Y / SSZ-13 / rare earth / ASA composite material, hydrocracking catalyst, catalyst carrier, and preparation method thereof

By preparing a Y/SSZ-13/rare earth/ASA composite material as a hydrocracking catalyst, the problems of narrow pores in existing catalysts leading to difficulty in feedstock entry and slow product diffusion were solved, achieving high-activity and selective hydrocracking effects and improving the yield and quality of jet fuel.

CN114130427BActive Publication Date: 2024-11-01PETROCHINA CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202010925489.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-09-04
Publication Date
2024-11-01
Estimated Expiration
2040-09-04

AI Technical Summary

Technical Problem

Existing hydrocracking catalysts, when processing straight-run diesel, suffer from problems such as small pore size and narrow, elongated channels, which make it difficult for reactants to enter the pores, reduce the utilization rate of acidic sites inside the molecular sieve channels, affect the diffusion of reaction products, result in low distillate oil yield, and low product octane number.

Method used

Y-type molecular sieve, SSZ-13 molecular sieve, rare earth elements, and amorphous silica-alumina were used as cracking centers to prepare a Y/SSZ-13/rare earth/ASA composite material by stepwise precipitation method. This formed a microporous-mesoporous structure, and the synergistic catalytic effect of each component improved the cracking activity and isomerization performance.

Benefits of technology

It achieves high catalyst activity and selectivity, and is suitable for producing high-quality jet fuel from straight-run diesel hydrocracking, thereby improving the yield and quality of jet fuel components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0002665935560000181
    Figure BDA0002665935560000181
  • Figure BDA0002665935560000191
    Figure BDA0002665935560000191
  • Figure BDA0002665935560000192
    Figure BDA0002665935560000192
Patent Text Reader

Abstract

The invention provides a Y / SSZ-13 / rare earth / ASA composite material and a preparation method thereof, a hydrocracking catalyst carrier and a preparation method thereof, a hydrocracking catalyst and a preparation method thereof, and the Y / SSZ-13 / rare earth / ASA composite material comprises the following steps: step 1, mixing a Y molecular sieve, an SSZ-13 molecular sieve, an aluminum source, an alkaline compound and water, heating and stirring; step 2, adding a silicon source and a rare earth precursor to the mixture of step 1, heating and stirring, and obtaining a Y / SSZ-13 / rare earth / ASA composite material. The catalyst prepared by the composite material of the present invention is suitable for a process of hydrocracking straight-run diesel to produce more aviation kerosene.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of oil refining catalysts, and specifically relates to a Y / SSZ-13 / rare earth / ASA composite material and a preparation method thereof, a hydrocracking catalyst carrier and a preparation method thereof, and a hydrocracking catalyst and a preparation method thereof. Background Art

[0002] As the scale of the international air transport industry continues to expand, the global demand for jet fuel has increased year by year, with an annual growth rate of about 5.0%, far higher than the annual growth rate of gasoline and diesel of 1.0% to 1.5%, which has greatly driven the demand for high-quality jet fuel products in the global oil market. China's domestic air transport industry showed a good development momentum in 2019. Against the backdrop of the overall slowdown in the growth rate of demand in the refined oil market, the jet fuel market still maintained a trend of strong supply and demand and rapid growth. According to data from the National Bureau of Statistics, China's kerosene consumption in 2019 was 36.84 million tons, an increase of 6.4% over the previous year. In 2019, the number of airports in China was close to 270, and by 2025, the total number of airports planned and laid out will reach 370. In the next five years, the civil aviation industry will still be in an upward period. By 2025, China's civil aviation kerosene demand will reach about 49.37 million tons, with an annual compound growth rate of 5%. This will greatly promote oil refining companies to produce more jet fuel products to meet market demand, and will also greatly promote the rapid development of jet fuel production technology. China's existing jet fuel production technologies mainly include straight-run jet fuel hydrorefining technology and hydrocracking technology. Jet fuel products have more profit advantages than diesel or gasoline products, which has greatly promoted major oil refineries to increase the production of jet fuel products. However, their output is restricted by the properties of the processed crude oil and the characteristics of the two jet fuel production technologies and cannot meet market demand.

[0003] At present, the distribution of oil products in my country is uneven and it is difficult to upgrade the quality of oil products. Changing the distribution of oil products and improving the quality of oil products by developing new processes, new catalysts, optimizing production plans, etc. has become the only way for refining and chemical companies to achieve efficient development. Hydrocracking technology has the advantages of flexible production plans, strong raw material adaptability, high selectivity of target products, and good product quality. Its importance is becoming increasingly prominent and its industrial applications are becoming increasingly widespread.

[0004] Generally, hydrocarbon molecules in straight-run diesel have a large carbon number, paraffins have a high freezing point, and cyclic hydrocarbons have a low smoke point. Hydrogenation conversion catalysts are required to have strong isomerization and cracking properties, which can convert components with higher freezing points in the raw materials into products with low freezing points and maintain a high yield of jet fuel products. In addition, hydrocracking catalysts also need to have strong aromatic hydrogenation saturation and ring opening capabilities so that the smoke point and naphthalene content of jet fuel products can meet the requirements of jet fuel quality indicators. Therefore, the selection of hydrocracking catalyst system is crucial.

[0005] The core of hydrocracking technology is hydrocracking catalyst. Hydrocracking catalyst is a bifunctional catalyst composed of a hydrogenation component with hydrogenation function and an acidic component with cracking function. The hydrogenation function is usually provided by a metal with hydrogenation function, which plays a role of hydrogenation / dehydrogenation in the reaction process, provides reaction raw materials for the acid center, and saturates the acid center products in time to prevent deep cracking. The cracking component is mainly provided by acidic amorphous silica-alumina or zeolite molecular sieves. The cracking components of the currently industrialized hydrocracking catalyst are usually mainly molecular sieves and amorphous silica-alumina. Among molecular sieves, Y molecular sieve is the most used. Y-type molecular sieve has the characteristics of strong acidity, good structural stability, good activity, high cracking performance, strong ring-opening performance, etc., but it has problems such as small pore size and narrow and slender pores. It is difficult for reaction raw materials such as large molecular organic matter to enter the pores, which will reduce the utilization rate of acidic sites inside the molecular sieve pores. At the same time, the narrow and slender pores will increase the diffusion resistance, affect the rapid diffusion and overflow of the reaction products, and lead to low distillate oil yields and low product octane numbers.

[0006] Although hydrocracking catalysts containing single cracking components have their own advantages, their disadvantages are also obvious. Catalysts containing composite cracking components can integrate their respective advantages, thereby improving both reaction activity and the yield of target products.

[0007] US6174429 discloses a hydrocracking catalyst, which contains 1-99wt% of at least one acidified aluminum-containing amorphous matrix, 0.1-80wt% of a Y-type molecular sieve with a unit cell parameter of 2.438nm, a SiO2 / Al2O3 chemical molar ratio of about 8, and a SiO2 / Al2O3 skeleton molar ratio of about 20, 0.1-30wt% of at least a metal component of Group VIII, 1-40wt% of at least one metal component of Group VIB, 0.1-20wt% of an auxiliary agent, and 0-20wt% of at least one metal element of Group VIIA. The catalyst adopts a preparation method of first preparing a carrier and then loading a hydrogenation metal. The catalyst has good activity and stability, but the yield of heavy naphtha and jet fuel is not high.

[0008] CN94117759.9 discloses a light oil type hydrocracking catalyst, the catalyst composition is low sodium high silicon Y type molecular sieve (prepared according to CN90102645.X) 50-65wt%, small pore alumina 10-26wt%, WO3 18-26wt%, NiO 4-6wt%. Its preparation method is to mix low sodium high silicon Y molecular sieve and small pore alumina and then extrude them into strips, the molded product is treated at high temperature in an ammonia-water vapor atmosphere, and the carrier is impregnated with a mixed solution containing tungsten and nickel after treatment, dried, and roasted to obtain the finished catalyst. The catalyst prepared by this technology has high cracking activity, but the liquid yield is low.

[0009] CN1393521A discloses a hydrocracking catalyst, which comprises 20-50 wt% amorphous silicon-alumina, 25-35 wt% alumina, and 10-30 wt% composite zeolite, wherein the composite zeolite comprises 30-90 wt% Y zeolite and 10-70 wt% ZSM-5 zeolite. The preparation method is to mechanically mix Y zeolite with ZSM-5 zeolite, and then add a mixture containing H + and NH 3+ The cation solution is treated, the treated composite zeolite is mechanically mixed with amorphous silicon aluminum and alumina, extruded into strips, dried and calcined, and the carrier is impregnated with a mixed solution containing tungsten and nickel, dried and calcined to obtain a catalyst. The catalyst has the advantages of flexible production plan and strong raw material adaptability, but its catalyst pore volume is small and the light oil yield is low.

[0010] Therefore, there is still a need in the art to conduct further research on hydrocracking catalysts, especially hydrocracking catalysts for producing more jet fuel. Summary of the invention

[0011] The main purpose of the present invention is to provide a Y / SSZ-13 / rare earth / ASA composite material and a preparation method thereof, a hydrocracking catalyst carrier and a preparation method thereof, a hydrocracking catalyst and a preparation method thereof. The Y / SSZ-13 / rare earth / ASA composite material has a microporous-mesoporous structure. The catalyst prepared from the composite material has strong adaptability to raw materials, has high cracking activity and isomerization performance, and is suitable for the hydrocracking process of using straight-run diesel as raw material to produce more aviation kerosene.

[0012] In order to achieve the above object, the present invention provides a method for preparing a Y / SSZ-13 / rare earth / ASA composite material, comprising the following steps:

[0013] Step 1, mixing Y molecular sieve, SSZ-13 molecular sieve, aluminum source, alkaline compound and water, heating and stirring;

[0014] Step 2: adding the silicon source and the rare earth precursor to the mixture of step 1, heating and stirring, to obtain a Y / SSZ-13 / rare earth / ASA composite material.

[0015] The preparation method of the Y / SSZ-13 / rare earth / ASA composite material of the present invention, wherein the step 1 is: dispersing the Y molecular sieve and the SSZ-13 molecular sieve in water, heating, then adding the aqueous solution of the aluminum source and the aqueous solution of the alkaline compound, and continuing heating and stirring.

[0016] The preparation method of the Y / SSZ-13 / rare earth / ASA composite material of the present invention, wherein the step 2 is: firstly adding the silicon source into the mixture of step 1, heating and stirring, and then adding the rare earth precursor.

[0017] In the method for preparing the Y / SSZ-13 / rare earth / ASA composite material of the present invention, the silicon source and the rare earth precursor are added to the mixture in step 1 in the form of aqueous solutions.

[0018] The method for preparing the Y / SSZ-13 / rare earth / ASA composite material of the present invention further comprises filtering, washing, drying and calcining steps after the heating and stirring in step 2.

[0019] The preparation method of the Y / SSZ-13 / rare earth / ASA composite material of the present invention, wherein the mass ratio of the Y molecular sieve to the SSZ-13 molecular sieve is 5-95:95-5; and / or the specific surface area of ​​the Y molecular sieve is 300-900m 2 / g, a total pore volume of 0.3-0.6 mL / g, a skeleton SiO2 / Al2O3 molar ratio of 5-20, and a relative crystallinity of 80-100%; the SiO2 / Al2O3 molar ratio of the SSZ-13 molecular sieve is 20-100, and the specific surface area is 200-500 m 2 / g, and the total pore volume is 0.4~0.8mL / g.

[0020] The preparation method of the Y / SSZ-13 / rare earth / ASA composite material of the present invention comprises the following steps: the aluminum source is an acidic aluminum source, which is one or more of aluminum sulfate, aluminum nitrate, and aluminum chloride; the alkaline compound is one or more of ammonia water, sodium hydroxide, potassium hydroxide, sodium carbonate, and ammonium carbonate; the silicon source is an alkaline silicon source; the rare earth precursor is one or more of rare earth chloride and rare earth nitrate; and the heating temperature in step 1 and the heating temperature in step 2 are both 60 to 90°C.

[0021] The preparation method of the Y / SSZ-13 / rare earth / ASA composite material of the present invention, wherein the mass content of the aluminum source in the aqueous solution of the aluminum source in terms of Al2O3 is 1 to 4 wt%; the mass content of the alkaline compound in the aqueous solution of the alkaline compound is 5 to 15 wt%.

[0022] The preparation method of the Y / SSZ-13 / rare earth / ASA composite material of the present invention comprises the following steps: the mass content of the silicon source in terms of SiO2 in the aqueous solution formed by the silicon source is 5 to 20 wt%; the mass content of the rare earth precursor in the aqueous solution formed by the rare earth precursor is 1 to 20 wt%.

[0023] In order to achieve the above-mentioned purpose, the present invention also provides a Y / SSZ-13 / rare earth / ASA composite material. Based on the total weight of the composite material, in the composite material, amorphous silicon aluminum accounts for 10-80wt%, molecular sieve accounts for 80-10wt%, and rare earth oxide accounts for 0.1-10%; based on the total weight of the molecular sieve, in the molecular sieve, Y molecular sieve accounts for 5-95wt%, and SSZ-13 molecular sieve accounts for 95-5wt%; the mass ratio of molecular sieve, aluminum source, alkaline compound, silicon source and rare earth precursor is: molecular sieve: Al2O3: alkaline compound: SiO2: rare earth precursor = (5-30): (5-10): (30-100): 10: (0.5-4), and the molecular sieve includes Y molecular sieve and SSZ-13 molecular sieve.

[0024] The Y / SSZ-13 / rare earth / ASA composite material of the present invention is prepared by a step-by-step precipitation method; the specific surface area of ​​the Y / SSZ-13 / rare earth / ASA composite material is 300-600 m 2 / g, a pore volume of 0.3-2.0 mL / g, an average pore diameter of 5-15 nm, and / or an infrared ester content of 100-500 μmol / g.

[0025] In order to achieve the above object, the present invention further provides a hydrocracking catalyst carrier, which includes the above Y / SSZ-13 / rare earth / ASA composite material.

[0026] In order to achieve the above object, the present invention further provides a method for preparing a hydrocracking catalyst carrier, which comprises the method for preparing the above Y / SSZ-13 / rare earth / ASA composite material.

[0027] In order to achieve the above object, the present invention further provides a hydrocracking catalyst, which comprises a carrier and an active component, wherein the carrier is the above hydrocracking catalyst carrier.

[0028] In order to achieve the above object, the present invention further provides a method for preparing a hydrocracking catalyst, the hydrocracking catalyst comprises a carrier and an active component, and the preparation method comprises the preparation method of the above Y / SSZ-13 / rare earth / ASA composite material.

[0029] In order to achieve the above object, the present invention provides the use of the above hydrocracking catalyst in oil processing to produce aviation kerosene.

[0030] Beneficial effects of the present invention:

[0031] The present invention adopts Y-type molecular sieve, SSZ-13 molecular sieve, rare earth and amorphous silicon aluminum as the cracking center, which not only gives full play to the performance of the cracking components, but also enables them to produce a synergistic catalytic effect. That is, the Y-type molecular sieve has a high ring-opening selectivity for aromatic hydrocarbons and a strong cracking selectivity for long-chain alkanes and alkenes; the SSZ-13 molecular sieve has good isomerization and shape selection performance; the amorphous silicon aluminum has the characteristics of good selectivity, high liquid yield, low hydrogen consumption and small product distribution changes during the operation cycle. Moreover, amorphous silicon aluminum has a dispersing effect on the Y-type molecular sieve and the SSZ molecular sieve, so that the molecular sieve particles are far apart, so that the product after the cracking of the crude oil molecules on the Y-type molecular sieve diffuses to the surface of the SSZ-13, and the isomerization and shape selection reactions occur on the surface of the SSZ-13 molecular sieve, producing more lighter components in the aviation kerosene components. At the same time, rare earth combines with amorphous silicon aluminum to improve the acidity of amorphous silicon aluminum, making amorphous silicon aluminum have a certain cracking activity, and the shallow cracking products on the amorphous silicon aluminum also diffuse to the surface of SSZ-13 to undergo isomerization and shape-selective reactions, generating more heavier components in the aviation kerosene components. In this way, the components of the catalyst prepared by the present invention cooperate with each other, so that the catalyst has high activity and good selectivity, and can be used in the process of producing high-quality aviation kerosene by hydrocracking of straight-run diesel. DETAILED DESCRIPTION

[0032] The following is a detailed description of the embodiments of the present invention. The embodiments are implemented based on the technical solution of the present invention, and detailed implementation methods and processes are given. However, the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments where specific conditions are not specified are usually based on conventional conditions.

[0033] The present invention provides a method for preparing a Y / SSZ-13 / rare earth / ASA composite material, comprising the following steps:

[0034] Step 1, mixing Y molecular sieve, SSZ-13 molecular sieve, aluminum source, alkaline compound and water, heating and stirring;

[0035] Step 2: adding the silicon source and the rare earth precursor to the mixture of step 1, heating and stirring, to obtain a Y / SSZ-13 / rare earth / ASA composite material.

[0036] The present invention adopts Y-type molecular sieve, SSZ-13 molecular sieve, rare earth and amorphous silicon aluminum as cracking centers, and the composite material prepared by the step-by-step precipitation method has a microporous-mesoporous structure. Among them, although the SSZ-13 molecular sieve is a small-pore molecular sieve, it has a significant isomerization function in the cracking reaction of heavy oil molecules, especially in the reaction of diesel hydrocracking to produce more aviation kerosene, and it shows a good effect. The SSZ-13 molecular sieve is combined with the Y-type molecular sieve, rare earth and amorphous silicon aluminum, which not only gives full play to the performance of several cracking components, but also enables the cracking components to produce synergistic catalytic effects with each other, thereby making the catalyst prepared by the composite material have higher activity and selectivity.

[0037] In one embodiment, the present invention has no special requirements on the crystals of the Y molecular sieve, and the Y molecular sieve can be a commercial Y molecular sieve of any crystal size. In another embodiment, the specific surface area of ​​the Y molecular sieve is 300 to 900 m 2 / g, the total pore volume is 0.3-0.6mL / g, the molar ratio of framework SiO2 / Al2O3 is 5-20, and the relative crystallinity is 80-100%. The present invention has no special requirements for the crystal grains of SSZ-13 molecular sieve, and it can be a commercial SSZ-13 molecular sieve of any crystal grain size. In another embodiment, the molar ratio of SiO2 / Al2O3 in SSZ-13 molecular sieve is 20-100, and the specific surface area is 200-500m 2 / g, and the total pore volume is 0.4-0.8 mL / g. In another embodiment, the mass ratio of Y molecular sieve to SSZ-13 molecular sieve is 5-95:95-5. The present invention does not particularly limit the preparation method of Y molecular sieve and SSZ-13 molecular sieve.

[0038] In one embodiment, the aluminum source is an acidic aluminum source, and further, the aluminum source can be one or more of aluminum sulfate, aluminum nitrate, and aluminum chloride. The alkaline compound is an inorganic base, such as one or more of ammonia water, sodium hydroxide, potassium hydroxide, sodium carbonate, and ammonium carbonate.

[0039] In one embodiment, step 1 is to disperse the Y molecular sieve and the SSZ-13 molecular sieve in water, heat it, then add the aqueous solution of the aluminum source and the aqueous solution of the alkaline compound, and continue heating and stirring. The heating temperature is, for example, 60 to 90°C.

[0040] In another embodiment, step 1 is to disperse the Y-type molecular sieve and SSZ-13 in water, heat to 60-90°C, and stir at a constant temperature for 1-8 hours to obtain a slurry of a mixture of the Y-type molecular sieve and the SSZ-13 molecular sieve; then add an aqueous solution of an aluminum source, and then add an aqueous solution of an alkaline compound, the addition time is, for example, 30min-8h, and then keep at 60-90°C for 0-8h to precipitate and obtain an aluminum sol. Wherein, the mass ratio of Y molecular sieve: SSZ-13 molecular sieve: water is 5-95:95-5:10-100. The mass content of the aluminum source in the aqueous solution of the aluminum source in terms of Al2O3 is, for example, 1-4wt%, and the mass content of the alkaline compound in the aqueous solution of the alkaline compound is, for example, 5-15wt%.

[0041] The present invention does not impose any particular limitation on the amount of aluminum source, as long as the amorphous silicon aluminum in the prepared Y / SSZ-13 / rare earth / ASA composite material accounts for 10-80 wt%. In one embodiment, the amount of the alkaline compound is such that the pH value of the mixed slurry is 7.5-10.0.

[0042] In one embodiment, step 2 is: first add the silicon source to the mixture of step 1, heat and stir, and then add the rare earth precursor. In another embodiment, step 2 is: under stirring and heating conditions, add the solution formed by the silicon source to the mixture of step 1, the addition time is 30min-10h, after adding the silicon source solution, keep it at 60-90°C for 0-8h, and then add the solution formed by the rare earth precursor. Then filter, wash, dry and calcine to obtain the Y / SSZ-13 / rare earth / ASA composite material.

[0043] In one embodiment, the silicon source is an alkaline silicon source, and further is water glass. The rare earth precursor is one or more of rare earth chloride and rare earth nitrate, and further is one or more of lanthanum chloride, cerium chloride, lanthanum nitrate, and cerium nitrate.

[0044] The present invention does not impose any particular limitation on the amount of silicon source, as long as the amorphous silicon aluminum accounts for 10-80 wt% in the prepared Y / SSZ-13 / rare earth / ASA composite material. The amount of rare earth precursor used should be such that the rare earth oxide accounts for 0.1-10% of the composite material based on the total weight of the composite material.

[0045] In one embodiment, the mass content of the silicon source in the silicon source solution is 5-20wt% in terms of SiO2; the mass content of the rare earth precursor in the aqueous solution formed by the rare earth precursor is 1-20wt%. In another embodiment, the aluminum source of the present invention is calculated as Al2O3, the silicon source is calculated as SiO2, and the mass ratio of the molecular sieve, the aluminum source, the alkaline compound, the silicon source and the rare earth precursor is: molecular sieve: Al2O3: alkaline compound: SiO2: rare earth precursor = (5-30): (5-10): (30-100): 10: (0.5-4), wherein the molecular sieve includes Y molecular sieve and SSZ-13 molecular sieve.

[0046] Thus, the present invention can obtain a Y / SSZ-13 / rare earth / ASA composite material through the above method. The composite material has a micro-mesoporous structure. Based on the total weight of the composite material, the amorphous silicon aluminum accounts for 10-80wt%, the molecular sieve accounts for 80-10wt%, and the rare earth oxide accounts for 0.1-10%; based on the total weight of the molecular sieve, the Y molecular sieve accounts for 5-95wt%, and the SSZ-13 molecular sieve accounts for 95-5wt%. The specific surface area of ​​the Y / SSZ-13 / rare earth / ASA composite material is 300-600m 2 / g, the pore volume is 0.3-2.0 mL / g, the average pore diameter is between 5-15 nm, the molar ratio of silicon to aluminum is 0.1-10 and / or the infrared acid content is 100-500 μmol / g.

[0047] The Y / SSZ-13 / rare earth / ASA composite material is kneaded, molded, dried and calcined with a binder, an extrusion aid and the like to obtain a hydrocracking catalyst carrier. The present invention does not particularly limit the preparation method of the catalyst carrier, and conventional carrier preparation methods in the art may be used.

[0048] Then, the hydrocracking catalyst carrier is loaded with the active component to obtain the hydrocracking catalyst. The present invention does not specifically limit the loading method, for example, it can be loaded by impregnation. The hydrocracking catalyst thus obtained has a specific surface area of ​​200 to 400 m 2 / g, the pore volume is 0.6~1.0mL / g, the average pore diameter is 8.0~13.0nm, and the infrared acid content is 100~500μmol / g.

[0049] The catalyst prepared by the invention has high activity and good selectivity, and can be used in the process of producing high-quality aviation kerosene by hydrocracking of straight-run diesel.

[0050] In order to better illustrate the present invention, the present invention is further described below in conjunction with specific embodiments. However, the scope of the present invention is not limited to the scope of these embodiments. The analysis method of the present invention: specific surface area, pore volume, and pore size are measured by low-temperature liquid nitrogen physical absorption method, relative crystallinity and skeleton silicon-aluminum ratio are measured by X-ray diffraction method, silicon-aluminum molar ratio is measured by chemical method, and infrared acid content is measured by pyridine infrared. In the present invention, wt% is mass percentage.

[0051] Example 1

[0052] (1) According to the addition amount of molecular sieve that accounts for 50wt% of the weight of the composite material, 19g of Y-type molecular sieve with a silicon-aluminum ratio of 7.5 and 1g of SSZ-13 with a silicon-aluminum ratio of 20 were weighed and added into the reactor.

[0053] (2) Solid aluminum sulfate was prepared into 500 mL of aluminum sulfate solution with a concentration of 20 g Al2O3 / L (A), concentrated ammonia water was diluted into a 10 wt% dilute ammonia solution by adding an appropriate amount of deionized water (B), and concentrated water glass solution was diluted into 72 mL of a 14 wt% water glass solution by adding an appropriate amount of deionized water (C). 2 g of cerium nitrate (Ce(NO3)3·6H2O) was added to 10 mL of water to obtain a solution with a CeO2 content of 6.61% (D).

[0054] (3) Add 100 mL of deionized water to the reactor and heat to 75° C. Then add (A) and (B) to make the mixed slurry have a pH of 8.0 and gel for 60 minutes. After the addition is completed, keep the temperature unchanged and age for 60 minutes.

[0055] (4) After aging, (C) is added to the mixture of step (3), keeping the temperature unchanged. After the feeding is completed, aging is carried out at the same temperature for 60 minutes.

[0056] (5) Add solution (D) to the slurry of step (4), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0057] (6) The slurry of step (5) was filtered, washed, dried at 120° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a composite material. The texture properties and acid properties of the composite material are shown in Table 1.

[0058] (7) 40 g of the composite material was added into a container, and water was added. Then, 4.7 g of aluminum sol and 2.4 g of sesbania powder were added, mixed, extruded, dried at 120° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a carrier.

[0059] (8) The carrier was impregnated with an impregnation solution prepared with equal volumes of 13.4 g of ammonium metatungstate and 6.7 g of nickel nitrate for 12 hours, dried at 50° C. for 4 hours, dried at 120° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a hydrocracking catalyst.

[0060] The textural properties and acid properties of the catalysts are shown in Table 2.

[0061] Example 2

[0062] (1) According to the addition amount of molecular sieves accounting for 50wt% of the weight of the composite material, 14g of Y-type molecular sieve with a silicon-aluminum ratio of 10 and 6g of SSZ-13 molecular sieve with a silicon-aluminum ratio of 50 were weighed and added into the reactor.

[0063] (2) Solid aluminum sulfate was prepared into 500 mL of aluminum sulfate solution with a concentration of 20 g Al2O3 / L (A), concentrated ammonia was diluted into a 10 wt% dilute ammonia solution by adding an appropriate amount of deionized water (B), and concentrated water glass solution was diluted into 72 mL of a 14 wt% water glass solution by adding an appropriate amount of deionized water (C). 2 g of lanthanum nitrate (La(NO3)3·6H2O) was added to 10 mL of water to obtain a solution with a La2O3 content of 3.76% (D).

[0064] (3) Add 100 mL of deionized water to the reactor and heat to 75° C. Then add (A) and (B) to make the pH of the mixed slurry 8.5 and gel for 30 minutes. After the addition is completed, keep the temperature unchanged and age for 60 minutes.

[0065] (4) Add solution (C) to the slurry of step (3), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0066] (5) Add solution (D) to the slurry of step (4), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0067] (6) The slurry of step (5) was filtered, washed, dried at 120° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a composite material. The texture properties and acid properties of the composite material are shown in Table 1.

[0068] (7) The steps for preparing the catalyst are the same as steps (7) and (8) of Example 1. The textural properties and acid properties of the catalyst are shown in Table 2.

[0069] Example 3

[0070] (1) According to the addition amount of molecular sieves accounting for 50wt% of the weight of the composite material, 10g of Y-type molecular sieve with a silicon-aluminum ratio of 12.5 and 10g of SSZ-13 with a silicon-aluminum ratio of 40 were weighed and added into the reactor.

[0071] (2) Solid aluminum sulfate was prepared into 500 mL of aluminum sulfate solution with a concentration of 20 g Al2O3 / L (A), concentrated ammonia was diluted into a 10 wt% dilute ammonia solution by adding an appropriate amount of deionized water (B), and concentrated water glass solution was diluted into 72 mL of a 14 wt% water glass solution by adding an appropriate amount of deionized water (C). 10 g of cerium nitrate (Ce(NO3)3·6H2O) was added to 50 mL of water to obtain a solution with a CeO2 content of 6.61% (D).

[0072] (3) Add 100 mL of deionized water to the reactor and heat to 75° C. Then add (A) and (B) to make the mixed slurry have a pH of 9.0 and gel for 90 minutes. After the addition is completed, keep the temperature unchanged and age for 50 minutes.

[0073] (4) Add solution (C) to the slurry of step (3), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0074] (5) Add solution (D) to the slurry of step (4), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0075] (6) The slurry of step (5) was filtered, washed, dried at 110° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a composite material. The texture properties and acid properties of the composite material are shown in Table 1.

[0076] (7) The steps for preparing the catalyst are the same as steps (7) and (8) of Example 1. The textural properties and acid properties of the catalyst are shown in Table 2.

[0077] The textural properties and acid properties of the catalysts are shown in Table 2.

[0078] Example 4

[0079] (1) According to the addition amount that the total weight of the molecular sieve accounts for 50wt% of the weight of the composite material, 6g of Y-type molecular sieve with a silicon-aluminum ratio of 15 and 14g of SSZ-13 with a silicon-aluminum ratio of 100 were weighed and added into the reactor.

[0080] (2) Solid aluminum sulfate was prepared into 500 mL of an aluminum sulfate solution with a concentration of 20 g Al2O3 / L (A), concentrated ammonia water was added with an appropriate amount of deionized water to dilute it into an 8 wt% dilute ammonia solution (B), concentrated water glass solution was added with an appropriate amount of deionized water to dilute it into 100 mL of a 10 wt% water glass solution (C), 5 g of cerium nitrate (Ce(NO3)3·6H2O) was taken and added to 50 mL of water to obtain a solution with a CeO2 content of 3.36% (D).

[0081] (3) Add 100 mL of deionized water to the reactor and heat to 75° C. Then add (A) and (B) to make the mixed slurry have a pH of 8.2 and gel for 150 min. After the addition is completed, keep the temperature unchanged and age for 60 min.

[0082] (4) Add solution (C) to the slurry of step (3), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0083] (5) Add solution (D) to the slurry of step (4), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0084] (6) The slurry of step (5) was filtered, washed, dried at 120° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a composite material. The texture properties and acid properties of the composite material are shown in Table 1.

[0085] (7) The steps for preparing the catalyst are the same as steps (7) and (8) of Example 1. The textural properties and acid properties of the catalyst are shown in Table 2.

[0086] The textural properties and acid properties of the catalysts are shown in Table 2.

[0087] Example 5

[0088] (1) According to the addition amount of molecular sieves accounting for 50wt% of the weight of the composite material, 19g of SSZ-13 with a silicon-aluminum ratio of 30 and 1g of Y-type molecular sieve with a silicon-aluminum ratio of 20 were weighed and added into the reactor.

[0089] (2) Solid aluminum sulfate was prepared into 1000 mL of aluminum sulfate solution with a concentration of 10 g Al2O3 / L (A), concentrated ammonia water was diluted with an appropriate amount of deionized water to obtain an 8 wt% dilute ammonia solution (B), concentrated water glass solution was diluted with an appropriate amount of deionized water to obtain 140 mL of 7 wt% water glass solution (C), 5 g of cerium nitrate (Ce(NO3)3·6H2O) was added to 50 mL of water to obtain a solution with a CeO2 content of 3.36% (D).

[0090] (3) Add 100 mL of deionized water to the reactor and heat to 85° C. Then add (A) and (B) to make the mixed slurry have a pH of 9.5 and gel for 60 minutes. After the addition is completed, keep the temperature unchanged and age for 60 minutes.

[0091] (4) Add solution (C) to the slurry of step (3), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0092] (5) Add solution (D) to the slurry of step (4), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0093] (6) The slurry of step (5) was filtered, washed, dried at 110° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a composite material. The texture properties and acid properties of the composite material are shown in Table 1.

[0094] (7) The steps for preparing the catalyst are the same as steps (7) and (8) of Example 1. The textural properties and acid properties of the catalyst are shown in Table 2.

[0095] The textural properties and acid properties of the catalysts are shown in Table 2.

[0096] Example 6

[0097] (1) According to the addition amount of molecular sieves accounting for 20wt% of the weight of the composite material, 2.5g of Y-type molecular sieve with a silicon-aluminum ratio of 15 and 2.5g of SSZ-13 molecular sieve with a silicon-aluminum ratio of 50 were weighed and added into the reactor.

[0098] (2) Solid aluminum sulfate was prepared into 1000 mL of an aluminum sulfate solution with a concentration of 10 g Al2O3 / L (A), concentrated ammonia water was diluted with an appropriate amount of deionized water to obtain a 10 wt% dilute ammonia solution (B), concentrated water glass solution was diluted with an appropriate amount of deionized water to obtain 150 mL of a 7 wt% water glass solution (C), 5 g of cerium nitrate (Ce(NO3)3·6H2O) was added to 50 mL of water to obtain a solution with a CeO2 content of 3.36% (D).

[0099] (3) Add 100 mL of deionized water to the reactor and heat to 95° C. Then add (A) and (B) to make the pH of the mixed slurry 8.5 and gel for 30 minutes. After the addition is completed, keep the temperature unchanged and age for 30 minutes.

[0100] (4) Add solution (C) to the slurry of step (3), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0101] (5) Add solution (D) to the slurry of step (4), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0102] (6) The slurry of step (5) was filtered, washed, dried at 110° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a composite material. The texture properties and acid properties of the composite material are shown in Table 1.

[0103] (7) The steps for preparing the catalyst are the same as steps (7) and (8) of Example 1. The textural properties and acid properties of the catalyst are shown in Table 2.

[0104] The textural properties and acid properties of the catalysts are shown in Table 2.

[0105] Example 7

[0106] (1) According to the addition amount that the total weight of the molecular sieve accounts for 30wt% of the weight of the composite material, 4.3g of Y-type molecular sieve with a silicon-aluminum ratio of 17.5 and 4.3g of SSZ-13 with a silicon-aluminum ratio of 50 were weighed and added into the reactor.

[0107] (2) Solid aluminum sulfate was prepared into 300 mL of aluminum sulfate solution with a concentration of 30 g Al2O3 / L (A), concentrated ammonia water was added with an appropriate amount of deionized water to dilute it into an 8 wt% dilute ammonia solution (B), concentrated water glass solution was added with an appropriate amount of deionized water to dilute it into 200 mL of 5 wt% water glass solution (C), 5 g of cerium nitrate (Ce(NO3)3·6H2O) was taken and added to 50 mL of water to obtain a solution with a CeO2 content of 3.36% (D).

[0108] (3) Add 100 mL of deionized water to the reactor and heat to 65° C. Then add (A) and (B) to make the mixed slurry have a pH of 8.5 and gel for 90 minutes. After the addition is completed, keep the temperature unchanged and age for 90 minutes.

[0109] (4) Add solution (C) to the slurry of step (3), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0110] (5) Add solution (D) to the slurry of step (4), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0111] (6) The slurry of step (5) was filtered, washed, dried at 110° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a composite material. The texture properties and acid properties of the composite material are shown in Table 1.

[0112] (7) The steps for preparing the catalyst are the same as steps (7) and (8) of Example 1. The textural properties and acid properties of the catalyst are shown in Table 2.

[0113] The textural properties and acid properties of the catalysts are shown in Table 2.

[0114] Example 8

[0115] (1) According to the addition amount of molecular sieves accounting for 40wt% of the weight of the composite material, 6.7g of Y-type molecular sieve with a silicon-aluminum ratio of 14 and 6.7g of SSZ-13 molecular sieve with a silicon-aluminum ratio of 20 were weighed and added into the reactor.

[0116] (2) Solid aluminum sulfate is prepared into 1000 mL of an aluminum sulfate solution with a concentration of 10 g Al2O3 / L (A), concentrated ammonia water is diluted with an appropriate amount of deionized water to obtain a 5 wt% dilute ammonia solution (B), concentrated water glass solution is diluted with an appropriate amount of deionized water to obtain 100 mL of a 5 wt% water glass solution (C), 5 g of cerium nitrate (Ce(NO3)3·6H2O) is added to 50 mL of water to obtain a solution with a CeO2 content of 3.36% (D).

[0117] (3) Add 200 mL of deionized water to the reactor and heat to 65° C. Then add (A) and (B) to make the mixed slurry have a pH of 8.0 and gel for 60 minutes. After the addition is completed, keep the temperature unchanged and age for 60 minutes.

[0118] (4) Add solution (C) to the slurry of step (3), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0119] (5) Add solution (D) to the slurry of step (4), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0120] (6) The slurry of step (5) was filtered, washed, dried at 110° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a composite material. The texture properties and acid properties of the composite material are shown in Table 1.

[0121] (7) The steps for preparing the catalyst are the same as steps (7) and (8) of Example 1. The textural properties and acid properties of the catalyst are shown in Table 2.

[0122] The textural properties and acid properties of the catalysts are shown in Table 2.

[0123] Example 9

[0124] (1) According to the addition amount of molecular sieves accounting for 60wt% of the weight of the composite material, 15g of Y-type molecular sieve with a silicon-aluminum ratio of 15 and 15g of SSZ-13 molecular sieve with a silicon-aluminum ratio of 30 were weighed and added into the reactor.

[0125] (2) Solid aluminum sulfate was prepared into 500 mL of an aluminum sulfate solution with a concentration of 10 g Al2O3 / L (A), concentrated ammonia water was added with an appropriate amount of deionized water to dilute it into a 7 wt% dilute ammonia solution (B), concentrated water glass solution was added with an appropriate amount of deionized water to dilute it into 100 mL of a 10 wt% water glass solution (C), 5 g of cerium nitrate (Ce(NO3)3·6H2O) was taken and added to 50 mL of water to obtain a solution with a CeO2 content of 3.36% (D).

[0126] (3) Add 200 mL of deionized water to the reactor and heat to 55° C., add (A) and (B) to make the mixed slurry gel at a pH of 8.0 for 90 minutes. After the addition is completed, age at 65° C. for 120 minutes.

[0127] (4) Add solution (C) to the slurry of step (3), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0128] (5) Add solution (D) to the slurry of step (4), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0129] (6) The slurry of step (5) was filtered, washed, dried at 110° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a composite material. The texture properties and acid properties of the composite material are shown in Table 1.

[0130] (7) The steps for preparing the catalyst are the same as steps (7) and (8) of Example 1. The textural properties and acid properties of the catalyst are shown in Table 2.

[0131] The textural properties and acid properties of the catalysts are shown in Table 2.

[0132] Example 10

[0133] (1) According to the addition amount of molecular sieves accounting for 50wt% of the weight of the composite material, 8.3g of Y-type molecular sieve with a silicon-aluminum ratio of 7.0 and 8.3g of SSZ-13 molecular sieve with a silicon-aluminum ratio of 30 were weighed and added into the reactor.

[0134] (2) Solid aluminum sulfate was prepared into 1000 mL of aluminum sulfate solution with a concentration of 10 g Al2O3 / L (A), concentrated ammonia water was diluted with an appropriate amount of deionized water to obtain a 6 wt% dilute ammonia solution (B), concentrated water glass solution was diluted with an appropriate amount of deionized water to obtain 90 mL of 7 wt% water glass solution (C), 5 g of cerium nitrate (Ce(NO3)3·6H2O) was added to 50 mL of water to obtain a solution with a CeO2 content of 3.36% (D).

[0135] (3) Add 300 mL of deionized water to the reactor and heat to 85° C. Then add (A) and (B) to make the mixed slurry gel at a pH of 8.5 for 60 min. After the addition is completed, age at 65° C. for 60 min.

[0136] (4) Add solution (C) to the slurry of step (3), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0137] (5) Add solution (D) to the slurry of step (4), keep the temperature unchanged, and after the feeding is completed, age at the same temperature for 60 minutes.

[0138] (6) The slurry of step (5) was filtered, washed, dried at 110° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a composite material. The texture properties and acid properties of the composite material are shown in Table 1.

[0139] (7) The steps for preparing the catalyst are the same as steps (7) and (8) of Example 1. The textural properties and acid properties of the catalyst are shown in Table 2.

[0140] The textural properties and acid properties of the catalysts are shown in Table 2.

[0141] Comparative Example 1

[0142] The conditions of Example 1 were used, but the materials were not subjected to step-wise precipitation but directly mixed and prepared.

[0143] (1) Solid aluminum sulfate is prepared into 500 mL of an aluminum sulfate solution with a concentration of 20 g Al2O3 / L (A), concentrated ammonia water is diluted with an appropriate amount of deionized water to obtain a 10 wt% dilute ammonia solution (B), concentrated water glass solution is diluted with an appropriate amount of deionized water to obtain 72 mL of a 14 wt% water glass solution (C), and 2 g of cerium nitrate (Ce(NO3)3·6H2O) is added to 10 mL of water to obtain a solution with a CeO2 content of 6.61% (D).

[0144] (2) Take a 1L container, add 300mL of deionized water and heat to 75°C, then add (A) and (B) to make the mixed slurry gel at pH 8.0 for 60 minutes. After the feeding is completed, age at 65°C for 60 minutes. Then continue to add solution (C) and keep the temperature unchanged. After the feeding is completed, age at the same temperature for 60 minutes. Filter, wash and dry to obtain amorphous silica-alumina.

[0145] (3) Take a 1L container, pour solution (D) into it, and heat it to 75°C, then add solution (B) to make the final pH value 8.5, and keep it at 75°C for 60 minutes after adding. Filter and wash to obtain the hydroxide of rare earth.

[0146] (4) Weigh 19 g of Y-type molecular sieve with a silicon-aluminum ratio of 7.5, 1 g of SSZ-13 with a silicon-aluminum ratio of 20, 20 g of amorphous silica-alumina, and 0.8 g of rare earth hydroxide into a 1-liter container, add 50 mL of water, then add 4.7 g of aluminum sol and 2.4 g of sesbania powder, mix and knead, extrude into strips, dry at 120°C for 5 hours, and calcine at 550°C for 3 hours to obtain a carrier.

[0147] (5) The carrier was impregnated with an impregnation solution prepared with equal volumes of 13.4 g of ammonium metatungstate and 6.7 g of nickel nitrate for 12 hours, dried at 50° C. for 4 hours, dried at 120° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a hydrocracking catalyst.

[0148] The textural properties and acid properties of the catalysts are shown in Table 2.

[0149] Comparative Example 2

[0150] The conditions of Example 3 were used, but the materials were not subjected to step-wise precipitation but directly mixed and prepared.

[0151] (1) Solid aluminum sulfate is prepared into 500 mL of an aluminum sulfate solution with a concentration of 20 g Al2O3 / L (A), concentrated ammonia water is diluted with an appropriate amount of deionized water to obtain a 10 wt% dilute ammonia solution (B), concentrated water glass solution is diluted with an appropriate amount of deionized water to obtain 72 mL of a 14 wt% water glass solution (C), 10 g of cerium nitrate (Ce(NO3)3·6H2O) is added to 50 mL of water to obtain a solution with a CeO2 content of 6.61% (D).

[0152] (2) Take a 1L container, add 300mL of deionized water and heat to 85°C, then add (A) and (B) to make the mixed slurry have a pH of 8.0 and gel for 60 minutes. After the feeding is completed, age at 65°C for 60 minutes. Then continue to add solution (C) and keep the temperature unchanged. After the feeding is completed, age at the same temperature for 60 minutes. Filter, wash and dry to obtain amorphous silica-alumina.

[0153] (3) Take a 1L container, pour solution (D) into it, and heat it to 75°C, then add solution (B) to make the final pH value 8.5, and keep it at 75°C for 60 minutes after adding. Filter and wash to obtain the hydroxide of rare earth.

[0154] (4) Weigh 9.1 g of Y-type molecular sieve with a silicon-aluminum ratio of 12.5, 9.1 g of SSZ-13 with a silicon-aluminum ratio of 40, 19.3 g of amorphous silica-alumina, and 4 g of rare earth hydroxide into a 1-liter container, add 50 mL of water, and then add 4.7 g of aluminum sol and 2.4 g of sesbania powder to mix and knead, extrude into strips, dry at 120°C for 5 hours, and calcine at 550°C for 3 hours to obtain a carrier.

[0155] (5) The carrier was impregnated with an impregnation solution prepared with equal volumes of 13.4 g of ammonium metatungstate and 6.7 g of nickel nitrate for 12 hours, dried at 50° C. for 4 hours, dried at 120° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a hydrocracking catalyst.

[0156] The textural properties and acid properties of the catalysts are shown in Table 2.

[0157] Comparative Example 3

[0158] The conditions of Example 5 were used, but the materials were not subjected to step-wise precipitation but directly mixed and prepared.

[0159] (1) Solid aluminum sulfate is prepared into 500 mL of an aluminum sulfate solution with a concentration of 20 g Al2O3 / L (A), concentrated ammonia water is diluted with an appropriate amount of deionized water to obtain a 10 wt% dilute ammonia solution (B), concentrated water glass solution is diluted with an appropriate amount of deionized water to obtain 72 mL of a 14 wt% water glass solution (C), 5 g of cerium nitrate (Ce(NO3)3·6H2O) is added to 50 mL of water to obtain a solution with a CeO2 content of 3.36% (D).

[0160] (2) Take a 1L container, add 300mL of deionized water and heat to 85°C, then add (A) and (B) to make the mixed slurry have a pH of 8.0 and gel for 60 minutes. After the feeding is completed, age at 65°C for 60 minutes. Then continue to add solution (C) and keep the temperature unchanged. After the feeding is completed, age at the same temperature for 60 minutes. Filter, wash and dry to obtain amorphous silica-alumina.

[0161] (3) Take a 1L container, pour solution (D) into it, and heat it to 75°C, then add solution (B) to make the final pH value 8.5, and keep it at 75°C for 60 minutes after adding. Filter and wash to obtain the hydroxide of rare earth.

[0162] (4) Weigh 0.9 g of Y-type molecular sieve with a silicon-aluminum ratio of 20, 18 g of SSZ-13 with a silicon-aluminum ratio of 30, 19.1 g of amorphous silica-alumina, and 2 g of rare earth hydroxide into a 1-liter container, add 50 mL of water, then add 4.7 g of aluminum sol and 2.4 g of sesbania powder, mix and knead, extrude into strips, dry at 120°C for 5 hours, and calcine at 550°C for 3 hours to obtain a carrier.

[0163] (5) The carrier was impregnated with an impregnation solution prepared with equal volumes of 13.4 g of ammonium metatungstate and 6.7 g of nickel nitrate for 12 hours, dried at 50° C. for 4 hours, dried at 120° C. for 5 hours, and calcined at 550° C. for 3 hours to obtain a hydrocracking catalyst.

[0164] The textural properties and acid properties of the catalysts are shown in Table 2.

[0165] Table 1 Texture and acid properties of Y / SSZ-13 / rare earth / ASA composites

[0166]

[0167]

[0168] Table 2 Catalyst texture properties and acid properties

[0169]

[0170] From the data in Table 2, it can be seen that the catalyst containing Y / SSZ-13 / rare earth / ASA composite material has a large specific surface area, a large pore volume, a wide pore size distribution, and a large infrared acid content. It has the advantages of strong raw material adaptability, good cracking activity, high product yield, and good product quality. It is suitable for the process of producing products of different purposes by hydrocracking reaction.

[0171] A 200mL medium-sized hydrocracking evaluation device was used to evaluate the catalyst performance. A one-stage series process was adopted. Before the evaluation, the catalyst was pre-sulfurized with cyclohexane containing 3wt% CS2. The properties of the feedstock oil and the reaction conditions used to evaluate the catalyst performance are shown in Tables 3 and 4, respectively. The evaluation results of each catalyst reaction are shown in Table 5.

[0172] Table 3 Raw oil properties

[0173] Crude oil Intermediate straight run diesel <![CDATA[Density (20 °C), g / cm 3 > 0.8149 Sulfur, μg / g 3750 Nitrogen, μg / g 75 Distillation range, ℃ IBP 174 10% 212 50% 252 90% 322 95% 350 EBP 363

[0174] Table 4 Reaction process conditions

[0175] <![CDATA[Partial pressure of H2, MPa]]> 10.0 Hydrogen to oil volume ratio 500 <![CDATA[Liquid hourly space velocity, h -1 > 1.5 Temperature, °C 355

[0176] Table 5 Catalyst reaction evaluation results

[0177]

[0178] It can be seen from the evaluation results of the catalysts in Table 5 that the hydrocracking catalyst containing the Y / SSZ-13 / rare earth / ASA composite material prepared by the method of the present invention has higher jet fuel selectivity than the catalyst prepared by direct mixing in the comparative example.

[0179] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing a Y / SSZ-13 / rare earth / ASA composite material, characterized in that: The steps include: Step 1, mixing Y molecular sieve, SSZ-13 molecular sieve, aluminum source, alkaline compound and water, heating and stirring; Step 2, adding a silicon source and a rare earth precursor to the mixture of step 1, heating and stirring, drying, and calcining to obtain a Y / SSZ-13 / rare earth / ASA composite material; Based on the total weight of the composite material, in the composite material, amorphous silicon aluminum ASA accounts for 10-80 wt%, molecular sieve accounts for 80-10 wt%, and rare earth oxide accounts for 0.1-10%; based on the total weight of the molecular sieve, in the molecular sieve, Y molecular sieve accounts for 5-95 wt%, and SSZ-13 molecular sieve accounts for 95-5 wt%.

2. The method for preparing the Y / SSZ-13 / rare earth / ASA composite material according to claim 1, characterized in that: The step 1 is: dispersing the Y molecular sieve and the SSZ-13 molecular sieve in water, heating, then adding the aqueous solution of the aluminum source and the aqueous solution of the alkaline compound, and continuing heating and stirring.

3. The method for preparing the Y / SSZ-13 / rare earth / ASA composite material according to claim 1, characterized in that: The step 2 is to first add the silicon source into the mixture of step 1, heat and stir, and then add the rare earth precursor.

4. The method for preparing the Y / SSZ-13 / rare earth / ASA composite material according to claim 3, characterized in that: The silicon source and the rare earth precursor are added to the mixture in step 1 in the form of aqueous solutions.

5. The method for preparing the Y / SSZ-13 / rare earth / ASA composite material according to claim 1, characterized in that: After the heating and stirring in step 2, the process also includes filtering and washing steps, and then drying and roasting.

6. The method for preparing the Y / SSZ-13 / rare earth / ASA composite material according to claim 1, characterized in that: The mass ratio of the Y molecular sieve to the SSZ-13 molecular sieve is 5-95:95-5; the specific surface area of ​​the Y molecular sieve is 300-900m 2 / g, the total pore volume is 0.3-0.6mL / g, the amount ratio of SiO2 / Al2O3 in the framework is 5-20, and the relative crystallinity is 80-100%; the amount ratio of SiO2 / Al2O3 in the SSZ-13 molecular sieve is 20-100, and the specific surface area is 200-500m 2 / g, and the total pore volume is 0.4~0.8mL / g.

7. The method for preparing the Y / SSZ-13 / rare earth / ASA composite material according to claim 1, characterized in that: The aluminum source is an acidic aluminum source, and the acidic aluminum source is one or more of aluminum sulfate, aluminum nitrate, and aluminum chloride; the alkaline compound is one or more of ammonia water, sodium hydroxide, potassium hydroxide, sodium carbonate, and ammonium carbonate; the silicon source is an alkaline silicon source; the rare earth precursor is one or more of rare earth chloride and rare earth nitrate; the heating temperature in step 1 and the heating temperature in step 2 are both 60~90°C; the mass ratio of molecular sieve, aluminum source, alkaline compound, silicon source and rare earth precursor is: molecular sieve: Al2O3: alkaline compound: SiO2: rare earth precursor = (5~30): (5~10): (30~100): 10: (0.5~4), and the molecular sieves are Y molecular sieve and SSZ-13 molecular sieve.

8. The method for preparing the Y / SSZ-13 / rare earth / ASA composite material according to claim 2, characterized in that: The mass content of the aluminum source in the aqueous solution of the aluminum source in terms of Al2O3 is 1-4 wt%; the mass content of the alkaline compound in the aqueous solution of the alkaline compound is 5-15 wt%.

9. The method for preparing the Y / SSZ-13 / rare earth / ASA composite material according to claim 4, characterized in that: The mass content of the silicon source in the aqueous solution formed by the silicon source in terms of SiO2 is 5-20 wt %; the mass content of the rare earth precursor in the aqueous solution formed by the rare earth precursor is 1-20 wt %.

10. A Y / SSZ-13 / rare earth / ASA composite material, characterized in that: The composite material is obtained by the preparation method described in claim 1. Based on the total weight of the composite material, in the composite material, amorphous silicon aluminum ASA accounts for 10-80 wt%, molecular sieve accounts for 80-10 wt%, and rare earth oxide accounts for 0.1-10%; based on the total weight of the molecular sieve, in the molecular sieve, Y molecular sieve accounts for 5-95 wt%, and SSZ-13 molecular sieve accounts for 95-5 wt%.

11. The Y / SSZ-13 / rare earth / ASA composite material according to claim 10, characterized in that: The specific surface area of ​​the Y / SSZ-13 / rare earth / ASA composite material is 300-600 m 2 / g, pore volume of 0.3-2.0 mL / g, average pore diameter of 5-15 nm, and / or, infrared acid content of 100-500 μmol / g.

12. A hydrocracking catalyst carrier, characterized in that: The hydrocracking catalyst carrier comprises the Y / SSZ-13 / rare earth / ASA composite material as claimed in claim 10 or 11.

13. A method for preparing a hydrocracking catalyst carrier, characterized in that: The hydrocracking catalyst carrier comprises a Y / SSZ-13 / rare earth / ASA composite material, and the preparation method comprises the preparation method of the Y / SSZ-13 / rare earth / ASA composite material according to claim 1.

14. A hydrocracking catalyst comprising a carrier and an active component, characterized in that: The carrier is the hydrocracking catalyst carrier according to claim 12.

15. A method for preparing a hydrocracking catalyst, the hydrocracking catalyst comprising a carrier and an active component, characterized in that: The carrier comprises a Y / SSZ-13 / rare earth / ASA composite material, and the preparation method comprises the preparation method of the Y / SSZ-13 / rare earth / ASA composite material according to claim 1.