Lightweight reinforced thermoplastic composite articles comprising bicomponent fibers

By introducing two-component fibers and leavening agents into thermoplastic composites to form porous mesh structures, the problem of insufficient performance of existing thermoplastic composites is solved, and higher peak load and bending strength are achieved in automotive and construction applications. , suitable for lightweight reinforced thermoplastic materials in complex structures.

CN114096389BActive Publication Date: 2024-11-22HANWA AZDEL INC
View PDF 22 Cites 0 Cited by

Patent Information

Application Number
CN202080027157.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-15
Filing Date
2020-01-31
Publication Date
2024-11-22
Estimated Expiration
2040-01-31

AI Technical Summary

Technical Problem

Existing thermoplastic composites have problems with insufficient performance in automotive and architectural applications, especially in terms of peak loads, stiffness and bending strength, which are difficult to meet the needs of complex structures.

Method used

Using a porous composite article containing bicomponent fibers, a mesh structure with a porosity of 20% to 80% is formed by combining reinforcing fibers, bicomponent fibers and a stump agent in the core layer, and in the longitudinal and transverse directions. Perform molding to improve the mechanical properties of the material.

Benefits of technology

The peak load, stiffness and bending modulus of the material are significantly improved, meeting the performance requirements of complex structures such as automotive roofs, internal components and furniture panels, providing a lighter and higher-strength solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114096389B_ABST
    Figure CN114096389B_ABST
Patent Text Reader

Abstract

A lightweight reinforced thermoplastic article having a core layer including bicomponent fibers in the core layer is described. In some examples, the core layer includes a thermoplastic material, reinforcing fibers, bicomponent fibers, and a bulking agent. After molding of the composite article, for a specific molded thickness, an increase in one or more of a peak load value, a stiffness value, a flexural strength value, and a flexural modulus value can be achieved.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Priority application

[0002] This application is related to and claims priority to and the benefit of U.S. Provisional Application No. 62 / 800,314 filed on February 1, 2019 and U.S. Provisional Application No. 62 / 874,036 filed on July 15, 2019, the disclosure of each of which is hereby incorporated by reference herein. Technical Field

[0003] Certain embodiments are directed to thermoplastic composite articles comprising bicomponent fibers. In some cases, a thermoplastic composite article having bicomponent fibers can provide improved properties over a thermoplastic composite article lacking bicomponent fibers. Background Art

[0004] Certain automotive and architectural applications often use thermoplastic-type materials in place of traditional steel or metal products. Using thermoplastic-type materials creates unique considerations that steel or metal products do not. Summary of the invention

[0005] Certain aspects are described herein to illustrate some configurations of thermoplastic composite articles having bicomponent fibers. Other configurations for producing thermoplastic composite articles including bicomponent fibers will be within the capabilities of one of ordinary skill in the art, given the benefit of this disclosure.

[0006] In one aspect, a molded porous composite article comprises a bulky core layer comprising a web formed of reinforcing fibers, bicomponent fibers, a bulking agent, and a thermoplastic material, wherein the web has a porosity of about 20% to about 80%, and wherein the bicomponent fibers comprise a core-shell arrangement, wherein the melting point of the shell material of the shell of the core-shell arrangement is substantially similar to the melting point of the thermoplastic material, and wherein the melting point of the core material of the core of the core-shell arrangement is at least twenty degrees Celsius higher than the melting point of the thermoplastic material, and wherein at a molded thickness of about 2 mm to about 4 mm in the longitudinal and transverse directions, the molded porous composite article comprises a peak load of 10 N to about 40 N in the longitudinal direction and a peak load of about 6 N to about 30 N in the transverse direction as tested by SAE J949_200904.

[0007] In certain embodiments, the bicomponent fiber comprises: a sheath comprising a polyolefin and a core comprising a polyester or a polyamide. In other examples, the bicomponent fiber comprises: a sheath comprising a polyolefin and a core comprising a polyester. In some examples, the polyolefin comprises polyethylene. In other examples, the polyethylene is a linear low density polyethylene. In some embodiments, the polyester comprises polyethylene terephthalate. In other examples, the polyamide comprises nylon.

[0008] In some cases, the thermoplastic material is polypropylene, the polyolefin of the shell comprises linear low density polyethylene, the bulking agent comprises expandable microspheres, and the polyester of the core comprises polyethylene terephthalate.

[0009] In other cases, the thermoplastic material is polypropylene, the polyolefin of the shell comprises linear low density polyethylene, the bulking agent comprises expandable microspheres, and the polyamide of the core comprises nylon.

[0010] In certain instances, the thermoplastic material comprises polypropylene, the reinforcing fibers comprise glass fibers, the bicomponent fibers comprise linear low density polyethylene in the sheath and a polyester or polyamide in the core, wherein the melting point of the polyester or polyamide in the core is at least twenty degrees Celsius higher than the melting point of the thermoplastic material, and wherein the bulking agent comprises expandable microspheres.

[0011] In some examples, the molded composite article further comprises a stiffness of about 10 N / cm to about 50 N / cm in the machine direction and about 7 N / cm to about 30 N / cm in the transverse direction as tested by SAE J949_200904.

[0012] In other examples, the molded composite article further comprises a flexural strength of about 6 MPa to about 17 MPa in the machine direction and about 4 MPa to about 11 MPa in the transverse direction as tested by SAE J949_200904.

[0013] In further examples, the molded composite article further comprises a flexural modulus of about 800 MPa to about 2000 MPa in the machine direction and about 500 MPa to about 1300 MPa in the transverse direction as tested by SAE J949_200904.

[0014] In some cases, the molded composite article also comprises a stiffness of about 10 N / cm to about 50 N / cm in the longitudinal direction and about 7 N / cm to about 30 N / cm in the transverse direction as tested by SAE J949_200904, and a flexural strength of about 6 MPa to about 17 MPa in the longitudinal direction and about 4 MPa to about 11 MPa in the transverse direction as tested by SAE J949_200904.

[0015] In some embodiments, the molded composite article further comprises a stiffness of about 10 N / cm to about 50 N / cm in the longitudinal direction and about 7 N / cm to about 30 N / cm in the transverse direction as tested by SAE J949_200904, and a flexural modulus of about 800 MPa to about 2000 MPa in the longitudinal direction and about 500 MPa to about 1300 MPa in the transverse direction as tested by SAE J949_200904.

[0016] In certain examples, the molded composite article further comprises a flexural strength of about 6 MPa to about 17 MPa in the machine direction and a flexural modulus of about 800 MPa to about 2000 MPa in the machine direction and about 500 MPa to about 1300 MPa in the transverse direction as tested by SAE J949_200904.

[0017] In some examples, the molded composite article further comprises a stiffness of about 10 N / cm to about 50 N / cm in the longitudinal direction and a stiffness of about 7 N / cm to about 30 N / cm in the transverse direction as tested by SAE J949_200904, a flexural strength of about 6 MPa to about 17 MPa in the longitudinal direction and a flexural strength of about 4 MPa to about 11 MPa in the transverse direction as tested by SAE J949_200904, and a flexural modulus of about 800 MPa to about 2000 MPa in the longitudinal direction and about 500 MPa to about 1300 MPa in the transverse direction as tested by SAE J949_200904.

[0018] In certain embodiments, the article is configured as an automotive headliner, an interior component, a partition panel, or a furniture panel.

[0019] In another aspect, the molded porous composite article comprises a bulky core layer comprising a web formed of reinforcing fibers, bicomponent fibers, a bulking agent, and a thermoplastic material, wherein the web has a porosity of about 20% to about 80%, and wherein the bicomponent fibers comprise a core-shell arrangement, wherein the melting point of the shell material of the shell of the core-shell arrangement is substantially similar to the melting point of the thermoplastic material, and wherein the melting point of the core material of the core of the core-shell arrangement is at least twenty degrees Celsius higher than the melting point of the thermoplastic material, and wherein the molded porous composite article comprises a stiffness of about 10 N / cm to about 50 N / cm in the machine direction and a stiffness of about 7 N / cm to about 30 N / cm in the transverse direction as tested by SAE J949_200904.

[0020] In some examples, the molded composite article further comprises a flexural strength of about 6 MPa to about 17 MPa in the machine direction and about 4 MPa to about 11 MPa in the transverse direction as tested by SAE J949_200904.

[0021] In other examples, the molded composite article further comprises a flexural modulus of about 800 MPa to about 2000 MPa in the machine direction and about 500 MPa to about 1300 MPa in the transverse direction as tested by SAE J949_200904.

[0022] In additional examples, the molded composite article further comprises a flexural strength of about 6 MPa to about 17 MPa in the longitudinal direction and about 4 MPa to about 11 MPa in the transverse direction as tested by SAE J949_200904, and a flexural modulus of about 800 MPa to about 2000 MPa in the longitudinal direction and about 500 MPa to about 1300 MPa in the transverse direction as tested by SAE J949_200904.

[0023] In another aspect, the molded porous composite article comprises a bulky core layer comprising a web formed of reinforcing fibers, bicomponent fibers, a bulking agent, and a thermoplastic material, wherein the web has a porosity of about 20% to about 80%, and wherein the bicomponent fibers comprise a core-shell arrangement, wherein the melting point of the shell material of the shell of the core-shell arrangement is substantially similar to the melting point of the thermoplastic material, and wherein the melting point of the core material of the core of the core-shell arrangement is at least twenty degrees Celsius higher than the melting point of the thermoplastic material, and wherein the molded porous composite article comprises a flexural strength of about 6 MPa to about 17 MPa in the machine direction and about 4 MPa to about 11 MPa in the transverse direction as tested by SAE J949_200904.

[0024] In certain examples, the molded composite article further comprises a flexural modulus of about 800 MPa to about 2000 MPa in the machine direction and about 500 MPa to about 1300 MPa in the transverse direction as tested by SAE J949_200904.

[0025] In additional aspects, the molded porous composite article comprises a bulky core layer comprising a mesh formed from reinforcing fibers, bicomponent fibers, a bulking agent, and a thermoplastic material, wherein the mesh has a porosity of about 20% to about 80%, and wherein the bicomponent fibers comprise a core-shell arrangement, wherein the melting point of the shell material of the shell of the core-shell arrangement is substantially similar to the melting point of the thermoplastic material, and wherein the melting point of the core material of the core of the core-shell arrangement is at least twenty degrees Celsius higher than the melting point of the thermoplastic material, and wherein the molded porous composite article comprises a flexural modulus of about 800 MPa to about 2000 MPa in the machine direction and about 500 MPa to about 1300 MPa in the transverse direction as tested by SAE J949_200904.

[0026] Additional aspects, examples, embodiments, and configurations are described in further detail below. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Certain aspects, embodiments and examples are described with reference to the accompanying drawings, in which:

[0028] Figure 1 is a diagrammatic representation of a core-sheath fiber arrangement according to some examples;

[0029] Figure 2 is an illustration of a side-by-side fiber arrangement according to certain embodiments;

[0030] Figure 3A and 3B each is an illustration of a side-by-side fiber arrangement with a shell according to some examples;

[0031] Figure 4 is a diagram of a core layer according to some examples;

[0032] Figure 5 illustrates methods that may be used to produce a core layer according to some examples;

[0033] Figure 6 Another method that can be used to produce a core layer according to certain examples is shown;

[0034] Figure 7 is a diagram of an article comprising a core layer and an outer skin layer according to some examples;

[0035] Figure 8 is a diagram of an article comprising a core layer and two outer skin layers according to some examples;

[0036] Fig. 9 is a diagram of an article including a core layer, an outer skin layer, and a decorative layer according to some examples;

[0037] Fig.10 is a diagram of a car roof according to some examples;

[0038] Fig.11 is a diagram of a rear trim panel of an automobile according to some examples;

[0039] Fig.12 is an illustration of a furniture article according to some embodiments;

[0040] Fig.13 is another illustration of an article of furniture according to some embodiments;

[0041] Fig.14 is another illustration of an article of furniture according to some embodiments;

[0042] Fig.15 is another illustration of an article of furniture according to some embodiments;

[0043] Fig.16 Photographs showing molded parts produced using hybrid lightweight reinforced thermoplastic sheets;

[0044] Fig.17 is a graph showing the tensile modulus of several samples measured in the machine direction (MD) and cross direction (CD);

[0045] Fig.18 is a graph showing the tensile strength of several samples measured in the machine direction (MD) and cross direction (CD);

[0046] Fig.19A A graph comparing the peak loads of various samples in the machine direction; and

[0047] Fig.19B Graph comparing the peak load in the transverse direction for various samples.

[0048] Those of ordinary skill in the art will recognize that the depictions and layers of the drawings are provided for illustration purposes only. Unless clearly described in conjunction with specific illustrations in the description herein, specific thicknesses, material sizes, etc. are not intended to be implied or required. DETAILED DESCRIPTION

[0049] Certain examples of composite articles are described herein that include a combination of thermoplastic materials and different fibers to provide improved properties. In some examples, one or more of peak load, stiffness, flexural strength, and flexural modulus can be increased.

[0050] In certain embodiments, in some cases, the articles produced herein are described as lightweight reinforced thermoplastic (LWRT) articles. Generally speaking, the articles comprise: a core layer comprising a web formed of a thermoplastic material, reinforcing fiber bicomponent fibers, and optionally a bulking agent. The presence of the combined materials may contribute to the enhanced properties.

[0051] In some configurations, the bicomponent fiber of the core layer may include two or more different materials that can be arranged in a variety of different ways. For example, the bicomponent fiber can be configured as a core-shell arrangement, a side-by-side arrangement, or a combination of these arrangements, wherein the shell surrounds the side-by-side arrangement of the fiber. The different fibers can be produced by extrusion, coextrusion, stretching, or in a similar manner for producing fibers. In some instances, the produced fiber can be coated with another material to provide a shell around the core fiber. In the case where there are more than a single fiber in the shell, the fibers can be coaxial, such as remaining unwound, or can be crossed or wound as desired.

[0052] refer to Figure 1, a diagram showing a cross section of a bicomponent fiber through a core-sheath arrangement is shown. The bicomponent fiber 100 includes a core material 110 surrounded by a sheath material 120. Each of the components 110, 120 may not be a fiber in the true sense, but rather the materials of the core 110 and the sheath 120 together form a fiber. Alternatively, each of the materials 110, 120 may be considered a fiber. The sheath material 120 does not have to completely surround the core material 110 or be symmetrical. Without wishing to be bound by any particular theory, the sheath material 120 is selected to be compatible with a thermoplastic material, such as a thermoplastic resin, used to produce the core layer. For example, the melting point of the sheath material 120 may be approximately the same or the same as the melting point of the thermoplastic material of the core layer. In some examples, the melting points of the sheath material 120 and the thermoplastic material may differ by about one degree Celsius to about ten degrees Celsius and the materials may still be considered compatible.

[0053] In certain embodiments, the core material 110 generally has a higher melting point than the shell material 120 and the thermoplastic material. For example, when forming the core layer, the shell material 120 and the thermoplastic material may melt or soften to form a web of the core layer. The core material 110 generally remains solid and does not melt or soften to any significant extent during material processing to form the core layer.

[0054] In some examples, the melting point of the core material 110 is at least fifteen degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material. In some examples, the melting point of the core material 110 is at least twenty degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material. In other examples, the melting point of the core material 110 is at least twenty-five degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material. In other examples, the melting point of the core material 110 is at least thirty degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material. In some examples, the melting point of the core material 110 is at least thirty-five degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material. In some embodiments, the melting point of the core material 110 is at least forty degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material. In other embodiments, the melting point of the core material 110 is at least forty-five degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material. In other embodiments, the melting point of the core material 110 is at least fifty degrees Celsius higher than the melting point of the shell material 120 or the melting point of the thermoplastic material.

[0055] In certain configurations, the materials present in the shell 120 and the core 110 are not the same materials. For example, the shell material 120 may include a polyolefin, and the core material 110 may include a material having a melting point higher than the melting point of the polyolefin of the shell material 120. In other cases, the core material 110 may include a polyester, a polyamide, or a copolyamide, and the shell material 120 may include a material having a melting point lower than the melting point of the polyester, polyamide, or copolyamide in the core material 110. In additional examples, the shell material 120 may include a polyolefin, and the core material 110 may include a polyester, a polyamide, or a copolyamide. In some examples, the shell material 120 includes a polyolefin, and the core material 110 includes a polyester. In other examples, the shell material 120 includes a polyolefin, and the core material 110 includes a polyamide. In some examples, the shell material 120 includes a polyolefin, and the core material includes a copolyamide.

[0056] In some examples, the polyolefin of the shell material 120 may be polyethylene, polypropylene, or other olefin polymers and copolymers. In some embodiments, the polyolefin material of the shell 120 may be considered to be a linear low-density polyolefin. For example, the polyolefin material of the shell 120 may be a linear low-density polyethylene (LLDPE) or a low-density polyethylene (LDPE). Although the exact material properties may vary, the density of the linear low-density polyethylene may be from about 0.91 g / cm3 to about 0.94 g / cm3. In some examples, the melting point of the LLDPE or LDPE may be at least fifteen degrees Celsius lower than the melting point of the core material 110. In certain examples, the melting point of the LLDPE or LDPE may be at least twenty degrees Celsius lower than the melting point of the core material 110. In other examples, the melting point of the LLDPE or LDPE may be at least twenty-five degrees Celsius lower than the melting point of the core material 110. In certain examples, the melting point of the LLDPE or LDPE may be at least thirty degrees Celsius lower than the melting point of the core material 110. In other examples, the melting point of the LLDPE or LDPE may be at least thirty-five degrees Celsius lower than the melting point of the core material 110. In certain examples, the melting point of the LLDPE or LDPE may be at least forty degrees Celsius lower than the melting point of the core material 110. In other examples, the melting point of the LLDPE or LDPE may be at least forty-five degrees Celsius lower than the melting point of the core material 110. In some examples, the melting point of the LLDPE or LDPE may be at least fifty degrees Celsius lower than the melting point of the core material 110.

[0057] In other examples, the core material 110 may include: a polyester including terephthalate monomer units. For example, the polyester may be polyethylene terephthalate, polybutylene terephthalate, or polynaphthyl terephthalate. In certain examples, the melting point of the polyester including terephthalate monomer units in the core material 110 may be at least fifteen degrees higher than the melting point of the material in the shell material 120. In some examples, the melting point of the polyester including terephthalate monomer units in the core material 110 may be at least twenty degrees higher than the melting point of the material in the shell material 120. In certain examples, the melting point of the polyester including terephthalate monomer units in the core material 110 may be at least twenty-five degrees higher than the melting point of the material in the shell material 120. In other examples, the melting point of the polyester including terephthalate monomer units in the core material 110 may be at least thirty degrees higher than the melting point of the material in the shell material 120. In certain examples, the melting point of the polyester containing terephthalate monomer units in the core material 110 may be at least thirty-five degrees higher than the melting point of the material in the shell material 120. In some examples, the melting point of the polyester containing terephthalate monomer units in the core material 110 may be at least forty degrees higher than the melting point of the material in the shell material 120. In other examples, the melting point of the polyester containing terephthalate monomer units in the core material 110 may be at least forty-five degrees higher than the melting point of the material in the shell material 120. In additional examples, the melting point of the polyester containing terephthalate monomer units in the core material 110 may be at least fifty degrees higher than the melting point of the material in the shell material 120.

[0058] In some embodiments, the core material 110 may include a polyamide or a copolyamide. For example, the core material 110 may include nylon, nylon 66, aramid, polyesteramide, polyetheramide, polyetheresteramide, or other polyamide-containing copolymers. In some instances, the melting point of the polyamide or copolyamide in the core material 110 may be at least fifteen degrees higher than the melting point of the material in the shell material 120. In some instances, the melting point of the polyamide or copolyamide in the core material 110 may be at least twenty degrees higher than the melting point of the material in the shell material 120. In some instances, the melting point of the polyamide or copolyamide in the core material 110 may be at least twenty-five degrees higher than the melting point of the material in the shell material 120. In other instances, the melting point of the polyamide or copolyamide in the core material 110 may be at least thirty degrees higher than the melting point of the material in the shell material 120. In some instances, the melting point of the polyamide or copolyamide in the core material 110 may be at least thirty-five degrees higher than the melting point of the material in the shell material 120. In some examples, the melting point of the polyamide or copolyamide in the core material 110 may be at least forty degrees higher than the melting point of the material in the shell material 120. In other examples, the melting point of the polyamide or copolyamide in the core material 110 may be at least forty-five degrees higher than the melting point of the material in the shell material 120. In additional examples, the melting point of the polyamide or copolyamide in the core material 110 may be at least fifty degrees higher than the melting point of the material in the shell material 120.

[0059] In some examples, the shell material 120 may include polyethylene, such as LLDPE, and the core material 110 may include polyester or polyamide. For example, the core material 110 may include nylon, polyethylene terephthalate, polybutylene terephthalate, polynaphthyl terephthalate, or a combination thereof. In some examples, the melting point of the polyester or polyamide in the core material 110 may be at least fifteen degrees higher than the melting point of the polyethylene material in the shell material 120. In some examples, the melting point of the polyester or polyamide in the core material 110 may be at least twenty degrees higher than the melting point of the polyethylene material in the shell material 120. In some examples, the melting point of the polyester or polyamide in the core material 110 may be at least twenty-five degrees higher than the melting point of the polyethylene material in the shell material 120. In other examples, the melting point of the polyester or polyamide in the core material 110 may be at least thirty degrees higher than the melting point of the polyethylene material in the shell material 120. In certain examples, the melting point of the polyester or polyamide in the core material 110 may be at least thirty-five degrees higher than the melting point of the polyethylene material in the shell material 120. In some examples, the melting point of the polyester or polyamide in the core material 110 may be at least forty degrees higher than the melting point of the polyethylene material in the shell material 120. In other examples, the melting point of the polyester or polyamide in the core material 110 may be at least forty-five degrees higher than the melting point of the polyethylene material in the shell material 120. In additional examples, the melting point of the polyester or polyamide in the core material 110 may be at least fifty degrees higher than the melting point of the polyethylene material in the shell material 120.

[0060] In other cases, the bicomponent fibers present in the LWRT article may comprise a side-by-side fiber arrangement. Figure 2 , shows a diagram showing a cross-section of a bicomponent fiber through a side-by-side fiber arrangement. The bicomponent fiber 200 includes a first fiber 210 arranged to one side of a second fiber 220. The fibers 210, 220 may be wound around each other or may remain unwound and extend generally coaxially with each other throughout the fiber 200. Without wishing to be bound by any particular theory, the melting point of the material in one of the fibers 210, 220 is generally about the same as or the same as the melting point of the thermoplastic material of the core layer. In some examples, the melting points of one of the fibers 210, 220 and the thermoplastic material may differ by about one degree Celsius to about ten degrees Celsius, and the materials may still be considered compatible.

[0061] In certain embodiments, the melting point of fiber 210 is usually higher than another fiber 220 and the thermoplastic material. For example, when forming the core layer, the fiber 220 and the thermoplastic material can melt or soften to form a web of the core layer. The fiber 210 usually remains solid and does not melt or soften to any significant extent during the material processing to form the core layer. In certain examples, the melting point of fiber 210 is at least 15 degrees Celsius higher than the melting point of fiber 220 or the melting point of the thermoplastic material. In some examples, the melting point of fiber 210 is at least 20 degrees Celsius higher than the melting point of fiber 220 or the melting point of the thermoplastic material. In other examples, the melting point of fiber 210 is at least 25 degrees Celsius higher than the melting point of fiber 220 or the melting point of the thermoplastic material. In other examples, the melting point of fiber 210 is at least 30 degrees Celsius higher than the melting point of fiber 220 or the melting point of the thermoplastic material. In some examples, the melting point of fiber 210 is at least thirty-five degrees Celsius higher than the melting point of fiber 220 or the melting point of the thermoplastic material. In some embodiments, the melting point of fiber 210 is at least forty degrees Celsius higher than the melting point of fiber 220 or the melting point of the thermoplastic material. In other embodiments, the melting point of fiber 210 is at least forty-five degrees Celsius higher than the melting point of fiber 220 or the melting point of the thermoplastic material. In other embodiments, the melting point of fiber 210 is at least fifty degrees Celsius higher than the melting point of fiber 220 or the melting point of the thermoplastic material.

[0062] In certain configurations, the materials present in the fibers 210, 220 are not the same material. For example, the fibers 220 may include a polyolefin, and the fibers 210 may include a material having a melting point higher than the melting point of the polyolefin of the shell material 120. In other cases, the fibers 210 may include a polyester, a polyamide, or a copolyamide, and the fibers 220 may include a material having a melting point lower than the melting point of the polyester, polyamide, or copolyamide in the fibers 210. In additional examples, the fibers 220 may include a polyolefin, and the fibers 210 may include a polyester, a polyamide, or a copolyamide. In some examples, the fibers 220 include a polyolefin, and the fibers 210 include a polyester. In other examples, the fibers 220 include a polyolefin, and the fibers 210 include a polyamide. In some examples, the fibers 220 include a polyolefin, and the fibers 210 include a copolyamide.

[0063] In some examples, the polyolefin of fiber 220 may be polyethylene, polypropylene, or other olefin polymers and copolymers. In some embodiments, the polyolefin material of fiber 220 may be considered to be a linear low-density polyolefin. For example, the polyolefin material of fiber 220 may be a linear low-density polyethylene (LLDPE) or a low-density polyethylene (LDPE). Although the exact material properties may vary, the density of linear low-density polyethylene may be about 0.91 g / cm3 to about 0.94 g / cm3. In some examples, the melting point of LLDPE or LDPE may be at least fifteen degrees Celsius lower than the melting point of fiber 210. In certain examples, the melting point of LLDPE or LDPE may be at least twenty degrees Celsius lower than the melting point of fiber 210. In other examples, the melting point of LLDPE or LDPE may be at least twenty-five degrees Celsius lower than the melting point of fiber 210. In certain examples, the melting point of LLDPE or LDPE may be at least thirty degrees Celsius lower than the melting point of core material 110. In other examples, the melting point of the LLDPE or LDPE may be at least thirty-five degrees Celsius lower than the melting point of the fiber 210. In certain examples, the melting point of the LLDPE or LDPE may be at least forty degrees Celsius lower than the melting point of the fiber 210. In other examples, the melting point of the LLDPE or LDPE may be at least forty-five degrees Celsius lower than the melting point of the fiber 210. In some examples, the melting point of the LLDPE or LDPE may be at least fifty degrees Celsius lower than the melting point of the fiber 210.

[0064] In other examples, the fiber 210 may include: a polyester including terephthalate monomer units. For example, the polyester may be polyethylene terephthalate, polybutylene terephthalate, or polynaphthyl terephthalate. In certain examples, the melting point of the polyester including terephthalate monomer units in the fiber 210 may be at least fifteen degrees higher than the melting point of the material in the fiber 220. In some examples, the melting point of the polyester including terephthalate monomer units in the fiber 210 may be at least twenty degrees higher than the melting point of the material in the fiber 220. In certain examples, the melting point of the polyester including terephthalate monomer units in the fiber 210 may be at least twenty-five degrees higher than the melting point of the material in the fiber 220. In other examples, the melting point of the polyester including terephthalate monomer units in the fiber 210 may be at least thirty degrees higher than the melting point of the material in the fiber 220. In certain examples, the melting point of the polyester including terephthalate monomer units in the fiber 210 may be at least thirty-five degrees higher than the melting point of the material in the fiber 220. In some examples, the melting point of the polyester containing terephthalate monomeric units in fiber 210 may be at least forty degrees higher than the melting point of the material in fiber 220. In other examples, the melting point of the polyester containing terephthalate monomeric units in fiber 210 may be at least forty-five degrees higher than the melting point of the material in fiber 220. In additional examples, the melting point of the polyester containing terephthalate monomeric units in fiber 210 may be at least fifty degrees higher than the melting point of the material in fiber 220.

[0065] In some embodiments, fiber 210 may include a polyamide or copolyamide. For example, fiber 210 may include nylon, nylon 66, aramid, polyesteramide, polyetheramide, polyetheresteramide, or other copolymers containing polyamide. In some examples, the melting point of the polyamide or copolyamide in fiber 210 may be at least fifteen degrees higher than the melting point of the material in fiber 220. In some examples, the melting point of the polyamide or copolyamide in fiber 210 may be at least twenty degrees higher than the melting point of the material in fiber 220. In some examples, the melting point of the polyamide or copolyamide in fiber 210 may be at least twenty-five degrees higher than the melting point of the material in fiber 220. In other examples, the melting point of the polyamide or copolyamide in fiber 210 may be at least thirty degrees higher than the melting point of the material in fiber 220. In some examples, the melting point of the polyamide or copolyamide in fiber 210 may be at least thirty-five degrees higher than the melting point of the material in fiber 220. In some examples, the melting point of the polyamide or copolyamide in fiber 210 may be at least forty degrees higher than the melting point of the material in fiber 220. In other examples, the melting point of the polyamide or copolyamide in fiber 210 may be at least forty-five degrees higher than the melting point of the material in fiber 220. In additional examples, the melting point of the polyamide or copolyamide in fiber 210 may be at least fifty degrees higher than the melting point of the material in fiber 220.

[0066] In some examples, fiber 220 may include polyethylene, such as LLDPE, and fiber 210 may include polyester or polyamide. For example, fiber 210 may include nylon, polyethylene terephthalate, polybutylene terephthalate, polynaphthyl terephthalate, or a combination thereof. In some examples, the melting point of the polyester or polyamide in fiber 210 may be at least fifteen degrees higher than the melting point of the polyethylene material in fiber 220. In some examples, the melting point of the polyester or polyamide in core fiber 210 may be at least twenty degrees higher than the melting point of the polyethylene material in fiber 220. In some examples, the melting point of the polyester or polyamide in fiber 210 may be at least twenty-five degrees higher than the melting point of the polyethylene material in fiber 220. In other examples, the melting point of the polyester or polyamide in fiber 210 may be at least thirty degrees higher than the melting point of the polyethylene material in fiber 220. In some examples, the melting point of the polyester or polyamide in fiber 210 may be at least thirty-five degrees higher than the melting point of the polyethylene material in fiber 220. In some examples, the melting point of the polyester or polyamide in fiber 210 may be at least forty degrees higher than the melting point of the polyethylene material in fiber 220. In other examples, the melting point of the polyester or polyamide in fiber 210 may be at least forty-five degrees higher than the melting point of the polyethylene material in fiber 220. In additional examples, the melting point of the polyester or polyamide in fiber 210 may be at least fifty degrees higher than the melting point of the polyethylene material in fiber 220.

[0067] refer to Figure 3A , shows a diagram showing a cross section through a side-by-side fiber arrangement with a shell surrounding a bicomponent fiber of the side-by-side fiber arrangement. For example, fiber 300 includes a shell 320 surrounding two fibers 310, 315. In Figure 3A In the embodiment, fibers 310, 315 may include the same or similar components. For example, each of fibers 310, 315 may independently include and combine Figure 1 The same materials described for core material 110 in FIG. 1 , for example, each of fibers 310 , 315 may independently comprise polyamide, polyester, or other polymers.

[0068] In certain embodiments, the shell material 320 may include a polyolefin. In some examples, the polyolefin of the shell material 320 may be polyethylene, polypropylene, or other olefin polymers and copolymers. In some embodiments, the polyolefin material of the shell 320 may be considered to be a linear low-density polyolefin. For example, the polyolefin material of the shell 320 may be a linear low-density polyethylene (LLDPE) or a low-density polyethylene (LDPE). Although the exact material properties may vary, the density of the linear low-density polyethylene may be from about 0.91 g / cm3 to about 0.94 g / cm3. In some examples, the melting point of the LLDPE or LDPE may be at least fifteen degrees Celsius lower than the melting point of the fibers 310, 315. In certain examples, the melting point of the LLDPE or LDPE may be at least twenty degrees Celsius lower than the melting point of the fibers 310, 315. In other examples, the melting point of the LLDPE or LDPE may be at least twenty-five degrees Celsius lower than the melting point of the fibers 310, 315. In certain examples, the melting point of the LLDPE or LDPE may be at least thirty degrees Celsius lower than the melting point of the fibers 310, 315. In other examples, the melting point of the LLDPE or LDPE may be at least thirty-five degrees Celsius lower than the melting point of the fibers 310, 315. In certain examples, the melting point of the LLDPE or LDPE may be at least forty degrees Celsius lower than the melting point of the fibers 310, 315. In other examples, the melting point of the LLDPE or LDPE may be at least forty-five degrees Celsius lower than the melting point of the fibers 310, 315. In some examples, the melting point of the LLDPE or LDPE may be at least fifty degrees Celsius lower than the melting point of the fibers 310, 315.

[0069] In some examples, the fibers 310, 315 may independently include polyester or polyamide. In some cases, the fibers 310, 315 may independently include nylon, polyethylene terephthalate, polybutylene terephthalate, polynaphthyl terephthalate, or a combination thereof. In some examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least fifteen degrees higher than the melting point of the polyethylene material in the shell material 320. In some examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least twenty degrees higher than the melting point of the polyethylene material in the shell material 320. In some examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least twenty-five degrees higher than the melting point of the polyethylene material in the shell material 320. In other examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least thirty degrees higher than the melting point of the polyethylene material in the shell material 320. In certain examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least thirty-five degrees higher than the melting point of the polyethylene material in the shell material 320. In some examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least forty degrees higher than the melting point of the polyethylene material in the shell material 320. In other examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least forty-five degrees higher than the melting point of the polyethylene material in the shell material 320. In additional examples, the melting point of the polyester or polyamide in the fibers 310, 315 may be at least fifty degrees higher than the melting point of the polyethylene material in the shell material 320.

[0070] Although Figure 3A Two side-by-side fibers are shown that may contain the same composition, but this configuration is not necessary. Figure 3B , showing fibers 360, 365 arranged side by side surrounded by a shell 370. The fibers 360, 365 do not have to have the same composition as each other, but the melting point of each of the fibers 360, 365 is generally higher than the melting point of the shell 370 in the fiber arrangement 350. In one configuration, one of the fibers 360, 365 is a reinforcing fiber as mentioned below, such as an inorganic fiber, such as glass fiber, graphite fiber, carbon fiber, etc., and the other of the fibers 360, 365 is an organic fiber, such as containing one or more covalently bonded carbon-hydrogen groups. By packaging inorganic and organic fibers in a shell, the addition of fibers during material processing to form a core layer can be simplified. In other examples, the fibers 360, 365 can each be an organic fiber with different compositions.

[0071] In certain embodiments, the shell material 370 may include a polyolefin. In some examples, the polyolefin of the shell material 370 may be polyethylene, polypropylene, or other olefin polymers and copolymers. In some embodiments, the polyolefin material of the shell 370 may be considered to be a linear low-density polyolefin. For example, the polyolefin material of the shell 370 may be a linear low-density polyethylene (LLDPE) or a low-density polyethylene (LDPE). Although the exact material properties may vary, the density of the linear low-density polyethylene may be from about 0.91 g / cm3 to about 0.94 g / cm3. In some examples, the melting point of the LLDPE or LDPE may be at least fifteen degrees Celsius lower than the melting point of the fibers 360, 365. In certain examples, the melting point of the LLDPE or LDPE may be at least twenty degrees Celsius lower than the melting point of the fibers 360, 365. In other examples, the melting point of the LLDPE or LDPE may be at least twenty-five degrees Celsius lower than the melting point of the fibers 360, 365. In certain examples, the melting point of the LLDPE or LDPE may be at least thirty degrees Celsius lower than the melting point of the fibers 360, 365. In other examples, the melting point of the LLDPE or LDPE may be at least thirty-five degrees Celsius lower than the melting point of the fibers 360, 365. In certain examples, the melting point of the LLDPE or LDPE may be at least forty degrees Celsius lower than the melting point of the fibers 360, 365. In other examples, the melting point of the LLDPE or LDPE may be at least forty-five degrees Celsius lower than the melting point of the fibers 360, 365. In some examples, the melting point of the LLDPE or LDPE may be at least fifty degrees Celsius lower than the melting point of the fibers 360, 365.

[0072] In some examples, the fibers 360 and 365 may independently include polyester or polyamide, or one of the fibers 360 and 365 may be an inorganic reinforcing fiber. In some cases, the fibers 360 and 365 may independently include nylon, polyethylene terephthalate, polybutylene terephthalate, polynaphthyl terephthalate, or a combination thereof. In some examples, the melting point of the material in the fibers 360 and 365 may be at least fifteen degrees higher than the melting point of the polyethylene material in the shell material 370. In some examples, the melting point of the material in the fibers 360 and 365 may be at least twenty degrees higher than the melting point of the polyethylene material in the shell material 370. In some examples, the melting point of the material in the fibers 360 and 365 may be at least twenty-five degrees higher than the melting point of the polyethylene material in the shell material 370. In other examples, the melting point of the material in the fibers 360 and 365 may be at least thirty degrees higher than the melting point of the polyethylene material in the shell material 370. In certain examples, the melting point of the material in the fibers 360, 365 may be at least thirty-five degrees higher than the melting point of the polyethylene material in the shell material 320. In some examples, the melting point of the material in the fibers 360, 365 may be at least forty degrees higher than the melting point of the polyethylene material in the shell material 370. In other examples, the melting point of the material in the fibers 360, 365 may be at least forty-five degrees higher than the melting point of the polyethylene material in the shell material 370. In additional examples, the melting point of the material in the fibers 360, 365 may be at least fifty degrees higher than the melting point of the polyethylene material in the shell material 370.

[0073] In certain embodiments and with reference to Figure 4, showing core layer 410 comprising thermoplastic material, reinforcing fibers, bicomponent fibers and a leavening agent. As discussed further below, the combination of these materials can provide improved mechanical properties. Although not in all configurations, the leavening agent is typically captured in the voids or holes of core layer 410. Core layer 410 can first be formed as a prepreg, which is typically a precursor to core layer 410 and does not have to be fully formed. For ease of illustration, the core layer is described below, but the properties of the core layer may also be the same as the prepreg. Core layer 410 includes a porous structure to allow gas to flow through the core layer. For example, the void content or porosity of the core layer can be 0%-30%, 10%-40%, 20%-50%, 30%-60%, 40%-70%, 50%-80%, 60%-90%, 0%-40%, 0%-50%, 0%-60%, 0%-70%, 0%-80%, 0%-90%, 10%-50%, 10%-60%, 10%-70%, 10%-80%, 10%-90%, 10%-95%, 20%-60% %, 20%-70%, 20%-80%, 20%-90%, 20%-95%, 30%-70%, 30%-80%, 30%-90%, 30%-95%, 40%-80%, 40%-90%, 40%-95%, 50%-90%, 50%-95%, 60%-95%, 70%-80%, 70%-90%, 70%-95%, 80%-90%, 80%-95%, or any illustrative value within these exemplary ranges. In some cases, the porosity or void content of the core layer 410 is greater than 0%, such as not fully consolidated, up to about 95%. Unless otherwise specified, reference to a core layer of a certain void content or porosity is based on the total volume of the core layer, and is not necessarily the total volume of the core layer plus any other materials or layers coupled to the core layer.

[0074] In certain embodiments, improved mechanical properties may be achieved by including polymer bicomponent fibers in the core layer 410. For example, increasing the amount of reinforcing fibers in the core layer 410 may generally reduce certain mechanical properties. Including bicomponent fibers in the core layer may, for example, increase one or more of the peak load value, stiffness value, flexural strength value, and flexural modulus value for a selected molded thickness. These values ​​may be measured, for example, using SAE J949 dated April 2009 (also referred to as SAE J949_200904). Briefly, the SAE J949 protocol used performs a three-point bend test on the sample and measures various performance values.

[0075] In certain embodiments, the thermoplastic material of core layer 410 may at least partially comprise one or more of the following: polyethylene, polypropylene, polystyrene, acrylonitrile styrene, butadiene, polyethylene terephthalate, polybutylene terephthalate, polybutylene tetrachloride, and polyvinyl chloride, plasticized and unplasticized, and blends of these materials with each other or with other polymeric materials. Other suitable thermoplastics include, but are not limited to, polyarylene ethers, polycarbonates, polyester carbonates, thermoplastic polyesters, polyimides, polyetherimides, polyamides, acrylonitrile-butyl acrylate-styrene polymers, amorphous nylons, polyarylene ether ketones, polyphenylene sulfides, polyarylene sulfones, polyether sulfones, liquid crystal polymers, commercially known as Poly(1,4-phenylene) compounds such as Bayer's The high heat polycarbonate of PC, high temperature nylon and silicone, and these materials each other or with other polymer materials alloy and blend can use the original thermoplastic material for forming the core layer in powder form, resin form, rosin form, fiber form or other suitable form. Various forms of exemplary thermoplastic materials are described herein, and are also described in U.S. Publication No. 20130244528 and US20120065283, for example. The exact amount of thermoplastic material present in the core layer 410 can vary, and the illustrative amount is in the range of about 20 weight % to about 80 weight %. As mentioned in this article, the material of the core layer 410 can be selected so that its melting point is approximately the same as one of the materials in the bicomponent fiber and is lower than the melting point of another material in the bicomponent fiber. The illustrative melting point range of the thermoplastic material includes, but is not limited to, about 120 degrees Celsius to about 260 degrees Celsius. If necessary, a thermoplastic material that melts between 100 degrees Celsius and 315 degrees Celsius can also be used.

[0076] In some examples, the reinforcing fibers of the core layer described herein may include glass fibers, carbon fibers, graphite fibers, synthetic organic fibers, particularly high modulus organic fibers, such as para- and meta-aramid fibers, nylon fibers, polyester fibers, or any high melt flow index resin suitable for use as fibers, natural fibers (such as hemp, sisal, jute, flax, coconut shell fibers, kenaf, and cellulose fibers), mineral fibers (such as basalt, mineral wool (such as rock or slag wool), wollastonite, alumina silica, etc., or mixtures thereof), metal fibers, metallized natural and / or synthetic fibers, ceramic fibers, yarn fibers, or mixtures thereof. In some cases, a type of reinforcing fiber may be used together with the mineral fiber, for example, a fiber formed by spinning or stretching a molten mineral. Illustrative mineral fibers include, but are not limited to, mineral wool fibers, glass wool fibers, asbestos fibers, and ceramic wool fibers. In some examples, the reinforcing fibers may be selected to be inorganic fibers, such as fibers that do not include covalently bonded carbon-hydrogen groups.

[0077] In certain embodiments, any of the aforementioned reinforcing fibers can be chemically treated before use to provide the required functional groups or to give the fiber other physical properties. The total fiber content (reinforcing fibers + bicomponent fibers) in the core layer can be about 20% by weight to about 90% by weight of the core layer, more specifically, about 30% by weight to about 70% by weight of the core layer. Typically, the total fiber content of the composite material product comprising the core layer is about 20% by weight to about 90% by weight of the composite material, more specifically about 30% by weight to about 80% by weight, such as about 40% by weight to about 70% by weight. The specific size and / or orientation of the reinforcing fibers used may depend at least in part on the required properties of the polymer material used and / or the resulting core layer. In view of the benefits of the present disclosure, those of ordinary skill in the art will easily select the additional type, fiber size and quantity of suitable fibers. In a non-limiting illustration, the diameter of the reinforcing fibers dispersed in the thermoplastic material to provide the core layer is generally greater than about 5 microns, more specifically about 5 microns to about 22 microns, and a length of about 5mm to about 200mm. More specifically, the reinforcing fiber diameter may be from about 5 microns to about 22 microns, and the fiber length may be from about 5 mm to about 75 mm. In some configurations, the flame retardant material may be present in fiber form. For example, the core layer may include a thermoplastic material, reinforcing fibers, bicomponent fibers, and fibers including a flame retardant material.

[0078] In some configurations, core layer 410 may be substantially halogen-free or halogen-free layer to meet the restrictions of harmful substances required for certain applications. In other cases, core layer 410 may include halogenated flame retardants (which may be present in flame retardant materials, or may be added in addition to flame retardant materials), for example, halogenated flame retardants comprising one or more of F, Cl, Br, I and At or compounds including such halogens, such as tetrabromobisphenol A polycarbonate or monohalogenated, dihalogenated, trihalogenated or tetrahalogenated polycarbonates. In some cases, the thermoplastic material used in core layer 410 may include one or more halogens to impart certain flame retardancy without the need to add another flame retardant. For example, in addition to the presence of flame retardant materials, thermoplastic materials may also be halogenated, or the original thermoplastic material may be halogenated and used alone. In the presence of halogenated flame retardants, it is desirable that the flame retardant exists in a flame retardant amount, which may vary according to other components present. For example, the halogenated flame retardant present in addition to the flame retardant material can be about 0.1 wt % to about 40 wt % (based on the weight of the prepreg), more specifically about 0.1 wt % to about 15 wt %, for example, about 5 wt % to about 15 wt % is present. If necessary, two different halogenated flame retardants can be added to the core layer 410. In other cases, non-halogenated flame retardants can be added, such as, for example, flame retardants comprising one or more of N, P, As, Sb, Bi, S, Se and Te. In certain embodiments, non-halogenated flame retardants may include phosphating materials, so the core layer 410 can be more environmentally friendly. In the presence of non-halogenated or substantially halogen-free flame retardants, it is desired that the flame retardant is present in a flame retardant amount, which can vary according to the other components present. For example, a substantially halogen-free flame retardant can be present in an amount of about 0.1% to about 40% by weight (based on the weight of the prepreg), more specifically in an amount of about 5% to about 40% by weight, such as about 5% to about 15% by weight, based on the weight of the core layer. If desired, two different substantially halogen-free flame retardants can be added to the core layer 410. In some cases, the core layer 410 described herein may include one or more halogenated flame retardants and one or more substantially halogen-free flame retardants. When there are two different flame retardants, a combination of the two flame retardants can be present in a flame retardant amount, which can vary according to the other components present. For example, the total weight of the flame retardant present can be about 0.1% to about 40% by weight (based on the weight of the prepreg or core), more specifically in an amount of about 5% to about 40% by weight, such as about 2% to about 14% by weight, based on the weight of the core layer. The flame retardants used in the core layers described herein may be added to the mixture comprising the thermoplastic material, bicomponent fibers, and reinforcing fibers (before the mixture is disposed on a screen or other processing assembly) or may be added after the core layer 410 is formed.

[0079] As mentioned herein, core layer 410 may include a leavening agent present in the pores or voids of the core layer. The leavening agent may take the form of expandable microspheres, the volume of which may increase upon exposure to heat or other stimuli. For example, the thickness of core layer 410 may be increased by expansion of the leavening agent. The exact amount of leavening agent present in core layer 410 may vary, but illustrative amounts include, but are not limited to, about 0.5% by weight to about 30% by weight.

[0080] In certain embodiments, the exact amount of the bicomponent fiber in the core layer described herein can vary. In general, the weight percentage of the bicomponent fiber in the core layer can vary in the range of about 2 wt % to about 30 wt %. In some instances, there are bicomponent fibers and reinforcing fibers of approximately the same amount in the core layer. In some instances, the total basis weight of the core layer 410 can vary in the range of about 500gsm to about 3500gsm. In some instances, the lighter core layer with suitable mechanical properties can be more desirable for reducing gross weight, for example, the basis weight of the core layer 410 can vary in the range of about 750gsm to about 1500gsm or about 750gsm to about 1250gsm.

[0081] In certain embodiments, the core layer and / or article described herein may be generally as Figure 5The preparation of reinforcing fiber, bicomponent fiber, bulking agent and thermoplastic material is shown. In order to produce the core layer, thermoplastic material, reinforcing fiber, bicomponent fiber, bulking agent and optional other materials can be added or metered into the dispersed foam in the open-top mixing tank equipped with an impeller in step 510 to provide an aqueous dispersion of the material. Without wishing to be bound by any particular theory, the presence of trapped air pockets of the foam can help disperse reinforcing fiber, bicomponent fiber, thermoplastic material, bulking agent and any other material. In some instances, the dispersed mixture of fiber, bulking agent and thermoplastic can be pumped to the headbox located above the wire section of the paper machine via a distribution manifold. For example, in step 520, the aqueous mixture can be deposited on a moving mesh screen or other supporting element. Then the foam can be removed without removing the fiber, bulking agent or thermoplastic material, while using pressure to provide the dispersed mixture to a moving support, such as a mesh screen, continuously producing a uniform fiber wet web, wherein the bulking agent is captured in the net. At step 530, the wet web may be passed through a dryer at a suitable temperature to reduce the moisture content and melt or soften at least one of the thermoplastic material and the bicomponent fiber to provide a core layer. When the hot web leaves the dryer, an optional surface or outer skin layer, such as a textured film, may be laminated to the web by passing the web of reinforcing fibers, bicomponent fibers, thermoplastic material, bulking agent, and textured film through the nip of a set of heated rollers. If desired, additional layers, such as another film layer, a scrim layer, etc., may also be attached to one or both sides of the web along with the textured film to facilitate easy handling of the produced composite material. The composite material may then be passed through a tension roller and continuously cut (cut) to the desired size for subsequent forming into a final composite product. Further information regarding the preparation of such composite materials, including suitable materials and processing conditions for use in forming such composite materials, is described, for example, in U.S. Patents 6,923,494; 4,978,489; 4,944,843; 4,964,935; 4,734,321; 5,053,449; 4,925,615; 5,609,966 and U.S. Patent Application Publications US 2005 / 0082881; US ​​2005 / 0228108; US 2005 / 0217932; US 2005 / 0215698; US 2005 / 0164023; and US 2005 / 0161865.

[0082] In another configuration, the core layer and / or article described herein may be generally as Figure 6The preparation of reinforcing fiber, bicomponent fiber and thermoplastic material is shown. In order to produce the core layer, thermoplastic material, reinforcing fiber, bicomponent fiber and optional other materials can be added or metered into the dispersed foam in the open-top mixing tank equipped with an impeller to provide an aqueous dispersion. Without wishing to be bound by any particular theory, the presence of trapped air pockets of the foam can help disperse reinforcing fiber, bicomponent fiber, thermoplastic material and any other material. In some examples, the dispersed mixture of fiber and thermoplastic can be pumped to the headbox located above the wire section of the paper machine via a distribution manifold. For example, the aqueous mixture can be deposited on a moving mesh screen or other supporting element to provide a wet web in step 620. Then the foam can be removed without removing the fiber or thermoplastic material, and the dispersed mixture is provided to a moving support, such as a mesh screen, using pressure to continuously produce a uniform fiber wet web. Then the leavening agent can be deposited or sprayed on the top of the wet web in step 625 to provide a wet web including a leavening agent. In step 630, the wet web containing the deposited bulking agent may be passed through a dryer, optionally under vacuum or by applying pressure, and heated at a suitable temperature to reduce the moisture content and melt or soften at least one of the thermoplastic material and the bicomponent fiber to provide a core layer. When the hot web leaves the dryer, an optional surface or outer skin layer, such as a textured film, may be laminated to the web by passing the web of reinforcing fibers, bicomponent fibers, thermoplastic material, bulking agent, and textured film through the nip of a set of heated rollers. If desired, additional layers, such as another film layer, a scrim layer, etc., may also be attached to one or both sides of the web along with the textured film to facilitate easy handling of the produced composite material. The composite material may then be passed through a tension roller and continuously cut (cut) to the desired size for subsequent forming into a final composite product.

[0083] In certain embodiments, the core layers described herein may be used with skin layers to provide a composite article. Figure 7, the skin layer 720 is shown as being disposed on the first surface of the core layer 410 to provide the composite article 700. The skin layer 720 may include, for example, a film, a scrim (e.g., a fibrous scrim), an inorganic fiberglass (inorganic fiberglass+scrim), a foil, a woven fabric, a nonwoven fabric, or as an inorganic coating, an organic coating, or a thermosetting coating disposed on the core layer. In other cases, the layer 720 may include a limiting oxygen index greater than about 22 as measured according to ISO 4589 dated 1996. In the case where the fibrous scrim is present as the skin layer 720 (or as part of the skin layer 720), the fibrous scrim may include at least one of glass fiber, aramid fiber, graphite fiber, carbon fiber, inorganic mineral fiber, metal fiber, metallized synthetic fiber, and metallized inorganic fiber. In the case where the thermosetting coating is present as the layer 720 (or as part of the layer 720), the coating may include at least one of unsaturated polyurethane, vinyl ester, phenolic, and epoxy resin. In the case where an inorganic coating is present as layer 720 (or as part of layer 720), the inorganic coating may include a mineral containing a cation selected from the group consisting of Ca, Mg, Ba, Si, Zn, Ti, and Al, or may include at least one of gypsum, calcium carbonate, and mortar. In the case where a nonwoven fabric is present as layer 720 (or as part of layer 720), the nonwoven fabric may include a thermoplastic material, a thermosetting binder, an inorganic fiber, a metal fiber, a metallized inorganic fiber, and a metallized synthetic fiber. If desired, an intermediate layer (not shown) may be present between the core layer and the outer skin layer 720. For example, an adhesive layer or a layer of other material may be present between the core layer 410 and the outer skin layer 720.

[0084] In some examples, the composite article may further include a second skin layer disposed on another surface of the core layer. Figure 8, a composite article 800 is shown comprising skin layers 720, 820 sandwiching core layer 410. Layer 820 may be the same as layer 720 or may be different. In some cases, layer 820 may comprise, for example, a film, a scrim (e.g., a fibrous scrim), an inorganic fiberglass (inorganic fiberglass + scrim), a foil, a woven fabric, a nonwoven fabric, or exists as an inorganic coating, an organic coating, or a thermosetting coating disposed on the core layer. In other cases, layer 820 may comprise a limiting oxygen index greater than about 22 as measured according to ISO 4589 dated 1996. In the case where a fibrous scrim is present as layer 820 (or as part of layer 820), the fibrous scrim may comprise at least one of glass fibers, aramid fibers, graphite fibers, carbon fibers, inorganic mineral fibers, metal fibers, metallized synthetic fibers, and metallized inorganic fibers. Where a thermosetting coating is present as layer 820 (or as part of layer 820), the coating may include at least one of unsaturated polyurethane, vinyl ester, phenolic, and epoxy resin. Where an inorganic coating is present as layer 820 (or as part of layer 820), the inorganic coating may include a mineral containing a cation selected from the group consisting of Ca, Mg, Ba, Si, Zn, Ti, and Al, or may include at least one of gypsum, calcium carbonate, and mortar. Where a nonwoven fabric is present as layer 820 (or as part of layer 820), the nonwoven fabric may include a thermoplastic material, a thermosetting binder, an inorganic fiber, a metal fiber, a metallized inorganic fiber, and a metallized synthetic fiber. If desired, an intermediate layer (not shown) may be present between the core layer and the outer skin layer 820. For example, an adhesive layer or a layer of other material may be present between the core layer 410 and the outer skin layer 820.

[0085] In certain configurations, the composite article may include a decorative layer disposed on a surface of the core layer or on an outer skin layer. Fig. 9 , showing an article 900 including a decorative layer 830 disposed on an outer skin layer 720. Although not shown, the decorative layer may be disposed on an opposite surface of the core layer 410 or may be disposed on Figure 8On the outer skin layer 820 shown in . In some examples, the decorative layer 930 can be configured as a decorative layer, a textured layer, a colored layer, etc. For example, the decorative layer 930 can be formed by a thermoplastic film such as polyvinyl chloride, polyolefin, thermoplastic polyester, thermoplastic elastomer, etc. The decorative layer 930 can also be a multilayer structure, which includes a foam core formed by, for example, polypropylene, polyethylene, polyvinyl chloride, polyurethane, etc. Fabrics can be bonded to the foam core, such as woven fabrics made of natural and synthetic fibers, organic fiber woven fabrics after needle punching or the like, raised fabrics, knitwear, flocked fabrics or other such materials. Fabrics can also be bonded to the foam core with thermoplastic adhesives, including pressure-sensitive adhesives and hot melt adhesives, such as polyamides, modified polyolefins, polyurethanes and polyolefins. The decorative layer 930 can also be produced using spunbond, thermal bonding, spunlace, meltblown, wet laying and / or dry laying processes. Insulating or sound absorbing layers may also be bonded to one or more surfaces of the articles described herein, and may be open or closed, such as open-cell foam or closed-cell foam, as desired.

[0086] In certain embodiments, the LWRT articles described herein may be molded to a specific thickness. Although not in all cases, the molding temperature may be selected to increase the total volume of the leavening agent, which may increase the thickness of the LWRT article. If compressed during formation of the LWRT article, the LWRT article without the leavening agent may also be expanded to some extent during molding. The exact molded thickness may vary as desired, and typical molded thicknesses vary in the range of about 1 cm to about 10 cm in the longitudinal and transverse directions, but other molded thicknesses may also be used.

[0087] In certain embodiments, as referred to herein, the presence of bicomponent fibers, reinforcing fibers, bulking agents, and thermoplastic materials in the core layer of an LWRT article may provide improved mechanical properties for selected molded thicknesses.

[0088] In certain embodiments, the LWRT article comprising a core layer and an outer skin layer may comprise a peak load value of about 10 N / cm to about 40 N / cm in the longitudinal direction and about 5 N / cm to about 30 N / cm in the transverse direction as measured by SAE J949_200904 at a molded thickness of 1.5 cm to 4 cm in the longitudinal and transverse directions.

[0089] In certain embodiments, the LWRT article comprising a core layer and an outer skin layer may comprise a stiffness value of about 6 N / cm to about 50 N / cm in the longitudinal direction and about 3 N / cm to about 30 N / cm in the transverse direction as measured by SAE J949_200904 at a molded thickness of 1.5 cm to 4 cm in the longitudinal and transverse directions.

[0090] In certain embodiments, the LWRT article comprising a core layer and an outer skin layer may comprise a tensile strength of about 6 N / m in the longitudinal direction as measured by SAE J949_200904 at a molded thickness of 1.5 cm to 4 cm in the longitudinal direction and in the transverse direction. 2 About 20N / m 2 and about 4 N / m in the transverse direction 2 About 12N / m 2 flexural strength value.

[0091] In some examples, the LWRT article comprising a core layer and an outer skin layer may comprise a tensile strength of about 800 N / m in the longitudinal direction as measured by SAE J949_200904 at a molded thickness of 1.5 cm to 4 cm in the longitudinal direction and in the transverse direction. 2 About 1800N / m 2 and about 500 N / m in transverse direction 2 To about 1600N / m 2 Flexural modulus.

[0092] In certain embodiments, the core layers and articles described herein may be used in architectural and automotive applications, such as headliners, rear window trim, trunk trim, office partitions, cabinet backs, automotive interior panels, or other automotive interior articles.

[0093] In certain embodiments and with reference to Fig.10 , the articles described herein may be present in the roof of a vehicle. Illustrative vehicles include, but are not limited to, automobiles, trucks, trains, subways, recreational vehicles, airplanes, ships, submarines, spacecraft, and other vehicles that can transport people or cargo. In some cases, the roof typically comprises at least one prepreg or core layer comprising bicomponent fibers, reinforcing fibers, thermoplastic materials, bulking agents, one or more optional outer skin layers disposed on the core layer or on the outer skin layer, and a decorative layer, such as a decorative fabric. In addition to being aesthetically pleasing and / or visually pleasing, the decorative layer may also enhance sound absorption and may optionally include foam, insulation, or other materials. In Fig.10, a top view of a canopy is shown in FIG. The canopy 1000 includes a body 1010 and an opening 1020, such as for a skylight, a roof window, etc. The body of the canopy 1010 can use one or more of the core layers described herein and be produced using a molding machine, wherein a decorative fabric is placed on the surface of the core layer and pressed with a desired mold to transform the article into a canopy having a desired shape. The opening 1020 can then be provided by trimming the canopy 1000. Non-visible surfaces of the canopy, such as those that rest on the roof, can include one or more additional layers or adhesives as desired. The overall shape and geometry of the canopy can be selected based on the area of ​​the vehicle to which the canopy is to be attached. For example, the length of the canopy can be sized and arranged so that it spans from the front windshield to the rear windshield, and the width of the canopy can be sized and arranged so that it spans from the left side of the vehicle to the right side of the vehicle. In some examples, the core layer of the canopy 1000 may include 20% to 80% by weight of reinforcing fibers and bicomponent fibers (total) and 20% to 80% by weight of thermoplastic material. In other embodiments, the reinforcing fibers include glass fibers and the thermoplastic material includes a polyolefin. The bicomponent fibers may include a core-shell arrangement or other arrangements as described herein. In some examples, the automotive canopy may provide peak load values, stiffness values, flexural strength values, and / or flexural modulus values ​​as discussed herein in conjunction with the core layer.

[0094] In some cases, the core layer can also be used to produce other automotive interior components, including panels, trim pieces, etc. Fig.11 An illustration of a rear window trim 1100 is shown in FIG. 1 (top view). The trim 1100 may include one or more of the core layers as described herein, optionally with an outer skin layer and / or a decorative layer. In some examples, the core layer of an automotive component such as a trim sheet may include 20 wt % to 80 wt % reinforcing fibers and bicomponent fibers (total) and 20 wt % to 80 wt % thermoplastic material. In other embodiments, the reinforcing fibers include glass fibers, and the thermoplastic material includes a polyolefin. The bicomponent fibers may include a core-shell arrangement or other arrangements as described herein. In some examples, an automotive trim or interior component may provide peak load values, stiffness values, flexural strength values, and / or flexural modulus values ​​as discussed herein in conjunction with the core layer.

[0095] In other configurations, the bicomponent fibers described herein can be used in non-automotive articles, such as furniture. Fig.12, a display cabinet 1200 is shown, which includes a top surface 1110, side surfaces 1212, 1214 connected to the front surface 1210, and a back surface 1220 connected to the side surfaces 1212, 1214. Surfaces 1210, 1212, 1214 and 1220 together form an internal storage area accessible to a user. Although not shown, the cabinet 1200 may include a front surface, such as a glass surface or other material to view the contents of the cabinet. Alternatively, a door or other device may be attached to the cabinet 1200 to shield the contents in the cabinet 1200 from being viewed. One or more surfaces of the cabinet 1200 may be configured as a LWRT product having a core layer comprising TP material, reinforcing fibers and bicomponent fibers. In some examples, the back surface 1220 may include a core layer, the reinforcing fibers and bicomponent fibers held together by a thermoplastic material. In the case where more than one of the surfaces of the product 1200 includes bicomponent fibers in one layer, the layers do not have to have the same composition, thickness or number of layers. In some examples, the core layer of the furniture article 1200 may include 20% to 80% by weight reinforcing fiber bicomponent fibers (total) and 20% to 80% by weight thermoplastic material. In other embodiments, the reinforcing fibers include glass fibers and the thermoplastic material includes a polyolefin. The bicomponent fibers may include a core-shell arrangement or other arrangements. In some examples, the furniture article 1200 or panels thereof may provide peak load values, stiffness values, flexural strength values, and / or flexural modulus values ​​as discussed herein in conjunction with the core layer.

[0096] In some configurations, the article of furniture may be configured to receive at least one drawer. Fig.13 , the cabinet 1300 is shown to include a drawer 1310 and a back surface 1320. For example, the back surface 1320 may include an LWRT article as described herein, such as an article having bicomponent fibers. Other surfaces of the cabinet 1300 may also include an LWRT article as described herein. In other configurations, the furniture article 1300 may be configured to receive (or may include) at least one door. See Fig.14 , cabinet 1400 includes door 1410 and back surface 1420. For example, back surface 1420 may include LWRT products as described herein. Other surfaces of cabinet 1400 may also include LWRT products as described herein. If desired, the outer surface of door 1410 may include LWRT as described herein. In the case where the cabinet includes a door, the door need not be closable by means of hinges 1412, 1414. In fact, the door may be configured as Fig.15 The sliding door 1510 is shown in the cabinet 1500.

[0097] Certain specific examples are described to illustrate additional aspects of the techniques described herein.

[0098] Example 1

[0099] Several samples were prepared and tested to determine the properties of composite articles including bicomponent fibers. The materials used in the test samples and their numbers are shown in Table 1 below. PP refers to polypropylene. The polymeric fibers tested were core-sheath bicomponent fibers, with LLDPE in the sheath and polyethylene terephthalate in the core.

[0100] Table 1

[0101]

[0102] Example 2

[0103] The composite articles of Example 1 were molded into different thicknesses. Table 2 below lists some different thicknesses for different articles. MD refers to the longitudinal direction of the test specimen matched to the machine direction, and CD refers to the longitudinal direction of the test specimen matched to the cross direction.

[0104] Table 2

[0105]

[0106] Example 3

[0107] The peak load values ​​of the test samples were measured using SAE J949_200904. In the three-point bending test, a three-point bending test was used, in which the film side of the test sample faced the load. The measured peak load values ​​of the test samples are shown in Table 3 below.

[0108] Table 3

[0109]

[0110] For all tested samples, along with the molded thickness increase, the peak load value in the longitudinal and transverse direction usually increases.When the peak load value of the sample (ST-12244 and ST-12245) with microballoon is compared with those samples (ST-12242 and ST-12243) without microballoon, under similar thickness, the peak load of the sample based on microballoon is usually higher.For example, under the thickness of 2.6cm, the peak load value of 990gsm ST-12242b sample in the longitudinal and transverse direction is respectively 25.2 and 17.0.Under the thickness of 2.5cm, the peak load value of 990gsm ST-12244a sample in the longitudinal and transverse direction is respectively 32.2 and 21.1.For 790gsm sample, observe similar results, for example, the MD and CD peak load values ​​of ST-12245a are greater than the MD and CD peak load values ​​of ST-12243c. These results are consistent with the combination of thermoplastic material, reinforcing fibers, polymeric fibers, and microspheres providing enhanced peak loads at selected basis weights and molded thicknesses.

[0111] Example 4

[0112] The stiffness values ​​of the test samples were measured using SAE J949_200904. In the three-point bending test, a three-point bending test was used, in which the film side of the test sample faced the load. The measured stiffness values ​​of the test samples are shown in Table 4 below.

[0113] Table 4

[0114]

[0115] The stiffness of the lighter products including less fiber is generally lower. When the stiffness values ​​of the samples (ST-12244 and ST-12245) with microspheres are compared with those samples (ST-12242 and ST-12243) without microspheres, under similar thickness, the sample stiffness based on microspheres is the same or higher. For example, under about 2.6cm molded thickness, the stiffness value of 990gsm ST-12242b sample in the longitudinal direction is 21.0. Under 2.5cm molded thickness, the stiffness value of 990gsm ST-12244a sample is 22.2. For these same samples, in the presence of microspheres, the stiffness in the transverse direction is reduced. For 790gsm sample, the MD and CD stiffness values ​​(10.1 and 7.6) of ST-12245a are less than the MD and CD stiffness values ​​(15.1 and 12.7) of ST-12243c. These results are consistent with the bicomponent fibers and microspheres providing an article that is equally or more flexible than the results without the microspheres present.

[0116] Example 5

[0117] The bending strength values ​​of the test samples were measured using SAE J949_200904. In the three-point bending test, a three-point bending test was used, in which the film side of the test sample faced the load. The measured bending strength values ​​of the test samples are shown in Table 5 below.

[0118] Table 5

[0119]

[0120] Flexural strength generally decreases with the increase of molded thickness. The flexural strength of the lighter product including less fiber is also generally lower. When the flexural strength of the sample (ST-12244 and ST-12245) with microspheres is compared with those samples (ST-12242 and ST-12243) without microspheres, under similar thickness, the flexural strength of the sample based on microspheres is the same or higher. For example, under the molded thickness of about 2.6cm, the flexural strength of 990gsm ST-12242b sample in the longitudinal direction is 11.3. Under the molded thickness of 2.5cm, the flexural strength of 990gsm ST-12244a sample is 15.1. For these same samples, in the presence of microspheres, the flexural strength in the transverse direction increases slightly.

[0121] For the 790 gsm sample, the MD and CD flexural strength values ​​of ST-12245a (14.5 and 10.2) are much higher than those of ST-12243c (8.9 and 6.3). These results are consistent with bicomponent fibers and microspheres providing equal or better flexural strength.

[0122] Example 6

[0123] The flexural modulus values ​​of the test samples were measured using SAE J949_200904. In the three-point bending test, a three-point bending test was used, in which the film side of the test sample faced the load. The measured flexural modulus values ​​of the test samples are shown in Table 6 below.

[0124] Table 6

[0125]

[0126] The flexural modulus of the sample (ST-12244 and ST-12245) with microballoon is compared with those samples (ST-12242 and ST-12243) without microballoon, under similar thickness, the flexural modulus of the sample based on microballoon is identical or higher.For example, under the molded thickness of about 2.6cm, the flexural modulus of 990gsmST-12242b sample in the longitudinal direction is 1389.6.Under the molded thickness of 2.5cm, the flexural modulus of 990gsmST-12244a sample is 1582.8.For these same samples, in the presence of microballoon, the flexural strength in the transverse direction increases. For the 790 gsm sample, the MD and CD flexural modulus values ​​of ST-12245a (1546.7 and 1204.8) are much higher than those of ST-12243c (1195.5 and 914.3). These results are consistent with bicomponent fibers and microspheres providing equal or better flexural modulus.

[0127] Example 7

[0128] Glass / bicomponent polymer fiber hybrid LWRT (H-LWRT) and standard glass fiber LWRT (S-LWRT) sheets are manufactured using the same wet laying process. The polyolefin resin, chopped glass fibers and bicomponent polymer fibers for H-LWRT are dispersed in water. The well-dispersed aqueous suspension of resin and fiber is transferred to the web forming section, and the swelling agent is added to the continuous web. The resulting web is drained, heated, laminated with surface materials (scrim and film) and consolidated to produce a flat LWRT composite sheet. Materials with various basis weights (areal density) can be produced by adjusting the manufacturing parameters. The basis weight of the control sample (S-LWRT) is 650g / m2, which is about 14.4% heavier than the basis weight of HLWRT, 568g / m2.

[0129] After being heated above the melting point of the resin, the material undergoes an increase in thickness due to bending of the fibers and the expansion / bulking agent releasing residual stresses. Thus, all materials were able to be molded to a thickness of 3.5 to 7 mm, which is thicker than the as-produced condition / thickness (Table 1). Fig.16 An example part molded from a sheet of Sample B (H-LWRT) is shown. The material shows good formability to fit the complex shape of the mold.

[0130] Analytical properties including basis weight (areal density), as-produced thickness, and glass (ash) content were measured according to standard internal testing procedures. Tensile properties of samples with a thickness of 3 mm were measured according to ASTM D790. Flexural properties of molded specimens with thicknesses of 3.5, 4, 5.5, and 7 mm were evaluated according to ASTM D638. Table 7 shows the physical properties of S-LWRT and H-LWRT.

[0131] Table 7

[0132] sample <![CDATA[Grammage (g / m 2 )]]> Thickness(mm) Ash content (%) Control (S-LWRT) 650 1.02 33.50 Sample A (H-LWRT) 568 1.12 29.72 Sample B (H-LWRT) 568 1.20 34.18

[0133] The control sample S-LWRT is 82 g / m heavier than the two H-LWRT samples. 2 (14.4%). S-LWRT shows a slightly lower thickness, indicating a slightly higher level of consolidation. Samples A and B (H-LWRT) have different glass contents due to the different weight percentages of the bicomponent polymeric fibers.

[0134] Example 8

[0135] To evaluate the tensile properties of the samples shown in Table 7, molded sheets having a thickness of 3.5 mm were cut into dog-bone tensile specimens by a punch. Fig.17 is a graph showing the tensile modulus of Sample A (H-LWRT), Sample B (H-LWRT) and Control (S-LWRT), and Fig.18 The following is a graph showing its tensile strength. For both tensile modulus and tensile strength, the results for all three samples in the machine direction (MD) are significantly better than those in the cross direction (CD). This may be due to the fiber orientation being biased toward the machine direction, which occurs primarily in the headbox. The flow in the headbox is a mixture of shear and stretching. The complex flow may have shear near the wall and stretching toward the machine direction throughout the domain. As a result, the fibers may be strongly aligned toward the flow direction, leading to better mechanical properties in the MD.

[0136] Sample B (H-LWRT) has the best average tensile modulus in MD, while the control (SLWRT) shows an average modulus in CD that is only slightly greater than both samples A and B. For tensile strength, all three samples show very similar performance in MD. In CD, sample A shows similar results to the control, and sample B is only slightly lower than the other two. It is worth noting that the control (S-LWRT) is 82 g / m heavier than the two H-LWRT samples. 2 This means that by hybridizing the glass fiber and bicomponent polymer fiber to achieve a full 82g / m 2 Weight reduction without sacrificing tensile properties. Especially for tensile properties, strength is highly dependent on the bond between resin and fiber. Bicomponent polymeric fibers have a component with a lower melting point than the matrix resin. During the heating and consolidation stage, the lower melting point component of the polymeric fiber melts and bonds to the glass fiber surface, which is believed to help better saturate the resin around the glass fiber.

[0137] Example 9

[0138] Bend tests were performed on specimens molded to 3.5, 4, 5.5 and 7 mm. Fig.19A and 19B The peak loads in MD and CD are compared between Sample A (H-LWRT), Sample B (HLWRT) and Control (S-LWRT). Just like the tensile properties, the peak load results in MD are also better than those in CD. Peak load decreases with increasing thickness due to the increase in porosity. All three samples show very similar peak load results throughout the molded thickness range. This indicates that weight reductions of up to 82 g / m2 can be achieved by hybridizing glass fibers with bicomponent polymeric fibers without sacrificing bending peak load.

[0139] When introducing elements of the examples disclosed herein, the articles "a," "an," "the," and "said" are intended to indicate that there are one or more of the elements. The terms "comprising," "including," and "having" are intended to be open ended and mean that there may be additional elements in addition to the listed elements. Given the benefit of this disclosure, one of ordinary skill in the art will recognize that various components in an example may be interchanged or replaced by various components in other examples.

[0140] While certain aspects, examples, and embodiments have been described above, those skilled in the art, given the benefit of this disclosure, will appreciate that additions, substitutions, modifications, and variations of the illustrative aspects, examples, and embodiments disclosed are possible.

Claims

1. A molded porous composite article comprising a bulky core layer, the core layer comprising a porous web formed of inorganic reinforcing fibers, organic bicomponent fibers, a bulking agent comprising expandable microspheres, and a thermoplastic polyolefin material, wherein the porous web has a porosity of about 20% to about 80%, wherein the organic bicomponent fibers comprise a core-shell arrangement, wherein the melting point of the core material of the core-shell arrangement is at least fifteen degrees Celsius higher than the melting point of the shell material of the core-shell arrangement, wherein the shell of the organic bicomponent fibers comprises a polyolefin, the polyolefin being polyethylene or polypropylene, and wherein the molded porous composite article has a peak load of about 10 N to about 40 N in the longitudinal direction and a peak load of about 6 N to about 30 N in the transverse direction as tested by SAE J949-200904 under the condition that the molded porous composite article has a molded thickness of about 2 mm to about 4 mm in the longitudinal and transverse directions.

2. The molded porous composite article according to claim 1, wherein the core material of the core-shell arrangement comprises polyamide.

3. The molded cellular composite article of claim 1, wherein the core material of the core-shell arrangement comprises polyester.

4. The molded porous composite article according to claim 1, wherein the thermoplastic polyolefin material of the porous web comprises polypropylene, the inorganic reinforcing fibers comprise glass fibers, the core material of the core-shell arrangement comprises polyester or polyamide, the shell material of the core-shell arrangement comprises polyethylene, and wherein the molded porous composite article also has a flexural strength of about 6 MPa to about 17 MPa in the longitudinal direction and a flexural modulus of about 800 MPa to about 2000 MPa in the longitudinal direction and a flexural modulus of about 500 MPa to about 1300 MPa in the transverse direction as tested by SAE J949_200904.

5. The molded porous composite article according to claim 1, wherein the thermoplastic polyolefin material of the porous web comprises polypropylene, the inorganic reinforcing fibers comprise glass fibers, the core material of the core-shell arrangement comprises polyester or polyamide in the core, and the shell material of the core-shell arrangement comprises polyethylene, wherein the molded porous composite article also has a stiffness of about 10 N / cm to about 50 N / cm in the longitudinal direction and a stiffness of about 7 N / cm to about 30 N / cm in the transverse direction as tested by SAE J949_200904, a flexural strength of about 6 MPa to about 17 MPa in the longitudinal direction and a flexural strength of about 4 MPa to about 11 MPa in the transverse direction as tested by SAE J949_200904, and a flexural modulus of about 800 MPa to about 2000 MPa in the longitudinal direction and about 500 MPa to about 1300 MPa in the transverse direction as tested by SAE J949_200904.

6. The molded porous composite article of claim 3, wherein the polyester comprises polyethylene terephthalate.

7. A molded porous composite article according to claim 3, wherein the thermoplastic polyolefin material of the porous web is polypropylene, the inorganic reinforcing fibers are glass fibers, the shell material of the core-shell arrangement is linear low density polyethylene, and the polyester of the core material comprises polyethylene terephthalate.

8. The molded porous composite article of claim 2, wherein the thermoplastic polyolefin material of the porous web is polypropylene, the inorganic reinforcing fibers are glass fibers, and the shell material of the core-shell arrangement is linear low density polyethylene.

9. A molded porous composite article according to claim 1, wherein the thermoplastic polyolefin material of the porous web comprises polypropylene, the inorganic reinforcing fibers comprise glass fibers, the organic bicomponent fibers comprise polyester or polyamide in the core, the shell material of the core-shell arrangement is linear low density polyethylene, and wherein the melting point of the polyester or polyamide in the core material is at least twenty degrees Celsius higher than the melting point of the shell material.

10. The molded porous composite article of claim 9, wherein the molded porous composite article further has a stiffness of about 10 N / cm to about 50 N / cm in the longitudinal direction and a stiffness of about 7 N / cm to about 30 N / cm in the transverse direction as tested by SAE J949_200904.

11. The molded porous composite article of claim 9, wherein the molded porous composite article further has a flexural strength of about 6 MPa to about 17 MPa in the longitudinal direction and about 4 MPa to about 11 MPa in the transverse direction as tested by SAE J949_200904.

12. The molded porous composite article of claim 9, wherein the molded porous composite article further has a flexural modulus of about 800 MPa to about 2000 MPa in the machine direction and about 500 MPa to about 1300 MPa in the transverse direction as tested by SAE J949_200904.

13. The molded porous composite article according to claim 9, wherein the molded porous composite article also has a stiffness of about 10 N / cm to about 50 N / cm in the longitudinal direction and a stiffness of about 7 N / cm to about 30 N / cm in the transverse direction as tested by SAE J949_200904, and a flexural strength of about 6 MPa to about 17 MPa in the longitudinal direction and about 4 MPa to about 11 MPa in the transverse direction as tested by SAE J949_200904.

14. The molded porous composite article according to claim 9, wherein the molded porous composite article also has a stiffness of about 10 N / cm to about 50 N / cm in the longitudinal direction and a stiffness of about 7 N / cm to about 30 N / cm in the transverse direction as tested by SAE J949_200904, and a flexural modulus of about 800 MPa to about 2000 MPa in the longitudinal direction and about 500 MPa to about 1300 MPa in the transverse direction as tested by SAE J949_200904.

15. The molded porous composite article according to claim 9, wherein the molded porous composite article also has a flexural strength of about 6 MPa to about 17 MPa in the longitudinal direction and a flexural modulus of about 800 MPa to about 2000 MPa in the longitudinal direction and about 500 MPa to about 1300 MPa in the transverse direction as tested by SAE J949_200904.

16. The molded porous composite article according to claim 9, wherein the molded porous composite article also has a stiffness of about 10 N / cm to about 50 N / cm in the longitudinal direction and a stiffness of about 7 N / cm to about 30 N / cm in the transverse direction as tested by SAE J949_200904, a flexural strength of about 6 MPa to about 17 MPa in the longitudinal direction and a flexural strength of about 4 MPa to about 11 MPa in the transverse direction as tested by SAE J949_200904, and a flexural modulus of about 800 MPa to about 2000 MPa in the longitudinal direction and about 500 MPa to about 1300 MPa in the transverse direction as tested by SAE J949_200904.

17. The molded cellular composite article of any one of claims 1 to 16, wherein the article is configured as an automotive headliner.

18. The molded cellular composite article of any one of claims 1 to 16, wherein the article is configured as an automotive interior component.

19. The molded porous composite article of any one of claims 1 to 16, wherein the article is configured as a partition panel or a furniture panel.

Citation Information

Patent Citations

  • Twin-sheet thermoformed products

    US20050082881A1

  • Methods of forming a layered article

    US20050161865A1

  • Structurally reinforced resinous article and method of making

    US20050164023A1

  • Fiber reinforced thermoplastic sheets with surface coverings

    US20050215698A1

  • Decorative interior sound absorbing panel

    US20050217932A1