Crosslinked adhesive composition
By combining the cross-linked thermoplastic polymer adhesive with interacting particles or fibers, the problem of contamination and pore accumulation in the whole part of the porous active medium is solved, and high-quality mechanical strength and performance are achieved , expanding the overall parts production of the processing window.
Patent Information
- Application Number
- CN202080047097.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-06-25
- Filing Date
- 2020-06-23
- Publication Date
- 2024-11-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
When the existing thermoplastic polymer adhesives make porous active media whole parts, it is easy to cause surface contamination of the media and pore size accumulation, affecting their performance, and the processing window is narrow, making it difficult to produce high-quality homogeneous parts.
Crosslinked thermoplastic polymer adhesive is used to combine with interacting particles or fibers to reduce the fluidity of the adhesive through the crosslinking process, ensure the interconnection and structural integrity of the medium, while expanding the range of processing temperature and time.
It significantly reduces the surface contamination and porosity loss of the active medium, improves the mechanical strength and performance of the entire part, expands the processing window, and can produce homogeneous block structures of various sizes.
Smart Images

Figure BDA0003435183010000281 
Figure BDA0003435183010000291 
Figure BDA0003435183010000292
Abstract
Description
Field of the Invention
[0001] The present invention relates to a crosslinked thermoplastic polymer binder and the use of the binder and an active medium made of interactive particles or fibers to form a porous article, a block structure or a monolith. The porous article can be used for filtering, separating or storing fluids, or for components of energy devices (e.g., electrodes of batteries and capacitors). Background of the Invention
[0003] It is well known that porous active media, such as activated carbon, benefit from being combined with a binder and transformed into a monolith or block by processing (e.g., compression molding or extrusion). The binder acts to connect the particles of the active media, thereby holding the structure together, making it easier to handle, and potentially densifying the active media. In order to maximize the performance of the monolith, it is important that the binder does not contaminate (or cover) the surface of the active media, as this can result in a loss of available specific surface area and pore volume, negatively impacting the performance of the media used for filtering, separating, or storing fluid components, or for components of energy devices such as electrodes in batteries and capacitors.
[0004] Thermoplastic polymers are known as binders for active media. They can be made into particulate materials of various particle sizes. During processing (such as compression molding, extrusion or calendaring) above their softening point (which can be described as the glass transition temperature of amorphous polymers and the melting point of crystalline and semi-crystalline polymers), they will experience sufficient deformation (polymer flow) to effectively anchor into the particles of the active media. However, this polymer flow can also lead to fouling of the surface and pores of the active media and reduce the performance of the active media for the intended use.
[0005] US 4,999,330 describes the need for and challenges of high density adsorbent monoliths for gas storage systems. The efficiency of the system depends on the level of surface area and pore volume of the adsorbent, the packing density of the adsorbent, the physical stability of the 3-D structure, and the degree of contamination of the adsorbent. US 4,999,330 uses an aqueous solution of methylcellulose or polyvinyl alcohol binder to coat high surface area carbon particles, then removes the solvent and compresses the binder-coated particles to reduce the total volume by 50% to 200%. The '330 system suffers from its complexity and multiple steps. It also involves coating the entire activated carbon particle - which blocks many of the adsorbent pores - and this contamination reduces the amount of surface area available for adsorption. US 6696384 also describes the use of methylcellulose as an aqueous binder for coating the surface of the active medium. It points out that the mechanical strength of the resulting monolith is low, which it attempts to address by crosslinking the cellulose binder after the monolith is formed. The crosslinking process has no positive impact on significant contamination of the active medium because it occurs while or after the medium is coated to form the monolith.
[0006] Other prior art describes the use of non-aqueous thermoplastic polymer binders in solid form or in the form of solid dispersions in water, which result in less contamination of the active medium because the binder does not coat the entire surface of the active medium, but rather attaches to active medium particles located at discrete points.
[0007] US 5,019,311, 5,147,722 and US 5,331,037 describe an extrusion method for producing a porous structure comprising interacting particles bonded together by a thermoplastic polymer binder. The porous structure is described as a "continuous web matrix" or "forced point bonding". The solid composite article can be used as a high performance water filter, such as a carbon block filter. US6,395,190 describes carbon filters having 15 to 25 weight percent of a polyolefin thermoplastic binder and methods for making them. (IR4203) US 2016 / 121249 notes that selected thermoplastic polymers such as PVDF and polyamides are exceptionally polarizable and have a reduced tendency to wet the carbon surface and cause adsorbent surface contamination compared to other thermoplastics described in the art. (IR4263) US2018 / 104670 describes the use of a PVDF binder with a high molecular weight, subjected to ASTM D-3835 at 450°F and 100 seconds -1 The melt viscosity is greater than 1.0 kp under the conditions of to minimize active particle contamination.
[0008] However, it is well known that all thermoplastic polymer binders will still contaminate the surface of the active medium to some extent, even those with high polarity or high molecular weight, high viscosity. This is because they undergo some deformation (polymer flow) under the temperature and pressure conditions required to make the monolith, which are usually at least 20°C, or at least 40°C, or at least 60°C, or at least 70°C, or at least 80°C, or at least 100°C higher than the softening point of the binder. If the temperature is low enough to prevent polymer flow, the thermoplastic polymer does not have enough chain mobility to anchor to the surface of the active medium and effectively act as a binder to produce a monolith with mechanical integrity. Mechanical integrity can be simply defined as pass / fail, where the mechanical integrity fails if more than 20% by weight of the block composition is not attached to the block structure after the block is formed. If the temperature is high enough to allow effective bonding, then polymer flow will occur and the binder will spread on the surface of the active medium and block the entrances of some pores.
[0009] Because the process equipment used to make monoliths generally does not apply pressure and temperature uniformly across the composition, the use of thermoplastic polymer adhesives generally results in gradients of bonding efficiency and contamination within the monolith, despite providing good structural integrity and mechanical strength. This is particularly true for larger monoliths, where contamination near the outer surface of the monolith in contact with the equipment metal tends to be severe, and bonding in the core of the monolith away from the metal tends to be poor.
[0010] Therefore, there is a need for improvements to the currently described thermoplastic polymer binders to further reduce contamination of the active medium and improve the overall performance of the monolith. There is also a need to widen the processing window to produce monoliths of any size with effective bonding and very low contamination of the active medium throughout the monolith.
[0011] We have now discovered that crosslinked thermoplastic polymers, which are crosslinked prior to use in the present invention, can be used to bind active media in a manner that results in interconnectivity of the media particles with minimal surface and pore contamination. Surprisingly, the crosslinked thermoplastic polymer particles were found to incorporate sufficient local chain mobility on the exterior of the particles to effectively bind particles of active media with little deformation (polymer flow) during fabrication of the monolith. The resulting monoliths have good to excellent mechanical strength and very low active media contamination.
[0012] The mechanical strength of the blocks was assessed visually and given a result of "pass" or "fail." "Pass" means that the block is structurally stable when placed on a flat surface, while "fail" means that the block does not hold together and is at least partially broken.
[0013] Contamination is measured by the loss of BET surface area per gram of active medium when going from pure active medium to a bulk structure. The percentage of contamination of the active medium is the percentage of BET surface area lost per gram of active medium when the active medium becomes a bulk. It is calculated as [1-(BET specific surface area of the bulk*100) / (BET specific surface area of the adsorbent*weight percentage of the adsorbent in the bulk)]*100. High contamination corresponds to contamination greater than 20%, low contamination corresponds to contamination of 1-10%, and very low contamination corresponds to contamination less than 1%. The percentage of contamination is defined as the percentage of BET surface area lost per gram of active medium when the active medium becomes a bulk or monolith. The BET surface area is measured using a QUANTACHROME NOVA-E gas adsorption instrument. Nitrogen adsorption and desorption isotherms are generated at 77K. The multi-point Brunauer-Emmett-Teller (BET) nitrogen adsorption method is used to determine the specific surface area.
[0014] Alternatively, contamination in a block may also be defined as a loss in porosity compared to a theoretical value calculated for zero contamination, which is in the range of 0.3 to 0.9 or 0.4 to 0.8 or 0.5 to 0.7. Porosity may be calculated from the bulk density and skeletal density of the block, since porosity = l - (bulk density / skeletal density). Bulk density is the mass of the block divided by the volume occupied by the block. Skeletal density is the mass of the block divided by the volume occupied by the solid matter in the block, which may be determined using a helium pycnometer method according to ASTM B923-10. Contamination is considered to be very low if the porosity loss is less than 20% or less than 10%; contamination is considered to be extremely low if the porosity loss is less than 9% or less than 5% or less than 1%.
[0015] The processing window can be wider because higher temperatures and / or longer times can be used in compression molding or extrusion without significantly increasing the polymer deformation of the adhesive, thereby achieving excellent bonding throughout the structure while keeping contamination at very low levels. For example, temperatures of more than 40°C above the softening point of the thermoplastic polymer adhesive, or more than 60°C above the softening point of the thermoplastic polymer adhesive, or more than 70°C, or more than 80°C, or more than 100°C above the softening point of the thermoplastic polymer adhesive can be used. This is particularly useful for generating larger blocks.
[0016] Combined active media can form porous articles for filtering, separating, or storing fluid components. Porous articles are particularly useful for removing contaminants from drinking water; separating contaminants from liquid or gaseous industrial streams; capturing and recovering small molecules, such as biologically and pharmaceutically active moieties, precious metals, and the performance of specific chemical reactions from fluid streams, such as by catalysis. Depending on the type of activity of the active media, it can separate dissolved or suspended substances by chemical reaction, physical capture, electrical (charge or ion) attraction, or the like. Porous articles can also be used to safely store or transport gases at moderate pressures due to the ability of the active media to adsorb gas molecules.
[0017] The present invention solves a common problem of monoliths made of active media and thermoplastic polymer binders, namely that the properties of the active media are partially lost due to contamination of its surface with the binder. Contamination occurs because the binder partially contaminates or covers the surface and / or blocks the entrance to the pores of the active media. This can occur in two ways. The first way is when the binder is used in the form of a solution, in which case the binder coats the surface of the active media in the form of a film. The second way is when the binder is used in a solid form dried or suspended in a liquid, in which case deformation of the binder (polymer flow) under the pressure and temperature conditions used to make the monolith leads to contamination. SUMMARY OF THE INVENTION
[0019] The present invention relates to a solid porous article having a cross-linked thermoplastic binder interconnected with one or more types of interacting powder materials or fibers. Interconnectivity refers to the binder connecting the powder materials or fibers at discrete points, rather than as a complete coating, to allow the materials or fibers to directly contact and interact with the fluid. The resulting article is a shaped multi-component, interconnected network with porosity. The article can be used for water purification, separation of dissolved or suspended substances in aqueous and non-aqueous systems in industrial applications, for gas storage, and for electrodes in energy storage devices.
[0020] The present invention provides a composition having: interactive particles and 0.5-30 weight percent, preferably 1-20 weight percent, of one or more types of cross-linked thermoplastic polymer binder particles, the percentages being based on the total weight of the interactive particles and the cross-linked polymer. The present invention also provides a solid porous article having at least 70 weight percent of interactive particles and 0.5 to 30 weight percent of cross-linked thermoplastic polymer binder particles, based on the total weight of the article. The present invention also provides a method for forming a solid porous article. The present invention also provides a method for separating fluids and a method for storing gases using a solid porous article.
[0021] Once the porous article is formed, the interacting particles exhibit interconnectivity. Interconnectivity refers to the binder connecting the powdered material or fibers as discrete particles at discrete points, rather than as a complete coating, to allow the material or fibers to directly contact and interact with the fluid. The resulting article is a formed multi-component, interconnected network that has porosity. The article can be used for water purification, and for separation of dissolved or suspended materials in aqueous, non-aqueous and gaseous systems in industrial applications. The separation article can operate at ambient temperatures as well as elevated temperatures. The article can be used in gas storage applications. The article can be used in energy storage applications. DETAILED DESCRIPTION OF THE INVENTION
[0023] As used herein, copolymer refers to any polymer having two or more monomeric units, and includes terpolymers and those polymers having more than three different monomeric units.
[0024] All references cited in this application are incorporated herein by reference.
[0025] As used herein, "interconnectivity" refers to the permanent bonding of active particles or fibers by fluoropolymer or polyamide adhesives without completely coating the interacting particles or fibers. The adhesive adheres the interacting particles together at specific discrete points to create an organized porous structure. The porous structure allows fluid to pass through the interconnected particles or fibers, and the fluid composition is directly exposed to the surface of the interacting particles or fibers, facilitating the interaction of the particles with the components of the fluid composition, resulting in separation of the components. Because the polymer adhesive only adheres to the interacting particles at discrete points, less adhesive is used for full connection compared to coating.
[0026] As used herein, percentages are by weight unless otherwise indicated, and molecular weights are weight average molecular weight unless otherwise indicated.
[0027] One or more cross-linked thermoplastic polymer binders are combined with one or more active media (eg, activated carbon) to form a solid structure.
[0028] The cross-linked thermoplastic polymer binder of the present invention results in little contamination of the active medium, resulting in a higher retention of its specific surface area and pore volume, and thus the bulk structure exhibits higher performance for the intended use.
[0029] The cross-linked thermoplastic material of the present invention allows a wider processing window for making bulk structures by compression molding or extrusion, and enables the production of homogeneous bulk structures of various sizes.
[0030] Thermoplastic polymers
[0031] The cross-linked thermoplastic material of the present invention does not include thermosetting polymers. Some examples of thermosetting polymers are epoxy resins, vulcanized rubber, melamine resins, standard polyurethane resins.
[0032] Thermoplastic polymers that can be crosslinked for use in the present invention include: fluoropolymers, polyamides, acrylic polymers, styrene-butadiene rubber (SBR), ethylene-vinyl acetate (EVA), polyimides, polyurethanes, styrenic polymers, polyolefins (including polyethylene and polypropylene), thermoplastic polyesters (including polyethylene terephthalate, polybutylene terephthalate and polylactic acid), cellulose, polyvinyl chloride, polycarbonate and thermoplastic polyurethane (TPU).
[0033] Preferred thermoplastic polymers that can be crosslinked for use in the present invention include: fluoropolymers, polyamides, acrylic polymers, styrenic polymers, polyolefins, polyesters.
[0034] Fluoropolymers
[0035] The term "fluoropolymer" means any polymer having in its chain at least one monomer selected from the following compounds, the compound containing a vinyl group capable of opening for polymerization and containing at least one fluorine atom, at least one fluoroalkyl group or at least one fluoroalkoxy group directly attached to the vinyl group. Examples of fluoropolymers include, but are not limited to: vinyl fluoride; vinylidene fluoride (VDF); trifluoroethylene (VF3); chlorotrifluoroethylene (CTFE); 1,2-difluoroethylene; tetrafluoroethylene (TFE); hexafluoropropylene (HFP); perfluoro(alkyl vinyl) ethers, such as perfluoro(methyl vinyl) ether (PMVE), perfluoro(ethyl vinyl) ether (PEVE) and perfluoro(propyl vinyl) ether (PPVE); perfluoro(1,3-dioxole); perfluoro(2,2-dimethyl-1,3-dioxole) (PDD).
[0036] Preferred fluoropolymers include homopolymers and copolymers, based on weight, copolymers having greater than 50 wt% fluoromonomer units, preferably greater than 65 wt%, more preferably greater than 75 wt%, and most preferably greater than 90 wt% of one or more fluoromonomers. Other monomer units in these polymers include any monomer containing a polymerizable C=C double bond.
[0037] The most preferred copolymers and terpolymers of the present invention are those wherein the vinylidene fluoride units constitute greater than 50% by weight of all monomer units in the polymer, more preferably greater than 70% by weight of the total units. Copolymers, terpolymers and higher polymers of vinylidene fluoride can be prepared by reacting vinylidene fluoride with one or more monomers selected from the group consisting of vinyl fluoride, trifluoroethylene, tetrafluoroethylene, partially or fully fluorinated α-olefins such as one or more of 3,3,3-trifluoro-1-propylene, 1,2,3,3,3-pentafluoropropylene, 3,3,3,4,4-pentafluoro-1-butene and hexafluoropropylene, partially fluorinated olefin hexafluoroisobutylene, perfluorinated vinyl ethers such as perfluoromethyl vinyl ether, perfluoroethyl vinyl ether, perfluoro-n-propyl vinyl ether and perfluoro-2-propoxypropyl vinyl ether, fluorinated dioxoles such as perfluoro(1,3-dioxole) and perfluoro(2,2-dimethyl-1,3-dioxole), allylic, partially fluorinated allylic or fluorinated allylic monomers such as 2-hydroxyethyl allyl ether or 3-allyloxypropylene glycol, and ethylene or propylene.
[0038] Fluoropolymers such as polyvinylidene fluoride based polymers are prepared by any method known in the art. Methods such as emulsion polymerization and suspension polymerization are preferred and are described in US6187885 and EP0120524.
[0039] Synthetic polyamide
[0040] Polyamides are polymers (substances made up of long molecules of many units) in which the repeating units in the molecular chain are linked together by amide groups. Amide groups have the general chemical formula CO-NH. They can be produced by the interaction of amine (NH2) groups and carboxyl (CO2H) groups, or they can be polymerized from amino acids or amino acid derivatives (molecules that contain both amino and carboxyl groups).
[0041] The synthesis of polyamides is well described in the art, examples are WO15 / 071604, WO14179034, EP0550308, EP0550315, US9637595.
[0042] The polyamides may be condensation or ring-opening products of:
[0043] - one or more amino acids, such as aminocaproic acid, 7-aminoheptanoic acid, 11-aminoundecanoic acid and 12-aminododecanoic acid, or one or more lactams, such as caprolactam, enantholactam and lauryl lactam; and
[0044] - one or more salts or mixtures of diamines with diacids, such as hexamethylenediamine, dodecamethylenediamine, meta-xylylenediamine, bis(p-aminocyclohexyl)methane and trimethylhexamethylenediamine, and diacids such as isophthalic acid, terephthalic acid, adipic acid, azelaic acid, suberic acid, sebacic acid and dodecanedicarboxylic acid.
[0045] Examples of polyamides may include PA 6, PA 7, PA 8, PA 9, PA 10, PA 11, and PA 12, and copolyamides such as PA 6,6.
[0046] The copolyamide may be derived from the condensation of at least two α,ω-aminocarboxylic acids, or of two lactams, or of a lactam and an α,ω-aminocarboxylic acid. The copolyamide may be derived from the condensation of at least one α,ω-aminocarboxylic acid (or a lactam), at least one diamine and at least one dicarboxylic acid.
[0047] Examples of lactams include lactams having 3 to 12 carbon atoms in the main ring, which may be substituted, for example, β,β-dimethylpropiolactam, α,α-dimethylpropiolactam, valerolactam, caprolactam, capryllactam and lauryl lactam.
[0048] Examples of α,ω-aminocarboxylic acids include aminoundecanoic acid and aminododecanoic acid. Examples of dicarboxylic acids include adipic acid, sebacic acid, isophthalic acid, succinic acid, 1,4-cyclohexanedicarboxylic acid, terephthalic acid, the sodium or lithium salts of sulfoisophthalic acid, dimer fatty acids (these dimer fatty acids have a dimer content of at least 98%, preferably hydrogenated) and dodecanedioic acid HOOC-(CH2) 10 -COOH.
[0049] The diamine may be an aliphatic diamine having 6 to 12 carbon atoms; it may be aromatic and / or saturated cyclic. Examples include hexamethylenediamine, piperazine, tetramethylenediamine, octamethylenediamine, decamethylenediamine, dodecamethylenediamine, 1,5-diaminohexane, 2,2,4-trimethyl-1,6-diaminohexane, diamine polyols, isophoronediamine (IPD), methylpentamethylenediamine (MPDM), bis(aminocyclohexyl)methane (BACM), and bis(3-methyl-4-aminocyclohexyl)methane (BMACM).
[0050] Examples of copolyamides include copolymers of caprolactam and lauryl lactam (PA 6 / 12), copolymers of caprolactam, adipic acid and hexamethylene diamine (PA 6 / 6-6), copolymers of caprolactam, lauryl lactam, adipic acid and hexamethylene diamine (PA 6 / 12 / 6-6), copolymers of caprolactam, lauryl lactam, 11-aminoundecanoic acid, azelaic acid and hexamethylene diamine (PA 6 / 6-9 / 11 / 12), copolymers of caprolactam, lauryl lactam, 11-aminoundecanoic acid, adipic acid and hexamethylene diamine (PA 6 / 6-6 / 11 / 12), and copolymers of lauryl lactam, azelaic acid and hexamethylene diamine (PA 6-9 / 12).
[0051] Polyamides also include polyamide block copolymers, such as polyether-b-polyamides and polyester-b-polyamides.
[0052] Another polyamide is Arkema's Ultrafine polyamide 6, 12 and 6 / 12 powders which are microporous and have open pores due to their manufacturing process. These powders have a very narrow particle size range which may be between 5 and 60 microns, depending on the grade. Lower average particle sizes of 5 to 20 are preferred.
[0053] Acrylic polymers used herein are intended to include polymers, copolymers and terpolymers formed from methacrylate and acrylate monomers, and mixtures thereof. Methacrylate monomers and acrylate monomers may constitute 51% to 100% of the monomer mixture, and there may be 0 to 49% of other ethylenically unsaturated monomers, including but not limited to styrene, α-methylstyrene, acrylonitrile. Suitable acrylate and methacrylate monomers and comonomers include but are not limited to methyl acrylate, ethyl acrylate and ethyl methacrylate, butyl acrylate and butyl methacrylate, isooctyl methacrylate and isooctyl acrylate, lauryl acrylate and lauryl methacrylate, stearyl acrylate and stearyl methacrylate, isobornyl acrylate and isobornyl methacrylate, methoxyethyl acrylate and methoxyethyl methacrylate, 2-ethoxyethyl acrylate and 2-ethoxyethyl methacrylate, dimethylaminoethyl acrylate and dimethylaminoethyl methacrylate monomers. (Meth) acrylic acid such as methacrylic acid and acrylic acid may be comonomers. Acrylic polymers include multilayer acrylic polymers, such as core-shell structures typically prepared by emulsion polymerization.
[0054] Styrenic polymers as used herein are intended to include polymers, copolymers and terpolymers formed from styrene and α-methylstyrene monomers, and mixtures thereof. Styrene and α-methylstyrene monomers may account for 50% to 100% of the monomer mixture, and there may be 0 to 50% of other ethylenically unsaturated monomers, including but not limited to acrylates, methacrylates, acrylonitrile. Styrenic polymers include but are not limited to polystyrene, acrylonitrile-styrene-acrylate (ASA) copolymers, styrene acrylonitrile (SAN) copolymers, styrene-butadiene copolymers such as styrene-butadiene rubber (SBR), methyl methacrylate-butadiene-styrene (MBS), and styrene-(meth)acrylate copolymers, such as styrene-methyl methacrylate copolymers (S / MMA).
[0055] As used herein, polyolefins are intended to include polyethylene, polypropylene, and copolymers of ethylene and propylene. Ethylene and propylene monomers may account for 51% to 100% of the monomer mixture, and there may be 0 to 49% of other ethylenically unsaturated monomers, including but not limited to acrylates, methacrylates, acrylonitrile, anhydrides. Examples of polyolefins include ethylene-ethyl acetate copolymers (EVA), ethylene-(meth)acrylate copolymers, ethylene-anhydride copolymers and grafted polymers, propylene-(meth)acrylate copolymers, propylene-anhydride copolymers and grafted polymers.
[0056] Cross-linked thermoplastic polymers
[0057] The crosslinked thermoplastic polymers used in the present invention have chemical bonds between adjacent polymer chains due to the use of a crosslinking agent and / or a radiation source. The crosslinked thermoplastic polymers used in the present invention can be blended (crosslinked before or after blending) or sequentially polymerized into an interpenetrating network or core-shell structure. An example of sequential polymerization is an acrylic modified fluoropolymer, which can be made from an emulsion fluoropolymer seed and subsequent acrylic polymerization.
[0058] The crosslinked thermoplastic polymers are insoluble in strong organic solvents known in the art as suitable solvents for the corresponding non-crosslinked thermoplastic polymers, for example, methyl isobutyl ketone, methyl ethyl ketone or N-methyl-2-pyrrolidone. According to ASTM D543, when the crosslinked thermoplastic polymer is exposed to the chemical by immersion at room temperature for 2 hours, 10 hours or 24 hours, the polymer does not dissolve in the solvent, but swells and forms a gel-like material that cannot be filtered through a 0.5 micron PTFE filter. If less than 20 weight percent, or less than 10 weight percent, or less than 5 weight percent of the polymer is present in the filtered solution, the polymer is considered a crosslinked polymer. According to ASTM D-3835 at 230°C and 100 seconds -1The viscosity of the crosslinked thermoplastic polymer is greater than 20 kpoise, preferably greater than 40 kpoise, and more preferably greater than 50 kpoise. The crosslinked thermoplastic polymer has a complex viscosity of greater than 10,000,000 seconds at 230°C when measured by ASTM D4440-01 or ISO 6721 Part 10 at a frequency of 0.1 Hz. -1 This is a dynamic mechanical analysis where the sample is placed in a parallel plate oscillating rheometer and the temperature is raised from room temperature to 250°C at a rate of 5°C per minute and then the complex viscosity is measured as a function of temperature as the temperature is decreased to room temperature at a rate of 2°C, 5°C, 10°C or 20°C per minute.
[0059] The crosslinked thermoplastic polymers may be prepared by any process known in the art, such as emulsion polymerization, suspension polymerization, solvent polymerization, bulk polymerization, and may include post-polymerization processes such as reactive extrusion and radiation curing. Examples of radiation are ultraviolet (UV), gamma rays, electron beams.
[0060] The crosslinked thermoplastic polymer for the present invention is in the form of granular material, is dry form or is suspended in an aqueous medium. The particles of crosslinked thermoplastic polymer can have any size and size distribution. When in powder form, the average particle size of the particles is 1 to 500 microns or 2 to 200 microns or 5 to 100 microns or 10 to 50 microns or 10 to 20 microns. In one embodiment, the particles are composed of aggregates of discrete particles, wherein the average particle size of the discrete particles is less than 10 microns, preferably less than 5 microns, more preferably less than 1 micron, more preferably less than 500nm, even less than 300nm. For example, polymers (such as polyvinylidene fluoride, acrylic polymers, styrene polymers, styrene-butadiene rubber, polyamide) prepared by emulsion polymerization can have discrete particle sizes. The polymers (such as polyolefins, polyamides, polyvinylidene fluoride, acrylic polymers, styrene polymers) made by other processes are composed of powder particles, wherein the particles are not composed of aggregates of discrete particles.
[0061] The particles of the crosslinked thermoplastic polymer can be in any shape, including circular, nearly circular, fibril or various irregular shapes. The crosslinked thermoplastic polymer can be advantageously prepared by polymerization in a dispersion medium, for example, suspension polymerization or emulsion polymerization. These processes will usually produce quite round particles suspended in an aqueous medium. After drying, suspension polymer powders contain particles that remain quite round, while emulsion polymers tend to produce powders with various irregular shapes, which are composed of aggregates of discrete round particles. Dried particles can be obtained by any process known in the art, such as spray drying, coagulation drying, pan drying, extrusion, grinding and milling.
[0062] The crosslinked thermoplastic polymer particles may be made from a single thermoplastic polymer, a blend of 2 or more thermoplastic polymers, or at least one crosslinked thermoplastic polymer layer.
[0063] US7868062 describes the preparation of highly cross-linked acrylic thermoplastic polymer particles by suspension polymerization. The cross-linked particulate material produced is insoluble in strong organic solvents such as tetrahydrofuran and dichloromethane. The particles made of multi-layer thermoplastic materials can be multi-stage, sequentially produced polymers having a core-shell particle structure. The core-shell particles can have two or more layers, wherein at least one layer is cross-linked using a cross-linking agent during the polymerization of the polymer layers. In one embodiment, all layers of the particles are cross-linked, and in another embodiment, the particles comprise at least one cross-linked inner layer and at least one non-cross-linked layer. The multi-stage polymer can be produced by any known technique for preparing multi-stage, sequentially produced polymers, for example, by emulsion polymerization of a subsequent stage monomer mixture in the presence of a previously formed polymer product. In this type of polymerization, the subsequent stage is attached to the previous stage and is closely connected to the previous stage. Examples of acrylic core-shell particles are described and referenced in US Pat. Nos. 3,661,994, 4,521,568, 2003 / 0216510, and 2013,317,175. Examples of fluorinated core-shell particles are described in JP 2018-172595A.
[0064] Crosslinked thermoplastic polymers can be obtained by chemical, thermal or radiation crosslinking processes. Chemical crosslinking agents can be used during the polymerization of thermoplastic monomers. For thermoplastic polymers produced by free radical or ionic processes, such as fluoropolymers, acrylic polymers, styrene polymers, typical crosslinking agents are multifunctional monomers containing 2 or more C=C double bonds, including aliphatic and aromatic vinyl, allyl, methallyl, and crotyl monomers. Examples of such crosslinking (sometimes referred to as grafting) monomers are described in US2013317175, including but not limited to: divinylbenzene, trivinylbenzene, butadiene, isoprene, diallyl phthalate, diallyl methacrylate, butanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate. Trymehylolpropane tri(meth)acrylate, divinyl sulfone, 1,3-butene dimethacrylate and combinations thereof. Preferred crosslinking monomers are polyvinylbenzene, polyallyl (meth) acrylate, poly (meth) acrylate and polyallyl phthalate, where "poly" can refer to di-, tri-, tetra- and greater than tetra-. The crosslinking monomer is incorporated into the monomer mixture in an amount of 0.1 to 55 wt%, preferably 0.2 to 20 wt%, and most preferably 0.5 to 10 wt%. For thermoplastic polymers (such as polyamides) produced by polycondensation processes, typical crosslinking agents include polyfunctional acids or polyfunctional amines with a functionality greater than or equal to 2, as described in US Pat. No. 8,546,614.
[0065] Chemical and / or radiation crosslinking of thermoplastic polymers can also be accomplished in post-polymerization processes such as solution crosslinking, reactive extrusion, reaction injection molding and / or radiation curing. Examples of reactive extrusion processes for crosslinking polyamides are described in EP2219698. In a first reactive extrusion step, the polyamide is modified a) with a difunctional or monofunctional crosslinking reactive compound (which contains at least one reactive site that allows crosslinking or reaction with a crosslinking agent) or b) with triallyl isocyanurate (TAIC) or a derivative thereof. In a second step, the modified polyamide undergoes a crosslinking reaction by treatment with at least one form of energy.
[0066] US8480917 describes the preparation of cross-linked PVDF by heating a solution of a PVDF-based polymer and a cross-linking agent. Examples of cross-linking agents may include dicumyl peroxide, benzoyl peroxide, bisphenol A, methylenediamine, ethylenediamine, isopropylethylenediamine, 1,3-phenylenediamine, 1,5-naphthalenediamine, 2,4,4-trimethyl-1,6-hexanediamine. The cross-linking agent is used in an amount of 0.1% to 10% by weight based on the weight of the polymer. Whether the PVDF-based polymer has been cross-linked can be determined by dynamic mechanical analysis (DMA), differential scanning calorimetry or solubility testing. When the PVDF-based polymer is cross-linked, the polymer molecular chains are linked together and therefore will not dissolve in a strong organic solvent, such as a solvent for a cross-linking reaction, such as methyl isobutyl ketone or methyl ethyl ketone. Similar processes for cross-linking fluoropolymers in the presence of an organic base are described in WO19027899. Examples of organic bases include: 1,8-diazabicycloundec-7-ene, 1.5-diazabicyclonon-5-ene, tetramethylguanidine, trimethylamine, hexanediamine, methylamine, dimethylamine, ethylamine, azetidine, isopropylamine, propylamine, 1,3-propylenediamine, pyrrolidine, N,N-dimethylglycine, butylamine, tert-butylamine, piperidine, choline, hydroquinone, cyclohexylamine, diisopropylamine, 4-dimethylaminopyridine, diethylenetriamine, 4-aminophenol. In one example, 1,8-diazabicycloundec-7-ene is used at 2% by weight based on the weight of the polymer.
[0067] US3923947 describes a process for crosslinking polyethylene by reactive extrusion in the presence of a peroxide compound, the peroxide compound being used at a loading of 0.1 to 5 wt%. Suitable peroxide compounds include 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 2,5-dimethyl-2,6-di(tert-butylperoxy)hexane, 1,3,5-tri-2-(tert-butylperoxy)diisopropylbenzene and 1,3,5-tri(tert-butylperoxy)isopropylbenzene.
[0068] It is also contemplated to use mixtures of one or more crosslinked thermoplastic polymers as binders in the present invention. In all cases, crosslinking occurs before the thermoplastic polymer is combined with the interacting particles or fibers to form a mass or monolith.
[0069] Interacting particles or fibers
[0070] One or more types of interactive particles can also be in the form of fibers that are combined with the cross-linked thermoplastic polymer binder of the present invention. The interactive particles or fibers of the present invention are particles or fibers that have physical, electrical or chemical interactions when they are close to or in contact with dissolved or suspended substances in a fluid (liquid or gas) composition. Depending on the type of activity of the interactive particles, the particles can separate dissolved or suspended substances by chemical reaction, physical capture, physical attachment, electrical (charge or ion) attraction or the like.
[0071] Examples of interactive particles or fibers include, but are not limited to: metal particles of 410, 304 and 316 stainless steel; copper, aluminum and nickel powders; ferromagnetic materials; activated alumina; activated carbon; carbon nanotubes; silica gel; glass beads; various abrasives; common minerals (such as silica or titanium dioxide); wood chips; ion exchange resins; zeolites; ceramics; ion exchange modified zeolites; diatomaceous earth; talc; graphite; carbon black; metal oxides; lithium ion transition metal salts. Examples of useful microbial interceptors include, but are not limited to: metal salts, particularly silver and copper salts, including AgBr, AgCl and silver zeolites. Other useful interactive particles or fibers include: iron hydroxyoxides (for adsorption of arsenic), calcium hydroxyapatite (for adsorption of fluoride), and phosphates, oxides and sulfates (for precipitation of metals such as lead, nickel and other toxic metals).
[0072] In one embodiment, two types of interactive particles or fibers are combined with the binder of the present invention, for example, activated carbon and ceramic, activated carbon and titanium dioxide, activated carbon and hydroxyapatite, activated carbon and zeolite, activated carbon and ion exchange resin, zeolite and ion exchange resin, metal particles and graphite, metal particles and carbon black.
[0073] The average particle size of the interactive particles or fibers of the present invention is from 0.1 microns to 3,000 microns and can have any aspect ratio. The aspect ratio of spherical particles is close to 1. The fibers can have essentially an infinite length to width aspect ratio. Although long fibers can be used with adhesives to produce fiber-reinforced structures to improve mechanical strength, the fibers are preferably cut to no more than 5 mm in length. Fiber reinforcement provides improved strength for porous separation products. The interactive particles or fibers should have sufficient thermal conductivity to allow the powder mixture to be heated. In addition, during extrusion or compression molding, the softening point or melting point of the particles and fibers must be sufficiently higher than the softening point or melting point of the thermoplastic polymer adhesive to prevent the material from melting and producing a continuous molten phase, but to produce the multiphase system that is generally required.
[0074] The ratio of the cross-linked thermoplastic polymer binder to the interacting particles or fibers is 0.5-35% by weight of dry binder: 65-99.5% by weight of interacting particles or fibers, preferably 0.5-20% by weight of dry binder: 80-99.5% by weight of interacting particles or fibers, more preferably 1-10% by weight of dry binder: 90-99% by weight of interacting particles or fibers. In one embodiment, it is 1-15% by weight of dry binder: 85-99% by weight of interacting particles or fibers. If less binder is used, complete interconnection may not be achieved, and if more binder is used, the contact between the interacting particles and the fluid passing through the separation product is reduced.
[0075] The separation articles of the present invention are different from membranes. Membranes work by cut-off filtration - having a specified pore size and preventing particles larger than the pore size from passing through the membrane. In contrast, the separation articles of the present invention rely on adsorption or absorption of interactive particles to remove materials from the fluid passing through the separation device.
[0076] Method for producing a solid porous article
[0077] The method of making the article of the present invention comprises: mixing the interactive particles or fibers, the crosslinked thermoplastic polymer and the optional additives into a homogeneous blend. The blend can be formed into an article by methods known in the art for forming solid articles. Available methods for forming the article of the present invention include, but are not limited to: extrusion, compression molding and roller pressing.
[0078] Mixing process
[0079] The mixing of interactive particles with binder particles is described in US 5019311, which is incorporated herein by reference. The process involves mixing at least one "binder" in dry form or suspended in an aqueous medium with one or more types of interactive particles or fibers, wherein the at least one "binder" is composed of a fine particulate material. The interactive particles or fibers can be composed of almost any granular, powdered or fine material or a series of fine fibers or coarse fibers. The melting point or softening point of the particles and fibers should be significantly higher than the melting point or softening point of the binder particles. Various additives and processing aids can be added to the mixture. "Additives" refer to materials that can cause the desired changes in the properties of the final product, for example, plasticizers that can produce a more elastic or rubbery consistency, or stiffeners that can produce a stronger, more brittle, more ceramic-like final product. "Processing aids" refer to materials that make the mixture easier to process, such as lubricants. An example of a lubricant is fumed silica. The binder should account for about 1% to about 30% of the total mixture weight, preferably about 4% to about 12%.
[0080] The mixing process usually used for mixing adhesives and interaction materials (particles and / or fibers) is intended to produce a final product that is as uniform as possible. In this process, the quality of the mixture produced by the mixing equipment is very important. Cold mixing processes usually require high shear levels to produce stable, compact mixtures that will be converted into strong composite materials during final processing. For example, ball milling usually must be carried out in a modified ball mill equipped with objects that increase shear. Plow mixers must also be improved with objects that "spread" the material. Usually, powder mixtures (mixtures that do not contain a large amount of long fibers) can be effectively mixed using modified ball mills or plow mixers, while mixtures of fibers and particles can be effectively dispersed in high-intensity chopping mixers.
[0081] In addition, it is suspected that the process requires a special distribution of particles in the mixture. The adhesive particles must be dispersed individually or as small groups dispersed between and on the surrounding interaction particles. The adhesive particles must stick to the interaction particles in such a way that a low dust, slow moving matrix is produced. In order to supplement this stickiness, the adhesive or interaction particles sometimes need to be coated with trace amounts of surfactants or similar materials.
[0082] As an alternative to the dry mixing process, (IR4215) WO / 16130410 describes mixing interactive particles with an aqueous dispersion of a thermoplastic polymer binder.
[0083] Forming a whole or block or solid porous product
[0084] As described in US 5019311, all particles and mixtures of components are processed according to the present invention by a procedure that may include any of a number of conventional methods commonly applied to plastics. These methods include extrusion to produce objects with two-dimensional uniform shapes, hot rolling compaction to produce thin sheets or thick plates, or compression molding or injection molding to produce complex block shapes.
[0085] To accomplish the fixation of interacting particles or fibers or to form forced point bonds, the plastic molding, extrusion, rolling or other forming equipment is operated in a manner to ensure that the critical combination of applied pressure, temperature and shear is achieved within the desired time sequence.
[0086] As described in US 5019311, US 5331037, the method for converting the particle blend into a block or monolith involves heating the blend to a temperature sufficiently above the softening or melting point of the polymer binder (usually 20° C. to 40° C.). Combined with the pressure and shear forces applied during processing, this temperature allows the thermoplastic polymer binder to "smear" into the film, acting as a bonding point.
[0087] In the present invention, the use of a cross-linked thermoplastic polymer binder inhibits or at least minimizes "smearing" of the binder particles. Sufficient polymer deformation is present only on the outside of the binder particles to effectively form bonding points, while the particle body has limited flowability. This produces significant benefits in minimizing contamination by interacting particles or fibers.
[0088] The speed of the method for preparing the block is mainly limited by the speed at which heat can be moved to the particle mixture. Unlike standard non-crosslinked thermoplastic polymers, crosslinked thermoplastic polymer adhesives can be processed over a wide temperature range, between its softening temperature and a temperature of 20°C, 40°C, 70°C, 80°C or 100°C above the softening temperature, and provide consistent bonding efficiency and extremely low pollution. In extrusion processing, the composition of the present invention can be greater than 5 inches / minute, preferably greater than 8 inches / minute, more preferably greater than 10 inches / minute, and most preferably greater than 15 inches / minute. The extrusion speed is converted into blocks of various sizes. In compression molding processing, the composition of the present invention can be converted into blocks of various sizes within a processing cycle time of less than 60 minutes, preferably less than 30 minutes, more preferably less than 20 minutes, most preferably less than 10 minutes or less than 5 minutes. For example, the block can be cylindrical, and the outer diameter range is 0.5 inches to 50 inches, preferably 1 inch to 20 inches, and more preferably 2 inches to 10 inches.
[0089] The size and shape of the block can vary depending on the target application. The block can have any shape and size. A typical example is a cylindrical block with a diameter greater than 1 inch, preferably greater than 2 inches, more preferably greater than 5 inches, and most preferably greater than 10 inches. Another typical example is a ring-shaped block with an outer diameter greater than 1 inch, preferably greater than 2 inches, more preferably greater than 5 inches, and most preferably greater than 10 inches, and an inner diameter greater than 0.1 inches, preferably greater than 0.2 inches, more preferably greater than 0.5 inches, and most preferably greater than 1 inch.
[0090] use
[0091] The articles of the present invention can be used for filtering, separating or storing fluids. They can also be used as components of energy storage devices, such as electrodes of batteries and capacitors. Filtration articles can purify and remove unwanted substances from fluids flowing through the articles, producing purer fluids for various commercial or consumer applications. The articles can also be used to capture substances from a fluid stream and concentrate them, and then remove these captured substances from the separation article for further use. The device can be used for drinking water (hot and cold water) purification, and can also be used for industrial purposes. Industrial use refers to use at high temperatures (greater than 50°C, greater than 75°C, greater than 100°C, greater than 125°C, even greater than 150°C, or up to the melting point of polymer binders); use with organic solvents, and for medical and biological cleaning and pure uses.
[0092] Due to the cross-linked nature of the thermoplastic adhesives of the present invention, they have significant advantages over standard thermoplastic polymers, including resistance to strong organic chemicals, excellent mechanical properties and thermomechanical properties. For example, the chemical resistance of the block to methyl isobutyl ketone or methyl ethyl ketone or N-methyl-2-pyrrolidone can be measured by ASTM D543, wherein a block made using a cross-linked thermoplastic polymer is exposed to a strain of 0.5% to 3% while the organic chemical is frequently applied to the surface of the block using a pipette to keep the surface wet for 2 to 24 hours. If the block maintains its mechanical integrity (defined as a simple pass / fail), its resistance to organic chemicals is considered good, and if there is more than 20% by weight of the block composition that is not attached to the block structure after chemical exposure, the mechanical integrity fails. Thermomechanical properties are measured by dynamic mechanical analysis at a frequency of 0.1 Hz or 1 Hz according to ASTM D4440-01 or ISO 6721 Part 10, where the G' and G" moduli are a function of temperature. Excellent thermomechanical properties are obtained when G' and G" exhibit a plateau between 200°C and 250°C.
[0093] The articles of the present invention can be used in a variety of different and demanding environments. High temperature, high reactivity, corrosive or acidic environment, sterile environment, contact with biological agents are environments where the separation articles of the present invention have obvious advantages over other non-crosslinked thermoplastic polymer binder systems.
[0094] The article of the present invention can be any size or any shape. In one embodiment, the article is a hollow tube formed by continuous extrusion of any length. Water or other fluids flow through the outside of the tube under pressure and are filtered from the outside of the tube to the inside and collected after passing through the filter.
[0095] Some articles of manufacture of the present invention include, but are not limited to:
[0096] a. Oil filter, wherein the composite latex may be coated on a paper filter medium;
[0097] b. Carbon block filtration systems, including for heavy metal reduction, biocide reduction, ionic contaminant reduction, and pharmaceutical reduction;
[0098] c. ion exchange membrane or column;
[0099] d. Catalytic media, used to promote chemical reactions;
[0100] e. Bioseparation and recovery of drugs and bioactive ingredients;
[0101] f. Gas separation of gases dissolved in aqueous and non-aqueous media and particles suspended in gases from other gases;
[0102] g. Chemical scrubbers, especially for flue gases in highly acidic environments;
[0103] h. Chemical resistant protective clothing and coverings;
[0104] i. Hot water treatment (>80℃) filtration to prevent the accumulation of organic pollutants and remove organic pollutants;
[0105] j. Automobile exhaust filtration;
[0106] k. Closed-loop industrial water system;
[0107] l. Industrial water treatment;
[0108] m. Greenhouse gas emissions (exhaust), exhaust (vent) and chimney capture;
[0109] n. Treatment of contaminated groundwater;
[0110] o. Treating brine and saline water into drinking water;
[0111] p. Use as a particle filter;
[0112] q. Treated with ozone exposure;
[0113] r. Gas storage;
[0114] s. Gas transportation;
[0115] t. Purification and / or filtration of the following substances:
[0116] - aliphatic solvents,
[0117] -strong acid,
[0118] - hot (>80°C) compounds,
[0119] -hydrocarbon,
[0120] - hydrofluoric acid,
[0121] - diesel and biodiesel fuels,
[0122] -ketone,
[0123] -amine,
[0124] -strong base,
[0125] - "Oleum" acid,
[0126] - strong oxidizing agents,
[0127] - aromatics, ethers, ketones, glycols, halogens, esters, aldehydes and amines,
[0128] -Compounds of benzene, toluene, butyl ether, acetone, ethylene glycol, ethylene dichloride, ethyl acetate, formaldehyde, butylamine, etc.;
[0129] u. Drinking water filtration, including filtration of salt water, well water and surface water;
[0130] v. Evaporation control device;
[0131] w. Hydrocarbon energy storage device
[0132] x. Removal of inorganic and ionic species from aqueous, non-aqueous and gaseous suspensions or solutions, including but not limited to: cations of hydrogen, aluminum, calcium, lithium, sodium and potassium; anions of nitrate, cyanide and chloride; metals, including but not limited to chromium, zinc, lead, mercury, copper, silver, gold, platinum, iron and other precious or heavy metals and metal ions; salts, including but not limited to sodium chloride, potassium chloride, sodium sulfate; and removal of organic compounds from aqueous solutions and suspensions.
[0133] Based on the list of exemplary uses and the description in this specification, one of ordinary skill in the art can imagine many other uses for the articles of the present invention.
[0134] Aspects of the Invention
[0135] Aspect 1: A composition comprising: a) one or more types of interactive particles; and b) 0.5-30%, preferably 1-20% by weight of one or more types of cross-linked thermoplastic polymer binder particles, based on the total weight of the interactive particles and the cross-linked thermoplastic polymer binder particles.
[0136] Aspect 2: A composition as described in Aspect 1, wherein the interactive particles are selected from: metal particles; activated alumina; activated carbon; carbon nanotubes; silica gel; glass beads; silicon dioxide; titanium dioxide; wood chips; ion exchange resins; zeolites, including ion exchange modified zeolites and silver modified zeolites; ceramics; diatomaceous earth; talc; graphite; carbon black; metal oxides; lithium ion transition metal salts, such as silver salts and copper salts; calcium hydroxyapatite; phosphates; oxides; and sulfates.
[0137] Aspect 3: The composition according to aspect 1, wherein the interactive particles are selected from the group consisting of activated carbon, zeolite, ceramic, hydroxyapatite, and titanium dioxide.
[0138] Aspect 4: The composition of Aspect 1, wherein the interactive particles comprise activated carbon.
[0139] Aspect 5: The composition of any one of Aspects 1 to 4, wherein the cross-linked thermoplastic polymer is selected from the group consisting of fluoropolymers, polyamides, acrylic polymers, polyimides, polyurethanes, styrenic polymers, polyolefins, polyesters, polyvinyl chloride, polycarbonates, and thermoplastic polyurethanes.
[0140] Aspect 6: The composition according to any one of aspects 1 to 4, wherein the cross-linked thermoplastic polymer is selected from the group consisting of fluoropolymers, polyamides, acrylic polymers, styrenic polymers, polyolefins, and polyesters.
[0141] Aspect 7: The composition of any one of Aspects 1 to 4, wherein the crosslinked thermoplastic polymer binder particles comprise a fluoropolymer selected from the group consisting of vinylidene fluoride homopolymers and copolymers, tetrafluoroethylene homopolymers and copolymers, or trifluorochloroethylene homopolymers and copolymers.
[0142] Aspect 8: The composition of any one of Aspects 1 to 4, wherein the cross-linked thermoplastic polymer binder particles comprise polyamide, wherein the polyamide is selected from the group consisting of polyamide 6, polyamide 6,6, polyamide 6,12, polyamide 11, polyamide 12, polyether-b-polyamide block copolymer, or polyester-b-polyamide block copolymer.
[0143] Aspect 9: The composition of any of Aspects 1 to 4, wherein the crosslinked thermoplastic polymer binder particles comprise an acrylic polymer, wherein the acrylic polymer is selected from the group consisting of homopolymers and copolymers comprising methacrylate or acrylate monomers.
[0144] Aspect 10: The composition of any one of aspects 1 to 4, wherein the styrenic polymer is selected from the group consisting of homopolymers and copolymers comprising styrene or α-methylstyrene monomers.
[0145] Aspect 11: The composition of any one of aspects 1 to 4, wherein the polyolefin is selected from the group consisting of homopolymers and copolymers containing ethylene or propylene monomers.
[0146] Aspect 12: The composition of any one of aspects 1 to 4, wherein the polyester is selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, and polylactic acid.
[0147] Aspect 13: The composition of any of Aspects 1 to 4, wherein the crosslinked thermoplastic polymer particles have a core-shell structure.
[0148] Aspect 14: The composition of any one of Aspects 1 to 13, wherein the -1 The crosslinked thermoplastic polymer has a melt viscosity greater than 20 kpoise, preferably greater than 40 kpoise, and more preferably greater than 50 kpoise.
[0149] Aspect 15: The composition of any one of Aspects 1 to 14, wherein the crosslinked thermoplastic polymer has a complex viscosity greater than 10 when measured by ASTM D4440-01 at a temperature of 230° C. and a frequency of 0.1 Hz. 8 Second -1 .
[0150] Aspect 16: The composition of any of Aspects 1 to 15, wherein the solubility of the crosslinked thermoplastic polymer particles in methyl ethyl ketone is less than 20%, preferably less than 10%, and most preferably less than 5% after 24 hours of immersion according to ASTM D543.
[0151] Aspect 17: The composition of any of Aspects 1 to 16, wherein the crosslinked thermoplastic polymer particles have a solubility in tetrahydrofuran of less than 10% after 24 hours of immersion according to ASTM D543.
[0152] Aspect 18: The composition of any of Aspects 1 to 17, wherein the crosslinked thermoplastic polymer particles have a solubility of less than 10% in N-methyl-2-pyrrolidone after 24 hours of immersion according to ASTM D543.
[0153] Aspect 19: The composition of any of Aspects 1 to 18, wherein the crosslinked thermoplastic polymer particles are in the form of a powder having an average particle size of 1 to 250 microns, preferably 5 to 30 microns.
[0154] Aspect 20: A composition as described in any of Aspects 1 to 19, wherein the cross-linked thermoplastic polymer particles are in the form of a powder composed of aggregates of discrete thermoplastic polymer particles, and the average particle size of the discrete particles is 20 nanometers to 10 micrometers, preferably 50 nanometers to 1 micrometer, and most preferably 80 nanometers to 500 nanometers.
[0155] Aspect 21: The composition of any one of Aspects 1 to 19, wherein the average particle size of the crosslinked thermoplastic polymer particles is from 20 nanometers to 250 micrometers, preferably from 100 nanometers to 150 micrometers, more preferably from 200 nanometers to 30 micrometers, and most preferably from 200 nanometers to 20 micrometers.
[0156] Aspect 22: A composition as described in any of Aspects 1 to 19, wherein the composition comprises at least 75 weight % of interactive particles and 1 to 25 weight % of cross-linked thermoplastic polymer particles, preferably at least 80 weight % of interactive particles and 2 to 20 weight % of cross-linked thermoplastic polymer particles, and most preferably at least 85 weight % of interactive particles and 1 to 15 weight % of cross-linked thermoplastic polymer particles.
[0157] Aspect 23: The composition of any one of Aspects 1 to 22, wherein the composition further comprises an additive selected from the group consisting of a plasticizer and a lubricant.
[0158] Aspect 24: A solid porous article comprising: a) at least 70 weight percent interactive particles and b) 0.5 to 30 weight percent crosslinked thermoplastic polymer binder particles, based on the total weight of the article.
[0159] Aspect 25: A solid porous article as described in Aspect 24, wherein the interacting particles are selected from: metal particles; activated alumina; activated carbon; carbon nanotubes; silica gel; glass beads; silicon dioxide; titanium dioxide; wood chips; ion exchange resins; zeolites, including ion exchange modified zeolites and silver modified zeolites; ceramics; diatomaceous earth; talc; graphite; carbon black; metal oxides; lithium ion transition metal salts, such as silver salts and copper salts; calcium hydroxyapatite; phosphates; oxides; and sulfates.
[0160] Aspect 26: The solid porous article of aspect 24, wherein the interactive particles are selected from the group consisting of activated carbon, zeolite, ceramic, hydroxyapatite, and titanium dioxide.
[0161] Aspect 27: The solid porous article of Aspect 24, wherein the interactive particles comprise activated carbon.
[0162] Aspect 28: A solid porous article as described in any of Aspects 24 to 27, wherein the cross-linked thermoplastic polymer is selected from the group consisting of fluoropolymers, polyamides, acrylic polymers, polyimides, polyurethanes, styrenic polymers, polyolefins, polyesters, polyvinyl chloride, polycarbonates, and thermoplastic polyurethanes.
[0163] Aspect 29: The solid porous article of any of Aspects 24 to 27, wherein the cross-linked thermoplastic polymer is selected from the group consisting of fluoropolymers, polyamides, acrylic polymers, styrenic polymers, polyolefins, polyesters, and combinations thereof.
[0164] Aspect 30: A solid porous article as described in any of Aspects 24 to 27, wherein the cross-linked thermoplastic polymer binder particles comprise a fluoropolymer, wherein the fluoropolymer is selected from the group consisting of vinylidene fluoride homopolymers and copolymers, tetrafluoroethylene homopolymers and copolymers, or trifluorochloroethylene homopolymers and copolymers.
[0165] Aspect 31: A solid porous article as described in any of Aspects 24 to 27, wherein the cross-linked thermoplastic polymer binder particles comprise polyamide, wherein the polyamide is selected from the following group: polyamide 6, polyamide 6,6, polyamide 6,12, polyamide 11, polyamide 12, polyether-b-polyamide block copolymer or polyester-b-polyamide block copolymer.
[0166] Aspect 32: The solid porous article of any of Aspects 24 to 27, wherein the crosslinked thermoplastic polymer binder particles comprise an acrylic polymer, wherein the acrylic polymer is selected from the group consisting of homopolymers and copolymers comprising methacrylate or acrylate monomers.
[0167] Aspect 33: The solid porous article of any of Aspects 24 to 27, wherein the styrenic polymer is selected from the group consisting of homopolymers and copolymers comprising styrene or α-methylstyrene monomers.
[0168] Aspect 34: The solid porous article of any one of Aspects 24 to 27, wherein the polyolefin is selected from the group consisting of homopolymers and copolymers containing ethylene or propylene monomers.
[0169] Aspect 35: The solid porous article of any one of Aspects 24 to 27, wherein the polyester is selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, and polylactic acid.
[0170] Aspect 36: The solid porous article of any of Aspects 24 to 27, wherein the crosslinked thermoplastic polymer particles have a core-shell structure.
[0171] Aspect 37: A solid porous article as described in any one of aspects 24 to 36, wherein the porous article is subjected to a temperature of 230° C. and 100 seconds according to ASTM D-3835. -1 The crosslinked thermoplastic polymer has a melt viscosity greater than 20 kpoise, preferably greater than 40 kpoise, and more preferably greater than 50 kpoise.
[0172] Aspect 38: A solid porous article as described in any one of aspects 24 to 37, wherein the crosslinked thermoplastic polymer has a complex viscosity greater than 10 when measured by ASTM D4440-01 at a temperature of 230° C. and a frequency of 0.1 Hz. 8 Second -1 .
[0173] Aspect 39: A solid porous article as described in any of Aspects 24 to 38, wherein the solubility of the crosslinked thermoplastic polymer particles in methyl ethyl ketone is less than 20%, preferably less than 10%, and most preferably less than 5% after 24 hours of immersion in accordance with ASTM D543.
[0174] Aspect 40: The solid porous article of any of Aspects 24 to 39, wherein the crosslinked thermoplastic polymer particles have a solubility in tetrahydrofuran of less than 10% after 24 hours of immersion in accordance with ASTM D543.
[0175] Aspect 41: The solid porous article of any of Aspects 24 to 40, wherein the crosslinked thermoplastic polymer particles have a solubility of less than 10% in N-methyl-2-pyrrolidone after 24 hours of immersion in accordance with ASTM D543.
[0176] Aspect 42: The solid porous article of any of Aspects 24 to 41, wherein the crosslinked thermoplastic polymer particles are in the form of a powder having an average particle size of 1 micrometer to 250 micrometers, preferably 5 micrometers to 30 micrometers.
[0177] Aspect 43: A solid porous article as described in any of Aspects 24 to 42, wherein the cross-linked thermoplastic polymer particles are in the form of a powder composed of aggregates of discrete thermoplastic polymer particles, and the average particle size of the discrete particles is 20 nanometers to 10 micrometers, preferably 50 nanometers to 1 micrometer, and most preferably 80 nanometers to 500 nanometers.
[0178] Aspect 44: The solid porous article of any of Aspects 24 to 42, wherein the crosslinked thermoplastic polymer particles are in the form of a powder and the powder has an average particle size of 1 micrometer to 250 micrometers.
[0179] Aspect 45: A solid porous article as described in any of Aspects 24 to 44, wherein, based on the weight of the article, the composition comprises at least 75 weight % of the interactive particles and 1 to 25 weight % of the cross-linked thermoplastic polymer particles, preferably at least 80 weight % of the interactive particles and 2 to 20 weight % of the cross-linked thermoplastic polymer particles, and most preferably at least 85 weight % of the interactive particles and 1 to 15 weight % of the cross-linked thermoplastic polymer particles.
[0180] Aspect 46: The solid porous article of any of Aspects 24 to 45, wherein the composition further comprises an additive selected from the group consisting of a plasticizer and a lubricant.
[0181] Aspect 47: A method of forming a solid porous article, the method comprising the steps of:
[0182] a) providing a composition as described in any one of aspects 1 to 23;
[0183] b) applying heat and pressure,
[0184] A solid porous article is thereby formed.
[0185] Aspect 48: The method according to aspect 47, wherein step b) is performed by compression molding or extrusion.
[0186] Aspect 49: The method of aspect 48, wherein the extrusion speed is greater than 5 inches / minute, preferably greater than 8 inches / minute, more preferably greater than 10 inches / minute, and most preferably greater than 15 inches / minute.
[0187] Aspect 50: The method according to aspect 48, wherein the compression molding time is less than 60 minutes, preferably less than 30 minutes, more preferably less than 20 minutes, and most preferably less than 10 minutes or less than 5 minutes.
[0188] Aspect 51: A method as described in any of Aspects 47 to 50, wherein the solid porous article is cylindrical and has an outer diameter ranging from 0.5 inches to 50 inches, preferably 0.1 to 20 inches, more preferably 0.25 to 10 inches, even more preferably 0.5 to 7 inches, or 1 to 20 inches, more preferably 2 to 10 inches.
[0189] Aspect 52: The method of any one of aspects 47 to 51, wherein step a) comprises: preparing the crosslinked thermoplastic polymer in the presence of at least one crosslinking agent.
[0190] Aspect 53: The method of any one of aspects 47 to 52, wherein step a) comprises: preparing the cross-linked thermoplastic polymer in the presence of a radiation source.
[0191] Aspect 54: The method of aspect 52, wherein the crosslinking agent is selected from the group consisting of polyvinylbenzene, polyallyl (meth)acrylate, poly (meth)acrylate, and polyallyl phthalate.
[0192] Aspect 55: The method as described in Aspect 53, wherein the radiation source is selected from the following group: ultraviolet rays, gamma rays, and electron beams.
[0193] Aspect 56: A method for separating fluid components, the method comprising the steps of: a) providing a solid porous article as described in any of Aspects 24 to 45, and b) passing a fluid through the article, wherein a selected component of the fluid is retained within the article.
[0194] Aspect 57: The method of Aspect 56, wherein the fluid is selected from the group consisting of gas, water, organic solvents, pharmaceutical preparations, and biological preparations.
[0195] Aspect 58: A gas storage method, the method comprising the following steps: a) providing a solid porous article as described in any one of Aspects 24 to 45, wherein the porous article is contained in a container, the container having at least one inlet and optionally at least one outlet; and b) providing gas to the inlet of the container having the solid porous article therein under a certain pressure, wherein at least 50 weight % of the total weight of the gas is maintained within the volume of the porous article, and wherein the container is capable of containing pressurized gas.
[0196] Aspect 59: A method as described in Aspect 58, wherein the gas is selected from the following group: inert gas, hydrocarbons, hydrogen-based gas, methane, natural gas, CO2, CO, O2, N2, fluorinated gas, halogenated gas, silane, phosphine, phosgene, boron trihalide, ammonia, hydrogen halide, sulfide and cyanide, preferably hydrocarbons, methane or natural gas.
[0197] Aspect 60: A method as described in aspect 57 or 58, wherein the container is capable of containing pressurized gas at a pressure of at least 14.7 psi to a maximum of 30 psi, preferably a maximum of 100 psi, preferably a maximum of 1000 psi, preferably a maximum of 3000 psi and preferably a maximum of 5000 psi. Example
[0198] Test method:
[0199] The particle size of the media (such as activated carbon) is measured using a TYLER RX-29 vibrating screen. The data is recorded as the weight average particle size or nominal "mxn" particle size, where at least 90% by weight of the particles are larger than "n" mesh and at least 90% by weight of the particles are smaller than "m" mesh.
[0200] The particle size of the polymer powder can be measured using a Malvern Masturizer 2000 particle size analyzer. The data is reported as weight average particle size (diameter).
[0201] NICOMP can be used TM The average discrete particle size of powder / latex was measured by 380 submicron particle size analyzer.
[0202] Data are reported as weight average particle size (diameter).
[0203] The BET specific surface area, pore volume and pore size distribution of the material can be determined using a QUANTACHROME NOVA-E gas adsorption instrument. Nitrogen adsorption and desorption isotherms are generated at 77K. The multi-point Brunauer-Emmett-Teller (BET) nitrogen adsorption method is used to characterize the specific surface area. Non-localized density functional theory (NLDFT, N2, 77K, slit pore model) is used to characterize the pore volume and pore size distribution.
[0204] The bulk density of a material or block is measured by measuring the weight of the material or block contained in a known volume after the material or block has been dried under vacuum at 110°C for 8 hours.
[0205] The porosity of a material or block is calculated as follows: Porosity = 1 - (bulk density / skeletal density). Proportion of contaminated pores: The percentage of contamination of the active medium is the percentage loss of BET surface area per gram of active medium when the active medium becomes a block. It is calculated as follows: [1 - (BET specific surface area of the block * 100) / (BET specific surface area of the adsorbent * weight % of adsorbent in the block)] * 100.
[0206] The chemical solubility of the polymer binder is determined according to ASTM D543 using an organic chemical such as methyl isobutyl ketone, methyl ethyl ketone or N-methyl-2-pyrrolidone. When 1 gram of a cross-linked thermoplastic polymer is exposed to an organic chemical by immersion at room temperature for 2 hours, 10 hours or 24 hours, the polymer does not dissolve in the solvent, but swells and forms a gel-like material that cannot be filtered through a 0.5 micron PTFE filter. If there is less than 20 weight % or less than 10 weight % or less than 5 weight % of the polymer in the filtered solution, the polymer is considered to be a cross-linked polymer.
[0207] The complex viscosity of a polymer is measured at a frequency of 0.1 Hz or 1 Hz according to ASTM D4440-01 or ISO 6721 part 10. This is a dynamic mechanical analysis in which the sample is placed in a parallel plate oscillating rheometer and the temperature is increased from room temperature to 250°C at a rate of 5°C per minute, and then the complex viscosity is measured as a function of temperature as the temperature is decreased to room temperature at a rate of 2°C, 5°C, 10°C or 20°C per minute.
[0208] The mechanical strength of the blocks was visually assessed and given a "pass" or "fail" result. A "pass" means that the block is structurally stable when set on a flat surface, while a "fail" means that the block does not hold together and is at least partially broken apart.
[0209] Example:
[0210] The powder blend is formed by dry blending Jacobi CX coconut shell activated carbon with one or more thermoplastic polymer binders. The activated carbon has a nominal 80 x 325 mesh particle size, a bulk density of about 0.3-0.4 g / cc, and a specific surface area BET (m 2 / g) is 1150 and the porosity is 0.67-0.92.
[0211] The binder used in Example 1 is cross-linked particles made by suspension polymerization using methyl methacrylate, ethyl acrylate and allyl methacrylate as cross-linking agents. The binder used in Example 2 is three-layer core-shell particles made by sequential emulsion polymerization, with the inner layer made of polymethyl methacrylate, the middle layer being a cross-linked polymer made of butyl acrylate, styrene and allyl methacrylate, and the outer layer being made of polymethyl methacrylate. The binder used in Comparative Example 1b is non-cross-linked particles made by suspension polymerization using methyl methacrylate and ethyl acrylate without a cross-linking agent.
[0212] The adhesives were characterized by dynamic mechanical analysis (DMA) according to ASTM D4440. The viscosity of the material was measured as a function of temperature at a constant frequency of 0.1 Hz. The viscosity of the crosslinked adhesives of all examples at 230°C was greater than 10 7 Second -1 , while the viscosity of the uncrosslinked adhesive used in the comparative example at 230°C was less than 10 7 Second -1 The chemical solubility of the adhesive was measured in methyl isobutyl ketone or methyl ethyl ketone according to ASTM D543. It was found that all the cross-linked adhesives used in the examples were insoluble in the chemicals after immersion for 24 hours, while the non-cross-linked adhesives used in the comparative examples were dissolved in both chemicals within 1 hour.
[0213] The following table lists the binder used in each example, its weight percent loading in the total blend, the average particle size of the binder powder, the average discrete particle size of the binder, and the melt viscosity of the binder at 230°C and 0.1 Hz. The powders were blended with a flat-bed tamping machine attachment. Artisa series 5-Quart tilted head vertical mixer is achieved, stirring at "Stir" speed for 20 minutes. Then, the powder blend is compressed into a self-supporting porous product by heating it at "T (heating)" for 30 minutes and then compressing it into a cylindrical mold using a cold shop press. Pressure is applied to reach the set height of the porous product so that the volume density of the structure is about 0.68g / cc. The porosity of the product is measured, and the carbon contamination rate % is calculated and recorded in a table. Carbon contamination is undesirable for target applications intended for fluid filtration or fluid storage because it reduces the ability of carbon to adsorb molecules in the fluid.
[0214] The porosity of the articles made from the cross-linked thermoplastic binder is virtually the same as the porosity of the initial carbon powder, which means that the contamination rate % is close to 0%, or less than 1%, or less than 0.4%, or less than 0.3%, or less than 0.1%. This is because the binder does not have the ability to flow during compression molding of the article. In contrast, the non-cross-linked thermoplastic of Comparative Example 1b results in an article with significantly lower porosity and, therefore, a higher carbon contamination rate. This is due to the fact that the binder can flow to the carbon surface during compression molding of the article and flow into some of the carbon pores. In addition, the binder tends to flow to the mold surface and stick to the metal, making it difficult to demold the article without destroying the article.
[0215]
[0216]
[0217]
Claims
1. A composition comprising: a) one or more types of interactive particles, wherein the interactive particles are particles that have physical, electrical or chemical interactions when they are in proximity to or in contact with dissolved or suspended matter in a fluid composition; and b) 0.5-30 wt % of one or more types of cross-linked thermoplastic polymer binder particles, based on the total weight of the interactive particles and the cross-linked thermoplastic polymer binder particles, wherein, The crosslinked thermoplastic polymer has a complex viscosity greater than 10 when measured by ASTM D4440-01 at a temperature of 230° C. and a frequency of 0.1 Hz. 8 Second -1 , wherein the cross-linked thermoplastic polymer is selected from the group consisting of fluoropolymers, polyamides, acrylic polymers, polyimides, polyurethanes, polyolefins, polyesters, polyvinyl chlorides and polycarbonates.
2. The composition according to claim 1, wherein The interactive particles are selected from the group consisting of: metal particles; activated carbon; carbon nanotubes; silica gel; glass beads; wood chips; ion exchange resins; zeolites, including ion exchange modified zeolites and silver modified zeolites; ceramics; diatomaceous earth; talc; graphite; carbon black; lithium ion transition metal salts; calcium hydroxyapatite; phosphates; oxides; and sulfates.
3. The composition according to claim 2, wherein The oxide is selected from silicon dioxide and metal oxides.
4. The composition according to claim 1, wherein The interactive particles are selected from the group consisting of activated carbon, zeolite, ceramic, hydroxyapatite, and titanium dioxide.
5. The composition according to claim 1, wherein The interactive particles include activated carbon.
6. The composition according to any one of claims 1 to 5, wherein The cross-linked thermoplastic polymer is selected from the group consisting of fluoropolymers, acrylic polymers, and styrenic polymers.
7. The composition according to any one of claims 1 to 5, wherein The cross-linked thermoplastic polymer is selected from the group consisting of acrylic polymers and styrenic polymers.
8. The composition according to any one of claims 1 to 5, wherein The fluorine-containing polymer is selected from the group consisting of vinylidene fluoride homopolymers and copolymers, tetrafluoroethylene homopolymers and copolymers, or trifluorochloroethylene homopolymers and copolymers.
9. The composition according to any one of claims 1 to 5, wherein The polyolefin is selected from the group consisting of homopolymers and copolymers containing ethylene or propylene monomers.
10. The composition according to any one of claims 1 to 5, wherein The crosslinked thermoplastic polymer particles have a core-shell structure.
11. The composition according to any one of claims 1 to 5, wherein According to ASTM D-3835 at 230°C and 100 seconds -1 At this time, the melt viscosity of the cross-linked thermoplastic polymer is greater than 20 kilopoise.
12. The composition according to any one of claims 1 to 5, wherein According to ASTM D-3835 at 230°C and 100 seconds -1 At this time, the melt viscosity of the cross-linked thermoplastic polymer is greater than 40 kilopoise.
13. The composition according to any one of claims 1 to 5, wherein The cross-linked thermoplastic polymer particles are in the form of a powder having an average particle size of 1 micron to 250 microns.
14. The composition according to any one of claims 1 to 5, wherein The cross-linked thermoplastic polymer particles are in the form of a powder having an average particle size of 5 to 30 microns.
15. The composition according to any one of claims 1 to 5, wherein The crosslinked thermoplastic polymer particles have an average particle size of 20 nanometers to 250 micrometers.
16. The composition according to any one of claims 1 to 5, wherein The crosslinked thermoplastic polymer particles have an average particle size of 200 nanometers to 30 micrometers.
17. The composition according to any one of claims 1 to 5, wherein The composition comprises at least 75 wt % of interactive particles and 1 to 25 wt % of crosslinked thermoplastic polymer particles.
18. The composition according to any one of claims 1 to 5, wherein The composition comprises at least 85 wt % of interactive particles and 1 to 15 wt % of crosslinked thermoplastic polymer particles.
19. A solid porous article comprising: a) at least 70 wt% of interactive particles, based on the total weight of the article, wherein the interactive particles are particles that have physical, electrical or chemical interactions when they are in proximity or contact with dissolved or suspended matter in a fluid composition; and b) 0.5 to 30 wt% of crosslinked thermoplastic polymer binder particles, wherein, The crosslinked thermoplastic polymer has a complex viscosity greater than 10 when measured by ASTM D4440-01 at a temperature of 230° C. and a frequency of 0.1 Hz. 8 Second -1 , wherein the cross-linked thermoplastic polymer is selected from the group consisting of fluoropolymers, polyamides, acrylic polymers, polyimides, polyurethanes, polyolefins, polyesters, polyvinyl chlorides and polycarbonates.
20. The solid porous article of claim 19, wherein: The interactive particles are selected from the group consisting of: metal particles; activated carbon; carbon nanotubes; silica gel; glass beads; wood chips; ion exchange resins; zeolites, including ion exchange modified zeolites and silver modified zeolites; ceramics; diatomaceous earth; talc; graphite; carbon black; lithium ion transition metal salts; calcium hydroxyapatite; phosphates; oxides; and sulfates.
21. The solid porous article of claim 20, wherein: The oxide is selected from silicon dioxide and metal oxides.
22. A solid porous article as claimed in any one of claims 19 to 21, wherein: The cross-linked thermoplastic polymer is selected from the group consisting of fluoropolymers, acrylic polymers, and styrenic polymers.
23. A solid porous article as claimed in any one of claims 19 to 21, wherein: The crosslinked thermoplastic polymer particles have a core-shell structure.
24. A solid porous article as claimed in any one of claims 19 to 21, wherein: According to ASTM D-3835 at 230°C and 100 seconds -1 At this time, the melt viscosity of the cross-linked thermoplastic polymer is greater than 20 kilopoise.
25. A solid porous article as claimed in any one of claims 19 to 21, wherein: According to ASTM D-3835 at 230°C and 100 seconds -1 At this time, the melt viscosity of the cross-linked thermoplastic polymer is greater than 40 kilopoise.
26. A solid porous article as claimed in any one of claims 19 to 21, wherein: The cross-linked thermoplastic polymer particles are in the form of a powder consisting of aggregates of discrete thermoplastic polymer particles, and the average particle size of the discrete particles is from 20 nanometers to 10 micrometers.
27. The solid porous article of claim 26, wherein: The average particle size of the discrete particles is between 80 nanometers and 500 nanometers.
28. A solid porous article as claimed in any one of claims 19 to 21, wherein: The solid porous article comprises at least 75 weight percent interactive particles and 1 to 25 weight percent crosslinked thermoplastic polymer particles, based on the weight of the article.
29. A solid porous article as claimed in any one of claims 19 to 21, wherein: The solid porous article comprises at least 80 weight percent interactive particles and 2 to 20 weight percent crosslinked thermoplastic polymer particles, based on the weight of the article.
30. A solid porous article as claimed in any one of claims 19 to 21, wherein: The interactive particles comprise activated carbon.
31. A method of forming a solid porous article, the method comprising the steps of: a) providing a composition as claimed in any one of claims 1 to 18; b) applying heat and pressure, A solid porous article is thereby formed.
32. The method of claim 31, wherein: Step b) is accomplished by compression molding or extrusion.
33. The method of claim 32, wherein: The extrusion speed is greater than 5 inches / minute.
34. The method of claim 32, wherein: The extrusion speed is greater than 10 inches / minute.
35. The method of claim 32, wherein: The compression molding time is less than 60 minutes.
36. The method of claim 32, wherein: The compression molding time is less than 10 minutes.
37. The method of claim 32, wherein: Step a) comprises preparing a crosslinked thermoplastic polymer in the presence of at least one crosslinking agent.
38. The method of claim 32, wherein: Step a) comprises preparing a crosslinked thermoplastic polymer in the presence of a radiation source.
39. A method for separating fluid components, the method comprising the steps of: a) providing a solid porous article as claimed in any one of claims 19 to 30, and b) passing a fluid through the article, wherein a selected component of the fluid is retained within the article.
40. The method of claim 39, wherein: The fluid is selected from the group consisting of gas, water, organic solvents, pharmaceutical preparations and biological preparations.
Citation Information
Patent Citations
Core-shell type particle, use thereof and method for production thereof
JP2018172595A
Weather-resistant, high-impact strength acrylic compositions
US20030216510A1
Light diffusing polymer composition, method of producing the same, and articles made therefrom
US20130317175A1
Block products incorporating small particle thermoplastic binders and methods of making same
US20160121249A1
Porous article having polymer binder sub-micron particle
US20180104670A1