triblock copolymer having a (c1)-(c2)-(c1) structure in which one end of the polymer block (c1) is connected to each of the two ends of the polymer block (c2).
[0120] Among them, diblock copolymers and triblock copolymers are preferred, and diblock copolymers having a (c1)-(c2) structure and triblock copolymers having a (c1)-(c2)-(c1) structure are more preferred.
[0121] The acrylic block copolymer (C) may have a functional group such as a hydroxyl group, a carboxyl group, an acid anhydride group, or an amino group in the molecular chain and / or at the molecular chain terminal as required.
[0122] The weight average molecular weight (Mw(C)) of the acrylic block copolymer (C) is 32000 to 300000, preferably 40000 to 250000, more preferably 45000 to 230000, and particularly preferably 50000 to 200000. By setting the Mw(C) within the above range, the amount of unmelted matter during melt kneading of the raw materials in the production of the resin composition, which causes the formation of pitting in the molded body, can be reduced to a very small amount.
[0123] The ratio (Mw(C) / Mn(C)) of the weight average molecular weight (Mw(C)) of the acrylic block copolymer (C) is preferably 1.0 to 2.0, more preferably 1.0 to 1.6. By setting Mw(C) / Mn(C) within the above range, the amount of unmelted matter during melt kneading of raw materials in the production of the resin composition, which causes the generation of pitting in the molded body, can be minimized.
[0124] The method for producing the acrylic block copolymer (C) is not particularly limited, and is generally a method of living polymerization of each polymer block. As living polymerization methods, there can be cited: a method of using an organic alkali metal compound as a polymerization initiator and performing anionic polymerization in the presence of an inorganic acid salt such as an alkali metal or alkaline earth metal salt; a method of using an organic alkali metal compound as a polymerization initiator and performing anionic polymerization in the presence of an organic aluminum compound; a method of using an organic rare earth metal complex as a polymerization initiator for polymerization; and a method of using an α-halogenated ester compound as a polymerization initiator and performing free radical polymerization in the presence of a copper compound. In addition, a method of polymerization using a polyvalent free radical polymerization initiator or a polyvalent free radical chain transfer agent can also be cited. Among them, from the perspective of obtaining an acrylic block copolymer (C) with high purity, easy control of the composition and molecular weight of each block, and economic efficiency, a method of using an organic alkali metal compound as a polymerization initiator and performing anionic polymerization in the presence of an organic aluminum compound is particularly preferred.
[0125] The refractive index of the acrylic block copolymer (C) is not particularly limited, but is preferably 1.485 to 1.495, and more preferably 1.487 to 1.493. If the refractive index is within the above range, the transparency becomes high. It should be noted that in this specification, the "refractive index" refers to the value measured at a wavelength of 587.6 nm (D-ray).
[0126] (Methacrylic resin composition)
[0127] By adding the acrylic multilayer polymer (B) of the present invention to the mixing step of the methacrylic resin (A) and the acrylic block copolymer (C) and kneading them, a methacrylic resin composition for producing a methacrylic melt extrusion molded product having excellent transparency, surface smoothness, resistance to whitening on bending, pencil hardness and bendability can be obtained.
[0128] There are the following four methods for mixing the methacrylic resin (A), the acrylic multilayer polymer (B), and the acrylic block copolymer (C), and any one of them can be selected.
[0129] (i) a two-stage mixing method of first mixing a methacrylic resin (A) and an acrylic multilayer polymer (B), and then mixing an acrylic block copolymer (C) into the mixture of (A) + (B);
[0130] (ii) a two-stage mixing method of first mixing the methacrylic resin (A) and the acrylic block copolymer (C), and then mixing the acrylic multilayer polymer (B) into the mixture of (A) + (C);
[0131] (iii) a two-stage mixing method of first mixing the acrylic multilayer polymer (B) and the acrylic block copolymer (C) and then mixing the methacrylic resin (A) into the mixture of (B) + (C);
[0132] (iv) A method in which a methacrylic resin (A), an acrylic multilayer polymer (B) and an acrylic block copolymer (C) are mixed in one stage.
[0133] As a mixing method, it can be carried out by using a Banbury mixer, a pressure kneading machine, a roller mill, a continuous mixer such as a single screw, a twin screw, a multi-screw extruder, etc. to mix the known methods. In addition, it can also be a method of melt mixing the product diluted after making a high-concentration masterbatch by the above method. From the viewpoint of productivity, a single screw method or a twin screw method is preferred. In particular, a single screw extruder is preferred because the shear energy of the resin composition is small.
[0134] (Rubber content)
[0135] In the present invention, the total amount of the rubber component layer (b1) of the acrylic multilayer polymer (B) and the acrylic polymer block (c2) of the acrylic block copolymer (C) is 5 to 60% by mass, preferably 6 to 50% by mass, and more preferably 7 to 30% by mass. If the total amount of the rubber component layer (b1) and the acrylic polymer block (c2) is less than 5% by mass, the impact strength is deteriorated, and if it exceeds 60% by mass, the rigidity is deteriorated.
[0136] (c2 rubber ratio)
[0137] In the present invention, the ratio of the content of the acrylic polymer block (c2) to the total rubber content of (b1) and (c2) is in the range of 5 to 90% by mass, preferably in the range of 10 to 85% by mass, and more preferably in the range of 15 to 80% by mass. When the ratio of the content of the acrylic polymer block (c2) to the rubber content is in the range of 5 to 90% by mass, the synergistic effect of the multilayered polymer particles and the block copolymer is exerted, and excellent impact strength is achieved.
[0138] (Optional Ingredients)
[0139] In addition to the methacrylic resin (A), the acrylic multilayer polymer (B), and the acrylic block copolymer (C), other polymers may be contained as needed within a range that does not impair the effects of the present invention. Examples of other polymers include olefin resins such as polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, and polynorbornene; ethylene ionomers; styrene resins such as polystyrene, styrene-maleic anhydride copolymer, high-impact polystyrene, AS resin, ABS resin, AES resin, AAS resin, ACS resin, and MBS resin; methyl methacrylate-styrene copolymers; ester resins such as polyethylene terephthalate and polybutylene terephthalate; amide resins such as nylon 6, nylon 66, and polyamide elastomers; and polyphenylene sulfide. Other thermoplastic resins such as polyetheretherketone, polysulfone, polyphenylene ether, polyimide, polyetherimide, polycarbonate, polyvinyl chloride, polyvinylidene chloride, polyvinylidene fluoride, polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polyacetal and phenoxy resins; thermosetting resins such as phenolic resins, melamine resins, silicone resins and epoxy resins; polyurethane; modified polyphenylene ether; silicone modified resin; acrylic rubber, silicone rubber; styrene thermoplastic elastomers such as SEPS, SEBS and SIS; olefin rubbers such as IR, EPR and EPDM, etc. Other polymers can be used alone or in combination.
[0140] The methacrylic melt extrusion molded product of the present invention may contain various additives as needed. As additives, antioxidants, heat-resistant agents, ultraviolet absorbers, light stabilizers, lubricants, mold release agents, polymer processing aids, antistatic agents, flame retardants, dyes / pigments, matting agents, anti-sticking agents, impact resistance modifiers and phosphors can be listed. The content of these additives can be appropriately set within the range that does not impair the effect of the present invention. For example, the content of the antioxidant is preferably set to 0.01 to 1 part by mass, the content of the ultraviolet absorber is preferably set to 0.01 to 3 parts by mass, the content of the light stabilizer is preferably set to 0.01 to 3 parts by mass, the content of the lubricant is preferably set to 0.01 to 3 parts by mass, the content of the dye / pigment is preferably set to 0.01 to 3 parts by mass, the content of the matting agent is preferably set to 0.1 to 20 parts by mass, and the anti-sticking agent is preferably set to 0.001 to 1 part by mass. Other additives can also be added in the range of 0.01 to 3 parts by mass.
[0141] Antioxidants are substances that have the effect of preventing the oxidative degradation of resins caused by their monomers in the presence of oxygen. Examples thereof include phosphorus antioxidants, phenolic antioxidants, sulfur antioxidants, and amine antioxidants. Among them, from the viewpoint of the effect of preventing the degradation of optical properties caused by coloration, phosphorus antioxidants and phenolic antioxidants are preferred, and phenolic antioxidants are more preferably used alone or in combination. When a phosphorus antioxidant and a phenolic antioxidant are used in combination, it is preferred to use a phosphorus antioxidant / phenolic antioxidant at a mass ratio of 0.2 / 1 to 2 / 1, and more preferably to use a phosphorus antioxidant / phenolic antioxidant at a mass ratio of 0.5 / 1 to 1 / 1.
[0142] As the phosphorus antioxidant, 2,2-methylenebis(4,6-di-tert-butylphenyl)octyl phosphite ("Adeka Stab HP-10" manufactured by ADEKA Corporation), tris(2,4-di-tert-butylphenyl)phosphite ("IRGAFOS168" manufactured by BASF Japan Co., Ltd.), and 3,9-bis(2,6-di-tert-butyl-4-methylphenoxy)-2,4,8,10-tetraoxa-3,9-diphosphaspiro[5.5]undecane ("Adeka Stab PEP-36" manufactured by ADEKA Corporation) are preferred.
[0143] As the phenolic antioxidant, pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] ("IRGANOX 1010" manufactured by BASF Japan Co., Ltd.) and octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate ("IRGANOX 1076" manufactured by BASF Japan Co., Ltd.) are preferred.
[0144] As the sulfur-based antioxidant, dilauryl 3,3'-thiodipropionate, distearyl 3,3'-thiodipropionate, pentaerythritol tetrakis (3-laurylthiopropionate), and the like are preferred.
[0145] As the amine antioxidant, octylated diphenylamine and the like are preferred.
[0146] The heat degradation inhibitor is a substance that can prevent thermal degradation of the resin by capturing polymer radicals generated when the resin is exposed to high temperature in a substantially oxygen-free condition. Preferred heat degradation inhibitors include 2-tert-butyl-6-(3'-tert-butyl-5'-methyl-hydroxybenzyl)-4-methylphenyl acrylate (Sumitomo Chemical Co., Ltd., "Sumilyzer GM") and 2,4-di-tert-amyl-6-(3',5'-di-tert-amyl-2'-hydroxy-α-methylbenzyl)phenyl acrylate (Sumitomo Chemical Co., Ltd., "Sumilyzer GS"), etc.
[0147] The ultraviolet absorber is a compound that has the ability to absorb ultraviolet rays and can be said to mainly have the function of converting light energy into heat energy. Examples of the ultraviolet absorber include benzophenones, benzotriazoles, triazines, benzoates, salicylates, cyanoacrylates, oxalanilides, malonic esters, and formamidines. Among them, benzotriazoles and triazines are preferred. One or more ultraviolet absorbers can be used.
[0148] Benzotriazoles are highly effective in suppressing the decrease in optical properties such as coloration due to ultraviolet irradiation and are therefore suitable for use in optical applications. Preferred benzotriazoles include 4-methyl-2-(2H-benzotriazol-2-yl)phenol ("JF-77" manufactured by Johoku Chemical Industry Co., Ltd.), 2-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol ("TINUVIN 329" manufactured by BASF Japan Co., Ltd.), 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol ("TINUVIN 234" manufactured by BASF Japan Co., Ltd.), and 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-tert-octylphenol] ("ADECAST LA-31" manufactured by ADEKA Corporation).
[0149] In addition, when it is desired to effectively absorb wavelengths near 380 nm, it is preferred to use a triazine-based ultraviolet absorber. Examples of such ultraviolet absorbers include 2,4,6-tris(2-hydroxy-4-hexyloxy-3-methylphenyl)-1,3,5-triazine ("Adeka Stab LA-F70" manufactured by ADEKA Co., Ltd.) and its analogs, hydroxyphenyltriazine-based ultraviolet absorbers ("TINUVIN477" and "TINUVIN460" manufactured by BASF JAPAN Co., Ltd.).
[0150] Light stabilizers are compounds that can be said to mainly have the function of capturing free radicals generated by photooxidation. Suitable light stabilizers include hindered amines such as compounds having a 2,2,6,6-tetraalkylpiperidine skeleton. For example, bis(2,2,6,6-tetramethyl-4-piperidyl) sebacate ("Adeka Stab LA-77Y" manufactured by ADEKA Co., Ltd.) and the like can be mentioned.
[0151] Lubricants are compounds that can be said to have the effects of adjusting the smoothness of the resin and metal surfaces, improving demoulding properties and processability by preventing aggregation or adhesion. Examples include higher alcohols, hydrocarbons, fatty acids, fatty acid metal salts, aliphatic amides, and fatty acid esters. Among them, from the perspective of compatibility with the methacrylic resin composition, aliphatic monohydric alcohols and aliphatic amides having 12 to 18 carbon atoms are preferred, and aliphatic amides are more preferred. Aliphatic amides are classified into saturated aliphatic amides and unsaturated aliphatic amides. Unsaturated aliphatic amides are more preferred because of the expected slip effect caused by preventing adhesion. As unsaturated aliphatic amides, N, N'-ethylene bisoleic acid amide ("Sripax O" manufactured by Nippon Chemical Co., Ltd.) and N, N'-dioleyl adipic acid amide ("Sripax ZOA" manufactured by Nippon Chemical Co., Ltd.) can be cited.
[0152] Examples of the release agent include: higher alcohols such as cetyl alcohol and stearyl alcohol; higher fatty acid glycerides such as stearic acid monoglyceride and stearic acid diglyceride. In the present invention, it is preferred to use higher alcohols and fatty acid glycerides in combination as the release agent. When higher alcohols and fatty acid glycerides are used in combination, the ratio is not particularly limited, and the amount of higher alcohols used: the amount of fatty acid glycerides used is preferably 2.5:1 to 3.5:1 in terms of mass ratio, and more preferably 2.8:1 to 3.2:1.
[0153] The polymer processing aid is a compound that exerts an effect on thickness accuracy and thin film formation when the methacrylic resin composition is molded. The polymer processing aid is generally a polymer particle having a particle size of 0.05 to 0.5 μm that can be produced by emulsion polymerization.
[0154] Examples of the antistatic agent include alkyl sulfonates such as sodium heptyl sulfonate, sodium octyl sulfonate, sodium nonyl sulfonate, sodium decyl sulfonate, sodium dodecyl sulfonate, sodium cetyl sulfonate, sodium octadecyl sulfonate, sodium diheptyl sulfonate, potassium heptyl sulfonate, potassium octyl sulfonate, potassium nonyl sulfonate, potassium decyl sulfonate, potassium dodecyl sulfonate, potassium cetyl sulfonate, potassium octadecyl sulfonate, potassium diheptyl sulfonate, lithium heptyl sulfonate, lithium octyl sulfonate, lithium nonyl sulfonate, lithium decyl sulfonate, lithium dodecyl sulfonate, lithium cetyl sulfonate, lithium octadecyl sulfonate, and lithium diheptyl sulfonate.
[0155] As flame retardants, there can be listed: metal hydrates having hydroxyl groups or water of crystallization, such as magnesium hydroxide, aluminum hydroxide, hydrated aluminum silicate, water and magnesium silicate, and hydrotalcite; phosphoric acid compounds such as polyphosphoric acid amine and phosphoric acid esters; silicon compounds, etc., preferably phosphate ester flame retardants such as trimethyl phosphate, triethyl phosphate, tripropyl phosphate, tributyl phosphate, tripentyl phosphate, trihexyl phosphate, tricyclohexyl phosphate, triphenyl phosphate, tricresyl phosphate, tri(xylyl) phosphate, dimethyl ethyl phosphate, methyl dibutyl phosphate, ethyl dipropyl phosphate, and hydroxyphenyl diphenyl phosphate.
[0156] Examples of dyes / pigments include red organic pigments such as para red, flame red, pyrazolone red, thioindigo red, and pyrene red; blue organic pigments such as cyanine blue and indanthrene blue; and green organic pigments such as cyanine green and naphthol green. These may be used alone or in combination of two or more.
[0157] Examples of the matting agent include glass fine particles, polysiloxane crosslinked fine particles, crosslinked polymer fine particles, mica, talc, calcium carbonate, and barium sulfate.
[0158] Examples of the anti-adhesion agent include fatty acids such as stearic acid and palmitic acid; fatty acid metal salts such as calcium stearate, zinc stearate, magnesium stearate, potassium palmitate, and sodium palmitate; waxes such as polyethylene wax, polypropylene wax, and montanic acid wax; low molecular weight polyolefins such as low molecular weight polyethylene and low molecular weight polypropylene; acrylic resin powder; polyorganosiloxanes such as dimethylpolysiloxane; octadecylamine; alkyl phosphate; fatty acid ester; amide resin powders such as ethylenebisstearamide; fluororesin powders such as tetrafluoroethylene resin; molybdenum disulfide powder; silicone resin powder; silicone rubber powder; silicon dioxide, etc.
[0159] Examples of the impact resistance modifier include a core-shell type modifier containing a diene rubber as a core layer component and a modifier containing a plurality of rubber particles.
[0160] Examples of the fluorescent substance include fluorescent pigments, fluorescent dyes, fluorescent white dyes, fluorescent brighteners, and fluorescent bleaching agents.
[0161] When the methacrylic resin composition contains other polymers and / or additives, they may be added during the polymerization of the methacrylic resin (A) and / or the acrylic multilayer polymer (B) and / or the acrylic block copolymer (C), may be added during the mixing of the methacrylic resin (A) and / or the acrylic multilayer polymer (B) and / or the acrylic block copolymer (C), or may be added after the mixing of the methacrylic resin (A) and / or the acrylic multilayer polymer (B) and / or the acrylic block copolymer (C).
[0162] The molded article of the present invention can be molded by melt extrusion on the basis of controlling the dispersed phase of the acrylic block polymer (C). The molded article is also useful as a film, for example, it can be well processed by using the inflation method and T-die extrusion method, or calendaring method, and solution casting method, which are usually used as melt extrusion methods. In addition, as required, both sides of the film are simultaneously contacted with rollers or metal belts, especially simultaneously contacted with rollers or metal belts heated to a temperature above the glass transition temperature, thereby obtaining a film with better surface properties. In addition, according to the purpose, the film can also be modified by lamination molding and biaxial stretching of the film. Among them, the T-die extrusion method is particularly preferred. The thickness of the film is preferably 20 to 200 μm, more preferably 30 to 100 μm.
[0163] In order to disperse the acrylic block polymer into a columnar phase, in the T-die extrusion method, the ratio Dr / Dt of the die lip opening (Dr) to the thickness (Dt) of the molded body is preferably in the range of 1≤Dr / Dt≤20, and more preferably in the range of 3≤Dr / Dt≤10. If Dr / Dt is less than 1, the acrylic block polymer will be a spherical phase with a large dispersed particle size, and whitening will occur when stress is applied. On the other hand, if Dr / Dt exceeds 20, a columnar phase with a large major diameter will be formed, whitening will occur when stress is applied, and the anisotropy will increase.
[0164] When using a T-die to manufacture, the shear rate applied when the die is discharged is preferably in the range of 200 to 650 / s, more preferably in the range of 300 to 550 / s. If the shear rate is less than 200 / s, the shear applied to the block copolymer is small, the dispersed particle size becomes larger, and whitening occurs. On the other hand, if the shear rate exceeds 650 / s, strong shear is applied to the block copolymer, the dispersed particle size becomes less than 1nm, and the bendability of the molded body cannot be expressed.
[0165] The methacrylic melt extrusion molded product of the present invention, particularly a film, can be used by laminating on metal, plastic, etc. Examples of the lamination method include wet lamination, dry lamination, extrusion lamination, hot melt lamination, etc., in which an adhesive is applied to a metal plate such as a steel plate, and then the film is placed on the metal plate and dry-laminated.
[0166] Examples of methods for laminating a film on a plastic component include film insert molding in which a film is placed in a mold and filled with resin by injection molding; lamination-injection-extrusion molding; and in-mold film injection molding in which a film is preformed and placed in a mold and filled with resin by injection molding.
[0167] The methacrylic melt-extruded film of the present invention may be further laminated with a functional layer or a thermoplastic resin film to form a laminated film.
[0168] When the molded article of the present invention is a methacrylic melt extruded film, the methacrylic melt extruded film and the functional layer can be stacked to form a laminated film. The functional layer can be formed on one side or both sides of the film. As the functional layer, a hard coat layer, an anti-glare layer, an anti-reflection layer, an antistatic layer, etc. can be listed, and at least one layer of these can be included.
[0169] When the methacrylic melt-extruded film as the molded product of the present invention is a laminated film in which a functional layer and a film are laminated, the thickness of the functional layer is preferably 0.1 to 20 μm, more preferably 1 to 10 μm, and the thickness of the laminated film is preferably 20 to 220 μm, more preferably 30 to 110 μm.
[0170] When the molded article of the present invention is a methacrylic melt extruded film, the methacrylic melt extruded film and the thermoplastic resin film can be stacked to form a laminated film. The thermoplastic resin film can be formed on one side or both sides of the methacrylic melt extruded film. As the thermoplastic resin of the thermoplastic resin film, for example, various thermoplastic resins such as polyolefins (polyethylene, polypropylene, polymethylpentene, etc.), polystyrene, polycarbonate, polyvinyl chloride, methacrylic resins, nylon, polyethylene terephthalate, and copolymers having a variety of monomer units constituting these thermoplastic resins can be cited. In the thermoplastic resin film, only one thermoplastic resin can be included, or two or more can be included.
[0171] In the case of a laminated film comprising the methacrylic melt extruded film of the present invention and a thermoplastic resin film, the thickness of the thermoplastic resin film is preferably 20 to 200 μm, more preferably 30 to 100 μm, and the thickness of the methacrylic melt extruded film is preferably 5 to 100 μm, more preferably 10 to 15 μm.
[0172] The methacrylic melt-extruded molded product of the present invention can be used for components for various purposes. Specific uses include, for example, surface materials for the following components: sign components or logo films such as advertising towers, vertical signs, cantilever signs, lintel signs, and roof signs; display components such as windows, partitions, and store displays; lighting components such as fluorescent lampshades, mood lighting covers, lampshades, lumen ceilings, light walls, and chandeliers; interior components such as furniture, hangings, and mirrors; architectural components such as doors, domes, safety window glass, partition walls, stair skirts, balcony skirts, and roofs of leisure buildings; aircraft windshields, pilot visors, motorcycle windshields, motorboat windshields, bus sunshades, automobile side visors, rear visors, front wings, headlight covers, skylights, window glass, automobile interior components, shock absorbers, and other automobile exterior components, and other transportation-related components. Components; signs for acoustic imaging, stereo covers, TV protection covers, vending machines, mobile phones, computers and other electronic equipment components; incubators, X-ray machine components and other medical equipment components; mechanical covers, measuring instrument covers, experimental equipment, rulers, dials, observation windows and other equipment-related components; liquid crystal protection panels, light guide plates, light guide films, Fresnel lenses, double convex lenses, front panels of various displays, diffusers and other optical-related components; road signs, navigation boards, curved convex mirrors, sound insulation walls and other traffic-related components; as well as greenhouses, large sinks, box sinks, bathroom components, clock panels, bathtubs, toilets, table mats, game components, toys, face protection masks for welding, back panels of solar cells, front panels for flexible solar cells; computers, mobile phones, furniture, vending machines, bathroom components, etc.
[0173] On the other hand, the methacrylic melt-extruded molded product of the present invention, particularly the laminated laminate of the film, can be used for automobile interior and exterior materials, daily necessities, wallpaper, paint alternative applications, furniture, housings of electrical equipment, housings of OA equipment such as facsimile machines, housings, parts of electrical or electronic devices, bathroom equipment, and the like.
[0174] As described above, the methacrylic melt-extruded molded product of the present invention comprises a methacrylic resin (A), an acrylic multilayer polymer (B) and an acrylic block copolymer (C), and the acrylic block polymer is controlled to be a specific dispersed phase, thereby providing a methacrylic molded product and film suitable for decorative applications and building material applications that are excellent in transparency, surface smoothness, resistance to whitening due to bending, pencil hardness and bendability.
[0175] Example
[0176] Next, the effects of the present invention are described by showing embodiments and comparative examples. It should be noted that the present invention is not limited by the following embodiments. In addition, in the following description, "part" means "part by mass" and "%" means "% by mass" unless otherwise stated.
[0177] The methacrylic acid-based melt-extrusion molded product as a film was evaluated by the following method.
[0178] [Morphology observation]
[0179] Using the films (75 μm thick) produced in the examples and comparative examples described later, cross-sectional slices were prepared at a thickness of 50 nm on a surface parallel to the extrusion direction using an ultramicrotome (Leica EM UC7rt manufactured by JEOL Ltd.). The prepared slices were stained with a 10% phosphotungstic acid aqueous solution, and the shape of the stained portion (the average particle size (de) of the rubber component layer (b1) in the acrylic multilayer polymer (B) and the morphology of the acrylic polymer block (c2) in the acrylic block copolymer (C)) was observed using STEM (main body: JSM-7600F, detector: SM-74240RTED manufactured by JEOL Ltd.).
[0180] (Dispersed into spherical phase)
[0181] When the acrylic block copolymer is dispersed in a sphere, two kinds of spherical dyed parts with different particle sizes are observed, in which the block copolymer and the acrylic multilayer polymer are dyed respectively. The average particle size of 30 dyed parts is measured for each of the two spherical dyed parts, and the component with the smaller average particle size is taken as the diameter of the block copolymer ( Figure 1 ).
[0182] (Dispersed into columnar phase)
[0183] When the acrylic block copolymer is dispersed in a cylinder, the dyed portion dispersed in a cylinder is regarded as the block copolymer, and the major diameter and the minor diameter are measured for 30 of the dyed portions, and the average value is regarded as the major diameter and the minor diameter ( Figure 2 ).
[0184] (acetone insoluble components)
[0185] 2 g of the prepared film (75 μm thick) (mass before separation) was placed in 50 mL of acetone and stirred at room temperature for 24 hours. All the liquid obtained was centrifuged at 20,000 rpm, 0°C, and 180 minutes using a centrifuge (manufactured by Hitachi Koki Co., Ltd.). The supernatant and the precipitate were collected separately and vacuum dried at 50°C for 8 hours to obtain an acetone-soluble component and an acetone-insoluble component. The mass of the obtained precipitate was measured, and the proportion of the acetone-insoluble component was calculated based on the following formula.
[0186] Acetone insoluble content (%) = [(mass of precipitate) / (mass before separation)] × 100
[0187] (Haze)
[0188] The resin film (thickness 75 μm) was cut into a 50 mm×50 mm test piece, and the haze was measured at 23° C. in accordance with JIS K7105 and evaluated according to the following criteria.
[0189] 〇: 0.5% or less
[0190] Δ: 0.5%~1.0%
[0191] ×: 1.0% or more
[0192] 〔ΔHaze before and after heating〕
[0193] The resin film (75 μm thick) was cut into 100 mm×100 mm test pieces and heated in an oven set at 100° C. for 30 minutes. The haze of the sample immediately after heating was measured, and the difference from the haze value before heating was calculated as Δ haze and evaluated according to the following criteria.
[0194] 〇: 0.5% or less
[0195] Δ: more than 0.5% and less than 1.0%
[0196] ×: 1.0% or more
[0197] 〔Film pencil hardness〕
[0198] The resin film (75 μm) was cut into a 10 cm×10 cm test piece, and the pencil hardness was measured in accordance with JIS K5600-5-4 and evaluated according to the following criteria.
[0199] ○: 2B or above
[0200] ×: 3B or below
[0201] (Stress whitening resistance)
[0202] A film having a thickness of 75 μm was bent at 90° at room temperature (23° C.), and the presence or absence of whitening at the bent portion was checked.
[0203] ○: No whitening
[0204] ×: Whitening
[0205] (MIT bendability)
[0206] A test piece was collected from the center of a film having a thickness of 75 μm, and the number of bends in a direction perpendicular to the film running direction was measured by a method based on ISO 5626 (JIS P8115 (2001)), and evaluated based on the following criteria.
[0207] ◎: More than 60 times
[0208] 0:30 times or more
[0209] ×: Less than 30 times
[0210] [Moldability (250% stretchability)]
[0211] The resin molded body (film with a thickness of 75 μm) was cut into 20 cm × 30 cm, and a single side thereof was subjected to corona discharge treatment, followed by aluminum deposition by vacuum evaporation to obtain a laminated film. The thickness of the aluminum layer was 30 nm. The laminated film was cut into 100 mm × 100 mm as a test piece, and was set in a biaxial stretching birefringence measuring device (manufactured by ヱトー Co., Ltd., SDR-563K), and stretched under the conditions of a temperature of 145 ° C, a stretching speed of 3600% / min, and a stretching ratio of 250%. In the method, 5 test pieces were stretched and evaluated as follows.
[0212] 0: No breakage occurred in any piece.
[0213] Δ: One or two sheets were broken.
[0214] ×: Three or more sheets were broken.
[0215] [Appearance after molding (evaporation properties)]
[0216] The laminated film obtained above was placed on a white paper (manufactured by FUJI Xerox Co., Ltd., C2r), and the appearance of the non-vapor-deposited surface was evaluated by visual inspection for specular glossiness under a fluorescent lamp (200 lux).
[0217] ○: Mirror gloss (no whitening)
[0218] Δ: Slightly mirror-like gloss (no whitening)
[0219] ×: No mirror gloss (whitening)
[0220] [Average particle size of rubber component layer (b1)]
[0221] Using the film (75 μm thick) produced in the examples and comparative examples described later, a cross-sectional slice of a surface parallel to the extrusion direction was prepared with a thickness of 50 nm using an ultra-thin slicer (Leica EM UC7rt manufactured by JEOL Ltd.). The prepared slice was electron stained with a 10% phosphotungstic acid aqueous solution, and the shape (morphology) of the stained portion was observed using an electron microscope (main body: JSM-7600F, detector: SM-74240RTED manufactured by JEOL Ltd.). For the observed spherical stained portions, the average particle size of 30 stained portions was measured, and this was taken as the average particle size of the rubber component layer (b1).
[0222] (Production Example 1) Acrylic Multilayer Polymer (B-1)
[0223] 150 parts by mass of deionized water, 0.10 parts by mass of sodium polyoxyethylene tridecyl ether acetate and 0.05 parts by mass of sodium carbonate were added to a reactor equipped with a stirrer, a thermometer, a nitrogen inlet pipe, a monomer inlet pipe and a reflux condenser. After the container was fully substituted with nitrogen to achieve a substantially oxygen-free state, the internal temperature was set to 80°C. 0.01 parts by mass of potassium persulfate was added thereto and stirred for 5 minutes. Then, 10 parts by mass of a mixture consisting of methyl methacrylate, methyl acrylate and allyl methacrylate in a mass ratio of 93.9 / 6.1 / 0.2 was continuously added dropwise for 50 minutes. After the addition was completed, the reaction was allowed to proceed for about 30 minutes until the polymerization rate reached 98% or more.
[0224] Next, 0.05 parts by mass of potassium persulfate was added to the reactor and stirred for 5 minutes. Then, 50 parts by mass of a mixture of n-butyl acrylate, styrene and allyl methacrylate in a mass ratio of 82.2 / 17.8 / 4.0 was added dropwise over 90 minutes. After the addition was completed, the reaction was allowed to proceed for about 60 minutes until the polymerization rate reached 98% or more.
[0225] Next, 0.04 parts by mass of potassium persulfate was added to the reactor and stirred for 5 minutes. Then, 40 parts by mass of a mixture of methyl methacrylate, methyl acrylate and n-octyl mercaptan in a mass ratio of 94.0 / 6.0 / 0.3 was continuously added dropwise for 30 minutes. After the addition was completed, the reaction was carried out for about 60 minutes until the polymerization rate reached 98% or more. A latex containing multilayer particles (B-1) with a volume average particle size of 110 nm was obtained. The average particle size of the rubber component layer (b-1) was 80 nm.
[0226] (Production Example 2) Acrylic Multilayer Polymer (B-2)
[0227] 150 parts by mass of deionized water, 0.03 parts by mass of sodium polyoxyethylene tridecyl ether acetate and 0.05 parts by mass of sodium carbonate were added to a reactor equipped with a stirrer, a thermometer, a nitrogen inlet pipe, a monomer inlet pipe and a reflux condenser. After the container was fully substituted with nitrogen to achieve a substantially oxygen-free state, the internal temperature was set to 80°C. 0.01 parts by mass of potassium persulfate was added thereto and stirred for 5 minutes. Then, 10 parts by mass of a mixture consisting of methyl methacrylate, methyl acrylate and allyl methacrylate in a mass ratio of 93.9 / 6.1 / 0.2 was continuously added dropwise for 50 minutes. After the addition was completed, the reaction was allowed to proceed for about 30 minutes until the polymerization rate reached 98% or more.
[0228] Next, 0.05 parts by mass of potassium persulfate was added to the reactor and stirred for 5 minutes. Then, 50 parts by mass of a mixture of n-butyl acrylate, styrene and allyl methacrylate in a mass ratio of 82.2 / 17.8 / 4.0 was continuously added dropwise over 90 minutes. After the addition was completed, the reaction was allowed to proceed for about 60 minutes until the polymerization rate reached 98% or more.
[0229] Next, 0.04 parts by mass of potassium persulfate was added to the reactor and stirred for 5 minutes. Then, 40 parts by mass of a mixture of methyl methacrylate, methyl acrylate and n-octyl mercaptan in a mass ratio of 94.0 / 6.0 / 0.3 was continuously added dropwise for 30 minutes. After the addition was completed, the reaction was carried out for about 60 minutes until the polymerization rate reached 98% or more. A latex containing multilayer structure polymer particles (B-2) with a volume average particle size of 220 nm was obtained. The average particle size of the rubber component layer (b-1) was 200 nm.
[0230] (Production Example 3) Methacrylic Resin (A-1)
[0231] Methacrylic resin (A-1): A methacrylic copolymer composed of methyl methacrylate (MMA) units (content 99.3 mass %) and methyl acrylate (MA) units (content 0.7 mass %), with Mw=84000 and Mw / Mn=2.1, was prepared according to a conventional method.
[0232] (Production Example 4) Methacrylic Resin (A-2)
[0233] Methacrylic resin (A-2): A methacrylic copolymer composed of methyl methacrylate (MMA) units (content 93.6 mass %) and methyl acrylate (MA) units (6.4 mass %), with Mw=120,000 and Mw / Mn=2.1, was prepared according to a conventional method.
[0234] (Production Example 5) Block Copolymer (C-1)
[0235] Block copolymer (C-1): A diblock copolymer composed of [methyl methacrylate (MMA) polymer block (c1)]-[n-butyl acrylate (BA) / benzyl acrylate (BzA) copolymer block (c2)] was prepared according to a conventional method, with a weight average molecular weight (Mw) of 120,000, a mass ratio of polymer blocks (c1): (c2) of 50:50, and a mass ratio of each monomer (MMA:BA) = (50:50).
[0236] (Production Example 6) Block Copolymer (C-2)
[0237] Block copolymer (C-2): A triblock copolymer composed of [methyl methacrylate (MMA) polymer block (c1)]-[n-butyl acrylate (BA) polymer block (c2)]-[methyl methacrylate (MMA) polymer block (c1)], with a weight average molecular weight (Mw) of 70,000, a mass ratio of polymer blocks (b1): (b2): (b1) of 14.3:50.0:35.7, and a mass ratio of each monomer (MMA:BA) = (50:50).
[0238] (Production Example 7) Block Copolymer (C-3)
[0239] Block copolymer (C-3): A triblock copolymer composed of [methyl methacrylate (MMA) polymer block (c1)]-[n-butyl acrylate (BA) polymer block (c2)]-[methyl methacrylate (MMA) polymer block (c1)], with a weight average molecular weight (Mw) of 65,000, a mass ratio of polymer blocks (c1): (c2): (c1) of 15:70:15, and a mass ratio of each monomer (MMA:BA) = (30:70).
[0240] (Production Example 8) Block Copolymer (C-4)
[0241] Block copolymer (C-4): A triblock copolymer composed of [methyl methacrylate (MMA) polymer block (c1)]-[n-butyl acrylate (BA) polymer block (c2)]-[methyl methacrylate (MMA) polymer block (c1)], with a weight average molecular weight (Mw) of 120,000, a mass ratio of polymer blocks (c1): (c2): (c1) of 8.5:83:8.5, and a mass ratio of each monomer (MMA:BA) = (17:83).
[0242] (Example 1)
[0243] 47 parts of pellets of an acrylic multilayer polymer (B-1), 50 parts of a methacrylic resin (A-1) (100% structural units from MMA, weight average molecular weight 80,000), and 3 parts of pellets of an acrylic block copolymer (C-1) were mixed using a twin-screw extruder and pelletized using a pelletizer to obtain a thermoplastic resin (R1).
[0244] A single screw vented extruder with a screw diameter of 50 mm and a T-die with a width of 500 mm and a lip opening of 0.5 mm was used to melt extrude a thermoplastic resin (R1) at a discharge rate of 40 kg / h and a resin temperature of 260°C to obtain a film-like melt. The shear rate was 480 / s. The melt was then clamped and pressed with a linear pressure of 30 kg / cm by a first clamping roll consisting of a mirror-finished metal elastic roll adjusted to 85°C and a mirror-finished metal rigid roll adjusted to 90°C with a gap of 50 μm, and then clamped and pressed with a second clamping roll consisting of a mirror-finished metal rigid roll adjusted to 90°C and a mirror-finished metal rigid roll adjusted to 85°C with a gap of 50 μm, to obtain a single-layer resin film (1) with a thickness of 75 μm (acetone insoluble content 28%).
[0245] The obtained resin film (1) was confirmed to have a morphology of block copolymer by the above-mentioned measuring method, and the result was spherical dispersion with a diameter of 20 nm. Various evaluations were performed on the film. The evaluation results are shown in Table 1. The resin film (1) was excellent in transparency, surface hardness, stress whitening resistance and bendability.
[0246] (Example 2)
[0247] A resin film (2) (acetone insoluble content 28%) was obtained by the same method as in Example 1 except that C-2 was used as the acrylic block copolymer. The morphology of the obtained resin film (2) was confirmed by the above-mentioned measurement method, and the result was that the block copolymer was dispersed in a columnar shape with a short diameter of 20 nm and a long diameter of 100 nm. The evaluation results are shown in Table 1. The resin film (2) was excellent in transparency, surface hardness, stress whitening resistance and bendability.
[0248] (Example 3)
[0249] A resin film (3) (acetone insoluble content 29%) was obtained by the same method as in Example 1 except that the acrylic multilayer polymer (B-1) was changed to 49 parts and the acrylic block copolymer was changed to 1 part of C-3. The morphology of the obtained resin film (3) was confirmed by the above-mentioned measurement method, and the result was that the block copolymer was dispersed in a columnar shape with a short diameter of 20 nm and a long diameter of 100 nm. The evaluation results are shown in Table 1. The resin film (3) was excellent in transparency, surface hardness, stress whitening resistance and bendability.
[0250] (Example 4)
[0251] A resin film (4) (39% acetone insoluble content) was obtained by the same method as in Example 1 except that the acrylic multilayer polymer (B-1) was changed to 65 parts, the methacrylic resin (A-1) was changed to 30 parts, and the acrylic block copolymer (C-2) was changed to 5 parts. The morphology of the obtained resin film (4) was confirmed by the above-mentioned measurement method, and the result was that the block copolymer was dispersed in a columnar shape with a short diameter of 20 nm and a long diameter of 200 nm. The evaluation results are shown in Table 1. The resin film (4) was excellent in transparency, surface hardness, and stress whitening resistance, and was particularly excellent in bendability.
[0252] (Example 5)
[0253] A resin film (5) (36% acetone insoluble content) was obtained by the same method as in Example 1 except that the acrylic multilayer polymer (B-1) was changed to 60 parts, the methacrylic resin (A-1) was changed to 30 parts, and the acrylic block copolymer (C-1) was changed to 10 parts. The morphology of the block copolymer was confirmed by the above-mentioned measurement method for the obtained resin film (5). The result was that the block copolymer was dispersed in a columnar shape with a short diameter of 20 nm and a long diameter of 300 nm. The evaluation results are shown in Table 1. The resin film (5) was excellent in transparency, surface hardness, and stress whitening resistance, and was particularly excellent in bendability.
[0254] (Example 6)
[0255] A resin film (6) (acetone insoluble component 28%) was obtained by the same method as in Example 1 except that the methacrylic resin (A-2) was changed to 50 parts and the acrylic block copolymer (C-2) was changed to 3 parts. The morphology of the obtained resin film (6) was confirmed by the above-mentioned measurement method, and the result was that the block copolymer was dispersed in a columnar shape with a short diameter of 20 nm and a long diameter of 200 nm. The evaluation results are shown in Table 1. The resin film (6) was excellent in transparency, surface hardness, and stress whitening resistance, and was particularly excellent in bendability.
[0256] (Example 7)
[0257] A resin film (7) (acetone insoluble component 27%) was obtained by the same method as in Example 1 except that the acrylic multilayer polymer (B-1) was changed to 40 parts, the acrylic multilayer polymer (B-2) was changed to 5 parts, and the acrylic block copolymer (C-2) was changed to 5 parts. The morphology of the obtained resin film (7) was confirmed by the above-mentioned measurement method, and the result was that the block copolymer was dispersed in a columnar shape with a short diameter of 20 nm and a long diameter of 200 nm. The evaluation results are shown in Table 1. The resin film (7) had poor transparency, but excellent pencil hardness and stress whitening resistance, and particularly excellent bendability.
[0258] (Comparative Example 1)
[0259] A resin film (8) (acetone insoluble component 28%) was obtained by the same method as in Example 1 except that the methacrylic resin (A-2) was changed to 50 parts and the acrylic block copolymer (C-3) was changed to 5 parts. The morphology of the block copolymer of the obtained resin film (8) was confirmed by the above-mentioned measurement method, and the result was that it was dispersed in a columnar shape with a short diameter of 30nm and a long diameter of more than 1000nm. The evaluation results are shown in Table 1. The dispersed particle size of the block copolymer of the resin film (8) was large, and whitening occurred when bent.
[0260] (Comparative Example 2)
[0261] A resin film (9) (acetone insoluble content 22%) was obtained by the same method as in Example 1 except that the acrylic multilayer polymer (B-1) was changed to 37 parts and the acrylic block copolymer (C-2) was changed to 10 parts. The morphology of the block copolymer in the obtained resin film (9) was confirmed by the above-mentioned measurement method, and the result was that it was dispersed in a columnar shape with a short diameter of 40 nm and a long diameter of 600 nm. The evaluation results are shown in Table 1. The dispersed particle size of the block copolymer in the resin film (9) was large, and whitening occurred when it was bent.
[0262] (Comparative Example 3)
[0263] A resin film (10) (37% acetone insoluble content) was obtained by the same method as in Example 1 except that the acrylic multilayer polymer (B-1) was changed to 40 parts and the acrylic multilayer polymer (B-2) was changed to 10 parts instead of the acrylic block copolymer. The evaluation results are shown in Table 1. The transparency of the resin film (10) was deteriorated due to the influence of the addition of the multilayer polymer with a large particle size.
[0264] (Comparative Example 4)
[0265] A resin film (11) (acetone insoluble component 30%) was obtained by the same method as in Example 1 except that the acrylic multilayer polymer (B-1) was changed to 50 parts and the acrylic block copolymer was changed to 0 parts. The evaluation results are shown in Table 1. Since the resin film (11) did not contain the block copolymer, it had poor bendability and was expected to be easily broken during processing.
[0266] (Comparative Example 5)
[0267] A resin film (12) (acetone insoluble content 54%) was obtained by the same method as in Example 1 except that the acrylic multilayer polymer (B-1) was changed to 90 parts, the methacrylic resin (A-1) was changed to 10 parts, and the acrylic block copolymer was changed to 0 parts. The evaluation results are shown in Table 1. Since the resin film (12) contained a large amount of the multilayer polymer, it had excellent bendability, but its surface hardness was poor.
[0268] (Comparative Example 6)
[0269] A resin film (13) with a thickness of 75 μm (36% acetone insoluble content) was obtained by the same method as in Example 5 except that the lip opening was set to 1.5 mm. The morphology of the block copolymer in the obtained resin film (13) was confirmed by the above-mentioned measurement method, and the result was that it was dispersed in spheres with a diameter of 200 nm. The evaluation results are shown in Table 1. The dispersed particle size of the block copolymer in the resin film (13) was large, and whitening occurred when bent.
[0270] (Example 8)
[0271] A resin film (14) (acetone insoluble content: 28.8% by mass) was obtained by the same method as in Example 1 except that 48 parts of the pellets of the multilayer structure polymer particles (B-1), 50 parts of the pellets of the methacrylic resin (A-1), and 2 parts of the pellets of the block copolymer (C-2) were used. The evaluation results are shown in Table 1. The resin film (14) was excellent in transparency, surface hardness, moldability, and vapor deposition properties.
[0272] (Example 9)
[0273] A resin film (15) (39.6% by mass of acetone insoluble components) was obtained by the same method as in Example 1 except that 66 parts of the pellets of the multilayer structure polymer particles (B-1), 30 parts of the pellets of the methacrylic resin (A-2), and 4 parts of the pellets of the block copolymer (C-2) were used. The evaluation results are shown in Table 1. The resin film (15) was excellent in transparency, surface hardness, moldability, and vapor deposition properties.
[0274] (Example 10)
[0275] A resin film (16) (acetone insoluble content: 27.0% by mass) was obtained by the same method as in Example 1 except that 45 parts of the pellets of the multilayer structure polymer particles (B-1), 52 parts of the pellets of the methacrylic resin (A-2), and 3 parts of the pellets of the acrylic block copolymer (C-3) were used. The evaluation results are shown in Table 1. The resin film (16) was excellent in transparency, surface hardness, moldability, and vapor deposition properties.
[0276] (Example 11)
[0277] A resin film (17) (16.8% by mass of acetone insoluble components) was obtained by the same method as in Example 1 except that 30 parts of the pellets of the multilayer structure polymer particles (B-1), 66 parts of the pellets of the methacrylic resin (A-1), and 4 parts of the pellets of the block copolymer (C-2) were used. The evaluation results are shown in Table 1. The resin film (17) was excellent in transparency, surface hardness, moldability, and vapor deposition properties.
[0278] (Example 12)
[0279] A resin film (18) (acetone insoluble content: 27.0% by mass) was obtained by the same method as in Example 1 except that 45 parts of the pellets of the multilayer polymer particles (B-1), 51 parts of the pellets of the methacrylic resin (A-2), and 4 parts of the pellets of the acrylic block copolymer (C-4) were used. The evaluation results are shown in Table 1. The resin film (18) had a slightly poor haze, but was excellent in surface hardness, moldability, and vapor deposition properties.
[0280] (Comparative Example 7)
[0281] A resin film (19) (acetone insoluble component: 23.8% by weight) was obtained by the same method as in Example 1 except that 36 parts of the pellets of the multilayered polymer particles (B-2), 59 parts of the pellets of the methacrylic resin (A-2), and 5 parts of the pellets of the block copolymer (C-2) were used. The evaluation results are shown in Table 1. The resin film (19) showed an increase in haze after heating, and white turbidity was observed in the appearance after vapor deposition and molding.
[0282] (Comparative Example 8)
[0283] A resin film (20) (acetone insoluble component 48.0 mass %) was obtained by the same method as in Example 1 except that 80 parts of the pellets of the multilayer structure polymer particles (B-1) and 20 parts of the pellets of the methacrylic resin (A-2) were used. The evaluation results are shown in Table 1. The pencil hardness of the resin film (20) was low, and the appearance after molding was turbid.
[0284] (Comparative Example 9)
[0285] A resin film (21) (acetone insoluble component 0 mass %) was obtained by the same method as in Example 1 except that 85 parts of the pellets of the methacrylic resin (A-1) and 15 parts of the pellets of the block copolymer (C-2) were used. The evaluation results are shown in Table 1. The resin film (21) was very brittle and cracked during molding.
[0286] (Comparative Example 10)
[0287] A resin film (22) (18.0% by mass of acetone insoluble components) was obtained by the same method as in Example 1 except that 30 parts of the pellets of the multilayered polymer particles (B-1), 20 parts of the pellets of the methacrylic resin (A-1), and 50 parts of the pellets of the block copolymer (C-2) were used. The evaluation results are shown in Table 1. The pencil hardness of the resin film (22) was reduced.
[0288] [Table 1]
[0289] Table 1
[0290]
[0291] Table 1 (continued)
[0292]
[0293] Table 1 (continued)
[0294]
[0295] Table 1 (continued)
[0296]
[0297] The above results demonstrate that the film of the present invention is excellent in transparency, surface smoothness, resistance to whitening on bending, pencil hardness, bendability, formability and appearance after forming, and is suitable for decorative purposes.
Claims
1. A methacrylic acid melt extrusion molded product, comprising: A methacrylic resin (A) comprising 80% by mass or more of methyl methacrylate units and having a weight average molecular weight of 60,000 or more and 200,000 or less; An acrylic multilayer polymer (B) having at least one rubber component layer (b1) inside and at least one thermoplastic resin component layer (b2), the outermost being the thermoplastic resin component layer (b2), and the average particle size of the rubber component layer (b1) being in the range of 0.05 to 0.15 μm; and an acrylic block copolymer (C) comprising a methacrylate polymer block (c1) and an acrylate polymer block (c2), The methacrylic acid melt extrusion molded product is characterized in that The content of the methacrylic resin (A) in the methacrylic melt-extrusion molded product is 20 to 79% by mass. The acetone insoluble content of the molded body is 1 to 60% by mass, and in a cross section of the molded body parallel to the extrusion direction, the acrylic ester polymer block (c2) forms a columnar phase, the short axis of the columnar phase is 1 nm to 100 nm, and the long axis of the columnar phase is 200 nm to 500 nm. In the acrylic multilayer polymer (B), the rubber component layer (b1) comprises a copolymer composed of 50 to 98.99% by mass of acrylic ester monomer units, 1 to 44.99% by mass of other monofunctional monomer units and 0.01 to 10% by mass of multifunctional monomer units, the thermoplastic resin component layer (b2) comprises a copolymer composed of 40 to 100% by mass of methacrylic ester monomer units and 60 to 0% by mass of other monomer units, and the content of the acrylic multilayer polymer (B) in the methacrylic melt-extruded molded product is 47 to 65% by mass, The acrylic block copolymer (C) comprises at least one methacrylate polymer block (c1) and at least one acrylate polymer block (c2), wherein the acrylic block copolymer (C) comprises 30 to 60% by mass of the methacrylate polymer block (c1) and 40 to 70% by mass of the acrylate polymer block (c2), and the content of the acrylic block copolymer (C) in the methacrylic melt extrusion molded product is 1 to 10% by mass. The total content of the rubber component layer (b1) and the acrylic acid ester polymer block (c2) in the methacrylic acid melt-extruded molded product is 7 to 60% by mass.
2. The methacrylic acid melt-extruded molded product according to claim 1, wherein The methacrylic acid melt-extruded molded product is a film having a thickness of 20 to 200 μm.
3. The methacrylic acid melt-extruded molded product according to claim 1, wherein Also contains matting agent.
4. The methacrylic acid melt-extruded molded product according to claim 1, wherein It also has a functional layer.
5. The methacrylic acid melt-extruded molded product according to claim 1, wherein The methacrylic melt-extruded molded product is a film, and the film is laminated with another thermoplastic resin film. The methacrylic acid melt-extruded molded product according to claim 1 , which is used for decoration.
7. The methacrylic acid melt-extruded molded product according to claim 1, which is used for building materials.
8. The method for producing a methacrylic melt-extruded molded product according to claim 1, comprising the step of melt-extruding a methacrylic resin composition using a T-die, wherein: The methacrylic resin composition comprises: a methacrylic resin (A) containing 80% by mass or more of methyl methacrylate units and having a weight average molecular weight of 60,000 or more and 200,000 or less; an acrylic multilayer polymer (B) having at least one rubber component layer (b1) inside and at least one thermoplastic resin component layer (b2), the outermost being the thermoplastic resin component layer (b2), the rubber component layer (b1) having an average particle size in the range of 0.05 to 0.15 μm; and an acrylic block copolymer (C) containing a methacrylate polymer block (c1) and an acrylate polymer block (c2), The content of the methacrylic resin (A) in the methacrylic melt-extrusion molded product is 20 to 79% by mass. The content of the acrylic multilayer polymer (B) in the methacrylic melt-extruded molded product is 47 to 65% by mass. The acrylic block copolymer (C) comprises 30 to 60% by mass of a methacrylate polymer block (c1) and 40 to 70% by mass of an acrylate polymer block (c2), and the content of the acrylic block copolymer (C) in the methacrylic melt extrusion molded product is 1 to 10% by mass. The total content of the rubber component layer (b1) and the acrylic ester polymer block (c2) in the methacrylic acid melt-extruded molded product is 7 to 60% by mass. In the melt extrusion step, the shear rate applied during extrusion from the die is in the range of 200 to 650 / s, and the ratio Dr / Dt of the die lip opening Dr to the thickness Dt of the molded product is 3≤Dr / Dt≤10.