Manufacturing method of OLED pixel forming mask, mask support template and frame integrated mask

By using mask support templates in OLED manufacturing, controlling the bonding and stretching of the mask on the frame, the mask deformation and alignment error problems are solved, and efficient OLED pixel formation is achieved.

CN114134459BActive Publication Date: 2024-11-26OLUM MATERIAL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202110902501.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-04
Filing Date
2021-08-06
Publication Date
2024-11-26
Estimated Expiration
2041-08-06

Smart Images

  • Figure CN114134459B_ABST
    Figure CN114134459B_ABST
Patent Text Reader

Abstract

The present invention relates to a mask for forming OLED pixels, a mask support template, and a method for manufacturing a frame-integrated mask. According to the mask for forming OLED pixels of the present invention, it is supported by a mask support template and attached to a frame, wherein the mask includes a mask unit formed with a plurality of mask patterns and a dummy portion around the mask unit, the mask has a pair of long sides and a pair of short sides, and on any straight line parallel to the long side or the short side of the mask, the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end is 0.1 μm to 20.0 μm greater than the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end in a mask using a predetermined design value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for manufacturing an OLED pixel forming mask, a mask support template, and a frame-integrated mask. More specifically, the present invention relates to a method for manufacturing an OLED pixel forming mask, a mask support template, and a frame-integrated mask, which can support and move the mask stably without causing deformation, and improve the positional precision by reducing the deformation of the mask when the mask is attached to a frame, thereby accurately aligning each mask. Background Art

[0002] As a technology for forming pixels in the OLED manufacturing process, the FMM (Fine Metal Mask) method is mainly used. In this method, a metal mask (Shadow Mask) in the form of a thin film is closely attached to a substrate and an organic substance is evaporated at a desired position.

[0003] In the existing OLED manufacturing process, after the mask is manufactured into a strip shape, a plate shape, etc., the mask is welded and fixed to the OLED pixel evaporation frame and used. A mask can have multiple units corresponding to one display. In addition, in order to manufacture large-area OLEDs, multiple masks can be fixed to the OLED pixel evaporation frame, and in the process of fixing them to the frame, each mask is stretched to make it flat. Adjusting the stretching force to make the entire part of the mask flat is a very difficult task. In particular, in order to flatten each unit while aligning the mask pattern with a size of several to tens of μm, it is necessary to perform a difficult task of finely adjusting the stretching force applied to each side of the mask while confirming the alignment status in real time.

[0004] Nevertheless, in the process of fixing multiple masks to a frame, there is still the problem of poor alignment between masks and between mask units. In addition, in the process of welding the mask to the frame, the thickness of the mask film is too thin and the area is too large, so there is a problem that the mask sags or twists due to the load; wrinkles and burrs generated in the welding part during the welding process lead to the problem of misalignment of the mask unit, etc.

[0005] In ultra-high-definition OLED, the existing QHD image quality is 500-600PPI (pixel per inch), and the pixel size is about 30-50μm, while 4K UHD and 8K UHD high-definition images have higher resolutions of ~860PPI and ~1600PPI. Considering the pixel size of ultra-high-definition OLED, the alignment error between units needs to be reduced to about a few μm. Exceeding this error will result in defective products, so the yield may be extremely low. Therefore, it is necessary to develop technologies that can prevent deformation such as sagging or twisting of the mask and enable accurate alignment, as well as technologies that fix the mask to the frame. Summary of the invention

[0006] Technical issues

[0007] Therefore, the present invention is proposed to solve the various problems of the prior art as described above, and its purpose is to provide a mask for forming OLED pixels, a mask support template and a frame-integrated mask manufacturing method that can prevent the mask from being deformed and being stably supported and moved, and prevent the mask from being deformed such as sagging or twisting, and can be accurately aligned.

[0008] In addition, an object of the present invention is to provide a method for manufacturing a frame-integrated mask that can significantly shorten the manufacturing time and significantly improve the yield.

[0009] Technical Solution

[0010] The above-mentioned object of the present invention is achieved by a mask for forming OLED pixels, wherein the mask for forming OLED pixels is supported by a mask support template and attached to a frame, wherein the mask includes a mask unit on which a plurality of mask patterns are formed and a dummy portion around the mask unit, the mask has a pair of long sides and a pair of short sides, and on any straight line parallel to the long sides or short sides of the mask, the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end is 0.1 μm to 20.0 μm greater than the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end in a mask using a predetermined design value.

[0011] When the mask is divided into three equal regions along the long side direction, in each region, any straight line is extended in a direction perpendicular to the long side, and the average value of the distance on any straight line from the mask pattern arranged at one end to the mask pattern arranged at the other end is set to A. When the mask is divided into three equal regions along the short side direction, in each region, any straight line is extended in a direction perpendicular to the short side, and the average value of the distance on any straight line from the mask pattern arranged at one end to the mask pattern arranged at the other end is set to B. For the case of a mask using a predetermined design value, when the mask is divided into three equal regions along the long side direction, in each region, any straight line is extended in a direction perpendicular to the long side, and the average value of the distance on any straight line from the mask pattern arranged at one end to the mask pattern arranged at the other end is set to C. When the mask is divided into three equal regions along the short side direction, in each region, any straight line is extended in a direction perpendicular to the short side, and the average value of the distance on any straight line from the mask pattern arranged at one end to the mask pattern arranged at the other end is set to D. At this time, the values ​​of AC and BD can be positive numbers respectively.

[0012] The value of AC may be 0.1 μm to 20.0 μm, and the value of BD may be 0.1 μm to 15.0 μm.

[0013] The coefficient of thermal expansion of the mask may be at least greater than 1, and the coefficient of thermal expansion of the template may be less than 1 (greater than 0).

[0014] The OLED pixel forming mask supported by the mask supporting template can be manufactured by the following steps: (a) preparing a template having a temporary adhesive portion formed on one side; (b) raising the process temperature to a temperature where the adhesive strength of the temporary adhesive portion becomes 0 to 5 kgf / cm 2 (c) lowering the process temperature to a temperature where the bonding strength of the temporary bonding portion is at least greater than 5 kgf / cm 2 (d) lowering the process temperature to room temperature; and (e) manufacturing a mask by forming a mask pattern on the mask metal film.

[0015] Step (d) may include the following steps: (d1) lowering the process temperature to below room temperature; (d2) lowering the process temperature to room temperature.

[0016] In step (b), the process temperature may be raised to 110° C. to 200° C., and in step (c), the process temperature may be lowered to a temperature lower than the process temperature in step (b) and higher than room temperature.

[0017] In step (b), the mask metal film is extended further to the side than the template in a state where there is no adhesion between the mask metal film and the template, and in step (c), the mask metal film is bonded to the template in an extended state.

[0018] As the process temperature in step (b) increases, the mask metal film can be bonded and fixed to the template in a state with a greater degree of extension.

[0019] In addition, the object of the present invention can be achieved by a mask for forming OLED pixels, wherein the mask for forming OLED pixels is supported by a mask support template and attached to a frame, wherein the mask includes a mask unit on which a plurality of mask patterns are formed and a dummy portion around the mask unit, the mask has a pair of long sides and a pair of short sides, and on any straight line parallel to the long sides or short sides of the mask, the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end is 0.1 μm to 20.0 μm greater than the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end in a mask manufactured by the following steps, wherein the steps are specifically: (1) preparing a template with a temporary bonding portion formed on one side; (2) raising the process temperature to a temperature at which the temporary bonding portion at least bonds the mask metal film and the template and bonds the mask metal film to the template; (3) lowering the process temperature to room temperature; and (4) manufacturing the mask by forming a mask pattern on the mask metal film.

[0020] The mask includes a mask unit having a plurality of mask patterns formed therein and a dummy portion around the mask unit, the mask having a pair of long sides and a pair of short sides, when the mask is equally divided into three regions along the long side direction, in each region, any straight line is extended in a direction perpendicular to the long side, and the average value of the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end on any straight line is set to A, and when the mask is equally divided into three regions along the short side direction, in each region, any straight line is extended in a direction perpendicular to the short side, and the average value of the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end on any straight line is set to B, for the following steps: (1) preparing a template having a temporary bonding portion formed on one side; (2) raising the process temperature to a temperature at which the temporary bonding portion is at a certain distance from the mask pattern arranged at one end to the mask pattern arranged at the other end; (1) reducing the temperature of the bonding mask metal film and the template and bonding the mask metal film to the template; (2) lowering the process temperature to room temperature; (3) manufacturing a mask by forming a mask pattern on the mask metal film; in the case of the manufactured mask, when the mask is divided into three equal regions along the long side direction, in each region, any straight line is extended in a direction perpendicular to the long side, and the average distance on any straight line from the mask pattern arranged at one end to the mask pattern arranged at the other end is set to C; when the mask is divided into three equal regions along the short side direction, in each region, any straight line is extended in a direction perpendicular to the short side, and the average distance on any straight line from the mask pattern arranged at one end to the mask pattern arranged at the other end is set to D, and at this time, the values ​​of AC and BD can be positive numbers respectively.

[0021] In addition, the above-mentioned purpose of the present invention is achieved by a mask supporting template, which is used to support a mask for forming OLED pixels and correspond the mask to a frame, and the mask supporting template includes: a template; a temporary bonding portion formed on the template; and a mask, which is bonded to the template by clamping the temporary bonding portion and has multiple mask patterns, the mask includes a mask unit having multiple mask patterns and a dummy portion around the mask unit, the mask has a pair of long sides and a pair of short sides, and on any straight line parallel to the long side or short side of the mask, the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end is 0.1μm to 20.0μm larger than the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end in a mask using a predetermined design value.

[0022] In addition, the purpose of the present invention can be achieved by a mask support template, the mask support template is used to support the OLED pixel formed with a mask and correspond the mask to the frame, the mask support template includes: a template; a temporary bonding portion, which is formed on the template; and a mask, which is bonded to the template by clamping the temporary bonding portion and is formed with a plurality of mask patterns, the mask includes a mask unit formed with a plurality of mask patterns and a dummy portion around the mask unit, the mask has a pair of long sides and a pair of short sides, on any straight line parallel to the long side or the short side of the mask, from the arranged The distance from the mask pattern at one end to the mask pattern arranged at the other end is 0.1 μm to 20.0 μm greater than the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end in a mask manufactured by the following steps, wherein: (1) preparing a template having a temporary bonding portion formed on one side; (2) raising the process temperature to a temperature at which the temporary bonding portion at least bonds the mask metal film and the template and bonds the mask metal film to the template; (3) lowering the process temperature to room temperature; and (4) manufacturing a mask by forming a mask pattern on the mask metal film.

[0023] In addition, the above-mentioned purpose of the present invention is achieved by a method for manufacturing a frame-integrated mask, which is integrally formed by at least one mask and a frame for supporting the mask, wherein the method may include the following steps: (a) loading the mask supporting template onto a frame having at least one mask unit area, and corresponding the mask to the mask unit area of ​​the frame; and (b) attaching the mask to the frame.

[0024] Effects of the Invention

[0025] According to the present invention having the above structure, the mask can be stably supported and moved without being deformed, and the mask can be accurately aligned without being deformed such as sagging or twisting.

[0026] In addition, according to the present invention, there is an effect that the production time can be significantly shortened and the yield can be significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 is a schematic diagram of an existing process of attaching a mask to a frame.

[0028] Figure 2 1 is a front view and a side cross-sectional view of a frame-integrated mask according to an embodiment of the present invention.

[0029] Figure 3 is a schematic diagram of a mask according to an embodiment of the present invention.

[0030] Figures 4 to 5 FIG. 4 is a schematic diagram of a process of forming a mask by bonding a mask metal film on a template to manufacture a mask support template according to an embodiment of the present invention.

[0031] Figure 6 This is a schematic diagram of a problem that occurs when the thermal expansion coefficient of the template is higher than that of the mask according to the comparative example.

[0032] Figure 7 3 is a schematic diagram of an interface state between a mask and a template and a state where the mask is attached to a frame when the thermal expansion coefficient of the template is lower than that of the mask according to an embodiment of the present invention.

[0033] Figure 8 Schematic diagram of the extension state of the mask metal film and the template in response to the process temperature change according to an embodiment of the present invention.

[0034] Fig. 9 1 is a comparison data between the initial design size of the mask and the size after the process is completed according to an experimental example of the present invention.

[0035] Fig.10 Schematic diagram of a method for measuring the total pitch of a mask before and after a process according to an experimental example of the present invention.

[0036] Fig.11 4 is a graph showing the measurement results of the total mask spacing before and after each process temperature according to an experimental example of the present invention.

[0037] Fig.12 2 is a schematic diagram of a process of attaching a mask to a frame and then placing a weight on the mask to measure tension according to an experimental example of the present invention.

[0038] Fig.13 2 is a schematic diagram of a state in which a template is loaded onto a frame and a mask is aligned to a unit area of ​​the frame according to an embodiment of the present invention.

[0039] Fig.14 is a schematic diagram of a process of separating the mask and the template after attaching the mask to the frame according to an embodiment of the present invention.

[0040] Fig.15 is a schematic diagram of a state where a mask is attached to a unit region of a frame according to an embodiment of the present invention.

[0041] [Reference Signs]

[0042] 23: First insulation part

[0043] 25: Second insulation part

[0044] 50: template

[0045] 51: Laser through hole

[0046] 55: Temporary bonding section

[0047] 100: Mask

[0048] 110: Mask metal film

[0049] 200: Framework

[0050] 210: Edge frame

[0051] 220: Mask unit sheet portion

[0052] 221: Edge sheet section

[0053] 223: First grid sheet portion

[0054] 225: Second grid sheet portion

[0055] C: Unit, mask unit

[0056] CR: Mask cell region

[0057] DM: dummy part, mask dummy part

[0058] L: Laser

[0059] P: Mask pattern

[0060] RT: room temperature

[0061] TS1, TS2, TS3: first, second, third process temperature

[0062] WB: Weld Bead DETAILED DESCRIPTION

[0063] Below, the present invention is described in detail with reference to the accompanying drawings, which are used to illustrate examples of specific embodiments that can be implemented as the present invention. These embodiments are described in detail so that those skilled in the art can fully implement the present invention. Various embodiments of the present invention should be understood to be different from each other but not mutually exclusive. For example, the specific shapes, structures and characteristics recorded can implement one embodiment as other embodiments without exceeding the spirit and scope of the present invention. In addition, the position or arrangement of individual components in each disclosed embodiment should be understood to be changeable without exceeding the spirit and scope of the present invention. The following detailed description is not intended to limit the present invention, and the scope of the present invention is limited only by the attached claims and all scopes equivalent thereto. Similar figure marks in the drawings refer to the same or similar functions in various aspects, and for convenience, length, area, thickness, etc. and their forms can also be exaggerated.

[0064] In the following, in order to enable those skilled in the art to easily implement the present invention, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0065] Figure 1 is a schematic diagram of an existing process of attaching a mask to a frame.

[0066] The existing mask 10 is a stick-type or a plate-type. Figure 1 The strip-type mask 10 can be used by welding both sides of the strip to the OLED pixel evaporation frame. The body (Body, or mask film 11) of the mask 10 has a plurality of display cells C. One cell C corresponds to one display of a smartphone, etc. A pixel pattern P is formed in the cell C so as to correspond to each pixel of the display.

[0067] Reference Figure 1 (a), a tensile force F1-F2 is applied along the long axis direction of the strip mask 10, and the strip mask 10 is loaded on a frame 20 in a stretched state. The cells C1-C6 of the strip mask 10 will be located in the blank area inside the frame 20.

[0068] Reference Figure 1 (b), the tensile forces F1-F2 applied to the respective sides of the stripe mask 10 are finely adjusted while being aligned, and then the stripe mask 10 and the frame 20 are connected to each other by welding a portion of the side surface of the stripe mask 10. Figure 1 (c) shows a side section of the stripe type mask 10 and the frame connected to each other.

[0069] Despite the fine adjustment of the tensile force F1-F2 applied to each side of the strip mask 10, the problem of poor alignment between the mask units C1-C3 still occurs. For example, the distances between the patterns P of the units C1-C6 are different from each other or the patterns P are skewed. Since the strip mask 10 has a large area including a plurality of units C1-C6 and has a very thin thickness of tens of μm, it is easy to sag or twist due to the load. In addition, it is a very difficult task to adjust the tensile force F1-F2 to make all the units C1-C6 flat while confirming the alignment status between the units C1-C6 in real time through a microscope. However, in order to avoid the mask pattern P with a size of several μm to tens of μm from having a bad influence on the pixel process of the ultra-high-quality OLED, the alignment error is preferably not more than 3 μm. The alignment error between such adjacent units is called pixel position accuracy (PPA).

[0070] Furthermore, it is a very difficult task to connect each strip mask 10 to a frame 20 respectively and to accurately align the multiple strip masks 10 and the multiple units C1-C6 of the strip mask 10, which will only increase the process time based on alignment, thereby becoming an important reason for reducing production efficiency.

[0071] In addition, after the strip mask 10 is connected and fixed to the frame 20, the tensile force F1-F2 applied to the strip mask 10 will act inversely on the frame 20. This tension will cause the frame 20 to deform slightly, and the alignment state of the plurality of cells C1-C6 will be distorted.

[0072] In view of this, the present invention proposes a frame 200 and a frame-integrated mask that can form an integrated structure of the mask 100 and the frame 200. The mask 100 integrated with the frame 200 can not only prevent deformation such as sagging or twisting, but also can be accurately aligned with the frame 200.

[0073] Figure 2 is a front view of a frame-integrated mask according to an embodiment of the present invention. Figure 2 (a)] and side cross-sectional view [ Figure 2 (b)].

[0074] Although this specification describes the configuration of the frame-integrated mask, the structure and manufacturing process of the frame-integrated mask include the entire contents of Korean Invention Patent Application No. 2018-0016186.

[0075] Reference Figure 2, the frame-integrated mask may include a plurality of masks 100 and a frame 200. In other words, the plurality of masks 100 are attached to the frame 200. Below, for the sake of convenience, a quadrangular mask 100 is used as an example for explanation, but before the mask 100 is attached to the frame 200, it may be a strip-shaped mask with protrusions on both sides for clamping, and the protrusions may be removed after being attached to the frame 200.

[0076] A plurality of mask patterns P are formed on each mask 100, and one cell C may be formed on one mask 100. One mask cell C may correspond to one display of a smartphone or the like.

[0077] The mask 100 may also be made of materials such as invar, super invar, nickel (Ni), nickel-cobalt (Ni-Co), etc. The mask 100 may be made of a metal sheet produced by a rolling process or electroforming.

[0078] The frame 200 may be formed in a form of attaching a plurality of masks 100. Considering thermal deformation, the frame 200 is preferably formed of a material such as Invar, Super Invar, nickel, nickel-cobalt, etc. having the same thermal expansion coefficient as the mask. The frame 200 may include an edge frame portion 210 having a substantially quadrangular shape or a square frame shape. The interior of the edge frame portion 210 may be hollow.

[0079] In addition, the frame 200 has a plurality of mask unit regions CR, and may include a mask unit sheet portion 220 connected to the edge frame portion 210. The mask unit sheet portion 220 may be composed of an edge sheet portion 221, a first grid sheet portion 223, and a second grid sheet portion 225. The edge sheet portion 221, the first grid sheet portion 223, and the second grid sheet portion 225 are portions divided on the same sheet, and they are integrated with each other.

[0080] The thickness of the edge frame portion 210 may be greater than that of the mask unit sheet portion 220, and may be formed with a thickness of several mm to several tens of cm. Although the thickness of the mask unit sheet portion 220 is thinner than that of the edge frame portion 210, it is thicker than the mask 100, and may be approximately 0.1 mm to 1 mm. The width of the first grid sheet portion 223 and the second grid sheet portion 225 may be approximately 1-5 mm.

[0081] In the planar sheet, a plurality of mask unit regions CR (CR11-CR56) may be provided except for the regions occupied by the edge sheet portion 221, the first grid sheet portion 223, and the second grid sheet portion 225.

[0082] The frame 200 has a plurality of mask unit regions CR, and each mask 100 can be attached in a manner that each mask unit C corresponds to each mask unit region CR. The mask unit C corresponds to the mask unit region CR of the frame 200, and part or all of the dummy portion can be attached to the frame 200 (mask unit sheet portion 220). Therefore, the mask 100 and the frame 200 can form an integrated structure.

[0083] Figure 3 is a schematic diagram of a mask 100 according to an embodiment of the present invention.

[0084] The mask 100 may include a mask unit C formed with a plurality of mask patterns P and a dummy portion DM around the mask unit C. The mask 100 may be manufactured using a metal sheet produced by a rolling process, electroforming, etc., in which one unit C is formed. The dummy portion DM corresponds to a portion of the mask metal film 110 other than the unit C, and may include only the mask metal film 110, or include the mask metal film 110 formed with a predetermined dummy portion pattern similar to the mask pattern P. The dummy portion DM corresponds to the edge of the mask 100, and a part or all of the dummy portion DM may be attached to the frame 200 (mask unit sheet portion 220).

[0085] The width of the mask pattern P may be less than 40 μm, and the thickness of the mask 100 may be about 5-20 μm. Since the frame 200 includes a plurality of mask unit regions CR (CR11-CR56), a plurality of masks 100 may be included, each of which includes a mask unit C (C11-C56) corresponding to each mask unit region CR (CR11-CR56).

[0086] Reference Figure 4 (a) may provide a template 50. The template 50 is a medium having a mask 100 attached to one side thereof and supporting the mask 100 to move the mask 100. One side of the template 50 is preferably a flat surface to support and carry the flat mask 100. The center portion 50a may correspond to the mask unit C of the mask metal film 110, and the edge portion 50b may correspond to the dummy portion DM of the mask metal film 110. In order to support the mask metal film 110 as a whole, the template 50 is a flat shape having an area larger than the mask metal film 110.

[0087] In order to allow the laser L irradiated from the upper part of the template 50 to reach the welding part WP (the area where welding is performed) of the mask 100, a laser passing hole 51 may be formed on the template 50. The laser passing hole 51 may be formed on the template 50 in a manner corresponding to the position and number of the welding part WP. Since a plurality of welding parts WP are arranged at predetermined intervals on the edge or dummy part DM of the mask 100, a plurality of laser passing holes 51 may also be formed at predetermined intervals corresponding thereto. As an example, since a plurality of welding parts WP are arranged at predetermined intervals on the dummy part DM on both sides (left / right) of the mask 100, a plurality of laser passing holes 51 may also be formed on both sides (left / right) of the template 50 at predetermined intervals.

[0088] The position and number of the laser through holes 51 do not necessarily correspond to the position and number of the welding part WP. For example, the laser L may be irradiated only to a part of the laser through holes 51 to perform welding. In addition, the laser through holes 51 that do not correspond to the welding part WP may also be used as alignment marks when aligning the mask 100 and the template 50. If the material of the template 50 is transparent to the laser L, the laser through holes 51 may not be formed.

[0089] A temporary adhesive part 55 may be formed on one side of the template 50. The temporary adhesive part 55 may temporarily attach the mask 100 or the mask metal film 110 to one side of the template 50 and support the template 50 before the mask 100 is attached to the frame 200.

[0090] The temporary adhesive portion 55 may use an adhesive that is removable by heating or an adhesive that is removable by irradiating UV.

[0091] As an example, the temporary adhesive portion 55 may use liquid wax. The liquid wax may use the same wax as that used in the polishing step of semiconductor wafers, etc., and its type is not particularly limited. As a resin component mainly used to control the adhesion force, impact resistance, etc. related to the retention force, the liquid wax may include substances such as acrylic acid, vinyl acetate, nylon and various polymers and solvents. As an example, the temporary adhesive portion 55 may use SKYLIQUIDABR-4016 including acrylonitrile butadiene rubber (ABR) as a resin component and n-propanol as a solvent component. The liquid wax is formed on the temporary adhesive portion 55 using a spin coating method.

[0092] The temporary adhesive part 55 as liquid wax has a lower viscosity at a temperature higher than 85° C.-100° C., and increases in viscosity at a temperature lower than 85° C., and a part of it is cured into a solid, thereby fixing and bonding the mask metal film 110 and the template 50 .

[0093] Secondly, refer to Figure 4(b), the mask metal film 110 may be bonded to the template 50. Liquid wax may be heated to above 85°C, and the mask metal film 110 may be brought into contact with the template 50, and then the mask metal film 110 and the template 50 may be passed between rollers for bonding.

[0094] According to one embodiment, the template 50 is baked at about 120° C. for 60 seconds to vaporize the solvent of the temporary adhesive portion 55, and then the mask metal film lamination process can be performed immediately. The lamination is performed by loading the mask metal film 110 on the template 50 having the temporary adhesive portion 55 formed on one side and passing it between an upper roll at about 100° C. and a lower roll at about 0° C. As a result, the mask metal film 110 can contact the template 50 by sandwiching the temporary adhesive portion 55.

[0095] After the mask metal film 110 is bonded to the template 50, one side of the mask metal film 110 may be planarized. The thickness of the mask metal film 110 manufactured by the rolling process may be reduced by the planarization process. In addition, the mask metal film 110 manufactured by the electroforming process may be planarized to control its surface characteristics and thickness. In addition, the mask metal film 110 may be planarized before being bonded to the template 50. The thickness of the mask metal film 110 may be about 5 μm to 20 μm.

[0096] In addition, when the mask metal film 110 is formed by etching the mask metal film 110, the etching liquid should be prevented from entering the interface between the mask metal film 110 and the temporary bonding portion 55 to damage the temporary bonding portion 55 / template 50, thereby causing an etching error of the mask pattern P. Therefore, in a state where the first insulating portion 23 is formed on one side of the mask metal film 110, the mask metal film 110 is bonded to the upper surface of the template 50. That is, the surface of the mask metal film 110 on which the first insulating portion 23 is formed can be directed toward the upper surface of the template 50. The mask metal film 110 and the template 50 can be bonded to each other by sandwiching the first insulating portion 23 and the temporary bonding portion 55.

[0097] The first insulating portion 23 may be formed on the mask metal film 110 by a printing method or the like using a photoresist material that is not etched by an etching solution. In addition, in order to maintain a circular shape after multiple wet etching processes, the first insulating portion 23 may include at least one of a curable negative photoresist and a negative photoresist containing an epoxy resin. As an example, it is preferred to use an epoxy-based SU-8 photoresist or a black matrix photoresist to achieve the baking of the temporary bonding portion 55 and the baking of the second insulating portion 25 (see Figure 5 (c) and the like are solidified together during the process.

[0098] Due to the material characteristics of the first insulating portion 23, even if the second insulating portion 25 is formed [refer to Figure 5 (c)] and then multiple subsequent etching processes will not be dissolved by the etching solution. If the first insulating portion 23 does not exist, the etching solution can enter the interface between the damaged temporary bonding portion 55 and the mask metal film 110, and further etch the lower part of the first mask pattern P, which will cause the pattern size to be too large or a local amorphous defect. As the present invention further sandwiches the first insulating portion 23, in the process of forming the mask pattern P using multiple processes, even if the mask metal film 110 is penetrated, the pattern width will not be further expanded, so that the pattern width of the second insulating portion 25 can be maintained.

[0099] Although the first insulating portion 23 and the temporary adhesive portion 55 are shown as being formed on the upper surface of the template 50, they may be formed on the lower surface of the mask metal film 110. In addition, the first insulating portion 23 and the temporary adhesive portion 55 may be formed on the template 50 and the mask metal film 110, respectively.

[0100] Then, refer to Figure 5 (c), the patterned second insulating portion 25 may be formed on the mask metal film 110. The second insulating portion 25 may be formed of photoresist using a printing method or the like.

[0101] Next, the mask metal film 110 may be etched. Dry etching, wet etching, or the like may be used without limitation, and as a result of the etching, the portion of the mask metal film 110 exposed by the empty space 26 between the second insulating portions 25 may be etched away. The etched portion of the mask metal film 110 forms a mask pattern P, and thus a mask 100 having a plurality of mask patterns P formed therein may be manufactured.

[0102] Then, refer to Figure 5 (d), the manufacturing of the template 50 supporting the mask 100 may be completed by removing the second insulating portion 25 .

[0103] in addition, Figure 5 Although the process of forming the mask pattern P after the mask metal film 110 is bonded to the template 50 is described in (d), it is not limited thereto and can be performed by Figure 4 (a) and (b) are to form a mask 100 having a mask pattern P (refer to Figure 3 ) is bonded to the template 50, thereby completing the manufacture of the template 50 for supporting the mask 100.

[0104] Since the frame 200 has a plurality of mask unit regions CR (CR11-CR56), a plurality of masks 100 having mask units C (C11-C56) corresponding to each mask unit region CR (CR11-CR56) may also be provided. In addition, a plurality of templates 50 may be provided for supporting each of the plurality of masks 100, respectively.

[0105] Figure 6 This is a schematic diagram of a problem that occurs when the thermal expansion coefficient of the template is higher than that of the mask according to the comparative example.

[0106] Reference Figure 6 (a), the process temperature of the space where the mask metal film 110 or the mask 100 and the template 50' are bonded is raised to a temperature T1 higher than the normal temperature. The process temperature T1 may be 85°C-100°C at which the viscosity of the temporary bonding part 55 is reduced. Next, the solvent of the temporary bonding part 55 is vaporized by baking, and the mask metal film 110 is bonded to the template 50'. Then, the process temperature may be lowered to a temperature T2 at which the viscosity of the temporary bonding part 55 becomes large and a part of it can be solidified.

[0107] Conventionally, glass, borosilicate glass, and the like have been used as materials for the template 50 ′. Among them, BOROFLOAT, which is borosilicate glass, is particularly ® The thermal expansion coefficient of 33 is about 3.3X10 -6 / ℃, and its thermal expansion coefficient is about 1.5-3 X 10 -6 The thermal expansion coefficient difference of the invar mask metal film 110 of 1.5477 W / °C is small, and the mask metal film 110 is easy to control, so it is often used.

[0108] The thermal expansion coefficient of the template 50' is higher than that of the mask metal film 110. Figure 6 As shown in (a), when the temperature T2 is lowered, the degree L2 of contraction of the mask metal film 110 due to the temperature change is relatively small, and on the contrary, the degree L1 of contraction of the template 50' is relatively large (L1>L2). At the same time, the template 50' and the mask metal film 110 are firmly bonded and fixed with the temporary bonding portion 55 sandwiched therebetween, and the mask metal film 110 is subjected to a force CT that further contracts than the original degree L2 of contraction. The force CT that further contracts is generated because the degree L1 of contraction of the template 50' is greater than the degree L2 of contraction of the mask metal film 110. Therefore, the mask metal film 110 is bonded to the template 50' in a state where a compressive force CT is applied in the lateral direction (inside the mask metal film 110).

[0109] If the thermal expansion coefficient of the template 50 ′ is higher than that of the mask 100 or the mask metal film 110 , the following problems may occur.

[0110] Reference Figure 6 (b), by Figure 6 The template 50 ′ of (a) is loaded on the frame 200 (or the edge sheet portion 221 , the first grid sheet portion 223 , and the second grid sheet portion 225 ) so as to correspond to the mask 100 , and a weld bead WB is formed by welding, so that the mask 100 can be attached to the frame 200 .

[0111] Furthermore, the template 50' can be separated from the mask 100. However, when the template 50' is separated from the mask 100, the compressive force CT applied to the mask 100 is released, which may cause the alignment state of the mask 100 to be disturbed. In other words, the mask 100 cannot be attached to the frame 200 in a state where both sides are pulled tightly toward the outside, but is attached to the frame 200 in a wrinkled or sagging state. This will cause product defects based on alignment errors of the mask 100, PPA errors between cells C, and the like.

[0112] Therefore, the template 50 of the present invention has a characteristic of having a lower thermal expansion coefficient than the mask 100 or the mask metal film 110 .

[0113] Figure 7 3 is a schematic diagram of an interface state between a mask and a template and a state where the mask is attached to a frame when the thermal expansion coefficient of the template is lower than that of the mask according to an embodiment of the present invention.

[0114] Reference Figure 7 (a), such as Figure 6 As shown in (a), the process temperature of the space where the process is performed is raised to a temperature T1 higher than the normal temperature, and the mask metal film 110 or the mask 100 having the pattern P formed thereon is bonded to the template 50. Then, the process temperature can be lowered to a temperature T2 at which the viscosity of the temporary bonding portion 55 becomes high and a part of it can be cured into a solid.

[0115] The mask metal 110 or the mask 100 is made of materials such as Invar, Super Invar, nickel, nickel-cobalt, etc., whose thermal expansion coefficient is at least greater than 1. Conversely, the thermal expansion coefficient of the template 50 may be less than 1 (greater than 0). It is preferred to use a template 50 made of quartz material with a thermal expansion coefficient of 0.55, but it is not limited thereto.

[0116] Since the thermal expansion coefficient of the template 50 is lower than that of the mask metal film 110, Figure 7 As shown in (a), when the temperature T2 is lowered, the template 50 hardly shrinks or shrinks to a relatively smaller extent than the mask metal film 110. The shrinkage degree of the mask metal film 110 [shrinkage Figure 7Although the L2 degree of (a) is relatively large, the mask metal film 110 is firmly bonded to the template 50 by sandwiching the temporary bonding portion 55, so it cannot shrink and is subjected to the internal force IT that wants to shrink. In other words, the mask metal film 110 is subjected to the tensile force IT in the lateral direction and is bonded to the template 50 in a taut state.

[0117] Reference Figure 7 (b) Figure 6 In the state (a), the template 50 is loaded on the frame 200 (or the edge sheet portion 221 , the first grid sheet portion 223 , and the second grid sheet portion 225 ) so as to correspond to the mask 100 , and a weld bead WB is formed by welding, so that the mask 100 can be bonded to the frame 200 .

[0118] In addition, the template 50 can be separated from the mask 100. However, when the template 50 is separated from the mask 100, the tensile force IT applied to the mask 100 is released and converted into a tension TS that tightens both sides of the mask 100. In other words, this state is a state in which the mask 100 is bonded to the template 50 after being pulled to a length longer than the original length of the mask 100 at the drop temperature T2. Since the mask 100 is welded and bonded to the frame 200 intact in this state, the pulled state (the state in which the mask unit sheet 220 itself applies tension TS to the surrounding mask unit sheet 220) can be maintained. The mask 100 is attached to the frame 200 in a state of being pulled tightly, so that wrinkles, deformation, etc. will not occur. Therefore, there is an effect of reducing the alignment error of the mask 100 and the PPA error between the units C.

[0119] Figure 8 FIG. 5 is a schematic diagram of the extension state of the mask metal film 110 and the template 50 in response to the process temperature change according to an embodiment of the present invention.

[0120] In addition, if Figure 7 Although the internal force IT (or tensile force IT) can be applied to the mask metal film 110 or the mask 100 by setting the thermal expansion coefficient of the template 50 to be lower than the thermal expansion coefficient of the mask metal film 110, the temperature rises to bond the mask metal film 110 to the template 50 is 85-100°C. Within this range, the difference in the degree of thermal expansion between the template 50 and the mask metal film 110 is not large, and the bonding is performed under the condition that the bonding strength of the temporary bonding portion 55 is sufficiently large. Therefore, there is a limitation that the tensile force IT contained in the mask metal film 110 is not large.

[0121] Therefore, the present invention is characterized in that Figure 8 As shown, compared Figure 7 In the embodiment, the process temperature is further controlled to further increase the stretching of the mask metal film 110 or the stretching force IT. Figure 8In (a), in order to compare the expansion and contraction degree of the mask metal film 110 and the template 50 , their initial lengths are the same, but the initial length of the template 50 may be greater than or equal to that of the mask metal film 110 .

[0122] Reference Figure 8 (a) prepare the template 50 and the mask metal film 110 or the mask 100 formed with the mask pattern P at room temperature (RT) of about 25° C. The first insulating portion 23 and the temporary adhesive portion 55 may be formed on one side of the template 50 or / and the mask metal film 110 .

[0123] Next, refer to Figure 8 (b), the process temperature may be raised to a level where the push-pull strength of the temporary adhesive portion 55 becomes 0 to 5 kgf / cm 2 The first process temperature TS1 may be about 110-200° C. The temporary bonding part 55 may be 0 to 5 kgf / cm 2 , the temporary adhesive portion 55 is equivalent to a state in which it does not have an adhesive force capable of bonding the mask metal film 110 and the template 50. That is, it is difficult to bond the mask metal film 110 and the template 50 when the temporary adhesive portion 55 is non-adhesive. This state can be understood as a state in which the mask metal film 110 and the template 50 are easily separated even without applying a load or external force. Therefore, even if the temporary adhesive portion 55 (and the first insulating portion 23) are sandwiched in between, there is only contact but no bonding between the mask metal film 110 and the template 50. The mask metal film 110 is not hindered by the temporary adhesive portion 55 and extends linearly as the temperature rises. In addition, the thermal expansion coefficient of the mask metal film 110 is smaller than the thermal expansion coefficient of the template 50, so the extension degree L1 of the mask metal film 110 at the first process temperature TS1 can be greater than the extension degree L2 of the template 50.

[0124] Next, refer to Figure 8 (c), the process temperature can be lowered to a second process temperature TS2 when the mask metal film 110 is in contact with the template 50, and the bonding strength of the temporary bonding portion 55 is at least greater than 5 kgf / cm 2 The second process temperature TS2 may be less than 85-100°C and greater than room temperature. As the temporary bonding portion 55 exhibits bonding force at the second process temperature TS2, the mask metal film 110 and the template 50 may be bonded. As the temperature decreases, the template 50 may shrink (L2->L3), and the mask metal film 110 may shrink accordingly.

[0125] only, Figure 8When the process temperature decreases (TS1->TS2) from step (b) to step (c), the temporary bonding portion 55 is cooled and solidified first, while the temperature decrease rate of the mask metal film 110 is delayed compared to the temporary bonding portion 55. Figure 7 In the case of the mask metal film 110, the mask metal film 110 can be bonded to the template 50 in a further extended state. Figure 7 When the mask metal film 110 and the template 50 are bonded after the temperature rises to the second process temperature TS2 immediately at room temperature RT, as shown in FIG. Figure 8 Between the room temperature T and the second process temperature TS2, by further adding a step of raising the temperature to the first process temperature TS1, the mask metal film 110 can be bonded to the template 50 in a further extended state. When the mask metal film 110 and the template 50 are bonded after the temperature is immediately raised to the second process temperature TS2 at the room temperature RT, the mask metal film 110 will be blocked by the temporary bonding part 55 due to the considerable bonding force in the temporary bonding part 55, and thus will not linearly extend even if the temperature rises. The further extension of the mask metal film 110 corresponds to a further increase in the tensile force IT contained in the mask metal film 110 or the mask 100 supported by the template 50, which means that the mask 100 can be kept in a more taut state after the mask 100 is matched / attached to the frame 200 in the subsequent process.

[0126] Next, refer to Figure 8 (e), the process temperature can be lowered to room temperature RT. As the temperature drops, the template 50 shrinks (about L3), and the mask metal film 110 shrinks accordingly. The template 50 can be restored to Figure 8 The length of the mask metal film 110 at the initial room temperature RT state is (a), and the mask metal film 110 can be bonded and fixed to the template 50 in a state further extended by L5 than the initial room temperature RT. The degree of extension L5 and the tensile force IT contained in the mask metal film 110 are greater than Figure 7 to the extent described in .

[0127] In addition, Figure 8 Between step (c) and step (e), a process of lowering the process temperature to a process temperature TS3 lower than the room temperature RT may be further performed. Then, the temperature may be raised to the room temperature RT again. As the temperature is lowered to the process temperature TS3, the template 50 will shrink more than the room temperature state by L4, and the mask metal film 110 will shrink accordingly. The process temperature TS3 may be about 5-15°C. In addition, the maintenance time of the process temperature TS3 may be at least greater than or equal to Figure 8The maintenance time of process temperatures TS1 and TS2 of (b) and (c) is determined. For example, assuming that the maintenance time of TS1 is 10 minutes and the maintenance time of TS2 is 5 minutes, the maintenance time of TS3 can be more than 10 minutes. By the above-mentioned rapid cooling rather than slow cooling, the viscosity of the temporary bonding part 55 increases, thereby further increasing the bonding strength. As the bonding strength of the temporary bonding part 55 is maximized, the mask metal film 110 and the template 50 can be further firmly bonded. Figure 8 The length of the mask metal film 110 further extended in step (b) can still be maintained after the temperature drops.

[0128] In addition, the process temperature of the process area for arranging the mask 100 and the template 50 can be controlled by heating / cooling means. In addition, the process temperature can also be controlled by applying specific energy such as plasma, UV, laser, etc. to the mask 100 and the template 50.

[0129] Fig. 9 1 is a comparison data between the initial design size of the mask and the size after the process is completed according to an experimental example of the present invention. Fig. 9 (a) and (c) show the initial state of the two samples, and (b) and (d) show the execution Figure 8 The state after the process. Three points are set at the upper, middle and lower parts of the mask metal film 110 or the mask 100 and the sizes are compared. The parts indicated by dotted lines in (a)-(d) correspond to the areas (mask units C) where the mask pattern P is arranged with predetermined design values, and the parts indicated by solid lines are actual measured values.

[0130] Comparing (a) with (b) and (c) with (d), we can see that when executing Figure 8 After the process, the dotted lines have a larger spacing than the solid lines. This means that the mask metal film 110 is extended compared to the same point. Comparing (a) and (b), it can be seen that it is further extended by about 1.6μm in the X-axis (short side) direction and about 4.3μm in the Y-axis (long side) direction. Comparing (c) and (d), it can be seen that it is further extended by about 0.9μm in the X-axis direction and about 3.3μm in the Y-axis direction.

[0131] Fig.10 Schematic diagram of a method for measuring the total pitch of a mask before and after a process according to an experimental example of the present invention.

[0132] The conditions in Table 1 were as follows. Figure 7 and Figure 8 technology.

[0133] Table 1

[0134]

[0135] Experimental Examples 1 to 3 correspond to Figure 7 Process, Experimental Examples 5, 6 and 8 correspond to Figure 8 In Experiment 4, only the initial rising temperature TS2 corresponds to Figure 8 process, Experimental Example 7 corresponds to Figure 8 A process in which the step of descending to TS2 is omitted and the process is directly cooled to TS3.

[0136] Fig.10 The method of measuring the extended state of the mask 100 after the process is performed is shown. The portion of the mask 100 that is actually attached to the frame 200 (mask unit sheet portion 220) and functions as the mask unit C is the portion where the mask pattern P is formed, so the extended state can be measured based on the position of the mask pattern P other than the dummy portion DM. The distance between the mask patterns P located at the end of the mask unit C is called the total pitch (TP).

[0137] Reference Fig.10 , when the mask 100 has a pair of long sides (X-axis sides) and a pair of short sides (Y-axis sides), if the mask 100 is equally divided into three regions along the short side direction, then in each region, any straight lines S1, S2, and S3 are extended in a direction perpendicular to the short side, and the average value (X-axis TP) of the distance from the mask pattern P arranged at one end to the mask pattern P arranged at the other end in the arbitrary straight lines S1, S2, and S3 can be calculated. In addition, if the mask 100 is equally divided into three regions along the long side direction, then in each region, any straight lines S4, S5, and S6 are extended in a direction perpendicular to the long side direction, and the average value (Y-axis TP) of the distance from the mask pattern P arranged at one end to the mask pattern P arranged at the other end in the arbitrary straight lines S4, S5, and S6 can be calculated.

[0138] The following table shows the X-axis (long axis) TP and Y-axis (short axis) TP of Experimental Examples 1-8. The average value of each axis can be calculated by measuring the TP of three areas. Figure 8 The TP value measured after the process is deducted from the execution Figure 7 The TP value is obtained by measuring the TP value after the process. Figure 8 The TP value measured after the process is deducted Fig. 9 The predetermined design values ​​described in Fig. 9 The TP was measured for three samples in Experimental Examples 1-7, and for two samples 2 in Experimental Example 8. The bonding strength of the temporary bonding portion 55 in each experimental example was about 40 kgf / cm 2 (-4MPa). The unit of the values ​​in the table is μm.

[0139] Table 2

[0140]

[0141] Referring to Table 2, it can be seen that the average of △TP in Experimental Examples 1 to 3 is negative rather than positive. Figure 8 The average of ΔTP is a positive number in Experimental Examples 5, 6, and 8 of the process. In particular, it can be confirmed that the absolute value of ΔTP increases as Experimental Examples 5, 6, and 8 are performed, that is, as the initial temperature rise TP2 increases.

[0142] In particular, ΔTP is preferably about 0.1 μm-20.0 μm based on the long axis, and is preferably about 0.1 μm-15.0 μm based on the short axis. If it is smaller than the above-mentioned reference, it is difficult for the mask 100 to maintain a sufficiently tight state on the frame 200. If it is larger than the above-mentioned reference, the tension applied by the mask 100 on the frame 200 increases, which increases the possibility of alignment errors in the mask pattern P, and may cause wrinkles in parts of the mask 100.

[0143] Fig.11 It is a curve diagram of the measurement results of the total mask spacing before and after each process according to an experimental example of the present invention. T1-T5 are the initial rising temperatures TP2, corresponding to 120°C-150°C respectively.

[0144] Reference Fig.11 It can be seen that Figure 8 The higher the initial temperature rise TP2 in the process, the larger △TP becomes. Fig.10 The same is true for Experimental Examples 5, 6, and 8. That is, it was confirmed that the mask metal film 110 was adhered and fixed to the template 50 in a state where the degree of extension became greater as the initial rise temperature TP2 increased.

[0145] Fig.12 2 is a schematic diagram of a process of placing a weight MS on the mask 100 to measure tension after the mask 100 is attached to the frame 200 according to an experimental example of the present invention.

[0146] The mask 100 was attached to the frame 200 (the mask unit sheet portions 220: 223, 225), and a 50 g weight MS was placed at the center of the mask 100 to measure the sagging amount of the mask unit sheet portions 220: 223, 225 relative to the mask 100. In the following table, Experimental Examples 9 and 10 were not performed. Figure 8 process, Experiments 11 and 12 were performed Figure 8 Process Status In the initial state, the height of the mask unit sheet portion 220 is 0, which is a reference value, and Δ(OM) shows the sagging amount (μm) of the mask unit sheet portion 220 when the weight MS is placed on the mask 100 .

[0147] Table 3

[0148]

[0149] Referring to Table 3, it can be seen that the mask 100 of Experimental Examples 11 and 12 has a large tensile force from the beginning and is tightly attached to the mask unit sheet portion 220, so the height is low. It can be confirmed that the deformation amount △ (OM) of the mask unit sheet portion 220 remains almost constant. In addition, for the case where the weight MS is placed on the mask 100, the average value in Experimental Examples 9 and 10 is -750, while the average value in Experimental Examples 11 and 12 is -708, and the sagging amount is reduced by 42μm. This means that the mask 100 is subjected to a large tensile force IT or tension TS (refer to Fig.15 ) is attached to frame 200.

[0150] Fig.13 1 is a schematic diagram of a state in which the template 50 is loaded on the frame 200 and the mask 100 is aligned with the unit region CR of the frame 200 according to an embodiment of the present invention. Fig.13 , a method of corresponding / attaching one mask 100 to the unit region CR is listed, but a process of simultaneously corresponding multiple masks 100 to all unit regions CR and attaching the masks 100 to the frame 200 can also be performed. In this case, there can be multiple templates 50, which are used to support each of the multiple masks 100 respectively.

[0151] The template 50 can be transferred by the vacuum suction cup 90. The vacuum suction cup 90 can be used to suck the opposite side of the template 50 to which the mask 100 is bonded and transferred. After the vacuum suction cup 90 sucks the template 50 and flips it, the bonding state and alignment state of the mask 100 are not affected during the process of transferring the template 50 to the frame 200.

[0152] Next refer to Fig.13 , the mask 100 can be matched to a mask unit region CR of the frame 200. The mask 100 can be matched to the mask unit region CR by loading the template 50 to the frame 200 (or the mask unit sheet portion 220). While controlling the position of the template 50 / vacuum suction cup 90, it is possible to observe through a microscope whether the mask 100 corresponds to the mask unit region CR. Since the template 50 presses the mask 100, the mask 100 can be closely attached to the frame 200.

[0153] In addition, a lower support 70 may be further disposed below the frame 200. The lower support 70 may press the reverse side of the mask unit region CR in contact with the mask 100. At the same time, since the lower support 70 and the template 50 press the edge of the mask 100 and the frame 200 (or the mask unit sheet portion 220) in opposite directions to each other, the alignment state of the mask 100 can be maintained and not disturbed.

[0154] Next, laser L is irradiated to the mask 100 and the mask 100 is attached to the frame 200 by laser welding. Welding beads WB are generated on the welding part WP of the mask by laser welding, and the welding beads WB may have the same material as the mask 100 / frame 200 and be integrally connected with them.

[0155] Fig.14 FIG. 2 is a schematic diagram of a process of separating the mask from the template after attaching the mask to the frame according to an embodiment of the present invention.

[0156] Reference Fig.14 After the mask 100 is attached to the frame 200, the mask 100 can be separated from the template 50 (debonding). The separation of the mask 100 from the template 50 can be performed by heating the temporary adhesive portion 55, chemically treating the temporary adhesive portion 55, applying ultrasonic waves, and applying ultraviolet rays. Since the mask 100 remains attached to the frame 200, only the template 50 can be lifted. As an example, if a heat ET higher than 85°C-100°C is applied, the viscosity of the temporary adhesive portion 55 is reduced, and the adhesive force between the mask 100 and the template 50 is weakened, so that the mask 100 and the template 50 can be separated. As another example, the temporary adhesive portion 55 can be separated from the template 50 by immersing the temporary adhesive portion 55 in a chemical substance such as IPA, acetone, ethanol, etc., so that the temporary adhesive portion 55 is dissolved, removed, etc. As another example, the adhesive force between the mask 100 and the template 50 is weakened by applying ultrasonic waves US or applying ultraviolet rays UV, so that the mask 100 and the template 50 can be separated.

[0157] If the template 50 is separated from the mask 100, the tensile force IT applied to the mask 100 is released and converted into a tension TS that tightens both sides of the mask 100. Thus, the mask 100 can be attached in a tightened state by applying the tension TS to the frame 200 (mask unit sheet 220).

[0158] Fig.15 2 is a schematic diagram of a state where the mask 100 is attached to the frame 200 according to an embodiment of the present invention. Fig.15 2 shows a state where all the masks 100 are attached to the unit region CR of the frame 200. Although the masks 100 may be attached one by one and then the templates 50 may be separated, all the masks 100 may be attached and then all the templates 50 may be separated.

[0159] Existing Figure 1The mask 10 of the present invention includes 6 units C1-C6 and thus has a longer length, while the mask 100 of the present invention includes one unit C and thus has a shorter length, so the degree of PPA (pixel position accuracy) distortion will be reduced. Moreover, since the present invention only needs to correspond to one unit C of the mask 100 and confirm the alignment state, the present invention can significantly shorten the manufacturing time compared to the existing method that corresponds to multiple units C (C1-C6) at the same time and needs to confirm all alignment states.

[0160] If each mask 100 is attached to the corresponding mask unit region CR and then the template 50 and the mask 100 are separated, since the multiple masks 100 will apply tension TS that shrinks in opposite directions, the tensions cancel each other out, so the mask unit sheet portion 220 will not be deformed. For example, on the first grid sheet portion 223 between the mask 100 attached to the CR11 unit region and the mask 100 attached to the CR12 unit region, the tension TS applied to the right direction by the mask 100 attached to the CR11 unit region and the tension TS applied to the left direction by the mask 100 attached to the CR12 unit region can cancel each other out. Therefore, the deformation of the frame 200 (or the mask unit sheet portion 220) due to the tension TS is minimized, thereby having the advantage of minimizing the alignment error of the mask 100 (or the mask pattern P).

[0161] As described above, the present invention lists preferred embodiments for illustration and description, and the present invention is not limited to the above embodiments. Those skilled in the art can make various modifications and changes without departing from the spirit of the present invention. Such modifications and changes all belong to the scope of the present invention and the appended claims.

Claims

1. A mask for forming an OLED pixel, which is supported by a mask support template and attached to a frame, wherein: The mask includes a mask unit formed with a plurality of mask patterns and a dummy portion around the mask unit, the mask having a pair of long sides and a pair of short sides, The mask is manufactured by the following steps (I) or (II), Step (I): (a) preparing a template having a temporary adhesive portion formed on one side; (b) The process temperature is raised to a level where the bonding strength of the temporary bonding portion is 0 to 5 kgf / cm 2 temperature and contacting the mask metal film to the template; (c) The process temperature is lowered to a level where the bonding strength of the temporary bonding portion is at least greater than 5 kgf / cm 2 temperature and bonding the mask metal film to the template; (d) lowering the process temperature to room temperature; (e) manufacturing a mask by forming a mask pattern on a mask metal film, Step (II): (a) preparing a mask having a mask pattern formed thereon; (b) preparing a template having a temporary adhesive portion formed on one side; (c) The process temperature is raised to a level where the bonding strength of the temporary bonding portion is 0 to 5 kgf / cm 2 temperature and contacting the mask to the template; (d) The process temperature is lowered to a level where the bonding strength of the temporary bonding portion is at least greater than 5 kgf / cm 2 temperature and bonding the mask to the template; (e) Lower the process temperature to room temperature, When a mask with a predetermined design value is used, it is manufactured through the following steps: (1) preparing a template having a temporary adhesive portion formed on one side; (2) raising the process temperature to a temperature at which the temporary bonding portion at least bonds the mask metal film and the template, and bonding the mask metal film to the template; (3) Lowering the process temperature to room temperature; (4) manufacturing a mask by forming a mask pattern on a mask metal film, On any straight line parallel to the long side or the short side of the mask, the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end is 0.1 μm to 20.0 μm greater than the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end in a mask using a predetermined design value, The thermal expansion coefficient of the mask is at least greater than 1X10 -6 / ℃, the thermal expansion coefficient of the template is less than 1X10 -6 / ℃ and greater than 0.

2. The OLED pixel forming mask according to claim 1, wherein: When the mask is equally divided into three regions along the long side direction, an arbitrary straight line is extended in a direction perpendicular to the long side in each region, and the average value of the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end on the arbitrary straight line is set as A. When the mask is equally divided into three regions along the short side direction, an arbitrary straight line is extended in a direction perpendicular to the short side in each region, and the average value of the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end on the arbitrary straight line is set as B. In the case of a mask with a predetermined design value, when the mask is equally divided into three regions along the long side direction, an arbitrary straight line is extended in a direction perpendicular to the long side in each region, and the average value of the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end on the arbitrary straight line is set as C. When the mask is equally divided into three regions along the short side direction, an arbitrary straight line is extended in a direction perpendicular to the short side in each region, and the average value of the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end on the arbitrary straight line is set as D. At this time, the values ​​of AC and BD are positive numbers.

3. The OLED pixel forming mask according to claim 2, wherein: The value of AC is 0.1 μm to 20.0 μm, and the value of BD is 0.1 μm to 15.0 μm.

4. The OLED pixel forming mask according to claim 1, wherein: Step (d) comprises the following steps: (d1) lowering the process temperature to below room temperature; (d2) Raise the process temperature to room temperature.

5. The OLED pixel forming mask according to claim 1, wherein: In step (b), the process temperature is raised to 110°C to 200°C, In step (c), the process temperature is lowered to a temperature lower than the process temperature in step (b) and higher than room temperature.

6. The OLED pixel forming mask according to claim 1, wherein: In step (b), the mask metal film is extended further to the side than the template in a state where there is no adhesion between the mask metal film and the template. In step (c), the mask metal film is bonded to the template in an extended state.

7. The OLED pixel forming mask according to claim 6, wherein: As the process temperature in step (b) increases, the mask metal film is bonded and fixed to the template in a state where the degree of extension becomes greater.

8. A mask support template, the template is used to support a mask for forming OLED pixels and correspond the mask to a frame, the mask support template comprising: template; a temporary bonding portion formed on the template; as well as A mask is bonded to the template by interposing a temporary bonding portion and is formed with a plurality of mask patterns, The mask includes a mask unit formed with a plurality of mask patterns and a dummy portion around the mask unit, the mask having a pair of long sides and a pair of short sides, The mask is manufactured by the following steps (I) or (II), Step (I): (a) preparing a template having a temporary adhesive portion formed on one side; (b) The process temperature is raised to a level where the bonding strength of the temporary bonding portion is 0 to 5 kgf / cm 2 temperature and contacting the mask metal film to the template; (c) The process temperature is lowered to a level where the bonding strength of the temporary bonding portion is at least greater than 5 kgf / cm 2 temperature and bonding the mask metal film to the template; (d) lowering the process temperature to room temperature; (e) manufacturing a mask by forming a mask pattern on a mask metal film, Step (II): (a) preparing a mask having a mask pattern formed thereon; (b) preparing a template having a temporary adhesive portion formed on one side; (c) raising the process temperature to a temperature at which the bonding strength of the temporary bonding portion is 0 to 5 kgf / cm2 and contacting the mask to the template; (d) The process temperature is lowered to a level where the bonding strength of the temporary bonding portion is at least greater than 5 kgf / cm 2 temperature and bonding the mask to the template; (e) Lower the process temperature to room temperature, When a mask with a predetermined design value is used, it is manufactured through the following steps: (1) preparing a template having a temporary adhesive portion formed on one side; (2) raising the process temperature to a temperature at which the temporary bonding portion at least bonds the mask metal film and the template, and bonding the mask metal film to the template; (3) Lowering the process temperature to room temperature; (4) manufacturing a mask by forming a mask pattern on a mask metal film, On any straight line parallel to the long side or the short side of the mask, the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end is 0.1 μm to 20.0 μm greater than the distance from the mask pattern arranged at one end to the mask pattern arranged at the other end in a mask using a predetermined design value, The thermal expansion coefficient of the mask is at least greater than 1X10 -6 / ℃, the thermal expansion coefficient of the template is less than 1X10 -6 / ℃ and greater than 0.

9. A method for manufacturing a frame-integrated mask, wherein the frame-integrated mask is integrally formed by at least one mask and a frame for supporting the mask, wherein: The manufacturing method comprises the following steps: (a) loading the mask support template of claim 8 onto a frame having at least one mask unit area, and aligning the mask to the mask unit area of ​​the frame; and (b) Attach the mask to the frame.