Ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst and its application

An ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst was prepared through a one-pot evaporation-induced self-assembly method, which solved the problems of low efficiency and poor stability of existing catalysts in the process of converting ethanol to n-butanol, and achieved high efficiency. It has excellent ethanol conversion and higher alcohol yield, and maintains excellent stability during long-term use, making it suitable for industrial applications.

CN114130399BActive Publication Date: 2024-10-22ZHEJIANG UNIV OF TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111209238.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-18
Publication Date
2024-10-22
Estimated Expiration
2041-10-18

AI Technical Summary

Technical Problem

Existing catalysts have problems such as low efficiency, complex processes, and poor catalyst stability in the process of converting ethanol to n-butanol. In particular, they show instability and low yields in large-scale production and long-term use.

Method used

A one-pot evaporation-induced self-assembly method is used to prepare ordered mesoporous copper-rare earth metal-aluminum composite oxide catalysts. Through highly dispersed copper and rare earth metal oxide active components and stable alumina carriers, a large specific surface area and pore size are formed. The moderate catalyst structure is used in the fixed-bed continuous catalytic conversion of ethanol to synthesize higher alcohols.

Benefits of technology

It achieved an ethanol conversion rate of up to 52.2% and a higher alcohol yield of 37.7%, and showed excellent stability in a long-term evaluation of 500 hours, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003308222250000101
    Figure BDA0003308222250000101
  • Figure BDA0003308222250000111
    Figure BDA0003308222250000111
  • Figure HDA0003490254790000011
    Figure HDA0003490254790000011
Patent Text Reader

Abstract

The ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst of the present invention has a highly ordered mesoporous structure and a high specific surface area, and copper, rare earth metal oxide and alumina carrier interact closely and are highly uniformly dispersed. The highly dispersed Cu active component provides a large amount of ethanol dehydrogenation activity or crotonaldehyde hydrogenation center, and the highly dispersed rare earth metal oxide cooperates with the alumina carrier to provide a large amount of acid-base active centers that promote acetaldehyde aldol condensation, thereby ultimately achieving efficient conversion of ethanol to higher alcohols. At the same time, the mutual doping and strong interaction between the oxides of copper, rare earth metals and aluminum limit the sintering and growth of Cu and rare earth metal oxides, so that the catalyst shows excellent stability in a long-term evaluation of 500h.
Need to check novelty before this filing date? Find Prior Art

Description

(I) Technical field

[0001] The present invention relates to an ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst (CuO-MO x -Al2O3) and its preparation method and application. The catalyst shows excellent catalytic activity, selectivity and stability in the reaction of ethanol to higher alcohols, and thus has good industrial application prospects. (II) Background technology

[0002] Due to the increasing depletion of fossil resources and the greenhouse effect caused by their use, the development and utilization of renewable biomass fuels have attracted more and more attention. As a renewable biomass fuel, bioethanol is widely used as a gasoline blending component in the United States, Brazil, China and other countries. However, ethanol has problems such as strong hygroscopicity, low energy density, and corrosion of engine cylinders, so it is not an ideal gasoline blending component. Compared with ethanol, n-butanol is insoluble in water, has high energy density, is less corrosive to automobile engines, can be mixed with gasoline in a higher ratio, and will not cause the problem of difficulty in starting the car due to fuel stratification, so it has become an ideal substitute for the current ethanol gasoline blending component. n-Butanol is also an important chemical raw material and product. It can be used as a platform molecule to prepare many chemicals and is widely used in petrochemical, food, medicine and other fields. In industry, petroleum-based propylene is mainly used as a raw material to synthesize n-butanol through carbonylation and hydrogenation reactions. Although n-butanol can also be produced by fermentation of biomass raw materials, the efficiency of producing n-butanol by biological fermentation is very low. At the same time, the production of n-butanol requires large evaporation, heating, cooling and other facilities, and the investment cost is high. On the other hand, the industrial process of producing biomass ethanol by biofermentation has become quite mature and has a certain scale, providing solid support for the development of downstream ethanol products. Therefore, the production of high-value-added chemicals through ethanol catalytic conversion has become one of the hot topics of current academic and industrial circles.

[0003] The preparation of n-butanol from bioethanol involves multiple catalytic processes such as ethanol dehydrogenation, acetaldehyde aldol condensation and crotonaldehyde hydrogenation, which restrict each other and result in a generally low yield of n-butanol. Designing and regulating the catalyst structure to achieve the synergistic effect of efficient ethanol dehydrogenation, acetaldehyde aldol condensation and crotonaldehyde hydrogenation is the key to effectively connect this series of tandem reactions. In the publicly published literature, iridium and ruthenium complex catalysts are used for the ethanol dehydrogenation condensation to produce n-butanol, and higher butanol selectivity and yield are achieved, but their preparation is complicated, and soluble strong bases such as sodium hydroxide and sodium ethoxide are used as catalysts for the acetaldehyde aldol condensation step. In particular, they use a tank reactor, catalyst separation is difficult, and the reaction cannot be carried out continuously, which is not conducive to the large-scale production of butanol fuel in the future [Angew. Chem. Int. Ed., 2013, 52, 9005-9008; J. Am. Chem. Soc. 2015, 137, 14264-14267]. Metal-supported multifunctional catalysts are widely used in the dehydrogenation condensation of ethanol to produce n-butanol, and exhibit excellent catalytic performance. For example, a copper-based catalyst supported by high specific surface area CeO2 achieved an ethanol conversion rate of 67% and a butanol yield of up to 30wt% at a reaction temperature of 250°C. However, it needs to be carried out in a supercritical CO2 medium. The reaction pressure greater than 10MPa places high demands on the material of the reaction equipment, the reaction process is more complicated, and the butanol production capacity per unit volume of the reactor is low, and its industrial application is restricted to a certain extent [Green Chem., 2015, 17: 3018-3025.]. Activated carbon-supported Cu-CeO2 / AC catalyst is used for the dehydrogenation condensation of ethanol to produce n-butanol. It has a high catalytic performance at 250°C, 2MPa (N2), LHSV=2h -1 Under the reaction conditions, the ethanol conversion rate was 46% and the butanol yield was nearly 20wt%, and no small molecule gas products were produced. However, the catalytic activity decreased slightly in the long-term reaction evaluation [Chem. Commun., 2016, 52, 13749-13752; Patent CN106076344].

[0004] Although copper-based catalysts are low in price and highly active, copper nanoparticles are prone to sintering due to the weak interaction between the metal and the carrier, and have poor thermal stability and durability [Prog. Solid State Chem., 1975, 9, 21-25.]. One way to improve the stability of copper-based catalysts is to form a copper spinel oxide structure. For example, Cu-based spinel oxide CuM2O4 (M = Fe, Al and other metals) exhibits higher catalytic activity and stability than CuO-ZnO-Al2O3 catalysts [Appl. Catal. A, 2008, 341, 139-145.]. Currently, partially embedding copper nanoparticles in mesoporous alumina with high thermal stability is an attractive method to inhibit the sintering of copper nanoparticles. At the same time, ordered mesoporous alumina (OMA) has the characteristics of large specific surface area, large pore size, ordered pore structure and good thermal stability, and is considered to be an ideal catalyst support for various catalytic reactions [J Catal., 2015, 326, 127-138; Catal Sci Technol., 2014, 4, 3169-3202.].

[0005] The invention adopts a one-pot evaporation induced self-assembly method to prepare an ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst, which realizes the high dispersion and stable existence of copper and rare earth metal oxide active components in the catalyst. At the same time, the catalyst has a large specific surface area and a pore size in the mesoporous range, which is conducive to the reaction and diffusion of reactants, intermediates and product molecules. It is applied to the reaction of ethanol fixed bed continuous catalytic conversion to synthesize higher alcohols, at 150-300°C, normal pressure-4.0MPa, LHSV=0.5-5mL / (h·g cat ), nitrogen / ethanol = 100:1 ~ 600:1 (volume ratio) reaction conditions, showing up to 52.2% ethanol conversion rate and 37.7% higher alcohol yield; at the same time, due to the strong restriction effect between the three oxides, the aggregation and sintering of the active centers are effectively prevented, thus showing excellent stability in 500h long-term evaluation, and has good industrial application prospects. (III) Summary of the invention

[0006] The present invention provides an ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst (CuO-MO x -Al2O3) and its preparation method and application, that is, a one-pot evaporation-induced self-assembly method is used to directly synthesize a catalyst with a large specific surface area, ordered mesoporous channels, highly dispersed active components and good stability, which is applied to the continuous and efficient catalytic conversion of ethanol fixed bed to synthesize higher alcohols.

[0007] The invention uses a one-pot method to synthesize an ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst in situ, which realizes the high dispersion and stable existence of copper and rare earth metal oxide active components on the catalyst. At the same time, the catalyst has a large specific surface area and a pore size in the mesoporous range, which is conducive to the reaction and diffusion of reactants, intermediates and product molecules. It is applied to the reaction of ethanol fixed bed continuous catalytic conversion to synthesize n-butanol, at 150-300°C, normal pressure-4.0MPa, LHSV=0.5-5mL / (h·g cat ), nitrogen / ethanol = 100:1~600:1 (volume ratio) reaction conditions, the yield of higher alcohols was as high as 15%~38%, and excellent stability was shown in a long-term evaluation of 500h.

[0008] In order to achieve the above object, the present invention adopts the following technical solution:

[0009] The present invention provides an ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst (CuO-MO x -Al2O3), the catalyst is prepared as follows:

[0010] The template agent is dissolved in anhydrous ethanol, and inorganic strong acid, salicylic acid and citric acid are added and mixed; soluble salts of copper, rare earth metals and aluminum are added and mixed; the solvent is evaporated at 25-80°C for 1-72h (preferably 60°C for 24h), and then dried at 60-120°C for 2-96h (preferably 65°C for 48h); the obtained mixture is heated to 350-550°C at a rate of 1-10°C / min (preferably 1°C / min) in a muffle furnace and calcined for 2-10h (preferably 400°C for 4h), and then the temperature is further increased to 600-800°C at a rate of 10-30°C / min (preferably 10°C / min) and calcined for 0.5-6h (preferably 700°C for 1h) to obtain the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst; the template agent is a triblock polymer surfactant;

[0011] The amount of aluminum in the soluble salt of aluminum is calculated based on the theoretical mass of aluminum oxide completely generated from the soluble salt of aluminum, and the ratio of the amount of the template, the hydrogen ions in the inorganic strong acid, salicylic acid, citric acid to the amount of aluminum in the soluble salt of aluminum is 0.015-0.02:1-5:0.05-0.1:0.03-0.08:1;

[0012] The masses of the soluble salts of copper, rare earth metals and aluminum are respectively calculated based on the theoretical mass of copper soluble salts completely generating copper oxide, rare earth metal soluble salts completely generating rare earth metal oxides and aluminum soluble salts completely generating aluminum oxide. The mass of copper oxide is 2.5-8.5% of the mass of the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst; the mass of the rare earth metal oxide is 3-15% of the mass of the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst; the mass of the aluminum oxide is 76.5-94.5% of the mass of the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst.

[0013] The catalyst can be used after the temperature drops naturally.

[0014] The ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst can be used for catalytic reaction after reduction activation in a reaction bed by any means known in the art before use. The reduction activation operation of the present invention is as follows: the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst is loaded into a fixed bed reactor, and ethanol is carried by N2 as a carrier gas and preheated before entering the fixed bed reactor for in-situ reduction at 100-325°C, and the liquid space velocity of ethanol is 2mL / (h·g cat ), the volume ratio of nitrogen to ethanol is 250:1.

[0015] Furthermore, the volume of the anhydrous ethanol is 2-20 mL / g (preferably 10 mL / g) based on the mass of the soluble aluminum salt.

[0016] Furthermore, the soluble copper salt is one or a mixture of soluble copper salts such as copper acetate, copper nitrate, copper chloride, etc.

[0017] The rare earth metal in the soluble salt of the rare earth metal may be one or a mixture of two or more rare earth metals; specifically, the rare earth metal in the soluble salt of the rare earth metal is one or a mixture of two or more of La, Ce, Sm, Pr, etc. The soluble salt of the rare earth metal is one or a mixture of several soluble rare earth metal salts such as acetates, nitrates, chlorides, etc. of the rare earth metal.

[0018] Furthermore, the soluble aluminum salt is one or a mixture of soluble aluminum salts such as aluminum nitrate, aluminum isopropoxide, and aluminum chloride.

[0019] In the above preparation method, the template is preferably P123 (EO 20 PO 70 EO 20 )、F127((C3H6O·C2H4O) x) and the like. The inorganic strong acid is preferably a mixture of one or more of hydrogen chloride or nitric acid, which can be added in the form of an aqueous solution, and is particularly preferably a mixture of one or two of inorganic acids such as 35wt% hydrochloric acid and 68wt% nitric acid.

[0020] The ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst of the present invention has a specific surface area of ​​190 to 400 m 2 / g, average pore diameter 6-15nm, pore volume 0.7-1.5mL / g.

[0021] The present invention also provides an application of the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst in the reaction of preparing higher alcohols by dehydrogenation condensation of ethanol.

[0022] The reaction is carried out continuously in a fixed bed reactor. The catalyst of the present invention has an ethanol conversion rate and a higher alcohol yield of up to 52.2% and 37.7% in the reaction, respectively, and no small molecule cracking products are produced; at the same time, due to the strong restriction effect between the three oxides, the catalyst performs well in a 500h stability test, thus showing good industrial application prospects.

[0023] Specifically, the application is: in a fixed bed reactor, the temperature is 150-300°C, the reaction pressure is normal pressure-4.0MPa, nitrogen and ethanol are introduced, and the liquid space velocity is 0.5-5mL / (h·g cat ), the volume ratio of nitrogen to ethanol is 100 to 600:1, and the ethanol is dehydrogenated and condensed to produce higher alcohols.

[0024] The ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst of the present invention has the highest selectivity and yield of higher alcohols and excellent stability. The main by-products of the reaction are acetaldehyde, ether, butyraldehyde, ethyl acetate, etc., and the unreacted ethanol can be recycled.

[0025] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0026] The ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst prepared by the method of the present invention has a highly ordered mesoporous structure and a high specific surface area (190-400m 2 / g), copper and rare earth metal oxides and alumina carriers interact closely and are highly uniformly dispersed. The highly dispersed Cu active component provides a large number of ethanol dehydrogenation activities or crotonaldehyde hydrogenation centers, and the highly dispersed rare earth metal oxides cooperate with the alumina carrier to provide a large number of acid-base active centers that promote acetaldehyde aldol condensation, thereby ultimately achieving efficient conversion of ethanol to higher alcohols. At the same time, the mutual doping and strong interaction between copper, rare earth metal M and aluminum oxides limit the sintering and growth of Cu and rare earth metal oxides, so that the catalyst shows excellent stability in a long-term evaluation of 500h.

[0027] In summary, the catalyst preparation method of the present invention is simple, effective and low-cost. When it is applied to the dehydrogenation condensation of ethanol to produce higher alcohols, a fixed-bed continuous reaction process is adopted. The process is simple and the reaction conditions are relatively mild. The yield of higher alcohols in the product can be as high as 37.7wt%. In particular, the catalyst has good stability and is suitable for industrial application. (IV) Description of the drawings

[0028] Figure 1 Schematic diagram of a fixed-bed reaction device for continuous catalytic conversion of ethanol to synthesize higher alcohols: 1-hydrogen cylinder, 2-nitrogen cylinder, 3-raw material bottle, 4-high-pressure constant flow pump, 5-three-way valve, 6-pressure reducing valve, 7-stop valve, 8-mass flow meter, 9-check valve, 10-reaction tube, 11-reaction furnace, 12-catalyst, 13-condenser, 14-condensed water, 15-back pressure valve, 16-collection tank.

[0029] Figure 2 High-resolution transmission electron microscopy (HRTEM) image (A), high-angle annular dark field scanning transmission (HAADF-STEM) image and corresponding element distribution image (B) of catalyst B prepared in Example 2 after reaction

[0030] Figure 3 X-ray diffraction (XRD) patterns of catalyst B prepared in Example 2 before and after the reaction: (a) before the reaction; (b) after the reaction.

[0031] Figure 4 The results of the stability test of the catalyst B prepared according to Example 2 in the fixed-bed continuous catalytic conversion of ethanol to synthesize higher alcohols; the reaction conditions are: temperature 260°C, pressure 3.0 MPa, liquid space velocity 2 mL / (h·g cat ), nitrogen / ethanol=250:1 (volume ratio).

[0032] Figure 5The stability test results of catalyst B prepared according to Example 2 and catalyst O prepared according to Comparative Example 3 in the fixed bed continuous catalytic conversion of ethanol to synthesize higher alcohols are compared; the reaction conditions are: temperature 260°C, pressure 3.0MPa, liquid space velocity 2mL / (h·g cat ), nitrogen / ethanol=250:1 (volume ratio). (V) Specific implementation methods

[0033] The present invention is further described below by means of specific embodiments, but the protection scope of the present invention is not limited thereto.

[0034] Example 1

[0035] At room temperature, 2.0 g P123 (EO 20 PO 70 EO 20 ) (0.00035 mol) was dissolved in 40 mL of anhydrous ethanol, and then 3.2 mL of 35 wt% hydrochloric acid (0.036 mol), 0.286 g of salicylic acid (0.0016 mol) and 0.2 g of citric acid (0.0010 mol) were added and stirred vigorously, and then 4.08 g of aluminum isopropoxide (0.02 mol), 0.0857 g of copper acetate (0.00047 mol) and 0.1616 g of lanthanum acetate (0.00051 mol) were added and stirred vigorously for 6 h to obtain a uniform mixed solution. The solvent was evaporated at 60 ° C for 24 h under air atmosphere, and then dried at 65 ° C for 48 h. Finally, the obtained dry sample was placed in a muffle furnace, and then the temperature was increased to 400 ° C at a rate of 1 ° C / min and calcined for 4 h, and then the temperature was continued to be increased to 700 ° C at a rate of 10 ° C / min and calcined for 1 h, and the catalyst A was obtained by natural cooling.

[0036] The above catalyst was loaded into a fixed bed reactor, the passage connecting the hydrogen bottle 1 to the reaction tube 10 was closed, and N2 was filled until the system pressure reached 3MPa, and then the reactor was heated to the reaction temperature of ethanol to higher alcohol (260°C or 300°C) at a rate of 10°C / min. At the same time, N2 was used as a carrier gas to carry the ethanol in the raw material bottle 3, which was preheated and then entered the reaction tube 10 to reduce the catalyst in situ. The liquid space velocity of ethanol was 2mL / (h·g cat ), the volume ratio of nitrogen to ethanol is 250:1. The material after the catalyst bed is cooled and collected by the condenser 13 and analyzed. When its composition is constant, it indicates that the catalyst reduction is completed. After the reduction is completed, the ethanol raw material is carried by N2 as a carrier gas and then enters the reaction tube for preheating to start the reaction. The liquid space velocity of ethanol is 2mL / (h·g cat ), the volume ratio of nitrogen to ethanol is 250:1. The reaction products after the catalyst bed and the unreacted ethanol are cooled and collected by the condenser 13 and analyzed.

[0037] Example 2

[0038] The preparation method of catalyst B is the same as that of Example 1, except that the amount of copper acetate added is 0.1429 g (0.00079 mol).

[0039] The reduction of catalyst B and the reaction method of ethanol to higher alcohols are the same as in Example 1.

[0040] from Figure 2 (A) The ordered mesoporous structure of catalyst B after the reaction can be clearly seen [Chem Eng J., 2017, 303, 1583-1592.], and no discernible Cu nanoparticles were found. Figure 2 In (B), the bright stripes correspond to the Al and O signals, which clearly form an ordered framework, while the Cu-K and La-L signals are evenly distributed on the ordered framework material. The above results indicate that the active components of copper and rare earth metal oxides are highly dispersed in the catalyst and are stable due to the strong interaction between the three oxides of copper, lanthanum and aluminum.

[0041] Figure 3 The XRD patterns of catalyst B before and after the reaction are shown in Figure 2. There are almost no obvious diffraction peaks on the XRD spectrum of the catalyst before the reaction, while there are no diffraction peaks of copper and lanthanum species in the XRD spectrum of catalyst B after the reaction, except for the γ-Al2O3 diffraction peak. Combining the results of HRTEM and HAADF-STEM analysis, it can be inferred that the three oxides in the one-pot evaporation-induced self-assembly synthesis method have a close interaction, thereby achieving a high dispersion of the active components in the catalyst and effectively preventing the aggregation and sintering of the active components.

[0042] In industrial applications, catalysts need to have not only good catalytic activity and selectivity for target products, but also good stability. Figure 4 As shown, catalyst B exhibited excellent stability in the 500 h continuous reaction evaluation, showing good prospects for industrial application.

[0043] Example 3

[0044] The preparation method of catalyst C is the same as that of Example 1, but the amount of copper acetate added is 0.1858 g (0.00102 mol).

[0045] The reduction of catalyst C and the reaction method of ethanol to higher alcohols are the same as in Example 1.

[0046] Example 4

[0047] The preparation method of catalyst D is the same as that of Example 1, except that the amount of copper acetate added is 0.2286 g (0.00126 mol).

[0048] The reduction of catalyst D and the reaction method of ethanol to higher alcohols are the same as in Example 1.

[0049] Example 5

[0050] The preparation method of catalyst E is the same as that of Example 1, except that the amount of lanthanum acetate added is 0.1347 g (0.00043 mol).

[0051] The reduction of catalyst E and the reaction method of ethanol to higher alcohols are the same as in Example 1.

[0052] Example 6

[0053] The preparation method of catalyst F is the same as that of Example 1, but the amount of lanthanum acetate added is 0.2155 g (0.00068 mol).

[0054] The reduction of catalyst F and the reaction method of ethanol to higher alcohols are the same as those in Example 1.

[0055] Example 7

[0056] The preparation method of catalyst G is the same as that of Example 2, but the amount of lanthanum acetate added is 0.2155 g (0.00068 mol).

[0057] The reduction of catalyst G and the reaction method of ethanol to higher alcohols are the same as in Example 1.

[0058] Example 8

[0059] At room temperature, 2.0 g P123 (EO 20 PO 70 EO 20 ) (0.00035 mol) was dissolved in 40 mL of anhydrous ethanol, and then 3.2 mL of 35 wt% hydrochloric acid (0.036 mol), 0.286 g of salicylic acid (0.0016 mol) and 0.2 g of citric acid (0.0010 mol) were added and stirred vigorously, and then 4.08 g of aluminum isopropoxide (0.02 mol), 0.1429 g of copper acetate (0.00079 mol) and 0.1623 g of cerium acetate (0.00051 mol) were added and stirred vigorously for 6 h to obtain a uniform mixed solution. The solvent was evaporated at 60 ° C for 24 h under air atmosphere, and then dried at 65 ° C for 48 h. Finally, the obtained dry sample was placed in a muffle furnace, heated to 400 ° C at a rate of 1 ° C / min and calcined for 4 h, and then continued to heat to 700 ° C at a rate of 10 ° C / min and calcined for 1 h, and naturally cooled to obtain catalyst H.

[0060] The reduction of catalyst H and the reaction method of ethanol to higher alcohols are the same as those in Example 1.

[0061] Example 9

[0062] At room temperature, 2.0 g P123 (EO 20 PO 70 EO 20 ) (0.00035 mol) was dissolved in 40 mL of anhydrous ethanol, and then 3.2 mL of 35 wt% hydrochloric acid (0.036 mol), 0.286 g of salicylic acid (0.0016 mol) and 0.2 g of citric acid (0.0010 mol) were added and stirred vigorously, and then 4.08 g of aluminum isopropoxide (0.02 mol), 0.1429 g of copper acetate (0.00079 mol) and 0.1866 g of samarium chloride (0.00051 mol) were added and stirred vigorously for 6 h to obtain a uniform mixed solution. The solvent was evaporated at 60 ° C for 24 h under air atmosphere, and then dried at 65 ° C for 48 h. Finally, the obtained dry sample was placed in a muffle furnace, heated to 400 ° C at a rate of 1 ° C / min and calcined for 4 h, and then continued to heat to 700 ° C at a rate of 10 ° C / min and calcined for 1 h, and naturally cooled to obtain catalyst I.

[0063] The reduction of catalyst I and the reaction method of ethanol to higher alcohols are the same as in Example 1.

[0064] Example 10

[0065] At room temperature, 2.0 g P123 (EO 20 PO 70 EO 20 ) (0.00035 mol) was dissolved in 40 mL of anhydrous ethanol, and then 3.2 mL of 35 wt% hydrochloric acid (0.036 mol), 0.286 g of salicylic acid (0.0016 mol) and 0.2 g of citric acid (0.0010 mol) were added and stirred vigorously, and then 4.08 g of aluminum isopropoxide (0.02 mol), 0.1429 g of copper acetate (0.00079 mol) and 0.1959 g of yttrium nitrate (0.00051 mol) were added and stirred vigorously for 6 h to obtain a uniform mixed solution. The solvent was evaporated at 60 ° C for 24 h under air atmosphere, and then dried at 65 ° C for 48 h. Finally, the obtained dry sample was placed in a muffle furnace, heated to 400 ° C at a rate of 1 ° C / min and calcined for 4 h, and then continued to heat to 700 ° C at a rate of 10 ° C / min and calcined for 1 h, and naturally cooled to obtain catalyst J.

[0066] The reduction of catalyst J and the reaction method of ethanol to higher alcohols are the same as those in Example 1.

[0067] Embodiment 11

[0068] At room temperature, 2.0 g P123 (EO 20 PO 70 EO 20) (0.00035 mol) was dissolved in 40 mL of anhydrous ethanol, and then 3.2 mL of 35 wt% hydrochloric acid (0.036 mol), 0.286 g of salicylic acid (0.0016 mol) and 0.2 g of citric acid (0.0010 mol) were added and stirred vigorously, and then 4.08 g of aluminum isopropoxide (0.02 mol), 0.1429 g of copper acetate (0.00079 mol) and 0.2225 g of praseodymium nitrate (0.00051 mol) were added and stirred vigorously for 6 h to obtain a uniform mixed solution. The solvent was evaporated at 60 ° C for 24 h under air atmosphere, and then dried at 65 ° C for 48 h. Finally, the obtained dry sample was placed in a muffle furnace, heated to 400 ° C at a rate of 1 ° C / min and calcined for 4 h, and then continued to heat to 700 ° C at a rate of 10 ° C / min and calcined for 1 h, and naturally cooled to obtain catalyst K.

[0069] The reduction of catalyst K and the reaction method of ethanol to higher alcohols are the same as those in Example 1.

[0070] Example 12

[0071] At room temperature, 2.0 g P123 (EO 20 PO 70 EO 20 ) (0.00035 mol) was dissolved in 40 mL of anhydrous ethanol, and then 3.2 mL of 68 wt% nitric acid (0.049 mol), 0.286 g of salicylic acid (0.0016 mol) and 0.2 g of citric acid (0.0010 mol) were added and stirred vigorously, and then 4.08 g of aluminum isopropoxide (0.02 mol), 0.1901 g of copper nitrate (0.00079 mol) and 0.1703 g of lanthanum nitrate (0.00051 mol) were added and stirred vigorously for 6 h to obtain a uniform mixed solution. The solvent was evaporated at 60 ° C for 24 h under air atmosphere, and then dried at 65 ° C for 48 h. Finally, the obtained dry sample was placed in a muffle furnace, heated to 400 ° C at a rate of 1 ° C / min and calcined for 4 h, and then continued to heat to 700 ° C at a rate of 10 ° C / min and calcined for 1 h, and naturally cooled to obtain catalyst L.

[0072] The reduction of catalyst L and the reaction method of ethanol to higher alcohols are the same as in Example 1.

[0073] Comparative Example 1

[0074] The preparation method of catalyst M is the same as that of Example 1, except that the amount of copper acetate added is 0.0286 g (0.00016 mol).

[0075] The reduction of catalyst M and the reaction method of ethanol to higher alcohols are the same as those in Example 1.

[0076] Comparative Example 2

[0077] The preparation method of catalyst N is the same as that of Example 1, except that the amount of copper acetate added is 0.2858 g (0.00157 mol).

[0078] The reduction of catalyst N and the reaction method of ethanol to higher alcohols are the same as those in Example 1.

[0079] Comparative Example 3

[0080] At room temperature, 2.0 g P123 (EO 20 PO 70 EO 20 ) (0.00035 mol) was dissolved in 40 mL of anhydrous ethanol, and then 3.2 mL of 35 wt% hydrochloric acid (0.036 mol), 0.286 g of salicylic acid (0.0016 mol) and 0.2 g of citric acid (0.0010 mol) were added and stirred vigorously, and then 4.08 g of aluminum isopropoxide (0.02 mol) was added and stirred vigorously for 6 h to obtain a uniform mixed solution. The solvent was evaporated at 60 ° C for 24 h under an air atmosphere, and then dried at 65 ° C for 48 h. Finally, the obtained dry sample was placed in a muffle furnace, heated to 400 ° C at a rate of 1 ° C / min and calcined for 4 h, and then continued to heat to 700 ° C at a rate of 10 ° C / min and calcined for 1 h, and naturally cooled to obtain an ordered mesoporous alumina carrier.

[0081] 0.1901g copper nitrate (0.00079mol) and 0.2214g lanthanum nitrate (0.00051mol) were dissolved in 5ml anhydrous ethanol to obtain a precursor solution, and then the ordered mesoporous alumina support was poured into the precursor solution, dried in the shade at room temperature, and then dried in an oven at 110°C for 4h. The dried solid was then calcined at 450°C in a muffle furnace at a rate of 10°C / min for 3h, and then cooled naturally to obtain catalyst O.

[0082] The reduction of catalyst O and the reaction method of ethanol to higher alcohols are the same as in Example 1.

[0083] according to Figure 5 It can be seen that the catalytic activity of catalyst O shows a clear downward trend. At the 200th hour, the yield of higher alcohols dropped to 36.1%, which is lower than the 37.3% of catalyst B. In addition, the activity of catalyst B did not drop significantly during the 500-hour reaction, further proving the excellent stability of catalyst B.

[0084] The reaction conditions and results are shown in Table 1.

[0085] Table 1 Reaction results of different catalysts in fixed bed ethanol continuous dehydrogenation condensation to produce higher alcohols

[0086]

[0087]

Claims

1. A method for preparing an ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst, characterized in that The catalyst is prepared as follows: The template agent is dissolved in anhydrous ethanol, and inorganic strong acid, salicylic acid and citric acid are added and mixed; soluble salts of copper, soluble salts of rare earth metals and soluble salts of aluminum are added and mixed; the solvent is evaporated at 25-80°C for 1-72 hours, and then dried at 60-120°C for 2-96 hours; the obtained mixture is heated to 350-550°C at a rate of 1-10°C / min in a muffle furnace and roasted for 2-10 hours, and then further heated to 600-800°C at a rate of 10-30°C / min and roasted for 0.5-6 hours to obtain the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst; the template agent is a triblock polymer surfactant, and the rare earth metal in the soluble salt of the rare earth metal is one or a mixture of two or more of La, Ce, Sm and Pr; The amount of aluminum in the soluble salt of aluminum is calculated based on the theoretical mass of aluminum oxide completely generated from the soluble salt of aluminum, and the ratio of the amount of the template, the hydrogen ions in the inorganic strong acid, salicylic acid, citric acid to the amount of aluminum in the soluble salt of aluminum is 0.015-0.02:1-5:0.05-0.1:0.03-0.08:1; The masses of the soluble salts of copper, rare earth metals and aluminum are respectively calculated based on the theoretical mass of copper soluble salts completely generating copper oxide, rare earth metal soluble salts completely generating rare earth metal oxides and aluminum soluble salts completely generating aluminum oxide. The mass of copper oxide is 2.5-8.5% of the mass of the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst; the mass of the rare earth metal oxide is 3-15% of the mass of the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst; the mass of the aluminum oxide is 76.5-94.5% of the mass of the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst.

2. The method for preparing the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst according to claim 1, characterized in that: The volume of the anhydrous ethanol is 2-20 mL / g based on the mass of the soluble salt of aluminum.

3. The method for preparing the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst according to claim 1, characterized in that: The soluble copper salt is one of copper acetate, copper nitrate and copper chloride or a mixture of several of them.

4. The method for preparing the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst according to claim 1, characterized in that: The rare earth metal in the soluble salt of the rare earth metal is one or a mixture of two or more rare earth metals.

5. The method for preparing the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst according to claim 1, characterized in that: The soluble salt of the rare earth metal is one or a mixture of acetate, nitrate and chloride of the rare earth metal.

6. The method for preparing the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst according to claim 1, characterized in that: The soluble aluminum salt is one or a mixture of aluminum nitrate, aluminum isopropoxide, and aluminum chloride.

7. The method for preparing the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst according to claim 1, characterized in that: The template is one of P123 and F127 or a mixture of several of them.

8. The method for preparing the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst according to claim 1, characterized in that: The inorganic strong acid is one of hydrogen chloride or nitric acid or a mixture of the two.

9. Use of the ordered mesoporous copper-rare earth metal-aluminum composite oxide catalyst prepared by the preparation method according to claim 1 in the reaction of ethanol dehydrogenation condensation to produce higher alcohols.

10. The use according to claim 9, characterized in that The application is as follows: in a fixed bed reactor, the temperature is 150-300°C, the reaction pressure is normal pressure-4.0MPa, nitrogen and ethanol are introduced, and the liquid space velocity is 0.5-5mL / (h·g cat ), the volume ratio of nitrogen to ethanol is 100 to 600:1, and the ethanol is dehydrogenated and condensed to produce higher alcohols.