Polyolefin-based microporous film, laminate, and non-aqueous electrolyte secondary battery using the same

By optimizing the internal pore structure and fibril distribution of the polyolefin-based microporous membrane, the problem of insufficient strength and capacity maintenance in lithium-ion secondary batteries is solved, and the efficient performance of the lithium-ion secondary battery separator is achieved.

CN114128031BActive Publication Date: 2024-11-05TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080051979.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-07-25
Filing Date
2020-07-22
Publication Date
2024-11-05
Estimated Expiration
2040-07-22

AI Technical Summary

Technical Problem

The existing polyolefin-based microporous membranes have problems inadequately taking into account both the strength and the capacity maintenance rate under rapid charging and discharge conditions in lithium-ion secondary batteries, especially the lack of optimization in the internal structure in the thickness direction and the overall impedance of the coating.

Method used

By adjusting the internal pore structure of the polyolefin-based microporous membrane, the number of pores in the thickness direction is 35 or more, the peak of tortuosity distribution is 1.30 or more and 1.80 or less, and the number of fibrils is 870 or more/μm3 or more/2800 or more/ μm3 or less, and the three-dimensional image parameters are optimized in FIB-SEM measurement to improve the compression resistance and charging impedance of the film.

Benefits of technology

The excellent strength of the lithium-ion secondary battery separator and the improved capacity maintenance rate under rapid charging and discharge conditions are achieved, ensuring the efficient performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003475264800000301
    Figure BDA0003475264800000301
  • Figure BDA0003475264800000311
    Figure BDA0003475264800000311
  • Figure BDA0003475264800000321
    Figure BDA0003475264800000321
Patent Text Reader

Abstract

This invention relates to a polyolefin-based microporous membrane. In a 2.7 μm × 2.7 μm three-dimensional image fabricated from cross-sectional images of the microporous membrane obtained by FIB-SEM measurements, the number of pores in the thickness direction is 35 pores / μm. 2 The peak value of the tortuosity distribution of the pores in the thickness direction is above 1.30 and below 1.80.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polyolefin-based microporous film, a laminate, and a nonaqueous electrolyte secondary battery using the same. Background Art

[0002] Thermoplastic resin microporous membranes are widely used as separation membranes, selective permeation membranes, and separators for objects. Specific uses of microporous membranes include separators for non-aqueous electrolyte secondary batteries such as lithium-ion secondary batteries, nickel-hydrogen batteries, nickel-cadmium batteries, and polymer batteries, separators for double-layer capacitors, various filters such as reverse osmosis filtration membranes, ultrafiltration membranes, and microfiltration membranes; waterproof and breathable clothing, medical materials, and fuel cell supports.

[0003] In particular, polyethylene microporous membranes are widely used as separators for lithium-ion secondary batteries. In addition to excellent mechanical strength that greatly contributes to the safety and productivity of the battery, the following features can also be listed: ensuring electrical insulation while having ion permeability that allows electrolyte to penetrate into the micropores, and automatically blocking ion permeation at around 120-150°C in the event of abnormal reactions outside / inside the battery, thereby having a pore blocking function that suppresses excessive temperature rise.

[0004] In addition, the use of lithium-ion secondary batteries in automobiles and household appliances has been expanded, and from the perspective of convenience, the demand for rapid charging and discharging in various applications has continued to increase. If a lithium-ion secondary battery is rapidly charged and discharged, the following issues will arise: the components such as electrodes and separators that constitute the lithium-ion secondary battery, and the impedance at the interface between the components will generate heat, and the thermal degradation of the battery components will be promoted. In addition, when a lithium-ion secondary battery is rapidly charged and discharged, since the charge and discharge time becomes shorter, there are the following problems: the time for lithium ions to penetrate into the fine parts of the electrode is reduced, the number of lithium ions that are effectively entered and exited is reduced, and the battery capacity will be reduced.

[0005] As a combination of separators for improving the long-term reliability of lithium-ion secondary batteries, a technology for improving the long-term compression resistance of a micro-region of a membrane has been proposed (Patent Document 1). In addition, a technology for improving the battery capacity (rate characteristics) under rapid charge and discharge conditions through specific stretching conditions has been proposed (Patent Document 2), and a technology for reducing the charging impedance by setting the parameters obtained by FIB-SEM image analysis of a coating on a polyolefin-based microporous membrane to a specific range has been proposed (Patent Document 3).

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Publication No. 2009-242631

[0009] Patent Document 2: Japanese Patent Application Publication No. 2016-121327

[0010] Patent Document 3: Japanese Patent Application Publication No. 2018-181649 Summary of the invention

[0011] Problems to be solved by the invention

[0012] Although Patent Documents 1 and 2 propose that: by adjusting the raw material composition and manufacturing conditions, the puncture strength, porosity, thermal shrinkage, film thickness retention rate due to puncture creep, etc. are adjusted, and the long-term reliability when applied to the separator of lithium-ion secondary batteries is improved, but the internal structure in the thickness direction of the microporous membrane is not fully considered, and there is insufficient balance between strength and capacity retention rate under rapid charge and discharge conditions. In addition, although Patent Document 3 proposes to reduce the charging impedance by making the fractal dimension of the insulating porous layer obtained by coating a specific range, the structure of the microporous membrane itself as the coated substrate and the internal structure in the thickness direction of the microporous membrane are not fully considered. When paying attention to the impedance in the substrate and the coating as a whole, there is insufficient balance between strength and capacity retention rate under rapid charge and discharge conditions.

[0013] Therefore, the purpose of the present invention is to overcome the above-mentioned defects and make the internal pore structure of the polyolefin-based microporous membrane within a specific range, thereby providing a polyolefin-based microporous membrane that has excellent strength when used as a separator for non-aqueous electrolyte secondary batteries represented by lithium-ion secondary batteries and can improve the capacity retention rate under rapid charge and discharge conditions.

[0014] Means for solving problems

[0015] The present invention for solving the above-mentioned problems has the following configurations.

[0016] (1) A polyolefin-based microporous membrane, wherein the number of pores in the thickness direction is 35 / μm in a 2.7 μm×2.7 μm×2.7 μm three-dimensional image prepared from each cross-sectional image obtained by FIB-SEM measurement of the microporous membrane 2 As described above, the peak value of the tortuosity distribution of the cell in the thickness direction is 1.30 or more and 1.80 or less.

[0017] (2) The polyolefin-based microporous membrane according to (1), wherein the frequency of the peak value of the tortuosity distribution of the pores in the thickness direction is 6% to 30%.

[0018] (3) The polyolefin-based microporous membrane according to (1) or (2), wherein the half value width of the tortuosity distribution of the pores in the thickness direction is 0.06 or more and 0.25 or less.

[0019] (4) The polyolefin-based microporous membrane according to any one of (1) to (3), wherein the number of fibrils in a 2.7 μm×2.7 μm×2.7 μm three-dimensional image prepared from each cross-sectional image obtained by FIB-SEM measurement of the microporous membrane is 870 fibers / μm 3 Above 2800 / μm 3 the following.

[0020] (5) A polyolefin-based microporous membrane, wherein the number of fibrils in a 2.7 μm×2.7 μm×2.7 μm three-dimensional image prepared from each cross-sectional image obtained by FIB-SEM measurement of the microporous membrane is 870 fibers / μm 3 Above 2800 / μm 3 the following.

[0021] (6) The polyolefin-based microporous membrane according to any one of (1) to (5), wherein the average fibril diameter is 25 nm to 60 nm.

[0022] (7) The polyolefin-based microporous membrane according to any one of (1) to (6), wherein the number of fibril intersections is 1350 / μm 3 Above 4400 / μm 3 the following.

[0023] (8) The polyolefin-based microporous membrane according to any one of (1) to (7), wherein the puncture strength is 180 gf or more and 700 gf or less.

[0024] (9) The polyolefin-based microporous membrane according to any one of (1) to (8), wherein the polyolefin-based microporous membrane has a thickness of 3 μm to 14 μm.

[0025] (10) The polyolefin-based microporous membrane according to any one of (1) to (9), wherein the porosity is 35% to 50%.

[0026] (11) The polyolefin-based microporous membrane according to any one of (1) to (10), wherein the maximum shrinkage stress temperature in the TD direction obtained by a thermomechanical analyzer (TMA) is 143° C. or higher, and the maximum shrinkage stress is 1.3 MPa or lower.

[0027] (12) A laminate obtained by further laminating a heat-resistant resin layer on the polyolefin microporous film according to any one of (1) to (11).

[0028] (13) A nonaqueous electrolyte secondary battery comprising the polyolefin microporous membrane according to any one of (1) to (11) or the laminate according to (12).

[0029] Effects of the Invention

[0030] The polyolefin-based microporous membrane according to the embodiment of the present invention, when used as a separator for non-aqueous electrolyte secondary batteries represented by lithium ion secondary batteries, exhibits the effects of excellent strength and improved capacity retention rate under rapid charge and discharge conditions. DETAILED DESCRIPTION

[0031] Hereinafter, the polyolefin-based microporous membrane according to the embodiment of the present invention will be described in detail. In the present specification, when a numerical range is described as "A to B", it means a range of not less than A and not more than B.

[0032] It is important that the polyolefin-based microporous membrane according to the embodiment of the present invention has a thickness direction of 35 cells / μm in a 2.7 μm×2.7 μm×2.7 μm three-dimensional image prepared from each cross-sectional image of the microporous membrane measured by FIB-SEM. 2 As described above, the peak value of the tortuosity distribution of the cell in the thickness direction is 1.30 or more and 1.80 or less.

[0033] The number of pores in the thickness direction and the peak value of the tortuosity distribution of the pores in the thickness direction can each be used as one of the indices representing the internal pore structure of the polyolefin-based microporous membrane.

[0034] The polyolefin-based microporous membrane in the embodiment of the present invention is mainly composed of a polyolefin-based resin. Here, the main component refers to a polyolefin-based resin containing more than 50% by mass and less than 100% by mass when the total mass of the polyolefin-based microporous membrane is 100% by mass. Here, as the polyolefin-based resin in the embodiment of the present invention, various polyethylene-based resins, various polypropylene-based resins, etc. can be cited, and the polyethylene-based resin in the embodiment of the present invention refers to a polymer having a total amount of more than 50% by mass and less than 100% by mass when the total mass of the polymer of the polyethylene-based resin is 100% by mass.

[0035] In this specification, the polyolefin-based microporous membrane is sometimes referred to as a “microporous membrane.” In addition, the polypropylene-based resin in the embodiment of the present invention refers to a polymer in which the total amount of propylene components exceeds 50% by mass and is less than 100% by mass when the total mass of the polymer of the polypropylene-based resin is 100% by mass.

[0036] Examples of the polyethylene resin in the embodiment of the present invention include homopolymers consisting only of ethylene, or copolymers obtained by copolymerizing chain olefins (α-olefins) such as propylene, 1-butene, 1-pentene, 1-hexene, 3-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene.

[0037] Examples of the polypropylene resin in the embodiment of the present invention include homopolymers consisting of propylene alone, various polypropylene resins such as ethylene-propylene copolymers, ethylene-propylene-butene copolymers, and propylene-butene copolymers.

[0038] The polyolefin-based resin in the embodiment of the present invention may be a single substance or a mixture of two or more different polyolefin-based resins.

[0039] Among these various polyolefin resins, polyethylene resins are particularly preferred from the viewpoint of excellent pore blocking performance. From the viewpoint of the pore blocking performance of the microporous membrane, the melting point (softening temperature) of the polyethylene resin is preferably 70 to 150°C.

[0040] The following is a detailed description of the polyolefin resin used in the embodiment of the present invention, taking polyethylene resin as an example. The types of polyethylene resin used in the embodiment of the present invention include polyethylene resins having a density of more than 0.94 g / cm 3 Such high-density polyethylene has a density of 0.93 to 0.94 g / cm 3 Medium density polyethylene in the range of 0.93 g / cm 3 However, from the viewpoint of controlling the internal pore structure of the polyolefin-based microporous membrane to be described later to be within the desired range, when the total mass of the polyolefin-based microporous membrane is 100 mass %, it is preferred that the composition contains 80 mass % or more of ultra-high molecular weight polyethylene.

[0041] The ultra-high molecular weight polyethylene used in the embodiment of the present invention preferably has a weight average molecular weight of 1.0×10 6 Above 1.0×10 7 If the weight average molecular weight is 1.0×10 6The above values ​​can prevent the relaxation time from being too short, suppress the increase of the stretching temperature and the heat treatment temperature, and prevent the fine fibrils from melting and the number of pores in the microporous membrane from decreasing. 6 The above ultra-high molecular weight polyethylene has increased molecular chain entanglement, and since the polyethylene resin layer is uniformly loaded with stress during the stretching process, various structures in the thickness direction described later can be controlled within a desired range. Therefore, the weight average molecular weight of the ultra-high molecular weight polyethylene is preferably 1.0×10 6 More preferably, 1.5×10 6 More preferably, 2.0×10 6 More than, most preferably 3.0×10 6 In addition, the upper limit of the weight average molecular weight is preferably 8.0×10 6 Below, more preferably 6.0×10 6 Below, more preferably 5.0×10 6 Below, the most preferred is 4.0×10 6 the following.

[0042] The molecular weight distribution (weight average molecular weight (Mw) / number average molecular weight (Mn)) of the ultra-high molecular weight polyethylene is preferably in the range of 3.0 to 100. The narrower the molecular weight distribution, the more uniform the system, and the easier it is to obtain uniform micropores, so it is preferred that the molecular weight distribution is as narrow as possible, but the narrower the distribution, the lower the molding processability. Therefore, the lower limit of the molecular weight distribution is preferably above 4.0, more preferably above 5.0, and further preferably above 6.0. Since the low molecular weight component increases if the molecular weight distribution increases, it is easy to cause a decrease in strength or the melting and hot bonding of fine fibrils during stretching and heat setting, so the upper limit is preferably below 80, more preferably below 50, further preferably below 20, and most preferably below 10. By being in the above range, good molding processability is obtained, and because the system is unified, uniform micropores are obtained.

[0043] The high-density polyethylene used in the embodiment of the present invention preferably has a weight average molecular weight (Mw) of 1.0×10 4 Above 1.0×10 6 Below, more preferably 1.0×10 5 Above 1.0×10 6 Below, particularly preferably 5.0×10 5 Above 9.0×10 5 By using a high-density polyethylene having a weight average molecular weight within the above range for the polyolefin-based microporous membrane according to the embodiment of the present invention, the pressure change of the resin in the extruder is unlikely to occur, and good quality may be obtained.

[0044] In addition, the polyolefin-based microporous membrane according to the embodiment of the present invention may contain various additives such as antioxidants, heat stabilizers, antistatic agents, ultraviolet light absorbers, anti-adhesive agents, and fillers, within the range that does not impair the effects of the present invention. In particular, an antioxidant is preferably added to inhibit oxidative degradation caused by thermal history of the polyolefin-based resin.

[0045] As the antioxidant, for example, it is preferred to use one or more selected from 2,6-di-tert-butyl-p-cresol (BHT: molecular weight 220.4), 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, tetrakis[methylene-3(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]methane, and the like.

[0046] The FIB-SEM determination in the embodiment of the present invention refers to the operation (FIB cutting) of cutting the cross section of the microporous film at a certain interval by repeatedly performing the operation of SEM (scanning electron microscope) image shooting of the surface after cutting with a focused ion beam (FIB), so as to measure the method of the continuous image at a certain interval in the depth direction. As a method for making a sample for FIB-SEM determination, it can be listed that the resin implemented with electronic dyeing is impregnated in the microporous film involved in the embodiment of the present invention, after the embedding treatment of the pore portion, the method of using a slicer to make a slice of the film cross section in the manner of the initial observation surface after the embedding treatment, etc. In addition, as a determination method of FIB-SEM, it can be listed that the sample (slice of the film cross section) made in the determination is cut at every interval of 10nm in the depth direction, and the method of sequentially shooting the SEM image of the depth direction, etc. It is explained that as a method for determining the position information of each SEM image, a part of the observation screen of the microporous membrane subjected to FIB cutting is marked with a metal component in advance, and the marked position is used as a basis to determine the correlation between the positions of each image. The image area is preferably about 3 μm square to 10 μm square, and when the observation surface is tilted, the scale can be converted taking into account the tilt.

[0047] In addition, as a method for producing a three-dimensional image from each cross-sectional image, for example, there can be listed a method in which, using image processing software such as "ExFact (registered trademark) Analysis for Porous / Particles" manufactured by Business Science Co., Ltd. of Japan, the portion of the resin in the microporous membrane that has been embedded and electron-stained (i.e., the portion corresponding to the pore portion of the microporous membrane) and the portion of the resin constituting the microporous membrane are binarized, and then three-dimensional stereoscopic imaging is performed based on the information from the binarization process, and the pore portion of the microporous membrane is thinned using image processing software such as "ExFact (registered trademark) Analysis for Porous / Particles" manufactured by Business Science Co., Ltd. of Japan, thereby producing a three-dimensional image of the pore portion inside the microporous membrane, etc. The size of the three-dimensional image to be created is set to be a cube surrounded by sides with a length of 2.7 μm from the viewpoint of analysis time and reproducibility of analysis parameters.

[0048] The number of channels in the thickness direction of the present application refers to the number of channels with the shortest distance among all the paths (channels) formed by the pores of the microporous membrane from the starting surface to the end surface in the thickness direction in the cube of the three-dimensional image surrounded by the side of 2.7 μm length produced by the above method, and is detected as one. The number of channels in the thickness direction of all the channels from the starting surface of the 2.7 μm×2.7 μm area to the end surface of the 2.7 μm×2.7 μm area in the cube of the three-dimensional image is counted and converted into per 1 μm 2 The obtained value is taken as the number of channels in the thickness direction in the embodiment of the present invention (channels / μm 2 ).

[0049] In the polyolefin-based microporous membrane according to the embodiment of the present invention, in a 2.7 μm×2.7 μm×2.7 μm three-dimensional image prepared from each cross-sectional image obtained by FIB-SEM measurement of the microporous membrane, the number of pores in the thickness direction is set to 35 / μm. 2 As described above, when used as a separator for a lithium-ion secondary battery, the paths for lithium ions to move are increased, and lithium ions can move smoothly, so the resistance of the separator can be reduced, and the capacity retention rate of the battery during rapid charge and discharge can be improved. From the perspective of reducing resistance and improving the capacity retention rate during rapid charge and discharge, the number of channels in the thickness direction is preferably 40 / μm 2 More preferably, 55 / μm 2 More preferably, 65 strands / μm 2 More than 80 / μm is particularly preferred 2In addition, from the viewpoint of reducing resistance, the more pores there are in the thickness direction of the microporous membrane in the three-dimensional image of 2.7 μm×2.7 μm×2.7 μm produced from each cross-sectional image obtained by FIB-SEM measurement, the more preferably the more pores there are, but from the viewpoint of maintaining operability during processing, the number of pores in the thickness direction is preferably 250 pores / μm. 2 Below, more preferably 200 strands / μm 2 the following.

[0050] The polyolefin-based microporous membrane involved in the embodiment of the present invention is important that in the three-dimensional image of 2.7 μm × 2.7 μm × 2.7 μm produced from each cross-sectional image obtained by FIB-SEM measurement of the microporous membrane, the peak value of the tortuosity distribution of the pores in the thickness direction is 1.30 or more and 1.80 or less. Here, the peak value of the tortuosity distribution of the pores in the thickness direction refers to the use of "ExFact (registered trademark) Analysis for Porous / Particles" and other image processing software to calculate the respective tortuosity for each pore in the thickness direction obtained by the above method, and the frequency distribution of tortuosity is made for all pores in the thickness direction of the analysis object, and the tortuosity with the highest frequency is shown in the figure of the tortuosity frequency distribution after smoothing. It should be noted that in the peak value of tortuosity, the larger the value, the more tortuosity the pores in the thickness direction of the microporous membrane are tortuous, and the smaller the value, the more the pores in the thickness direction of the microporous membrane have a path close to a straight line. In the present application, when two or more peaks of the tortuosity of the pores in the thickness direction are observed, the peak with the highest frequency is adopted, and when two or more peaks with the same frequency are observed, the peak with the lowest tortuosity is adopted.

[0051] The polyolefin-based microporous membrane according to the embodiment of the present invention is a three-dimensional image of 2.7 μm × 2.7 μm × 2.7 μm prepared from each cross-sectional image obtained by FIB-SEM measurement of the microporous membrane. By making the peak value of the tortuosity distribution of the pores in the thickness direction 1.30 or more and 1.80 or less, the path of lithium ion movement becomes close to a straight line when used as a separator of a lithium ion secondary battery. Since lithium ions can move smoothly, the resistance of the separator can be reduced, and the capacity retention rate of the battery during rapid charge and discharge can be improved. From the perspective of reducing resistance and improving the capacity retention rate during rapid charge and discharge, the peak value of the tortuosity distribution of the pores in the thickness direction is preferably 1.75 or less, more preferably 1.70 or less, further preferably 1.65 or less, and particularly preferably 1.60 or less. In addition, from the viewpoint of reducing resistance, the lower the peak value of the tortuosity distribution of the pores in the thickness direction in the three-dimensional image of 2.7μm×2.7μm×2.7μm made from each cross-sectional image obtained by FIB-SEM measurement, the better. However, if the peak value of the tortuosity distribution is too low, dendritic lithium metallic precipitates called dendrites are easily generated on the electrode surface when used as a separator for a lithium ion battery. Since this can easily cause a short circuit between the positive and negative electrodes, the peak value of the tortuosity distribution is preferably above 1.30.

[0052] In the embodiment of the present invention, in a 2.7 μm×2.7 μm×2.7 μm three-dimensional image prepared from each cross-sectional image obtained by FIB-SEM measurement of the microporous membrane, the number of pores in the thickness direction is set to 35 / μm. 2 The method of the present invention is as follows: 80% or more of the constituent resin of the polyolefin-based microporous membrane is ultra-high molecular weight polyethylene, and the surface ratio of wet stretching is 60 times or more, and the resin concentration during manufacturing is lower than 30% by mass. In the embodiment of the present invention, it is found that by making 80% or more of the constituent resin of the polyolefin-based microporous membrane ultra-high molecular weight polyethylene, and the resin concentration during manufacturing is lower than 30% by mass, the spherulite growth of polyethylene in the cast sheet before stretching can be suppressed, and the cast sheet structure can be made uniform. Furthermore, by combining with wet stretching with a wet surface ratio of 60 times or more, the site of insufficient pore opening is greatly reduced, and uniform pore opening of the polyolefin-based microporous membrane becomes possible. In addition, by utilizing the uniform pore opening of the polyolefin-based microporous membrane, the number of pores in the thickness direction can be increased by reducing the number of insufficiently opened pores. By reducing the number of insufficiently opened pores, the tortuosity of the pores in the thickness direction can be suppressed, and the peak value of the tortuosity distribution can be controlled to a low specific range.

[0053] The polyolefin-based microporous membrane involved in the embodiment of the present invention is preferably 6% or more and 30% or less in frequency of the peak value of the tortuosity distribution of the pores in the thickness direction from the viewpoint of reducing resistance when used as a separator of a lithium-ion secondary battery and improving the capacity retention rate during rapid charge and discharge. Here, the frequency of the peak value of the tortuosity distribution represents the value of the frequency in the peak value of the aforementioned tortuosity frequency distribution, and the larger the value, the greater the proportion of the pores representing the peak value of the tortuosity, that is, the more uniform the tortuosity of each pore in the thickness direction.

[0054] The frequency of the peak value of the tortuosity distribution of the channels in the thickness direction in the embodiment of the present invention is more preferably 7% or more, more preferably 9% or more, and particularly preferably 12% or more from the viewpoint of further improving the effect of reducing resistance and improving the capacity retention rate during rapid charge and discharge. On the other hand, from the viewpoint of improving mechanical properties such as strength, the frequency of the peak value of the tortuosity distribution of the channels in the thickness direction is preferably 30% or less.

[0055] In an embodiment of the present invention, as a method for making the frequency of the peak value of the tortuosity distribution of the channels in the thickness direction greater than 6% and less than 30%, there can be listed a method of making the wet stretching speed within a specific low range to make the openness during stretching uniform; and a method of applying multi-stage stretching of more than two stages to slowly open the holes, thereby increasing the number of channels with the same tortuosity, etc.

[0056] The polyolefin-based microporous membrane involved in the embodiment of the present invention is preferably 0.06 or more and 0.25 or less in half width of the tortuosity distribution of the pores in the thickness direction from the viewpoint of reducing resistance when used as a separator of a lithium-ion secondary battery and improving the capacity retention rate during rapid charge and discharge. Here, the half-value width of the tortuosity distribution represents the arithmetic half-value full width of the graph of the tortuosity frequency distribution described above, and the smaller the value, the sharper the distribution of the tortuosity, and the more uniform the tortuosity of each pore in the thickness direction.

[0057] In the embodiment of the present invention, the half-value width of the tortuosity distribution of the channels in the thickness direction is more preferably 0.20 or less, more preferably 0.15 or less, and particularly preferably 0.11 or less from the viewpoint of further improving the effect of reducing resistance and improving the capacity retention rate during rapid charge and discharge. On the other hand, from the viewpoint of improving mechanical properties such as strength, the half-value width of the tortuosity distribution of the channels in the thickness direction is more preferably 0.06 or more, and more preferably 0.07 or more.

[0058] In an embodiment of the present invention, as a method for making the half-value width of the tortuosity distribution of the channels in the thickness direction greater than or equal to 0.06 and less than or equal to 0.25, there can be listed a method of greatly setting the relaxation ratio (relaxation rate) in the heat treatment process after wet stretching, performing shrinkage in the surface direction to make the channel path in the thickness direction uniform along the straight line direction, etc.

[0059] The polyolefin-based microporous membrane according to the embodiment of the present invention preferably has a fibril number of 870 fibers / μm in a 2.7 μm×2.7 μm×2.7 μm three-dimensional image prepared from each cross-sectional image of the microporous membrane measured by FIB-SEM. 3 Above 2800 / μm 3 the following.

[0060] As a method for producing a three-dimensional image from each cross-sectional image obtained by FIB-SEM measurement in order to determine the number of fibrils, for example, a method of using image processing software such as "ExFact (registered trademark) Analysis for Fiber" manufactured by Business Science Co., Ltd. of Japan to binarize the portion of the resin embedded and electron-stained and observed as a bright portion in the polyolefin-based microporous membrane (i.e., the portion corresponding to the pore portion of the microporous membrane) and the portion of the resin constituting the polyolefin-based microporous membrane (constituent resin portion), and then using the binarized information as a basis to produce a three-dimensional stereoscopic image, and using image processing software such as "ExFact (registered trademark) Analysis for Fiber" manufactured by Business Science Co., Ltd. of Japan to perform a line thinning process on the resin portion constituting the polyolefin-based microporous membrane, thereby producing a three-dimensional image of the constituent resin portion inside the polyolefin-based microporous membrane, etc. The size of the three-dimensional image to be created is set to be a cube surrounded by sides with a length of 2.7 μm from the viewpoint of analysis time and reproducibility of analysis parameters.

[0061] The number of fibrils in the present invention is as follows: For the constituent resin portion obtained from the three-dimensional image, the image processing software such as "ExFact (registered trademark) Fiber Analysis (Analysis for Fiber)" manufactured by Japan Business Science Co., Ltd. is used to divide the thinned lines of the constituent resin portion at the intersection and branching parts, and the number of thin lines obtained thereby is calculated, and then converted into per 1 μm 3 The value obtained by the number of roots.

[0062] The polyolefin-based microporous membrane according to the embodiment of the present invention has cracks in the higher-order structure during the stretching step of the production method example described below. In the present invention, the number of fibrils is 870 / μm. 3The above indicates that the number of fibrous resin portions after cleavage is sufficiently large and that pores in the polyolefin-based microporous membrane are sufficiently formed, so that lithium ions can smoothly move when used as a separator for a lithium ion secondary battery.

[0063] The polyolefin-based microporous membrane according to the embodiment of the present invention is characterized in that the number of fibrils in a 2.7 μm×2.7 μm×2.7 μm three-dimensional image prepared from each cross-sectional image obtained by FIB-SEM measurement of the microporous membrane is 870 / μm. 3 As a result, the resistance of the separator can be reduced, and the thermal degradation of the battery can be suppressed or the capacity retention rate during rapid charge and discharge can be improved. From the perspective of reducing the resistance, suppressing the thermal degradation and improving the capacity retention rate during rapid charge and discharge, the number of fibrils is preferably 1000 / μm. 3 More preferably, 1250 strands / μm 3 More than 1400 strands / μm is particularly preferred 3 On the other hand, if the number of fibrils is too large, the number of channels through which lithium ions pass may decrease, and the impedance may increase. Therefore, 2800 fibrils / μm is preferred. 3 the following.

[0064] In the present invention, a 2.7 μm×2.7 μm×2.7 μm three-dimensional image prepared from each cross-sectional image obtained by FIB-SEM measurement of the microporous membrane was used as the number of fibrils to be 870 / μm. 3 ~2800 / μm 3 The method can include making more than 80% by mass of the resin constituting the polyolefin-based microporous membrane an ultra-high molecular weight polyethylene, and the surface ratio of the wet stretching is more than 60 times, thereby making the resin concentration during manufacturing less than 30% by mass. In the embodiment of the present invention, it is found that by making more than 80% by mass of the resin constituting the polyolefin-based microporous membrane an ultra-high molecular weight polyethylene, the spherulite growth of polyethylene in the cast sheet before stretching can be suppressed, and the cast sheet structure can be made uniform. In addition, by combining with a wet stretching with a wet surface ratio of more than 60 times, the part where the pores are not formed sufficiently can be greatly reduced, and the pores of the polyolefin-based microporous membrane can be uniformly formed. In addition, by uniformly forming the pores of the polyolefin-based microporous membrane, the part where the pores are not formed sufficiently can be reduced, thereby increasing the number of fibrils.

[0065] The polyolefin-based microporous membrane involved in the embodiment of the present invention is preferably analyzed from the viewpoint of reducing the resistance inside the battery when used as a separator of a lithium-ion secondary battery and improving the capacity retention rate during rapid charge and discharge. The average diameter of the fibrils obtained by analyzing the three-dimensional image of 2.7 μm × 2.7 μm × 2.7 μm made from each cross-sectional image obtained by FIB-SEM is 25 nm or more and 60 nm or less. Here, the average diameter of the fibrils refers to the average value of the diameters of all fibrils contained in the three-dimensional image of 2.7 μm × 2.7 μm × 2.7 μm obtained by image processing software such as "ExFact (registered trademark) Analysis for Fiber" made by Japan Business Science Co., Ltd. in the same way as the evaluation method of the number of fibrils. By making the fibril diameter a specific range, lithium ions can move smoothly when used as a separator of a lithium-ion secondary battery.

[0066] The average diameter of the fibrils in the embodiment of the present invention is more preferably 55 nm or less, more preferably 45 nm or less, and particularly preferably 35 nm or less from the viewpoint of further improving the effect of reducing resistance and improving the capacity retention rate during rapid charge and discharge. On the other hand, from the viewpoint of making mechanical properties such as strength good, the average diameter of the fibrils is preferably 25 nm or more.

[0067] In an embodiment of the present invention, as a method for making the average diameter of the fibrils greater than 25 nm and less than 60 nm, there are listed a method of making the wet stretching speed within a specific low range to make the formation of the pore portion during stretching uniform, and a method of applying multi-stage stretching of more than two stages to gradually form the pore portion.

[0068] The polyolefin-based microporous membrane according to the embodiment of the present invention preferably has a fibril cross number of 1350 / μm from the viewpoint of reducing resistance when used as a separator of a lithium ion secondary battery and improving the capacity retention rate during rapid charge and discharge. 3 More than 4400 / μm 3 Here, the fibril crossing number is as follows: In the same way as the evaluation method for the fibril root number, when the lines of the constituent resin part of the microporous membrane are segmented using image processing software such as "ExFact (registered trademark) Analysis for Fiber" manufactured by Japan Business Science Co., Ltd., the number of locations where the constituent resin parts cross each other is calculated, that is, in a three-dimensional image of 2.7μm×2.7μm×2.7μm, the number of crossing locations is calculated, and then converted into per 1μm 3 The value obtained by the number of .

[0069] In the embodiment of the present invention, a large number of fibril intersections indicates that a fine network structure is formed in the microporous membrane, and that pores in the polyolefin microporous membrane are sufficiently formed, and lithium ions can smoothly move when used as a separator for a lithium ion secondary battery.

[0070] The number of fibril intersections in the embodiment of the present invention is more preferably 1700 / μm from the viewpoint of further improving the effect of reducing resistance and improving the capacity retention rate during rapid charge and discharge. 3 More preferably, 2200 pieces / μm 3 More than 3000 pieces / μm is particularly preferred 3 On the other hand, from the viewpoint of improving mechanical properties such as strength, the number of fibril intersections is more preferably 4200 / μm. 3 the following.

[0071] In the embodiment of the present invention, the number of fibril intersections is 1350 / μm. 3 More than 4400 / μm 3 The following method includes the following method, etc., in which the relaxation rate in the heat treatment step after wet stretching is set to a large value to shrink in the plane direction and make the pore path in the thickness direction uniform in the linear direction.

[0072] The polyolefin-based microporous membrane involved in the embodiment of the present invention, from the perspective of the safety of the lithium-ion secondary battery, preferably has a maximum shrinkage stress temperature of 143°C or more in the TD direction measured by a thermomechanical analyzer (TMA) and a maximum shrinkage stress of 1.3MPa or less. When the lithium-ion secondary battery is in a high temperature state by rapid charge and discharge, the shrinkage stress of the polyolefin-based microporous membrane contained in the lithium-ion secondary battery becomes larger, especially easily causing deformation in the unwound TD direction. Because the insulation in the lithium-ion secondary battery is sometimes insufficient due to the deformation of the polyolefin-based microporous membrane in the TD direction, the lithium-ion battery becomes a cause of thermal runaway and fire, so from the perspective of improving the safety of the lithium-ion secondary battery, in the embodiment of the present invention, it is preferred that the maximum shrinkage stress temperature in the TD direction measured by a thermomechanical analyzer (TMA) is higher and the maximum shrinkage stress is lower. Among them, from the perspective of the balance between the pore structure, fibril structure, strength, etc. of the polyolefin-based microporous membrane, the maximum shrinkage stress temperature in the TD direction measured by a thermomechanical analyzer (TMA) is preferably below 150°C, and the maximum shrinkage stress is preferably above 0.6 MPa.

[0073] In an embodiment of the present invention, as a method for achieving a maximum shrinkage stress temperature of 143°C or higher and a maximum shrinkage stress of 1.3 MPa or lower in the TD direction as measured by a thermomechanical analyzer (TMA), there can be cited a method of strengthening the deformation relaxation of a polyolefin-based microporous membrane by setting a heat setting temperature of 130°C or higher and a relaxation rate of 15% or higher in a structure having ultra-high molecular weight polyethylene as a main component.

[0074] The polyolefin-based microporous membrane involved in the embodiment of the present invention is preferably 180 gf or more and 700 gf or less from the viewpoint of improving the impact resistance of the battery when used as a separator of a lithium ion secondary battery. From the viewpoint of further improving the impact resistance of the battery when used as a separator of a lithium ion secondary battery, the puncture strength is more preferably 250 gf or more, more preferably 350 gf or more, and particularly preferably 500 gf or more. In addition, from the viewpoint of the impact resistance of the battery, the higher the strength of the polyolefin-based microporous membrane, the more preferred, but from the viewpoint of making the balance with other physical properties such as thermal shrinkage a good one, it is preferably 700 gf or less. It should be noted that the puncture strength in the embodiment of the present invention is the puncture strength when the thickness is converted to 10 μm.

[0075] In an embodiment of the present invention, as a method for achieving a puncture strength of a polyolefin-based microporous membrane of 180 gf to 700 gf, there can be cited a method in which 70% by mass or more of the constituent resin of the polyolefin-based microporous membrane is ultra-high molecular weight polyethylene, the surface ratio of wet stretching is set to 60 times or more, and the porosity of the polyolefin-based microporous membrane is set to 35% to 55%.

[0076] The thickness of the polyolefin-based microporous membrane involved in the embodiment of the present invention is 3 μm or more and 14 μm or less. Since it can reduce the distance between electrodes and increase the number of battery component stacking when used as a separator of a lithium-ion battery, it is preferred from the perspective of high capacity of the battery. As a method of setting the thickness to 3 μm or more and 14 μm or less, a method of using a wet stretching method and increasing the stretching ratio and the line speed during manufacturing can be used. From the perspective of making the battery high capacity, the thickness of the polyolefin-based microporous membrane is more preferably 12 μm or less, further preferably 10 μm or less, and particularly preferably 7 μm or less.

[0077] The polyolefin-based microporous membrane according to the embodiment of the present invention preferably has a porosity of 35% to 50% from the viewpoint of making various structures of pores in the thickness direction within a specific range or making the puncture strength and safety when used as a separator of a lithium ion secondary battery good.

[0078] In the embodiment of the present invention, examples of methods for adjusting the porosity to 35% or more and 50% or less include methods of adjusting various production conditions such as stretching ratio, stretching temperature, heat treatment temperature, and heat treatment time.

[0079] The polyolefin-based microporous membrane according to the embodiment of the present invention may be formed into a laminate further including a heat-resistant resin layer from the viewpoint of improving heat resistance when mounted in a lithium ion battery.

[0080] As the heat-resistant resin layer, it is preferred to use various fluorine-based resins, acrylic resins, aromatic polyamide resins, etc., which are insoluble in the electrolyte of the battery and electrically stable within the range of battery use conditions. In addition, from the viewpoint of further improving heat resistance, the heat-resistant resin layer may also contain organic powders, inorganic powders, or a mixture of these as fillers. For example, as organic powders, fluorine-based resins, melamine-based resins, aromatic polyamide-based resins, etc. can be used, and as inorganic powders, metal oxides, metal nitrides, metal carbides, metal hydroxides, carbonates, sulfates, etc. can be used. More specifically, aluminum oxide, silicon dioxide, titanium dioxide, aluminum hydroxide, calcium carbonate, etc. can be used.

[0081] Next, an example of a method for producing a polyolefin-based microporous membrane according to an embodiment of the present invention will be described below, but the present invention is not limitedly interpreted by the example.

[0082] The method for producing a polyolefin-based microporous film according to an embodiment of the present invention preferably includes the following steps (a) to (e).

[0083] (a) a step of preparing a polyolefin resin solution by melting and kneading a polymer material containing one or more polyolefin resins and a solvent added as needed.

[0084] (b) Process of extruding the dissolved substance, forming it into a sheet, and cooling and solidifying it

[0085] (c) Step of stretching the obtained sheet by a roll method or a tenter method

[0086] (d) Then, a step of extracting the plasticizer from the obtained stretched film and drying the film

[0087] (e) Heat treatment / re-stretching process

[0088] Each step is described below.

[0089] (a) Preparation process of polyolefin resin solution

[0090] The polyolefin resin used in the embodiment of the present invention is heated and dissolved in a plasticizer to prepare a polyolefin resin solution. The plasticizer is not limited as long as it is a solvent that can fully dissolve the polyolefin resin. Since a relatively high ratio of stretching can be achieved, the solvent is preferably liquid at room temperature.

[0091] Examples of the solvent include aliphatic, cycloaliphatic or aromatic hydrocarbons such as nonane, decane, decalin, p-xylene, undecane, dodecane and liquid paraffin, mineral oil fractions having boiling points corresponding to these, and phthalic acid esters such as dibutyl phthalate and dioctyl phthalate that are liquid at room temperature. In order to obtain a gel-like sheet with a stable content of the liquid solvent, it is preferred to use a non-volatile liquid solvent such as liquid paraffin.

[0092] The ratio of the solvent is preferably 400 parts by mass or more and 900 parts by mass or less based on 100 parts by mass of the total mass of the polyethylene resin from the viewpoint of easily controlling the cell structure in the thickness direction to fall within a specific range.

[0093] In the melt mixing state, although it is mixed with the polyolefin resin, a solid solvent can be mixed in a liquid solvent at room temperature. As such a solid solvent, stearyl alcohol, cetyl alcohol, paraffin, etc. can be listed. Wherein, if only a solid solvent is used, uneven stretching, etc. may occur.

[0094] The viscosity of the liquid solvent is preferably 20 to 200 cSt at 40°C. If the viscosity at 40°C is 20 cSt or more, the sheet formed by extruding the polyolefin resin solution from the die head is less likely to be uneven. On the other hand, if the viscosity at 40°C is 200 cSt or less, the liquid solvent can be easily removed. It should be noted that the viscosity of the liquid solvent is the viscosity measured at 40°C using an Ubbelohde viscometer.

[0095] (b) Extrudate formation and gel sheet formation

[0096] The method for uniformly melting and kneading the polyolefin resin solution is not particularly limited, but when a high-concentration polyolefin resin solution is to be prepared, it is preferably carried out in a twin-screw extruder. As required, known additives such as metal soaps such as calcium stearate, ultraviolet absorbers, light stabilizers, antistatic agents, etc. may also be added within the range that does not damage the film-forming property and the effect of the present invention. In particular, an antioxidant is preferably added to prevent oxidation of the polyolefin resin.

[0097] In the extruder, the polyolefin resin solution is uniformly mixed at a temperature at which the polyolefin resin is completely melted. The melting and kneading temperature varies depending on the polyolefin resin used, but is preferably (melting point of the polyolefin resin + 10°C) to (melting point of the polyolefin resin + 120°C). More preferably, it is (melting point of the polyolefin resin + 20°C) to (melting point of the polyolefin resin + 100°C).

[0098] Here, the melting point refers to the value obtained by DSC (Differential scanning calorimetry) measurement based on JIS K7121 (1987). For example, when the polyolefin resin is a polyethylene resin, the melt-kneading temperature of the polyethylene resin is preferably in the range of 140 to 250° C. More preferably, it is 160 to 230° C., and most preferably, it is 170 to 200° C. Specifically, since the polyethylene resin has a melting point of about 130 to 140° C., the melt-kneading temperature is preferably 140 to 250° C., and most preferably, it is 180 to 230° C.

[0099] From the viewpoint of suppressing the deterioration of polyolefin resin, preferably the melt-mixing temperature is low, but if it is lower than the above-mentioned temperature, then there is the extrudate after extruding from the die head and will produce unmelted material, and in the subsequent stretching process, it becomes the situation causing the reasons such as broken film. In addition, if it is higher than the above-mentioned temperature, then there is the thermal decomposition of polyolefin resin and becomes violent, and the physical property of the obtained polyolefin microporous film, such as intensity and porosity, etc., deteriorates. In addition, the decomposed product is separated out on the roller on the cooling roll or the stretching process, etc., and is related to the appearance deterioration because of adhering to the sheet. Therefore, preferably the melt-mixing temperature is mixed within the above-mentioned range.

[0100] In addition, a gel sheet is obtained by cooling the obtained extrudate, and the microphase of the polyolefin resin separated by the solvent can be fixed by cooling. In the cooling process, the gel sheet is preferably cooled to 10 to 50°C. This is because the final cooling temperature is set below the crystallization end temperature, so that the high-order structure is refined, which makes it easy to stretch uniformly in the subsequent stretching. Therefore, cooling is preferably performed at least below the gelation temperature at a rate of 30°C / min or more.

[0101] Generally, if the cooling rate is slow, relatively large crystals are formed, so the higher-order structure of the gel-like sheet becomes coarse, and the gel structure forming the crystals also becomes a larger structure. On the other hand, if the cooling rate is fast, small and uniform crystals are formed, so the higher-order structure of the gel-like sheet becomes dense, which is related to uniform stretching and a reduction in the unopened portion.

[0102] As a cooling method, there are a method of directly bringing it into contact with cold air, cooling water, or other cooling media, a method of bringing it into contact with a roll cooled with a refrigerant, a method of using a casting drum, etc.

[0103] Herein, the case where the polyolefin-based microporous membrane is a single layer is described, but the polyolefin-based microporous membrane according to the embodiment of the present invention is not limited to a single layer, and may be a laminate. The number of laminates is not particularly limited, and may be a laminate of 2 layers or a laminate of 3 or more layers.

[0104] As a method for making a polyolefin-based microporous membrane into a laminate, for example, the following method can be listed: prepare the desired resins as needed, and supply these resins to an extruder separately, melt them at a desired temperature, make them merge in a polymer tube or a die, and extrude them from a slit-shaped die with the thickness of each target layer, thereby forming a laminate.

[0105] (c) Stretching process

[0106] The obtained gel-like (including laminated sheets) sheet is stretched. Examples of the stretching method used include uniaxial stretching in the sheet conveying direction (MD direction) using a roll stretcher, uniaxial stretching in the sheet width direction (TD direction) using a tenter, sequential biaxial stretching using a roll stretcher and a tenter, or a combination of a tenter and a tenter, or simultaneous biaxial stretching using a simultaneous biaxial tenter.

[0107] From the perspective of uniformity of the thickness of the film, the stretching ratio varies depending on the thickness of the gel-like sheet, and it is preferred that the stretching ratio be 7 times or more in any direction. In addition, from the perspective of making the various pore structures in the thickness direction within a desired range, the surface ratio is preferably 60 times or more, more preferably 80 times or more, and particularly preferably 100 times or more. In addition, from the perspective of suppressing rupture during the manufacture of the polyolefin-based microporous membrane, the surface ratio is preferably 150 times or less.

[0108] From the viewpoint of improving the stretching uniformity in the stretching process, the preferred form of the stretching ratio and the raw material composition is that when the total mass of all polyolefin resins contained in the gel-like sheet is 100 mass%, the composition contains 80 mass% or more of ultra-high molecular weight polyethylene with a weight average molecular weight (Mw) of 1,000,000 or more, and the gel-like sheet is stretched to a surface ratio of 60 times or more in a wet state, and more preferably stretched to 10×10 times or more in a wet state. A further preferred form is that when the total mass of all polyolefin resins contained in the gel-like sheet is 100 mass%, the composition contains 80 mass% or more of ultra-high molecular weight polyethylene with a weight average molecular weight (Mw) of 2,000,000 or more, and the gel-like sheet is stretched to a surface ratio of 60 times or more in a wet state, and most preferably stretched to 10×10 times or more in a wet state.

[0109] The stretching temperature is preferably the melting point of the gel sheet + 10°C or less, and more preferably in the range of (the crystal dispersion temperature Tcd of the polyolefin resin) to (the melting point of the gel sheet + 5°C). Specifically, in the case of a polyethylene composition, since it has a crystal dispersion temperature of about 90 to 110°C, the stretching temperature is preferably 100 to 130°C, more preferably 115 to 125°C, and further preferably 117.5 to 125°C. The crystal dispersion temperature Tcd is obtained from the temperature characteristics of the dynamic viscoelasticity measured according to ASTM D4065 (2012).

[0110] If the stretching temperature is lower than 100°C, the pores are insufficiently opened due to low-temperature stretching, making it difficult to obtain uniform film thickness and the porosity is also low. If the stretching temperature is higher than 130°C, the sheet may melt and the pores may be easily blocked.

[0111] The above stretching causes the high-order structure of the film to crack, and the crystal phase is refined to form a plurality of fibrils. The fibrils form a three-dimensional irregularly connected network structure. Since the mechanical strength is improved by stretching and pores are formed, the polyolefin-based microporous membrane involved in the embodiment of the present invention is suitable for battery separators.

[0112] In addition, by stretching before removing the plasticizer, the polyolefin resin is in a fully plasticized and softened state, so the cracking of the high-order structure becomes smooth, and the crystal phase can be uniformly refined. In addition, by stretching before removing the plasticizer, the high-order structure is easy to crack, so the strain during stretching is not easy to remain, and the thermal shrinkage rate can be reduced compared with the case of stretching after removing the plasticizer.

[0113] (d) Plasticizer extraction (washing) and drying process

[0114] Next, the plasticizer (solvent) remaining in the gel-like sheet is removed using a washing solvent. Since the polyolefin resin phase and the solvent phase are separated, a polyolefin microporous membrane is obtained by removing the solvent.

[0115] Examples of the washing solvent include saturated hydrocarbons such as pentane, hexane, and heptane; chlorinated hydrocarbons such as dichloromethane and carbon tetrachloride; ethers such as diethyl ether and dioxane; ketones such as methyl ethyl ketone; and chain fluorinated carbons such as trifluoroethane.

[0116] These washing solvents have low surface tension (e.g., 24 mN / m or less at 25°C). By using a washing solvent with low surface tension, shrinkage caused by the surface tension of the gas-liquid interface during drying after washing is suppressed in the formation of a microporous network structure, thereby obtaining a polyolefin-based microporous membrane with excellent porosity and permeability. These washing solvents can be appropriately selected according to the plasticizer, and can be used alone or in combination.

[0117] The washing method includes a method of immersing the gel sheet in a washing solvent and extracting the gel sheet, a method of showering the washing solvent on the gel sheet, or a method obtained by combining these methods, etc. The amount of the washing solvent used varies depending on the washing method, but is usually preferably 300 parts by mass or more relative to 100 parts by mass of the gel sheet.

[0118] The washing temperature is preferably 15 to 30° C., and may be heated to 80° C. or less as needed. At this time, the longer the gel sheet is immersed in the washing solvent, the better, from the viewpoint of improving the washing effect of the washing solvent, avoiding uneven physical properties (e.g., physical properties in the TD direction and / or MD direction) of the obtained polyolefin-based microporous membrane, and improving the mechanical and electrical properties of the polyolefin-based microporous membrane.

[0119] The above-mentioned washing is preferably performed until the residual solvent in the washed gel-like sheet, that is, the polyolefin-based microporous membrane, is less than 1% by mass.

[0120] Then, the solvent in the polyolefin-based microporous membrane is dried and removed by a drying step. The drying method is not particularly limited, and a method using a metal heating roller, a method using hot air, etc. can be selected. The drying temperature is preferably 40 to 100° C., and more preferably 40 to 80° C. If the drying is insufficient, the porosity of the polyolefin-based microporous membrane may decrease in the subsequent heat treatment, and the permeability may deteriorate.

[0121] (e) Heat treatment / re-stretching process

[0122] The dried polyolefin-based microporous membrane can be stretched (re-stretched) at least in a uniaxial direction. The re-stretching can be performed by a tentering method or the like while heating the polyolefin-based microporous membrane in the same manner as the above-mentioned stretching. The re-stretching can be uniaxial stretching or biaxial stretching. In the case of multi-stage stretching, it is performed by combining simultaneous biaxial or sequential stretching.

[0123] The re-stretching temperature is preferably below the melting point of the polyolefin resin, and more preferably in the range of (Tcd of the polyolefin resin composition - 20°C) to the melting point of the polyolefin resin. Specifically, in the case of a polyethylene resin, the re-stretching temperature is preferably 70 to 135°C, more preferably 110 to 135°C, further preferably 125 to 135°C, and further preferably 130 to 135°C.

[0124] The re-stretching ratio is preferably 1.01 to 2.0 times in the case of uniaxial stretching, and the ratio in the TD direction is preferably 1.1 to 1.6 times, and more preferably 1.2 to 1.4 times. In the case of biaxial stretching, it is preferably stretched 1.01 to 2.0 times in the MD direction and the TD direction, respectively. It should be noted that the re-stretching ratio may be different in the MD direction and the TD direction. By re-stretching within the above range, the porosity and permeability can be improved, and the re-aggregation of the original fibers caused by shrinkage can be suppressed, and uniform pore opening of the polyolefin-based microporous membrane becomes possible.

[0125] From the viewpoint of heat shrinkage, wrinkles and relaxation, the relaxation rate from the maximum re-stretching ratio is preferably 20% or less, more preferably 10% or less, and further preferably 5% or less. When the relaxation rate is 20% or less, a uniform fibril structure is obtained.

[0126] (f) Other processes

[0127] In addition, the polyolefin-based microporous membrane may be subjected to a hydrophilization treatment according to other uses. The hydrophilization treatment may be performed by monomer grafting, surfactant treatment, corona discharge, etc. Monomer grafting is preferably performed after crosslinking treatment.

[0128] The present invention also relates to a nonaqueous electrolyte secondary battery including the polyolefin microporous membrane or laminate according to the embodiment of the present invention.

[0129] Example

[0130] The method for measuring the characteristics and the method for evaluating the effects in the embodiments of the present invention are as follows. However, the embodiments of the present invention are not limited to these examples.

[0131] (1) Weight average molecular weight (Mw)

[0132] The weight average molecular weight of the polyethylene resin is determined by gel permeation chromatography (GPC) under the following conditions.

[0133] ·Measurement device: GPC-150C manufactured by WATERS CORPORATION

[0134] ·Pillar: SHODEX UT806M manufactured by Showa Denko Co., Ltd.

[0135] Column temperature: 135°C

[0136] Solvent (mobile phase): o-dichlorobenzene

[0137] Solvent flow rate: 1.0 mL / min

[0138] · Sample concentration: 0.1wt% (dissolution conditions: 135℃ / 1H)

[0139] Injection volume: 500μL

[0140] Detector: Differential refractometer (RI detector) manufactured by WATERS CORPORATION

[0141] · Calibration curve: A calibration curve obtained using a monodisperse polystyrene standard sample was prepared using a predetermined conversion constant.

[0142] (2) Thickness

[0143] The evaluation sample was cut from the polyolefin microporous membrane in a size of 95 mm × 95 mm, and then marked in a manner that 40 mm square grids were connected in two vertical and horizontal directions, and a total of 4 were connected. It should be noted that when marking, the marking was performed in the following manner: the vertex of the center where the 4 grids overlapped overlapped with the center position of the evaluation sample, and the edges of the vertical and horizontal grids were parallel to the edges of the evaluation sample. The thickness of a total of 9 locations corresponding to the vertices of the 4 connected grids was measured by a contact thickness meter (Lite Machik, Mitsutoyo Co., Ltd.), and the average thickness of the 9 points was calculated.

[0144] (3) Porosity

[0145] A sample for evaluation was cut out of the polyolefin microporous membrane in a size of 5 cm square, and its volume (cm 3 ) and mass (g), and these are related to the resin density (g / cm 3 ) is calculated using the following formula. Five or more measurements are performed at different random locations in the same polyolefin-based microporous membrane, and the average porosity of the five points is obtained. It should be noted that the resin density is obtained using JIS K6922-2-2010 after the polyolefin-based microporous membrane is heated and melted to form a sheet in a non-porous state.

[0146] Porosity = [(volume-mass / resin density) / volume] × 100

[0147] (4) Puncture strength

[0148] A puncture meter manufactured by MARUBI SHI Co., Ltd. was used to measure the maximum load when a polyolefin microporous membrane having a thickness of T1 (μm) was punctured at a speed of 2 mm / sec using a needle having a spherical tip (radius of curvature R: 0.5 mm) and a diameter of 1 mm. The measured value was taken as the puncture strength L1 (gf).

[0149] The puncture strength L1(gf) is converted to the maximum load when the thickness is 10 μm using the formula: L2(gf)=L1(gf) / T1(μm)×10 μm, and is taken as the puncture strength L2(gf) converted to a thickness of 10 μm.

[0150] More than three measurements are performed at different randomly selected locations in the same polyolefin-based microporous membrane, and the average values ​​of the puncture strength L1 (gf) at the three points and the puncture strength L2 (gf) converted to a thickness of 10 μm are calculated respectively. The average value of the puncture strength L2 (gf) converted to a thickness of 10 μm is recorded in the table as "Puncture Strength (10 μm converted)".

[0151] (5) FIB-SEM

[0152] The continuous images were measured by FIB-SEM under the following conditions.

[0153] · Sample preparation: After embedding a polyolefin-based microporous membrane with an epoxy-based resin, electron staining was performed using OsO 4 and the sample was used for measurement.

[0154] Observation device: FEI Helios G4

[0155] Observation conditions: Acceleration voltage 1 kV

[0156] · Sample tilt: 52°

[0157] Pixel size: Horizontal image: 5.4nm, vertical image: 6.8nm (after tilt correction)

[0158] Slice interval in FIB: 10nm

[0159] Image adjustment method: A mark was made by depositing Pt on the upper part of the film, and the position between each image was checked.

[0160] Tilt correction: Since FIB-SEM observation starts at a tilt of 52°, the SEM image is observed while being reduced in the longitudinal direction. Therefore, in order to obtain an image observed from the front, the image needs to be magnified by 1.27 times (= / sin52°) in the longitudinal direction. The image after tilt correction is used to create the three-dimensional image described later.

[0161] Measurement size: A 5 μm×5 μm section of a thin film was sequentially processed by FIB, sliced ​​until it reached 4 μm in the depth direction, and a volume of 5 μm×5 μm×4 μm was measured (400 images were taken).

[0162] (6) Production of three-dimensional images for pore analysis

[0163] For the FIB-SEM image obtained in (5), the image processing software "ExFact (registered trademark) Analysis for Porous / Particles" manufactured by Japan Business Science Co., Ltd. is used to perform a binarization process on the resin portion of the microporous membrane that is embedded and electronically stained (i.e., the portion corresponding to the pore portion of the microporous membrane) and the portion of the resin constituting the microporous membrane, and then a three-dimensional stereoscopic image is formed based on the binarization information. After that, the pore portion of the microporous membrane is subjected to a thinning process using the image processing software "ExFact (registered trademark) Analysis for Porous / Particles" manufactured by Japan Business Science Co., Ltd., thereby producing a three-dimensional image of the pore structure inside the microporous membrane. The size of the produced three-dimensional image was a cube surrounded by a side having a length of 2.7 μm at the center in the FIB-SEM measurement size of 5 μm×5 μm×4 μm from the viewpoint of analysis time and reproducibility of analysis parameters.

[0164] (7) Number of holes in the thickness direction

[0165] For the three-dimensional image obtained in (6), the following operation was performed using the image processing software "ExFact (registered trademark) Analysis for Porous / Particles" manufactured by Japan Business Science Co., Ltd.: Among all the paths (pores) formed by the pores of the microporous membrane from the starting surface to the end surface in the thickness direction of the polyolefin-based microporous membrane, the pore with the shortest distance was detected as one and operated. In the cube of the three-dimensional image surrounded by sides with a side length of 2.7 μm, all the pores in the thickness direction from the starting surface of the area of ​​2.7 μm×2.7 μm to the end surface of 2.7 μm×2.7 μm were counted, and the number of pores converted to 1 μm was calculated. 2 The value obtained by calculating the number of roots is used as the number of channels in the thickness direction in the present invention.

[0166] (8) Peak value of the tortuosity distribution of the pores in the thickness direction

[0167] After calculating the tortuosity of each pore in the thickness direction obtained in (7) using the image processing software "ExFact (registered trademark) Analysis for Porous / Particles", a frequency distribution of tortuosity is made for all pores in the thickness direction of the analysis object, and a graph of the tortuosity frequency distribution after smoothing is made. The resulting graph will show the tortuosity with the highest frequency as the peak of the tortuosity distribution of the pores in the thickness direction. When the peak of the tortuosity of the pores in the thickness direction is observed at more than two locations, the peak with the highest frequency is used. When the peak with the highest frequency is observed at more than two locations with the same frequency, the peak with the lowest tortuosity is used.

[0168] (9) Frequency of peak values ​​of channel tortuosity distribution in the thickness direction

[0169] The value of the frequency at the peak of the tortuosity distribution obtained in (8) is taken.

[0170] (10) Half-value width of the channel tortuosity distribution in the thickness direction

[0171] For the tortuosity frequency distribution graph obtained in the same manner as in (8), function fitting was performed using numerical analysis software to obtain the arithmetic full width at half maximum.

[0172] (11) Capacity retention rate under rapid charge and discharge conditions

[0173] In order to evaluate the capacity retention rate under rapid charge and discharge conditions in the configuration of a lithium ion secondary battery, a polyolefin microporous membrane was incorporated as a separator in a non-aqueous electrolyte secondary battery composed of a positive electrode, a negative electrode, a separator and an electrolyte, and a charge and discharge test was performed.

[0174] The following negative electrode and positive electrode were used: the negative electrode was formed on an aluminum foil with a size of 38 mm wide×33 mm long×20 μm thick with a mass per unit area of ​​9.5 mg / cm 2 Laminated NMC532 (lithium nickel manganese cobalt composite oxide (Li 1.05 Ni 0.50 Mn 0.29 Co 0.21 O2)), the positive electrode is on a copper foil with a width of 40 mm × a length of 35 mm × a thickness of 10 μm with a unit area mass of 5.5 mg / cm 2 Lamination density 1.45g / cm 3 The positive and negative electrodes are dried in a vacuum oven at 120°C before use.

[0175] As a separator, a polyolefin microporous membrane with a length of 50 mm and a width of 50 mm was dried in a vacuum oven at room temperature. As for the electrolyte, vinylene carbonate (VC) and LiPF6 were dissolved in a mixture of ethylene carbonate, ethyl methyl carbonate, and dimethyl carbonate (30 / 35 / 35, volume ratio) to prepare a solution with a VC concentration of 0.5 mass% and a LiPF6 concentration of 1 mol / L.

[0176] The positive electrode, the separator, and the negative electrode are stacked, the obtained stack is arranged in a laminate, an electrolyte is injected into the laminate, and the laminate is vacuum-sealed to produce a lithium ion secondary battery.

[0177] The manufactured lithium ion secondary battery was charged 10 to 15% at a temperature of 35°C and 0.1C as the initial charge, and was left at 35°C for one night (more than 12 hours) to perform exhaust. Next, at a temperature of 35°C and a voltage range of 2.75 to 4.2V, CC-CV charging with a charging current value of 0.1C (constant current constant voltage charging (termination current condition 0.02C)) and CC discharge with a discharge current value of 0.1C (constant current discharge) were performed. Then, at a temperature of 35°C and a voltage range of 2.75 to 4.2V, three cycles of CC-CV charging with a charging current value of 0.2C (constant current constant voltage charging (termination current condition 0.05C)) and CC discharge with a discharge current value of 0.2C (constant current charging) were performed, and the time after the cycle was regarded as the initial stage of the non-aqueous electrolyte secondary battery.

[0178] In addition, after CC-CV charging (constant current constant voltage charging (termination current condition 0.05C)) with a charging current value of 0.2C at a temperature of 35°C and a voltage range of 2.75 to 4.2V, a CC discharge (low current discharge) of 0.2C was performed at 15°C, and the discharge capacity at this time was 0.2C capacity. Next, CC-CV charging (constant current constant voltage charging (termination current condition 0.05C) with a charging current value of 0.5C was performed at a temperature of 35°C and a voltage range of 2.75 to 4.2V, and a 10C (180mA, 14.4mA / cm 2 ) in the rate test. From the results, the ratio of 10C capacity to 0.2C capacity {(10C capacity / 0.2C capacity)×100} (%) was taken as the capacity retention rate (%) under rapid charge and discharge conditions. 55% or more indicates good characteristics.

[0179] (12) Production of three-dimensional images for fibril analysis

[0180] Regarding the FIB-SEM image obtained in (5), the image processing software "ExFact (registered trademark) Analysis for Fiber" manufactured by Japan Business Science Co., Ltd. was used to perform a binarization process on the part of the resin embedded in the microporous membrane and subjected to electron staining (i.e., the part corresponding to the pores of the microporous membrane) and the part of the resin constituting the microporous membrane, and then a three-dimensional stereoscopic image was obtained based on the binarization information. Then, the image processing software "ExFact (registered trademark) Analysis for Porous / Particles" manufactured by Japan Business Science Co., Ltd. was used to perform a thinning process on the resin part constituting the microporous membrane to produce a three-dimensional image of the resin part inside the microporous membrane. The size of the produced three-dimensional image was a cube surrounded by a side of 2.7 μm in the center within the FIB-SEM measurement size of 5 μm×5 μm×4 μm, from the viewpoint of analysis time and reproducibility of analysis parameters.

[0181] (13) Number of fibrils

[0182] For the three-dimensional image obtained in (12), the image processing software "ExFact (registered trademark) Analysis for Fiber" manufactured by Japan Business Science Co., Ltd. was used to segment the lines constituting the resin part that had been subjected to line thinning processing at the intersection and branching parts, and the number of thin lines after this operation was calculated, and then converted into per 1 μm 3 The value obtained by calculating the number of fibers is taken as the number of fibrils in the present invention.

[0183] (14) Average diameter of fibrils

[0184] The average diameter of all fibrils contained in the 2.7 μm×2.7 μm×2.7 μm three-dimensional image obtained in (13) was calculated using the image processing software "ExFact (registered trademark) Analysis for Fiber" manufactured by Business Science Corporation of Japan as the average fibril diameter.

[0185] (15) Number of fibril crossings

[0186] In (13), the image processing software "ExFact (registered trademark) Analysis for Fiber" manufactured by Japan Business Science Co., Ltd. was used to segment the lines of the constituent resin parts of the microporous membrane. The number of intersections between the constituent resin parts was calculated and converted into the number of intersections per 1 μm. 3 The value obtained by the number of is taken as the fibril crossing number in the present invention.

[0187] (16) Maximum shrinkage stress in the TD direction measured by thermomechanical analysis (TMA)

[0188] A 3 mm rectangle and a 15 mm rectangle were cut from the polyolefin microporous film in the MD direction and in the TD direction to prepare the evaluation sample. The evaluation sample was fixed to the chuck with a chuck spacing (TD direction) of 10 mm using the "TMA 7100" manufactured by Hitachi HiTech Nologi, and the temperature was raised from 30°C to 200°C at a rate of 5°C / min in a fixed length mode. The temperature and shrinkage force when the temperature was raised to 200°C were measured at 1 second intervals, and the value obtained by dividing the maximum shrinkage force (gf) by the cross-sectional area of ​​the evaluation sample was taken as the maximum shrinkage stress (MPa) in the TD direction measured by the thermomechanical analyzer (TMA).

[0189] (17) Maximum shrinkage stress temperature in the TD direction measured by a thermomechanical analyzer (TMA)

[0190] In (16), the temperature at which the maximum shrinkage stress in the TD direction measured by the thermomechanical analyzer (TMA) is shown is referred to as the maximum shrinkage stress temperature (° C.) in the TD direction measured by the thermomechanical analyzer (TMA).

[0191] (18) Safety evaluation

[0192] The lithium ion secondary battery prepared in the same manner as (11) was charged at a constant current of 0.2 C until the voltage reached 4.2 V, then charged at a constant voltage of 4.2 V, and then discharged at a current of 1 C until the final voltage reached 3.0 V. Next, constant current charging was performed at a current of 0.2 C until the voltage reached 4.2 V, and then constant voltage charging was performed at 4.2 V. Thereafter, the charged battery was placed in an oven, the temperature was raised from room temperature at 5°C / min, and then placed at 150°C for 60 minutes, and evaluated according to the following criteria.

[0193] A: No fire or smoke was observed after 60 minutes.

[0194] B: Fire or smoke was observed more than 30 minutes and within 60 minutes after reaching 150°C.

[0195] C: Fire or smoke was observed more than 10 minutes and within 30 minutes after the temperature reached 150°C.

[0196] D: Fire or smoke was observed within 10 minutes after reaching 150°C.

[0197] (Example 1)

[0198] The weight average molecular weight (Mw) was 10×10 5The ultra-high molecular weight polyethylene and the weight average molecular weight (Mw) are 5×10 5 High-density polyethylene is used as a raw material. 80 parts by mass of liquid paraffin is added to 16 parts by mass of ultra-high molecular weight polyethylene and 4 parts by mass of high-density polyethylene, and then 0.5 parts by mass of 2,6-di-tert-butyl-p-cresol and 0.7 parts by mass of tetrakis[methylene-3-(3,5-di-tert-butyl-4-hydroxyphenyl)-propionate]methane are added and mixed as an antioxidant based on the total mass of the polyethylene resin to prepare a polyethylene resin solution. It should be noted that the ratio of ultra-high molecular weight polyethylene when the mass of all polyethylene resins is 100% by mass is 80% by mass. Since most of the liquid paraffin and antioxidant are removed in the manufacturing process, in the present invention, the ratio of ultra-high molecular weight polyethylene when the mass of all polyethylene resins is 100% by mass is used as the ratio of ultra-high molecular weight polyethylene in the polyolefin microporous membrane.

[0199] The obtained polyethylene resin solution was put into a twin-screw extruder, kneaded at 180° C., supplied to a T-die, and the extrudate was cooled with a cooling roll controlled at 15° C. to form a gel-like sheet.

[0200] The obtained gel-like sheet was longitudinally stretched 8 times in the longitudinal direction (MD direction) at 118°C by a roll stretcher (recorded as longitudinal stretching (MD1) in the table), cooled, and then transversely stretched 8 times in the width direction (TD direction) at 118°C by a tenter stretcher (recorded as transverse stretching (TD) in the table). In this state, the sheet width was fixed in the tenter stretcher and maintained at a temperature of 115°C for 10 seconds. It should be noted that the product of the ratio of longitudinal stretching (MD1) and the ratio of transverse stretching (TD), that is, the area ratio, was 64 times.

[0201] Then, the stretched gel-like sheet was immersed in a dichloromethane bath using a washing tank, and the liquid paraffin was removed and then dried to obtain a polyolefin-based microporous membrane. Finally, an oven was used to shorten the film by 5% in the width direction (recorded as relaxation rate in the table), and heat-set for 10 minutes at 130°C in the relaxed state to obtain a polyolefin-based microporous membrane. It should be noted that in the table, the shortening ratio in the width direction during heat setting is recorded as relaxation rate, and the time for heat setting is recorded as heat setting time.

[0202] (Example 2)

[0203] For the stretching in the longitudinal direction (MD direction) performed by a roller stretching machine, the first stage (MD1) was set to 118°C and 4 times (recorded in the table as longitudinal stretching (MD1)), and the second stage (MD2) was set to 118°C and 2 times (recorded in the table as longitudinal stretching (MD2)). Stretching was carried out in these two stages. Except for this, a polyolefin-based microporous membrane was obtained in the same manner as in Example 1.

[0204] (Examples 3 to 5, 8 to 19)

[0205] A polyolefin-based microporous membrane was obtained in the same manner as in Example 2 except that the raw material composition and production conditions were as shown in the table.

[0206] (Examples 6 and 7)

[0207] A polyolefin-based microporous membrane was obtained in the same manner as in Example 1 except that the raw material composition and production conditions were as shown in the table.

[0208] (Comparative Examples 1 to 4)

[0209] A polyolefin-based microporous membrane was obtained in the same manner as in Example 1 except that the raw material composition and production conditions were as shown in the table.

[0210]

[0211]

[0212]

[0213]

[0214] Table 5

[0215]

[0216] Industrial Availability

[0217] The polyolefin-based microporous membrane according to the embodiment of the present invention is suitable for use as a separator for non-aqueous electrolyte secondary batteries such as lithium-ion secondary batteries because it has excellent strength and can improve the capacity retention rate under rapid charge and discharge conditions.

[0218] While the invention has been described in detail and with reference to specific embodiments thereof, it will be apparent to one skilled in the art that various changes and modifications can be made therein without departing from the spirit and scope of the invention.

[0219] This application is based on Japanese patent application (Japanese Patent Application No. 2019-137306) filed on July 25, 2019, and Japanese patent application (Japanese Patent Application No. 2019-137307) filed on July 25, 2019, and the contents of these are incorporated herein by reference.

Claims

1. A polyolefin-based microporous membrane having a composition in which, when the total mass of the polyolefin-based resin used as a raw material is set to 100 mass %, the raw material contains 80 mass % of an ultra-high molecular weight polyethylene having a weight average molecular weight Mw of 1,000,000 or more, In the 2.7 μm×2.7 μm×2.7 μm three-dimensional image prepared from each cross-sectional image obtained by FIB-SEM measurement of the microporous membrane, the number of pores in the thickness direction was 35 / μm. 2 The peak value of the tortuosity distribution of the pores in the thickness direction is 1.30 or more and 1.80 or less. The maximum shrinkage stress temperature in the TD direction measured by a thermomechanical analyzer (TMA) is 143° C. or higher, and the maximum shrinkage stress is 1.3 MPa or lower.

2. The polyolefin-based microporous membrane according to claim 1, wherein The frequency of the peak value of the tortuosity distribution of the cell in the thickness direction is 6% or more and 30% or less.

3. The polyolefin-based microporous membrane according to claim 1 or 2, wherein The half value width of the tortuosity distribution of the cell in the thickness direction is 0.06 or more and 0.25 or less.

4. The polyolefin-based microporous membrane according to claim 1 or 2, wherein In the 2.7 μm×2.7 μm×2.7 μm three-dimensional image prepared from each cross-sectional image obtained by FIB-SEM measurement of the microporous membrane, the number of fibrils was 870 / μm. 3 Above and 2800 / μm 3 the following.

5. A polyolefin-based microporous membrane having a composition in which, when the total mass of the polyolefin-based resin used as a raw material is set to 100 mass %, the raw material contains 80 mass % of an ultra-high molecular weight polyethylene having a weight average molecular weight Mw of 1,000,000 or more, In the 2.7 μm×2.7 μm×2.7 μm three-dimensional image prepared from each cross-sectional image obtained by FIB-SEM measurement of the microporous membrane, the number of fibrils was 870 / μm. 3 Above and 2800 / μm 3 the following, The maximum shrinkage stress temperature in the TD direction measured by a thermomechanical analyzer (TMA) is 143° C. or higher, and the maximum shrinkage stress is 1.3 MPa or lower.

6. The polyolefin-based microporous membrane according to claim 1, 2 or 5, wherein The average fibril diameter is 25 nm or more and 60 nm or less.

7. The polyolefin-based microporous membrane according to claim 1, 2 or 5, wherein The number of fibril crossings is 1350 / μm 3 Above and 4400 / μm 3 the following.

8. The polyolefin-based microporous membrane according to claim 1, 2 or 5, wherein The puncture strength is 180 gf or more and 700 gf or less.

9. The polyolefin-based microporous membrane according to claim 1, 2 or 5, wherein The thickness is 3 μm or more and 14 μm or less.

10. The polyolefin-based microporous membrane according to claim 1, 2 or 5, wherein The porosity is 35% or more and 50% or less. 11 . A laminate comprising the polyolefin-based microporous film according to claim 1 , further comprising a heat-resistant resin layer laminated thereon. 12 . A non-aqueous electrolyte secondary battery comprising the polyolefin-based microporous membrane according to claim 1 or the laminate according to claim 11 .