Preparation method of high-corrosion-resistance and high-strength precise pipeline

By using silicon nitride ceramic powder lining on 316 stainless steel pipes, the problem of insufficient corrosion resistance and strength in extreme environments of traditional pipes is solved, and high corrosion resistance and high strength precision pipeline preparation is achieved, improving flow efficiency and use Lifespan, while reducing maintenance costs.

CN119061393AInactive Publication Date: 2024-12-03ZHEJIANG JNDIA PIPELINE IND

Patent Information

Application Number
CN202411560073.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-04
Publication Date
2024-12-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional pipes have insufficient corrosion resistance in extreme corrosion environments, insufficient strength and wear resistance, and it is difficult to control the inner wall finish and dimensional accuracy during the preparation process, resulting in reduced performance and high maintenance costs.

Method used

316 stainless steel is used as the substrate, and 70%-80% silicon nitride ceramic powder, 10%-20% water, 1%-10% binder and 1%-5% other additives are used as the lining material. Prepare high corrosion-resistant, high-strength precision pipes through pretreatment, coating, drying and sintering to ensure that the ceramic lining is closely integrated with the substrate.

Benefits of technology

It significantly improves the corrosion resistance and strength of the pipe, improves the inner wall finish and dimensional accuracy, reduces fluid resistance, extends service life and reduces maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119061393A_ABST
    Figure CN119061393A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-corrosion-resistance and high-strength precise pipeline, and relates to the technical field of pipeline preparation, preparation materials of the high-corrosion-resistance and high-strength precise pipeline comprise a base body and a lining, the base body is made of 316 stainless steel, and the lining is prepared from the following materials: 70-80% of ceramic powder made of silicon nitride; 10%-20% of water; 1%-10% of a binder; the total amount of other additives is 1%-5%; the corrosion-resistant pipeline has the beneficial effects that the corrosion resistance of the pipeline is greatly improved by introducing the silicon nitride lining, and the pipeline can stably run for a long time in an extreme corrosion environment without being damaged; through a fine preparation process and strict quality control, the smoothness and the size precision of the inner wall of the pipeline are remarkably improved, the fluid resistance is effectively reduced, and the flowing efficiency is improved; the overall performance of the pipeline is also enhanced by the high strength and wear resistance of the silicon nitride lining, so that the pipeline can bear higher pressure and flow velocity without deformation or wear; the preparation method also has relatively high production efficiency and relatively low cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of pipeline preparation, and in particular to a method for preparing a high-corrosion-resistant and high-strength precision pipeline. Background Art

[0002] In the existing technology, although traditional pipelines such as stainless steel pipelines have good corrosion resistance and mechanical strength to a certain extent, they still have many shortcomings, as detailed below: First, in extremely corrosive environments, such as strong acid, strong alkali, or high temperature and high pressure conditions, the corrosion resistance of traditional pipelines often cannot meet the requirements of long-term stable operation, and they are prone to corrosion perforation or leakage. Secondly, when traditional pipes are subjected to high pressure or high flow rate media, their strength and wear resistance may be insufficient, resulting in the need to increase the pipe wall thickness to enhance strength, but this in turn increases material costs and processing difficulty; In addition, it is often difficult to accurately control the inner wall finish and dimensional accuracy of traditional pipes during the preparation process, which affects the flow efficiency of the fluid and the overall performance of the pipe. Finally, the performance of traditional pipelines will gradually decline due to medium erosion and mechanical wear during long-term use, requiring frequent replacement or repair, which increases maintenance costs and downtime; Therefore, a method for preparing high-corrosion-resistant and high-strength precision pipeline is proposed. Summary of the invention

[0003] 1. Technical issues to be resolved In view of the deficiencies in the prior art, the present invention provides a method for preparing a high-corrosion-resistant and high-strength precision pipeline to solve the problems raised in the above-mentioned background technology.

[0004] (II) Technical solution To achieve the above object, the present invention provides the following technical solution: a method for preparing a high-corrosion-resistant and high-strength precision pipeline, wherein the preparation materials include a substrate and a lining, wherein the substrate is 316 stainless steel, and the preparation materials of the lining include the following: Ceramic powder: 70%-80%, made of silicon nitride; Water: 10%-20%; Binder: 1%-10%; Total amount of other additives: 1%-5%; The preparation method includes the following: 1) Matrix pretreatment: S1. Matrix inspection: Check whether there are cracks on the surface of the pipeline; S2. Matrix treatment: ①. Cleaning: Clean the pipes to remove impurities such as oil, rust, etc. to ensure that the surface is clean and pollution-free; ② Roughening treatment: roughening the inner wall of the substrate; ③ Drying: Dry the pipe thoroughly to prevent moisture from affecting the later sintering effect; 2) Lining preparation: Mixing: Mix the materials for lining preparation; 3) Coating treatment: The detailed process of coating treatment includes the following: Pipe preheating: Before coating, the stainless steel pipe is preheated to improve the adhesion and drying efficiency of the ceramic slurry; Initial coating: Use coating equipment to evenly coat the ceramic slurry on the inner wall of the stainless steel pipe; Layer-by-layer coating: For pipes that require a thicker lining layer, coating should be done layer by layer. After each layer is coated, it is necessary to wait for it to dry to a certain degree (usually surface dry) before coating the next layer; Inspection and repair: After each layer is applied, carefully check whether there are bubbles, cracks or uncovered areas in the coating layer, and repair them in time; 4) Drying and curing: Allow the coating to dry naturally at room temperature; 5) Sintering treatment: Sinter the dried and solidified substrate to ensure that the ceramic lining layer is dense, defect-free and tightly bonded to the stainless steel substrate; 6) Quality inspection: Appearance inspection: Check whether the coating layer is flat, smooth, free of cracks, bubbles and other defects; Performance test: Conduct corrosion resistance and strength performance tests on the coated pipes; Preferably, other additives include dispersants, thickeners, defoamers, preservatives, pH regulators, and leveling agents.

[0005] Preferably, the stirring furnace needs to be heated when the lining materials are mixed, and the detailed processing parameters are as follows: Stirring time: 30-50min; Stirring speed: 500-800n / min; Stirring temperature: 20-35℃; Stir until the slurry has no obvious particles, lumps, or bubbles.

[0006] Preferably, the substrate is roughened by sandblasting or chemical etching.

[0007] Preferably, the equipment required for sintering is a high temperature furnace, and the sintering parameters of the high temperature furnace are as follows: Sintering time: 1.5-2h; Sintering temperature: 1300-1450℃.

[0008] Preferably, during the initial coating, it is necessary to ensure that there are no bubbles or gaps on the surface.

[0009] Preferably, in the drying process step proposed in step 4), accelerated drying is required when the following situations are encountered: ①. Time constraints: There are strict time limits for production or repair tasks; ②. Unfavorable environmental conditions: If the production environment has high humidity, low temperature or poor ventilation; ③. The coating thickness is large: When the coated silicon nitride ceramic slurry layer is thicker, it takes longer for natural drying to ensure that the moisture and solvent inside the coating are completely volatilized; ④. Improve production efficiency: In large-scale production, in order to improve production efficiency and output, accelerated drying is often used to shorten the production cycle of each batch of products; The methods for accelerating drying include heating drying, vacuum drying and forced ventilation drying; Among them: the heating and drying uses a hot air circulation oven, the hot air temperature is 240-320℃, the hot air time is 1.5-2h, and the wind speed is 2-3.5m / s; Among them: vacuum drying uses a vacuum oven, the vacuum atmospheric pressure is 110-133Pa, the vacuum temperature is 340-460℃, and the time is 1.5-2h; Among them: forced ventilation drying requires the use of a forced ventilation dryer, with a temperature of 65-125°C, a time of 35-85 minutes, a wind speed of 5-6.3m / s, and a humidity of 10%-15%. Preferably, during and after sintering, the following should be noted: ①. Insulation: A insulation stage is set during the sintering process to keep the material at the set temperature for a certain period of time to ensure that the material is fully sintered and achieves the required performance; Among them: the insulation time is 15-20min, and the insulation triggering condition is that the furnace body rises 300-350℃ every time as one cycle.

[0010] ② Heating rate: Control the heating rate to avoid excessive thermal stress inside the material due to rapid heating, which may cause cracking or deformation; Among them: the heating rate does not exceed 8-9℃ / min; ③. Cooling rate: Control the cooling rate to avoid excessive cooling, which may cause residual stress inside the material and affect the performance and service life of the material; Among them: the cooling rate is 5-6.5℃ / min.

[0011] ④. After sintering is completed, the material is cooled to room temperature by natural cooling.

[0012] (III) Beneficial effects Compared with the prior art, the present invention provides a method for preparing a high-corrosion-resistant and high-strength precision pipeline, which has the following beneficial effects: The high-corrosion-resistant and high-strength precision pipelines prepared by the above preparation method have shown significant advantages in overcoming the shortcomings of traditional pipelines, as detailed below: First, the introduction of silicon nitride lining greatly improves the corrosion resistance of the pipeline, enabling it to operate stably for a long time in an extremely corrosive environment without being damaged; Secondly, through sophisticated preparation technology and strict quality control, the inner wall finish and dimensional accuracy of the pipeline have been significantly improved, effectively reducing fluid resistance and improving flow efficiency; In addition, the high strength and wear resistance of the silicon nitride lining also enhances the overall performance of the pipeline, allowing it to withstand higher pressures and flow rates without deformation or wear; Finally, the preparation method also has high production efficiency and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 It is a schematic diagram of the preparation process of the present invention. DETAILED DESCRIPTION

[0014] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0015] The present invention provides a technical solution, embodiment 1: Figure 1 As shown, a method for preparing a high-corrosion-resistant and high-strength precision pipeline, wherein the preparation materials include a substrate and a lining, wherein the substrate is 316 stainless steel, and the preparation materials of the lining include the following: Ceramic powder: 70%-80%, made of silicon nitride; Water: 10%-20%; Binder: 1%-10%; Total amount of other additives: 1%-5%; The preparation method includes the following: 1) Matrix pretreatment: S1. Matrix inspection: Check whether there are cracks on the surface of the pipeline; S2. Matrix treatment: ①. Cleaning: Clean the pipes to remove impurities such as oil, rust, etc. to ensure that the surface is clean and pollution-free; ② Roughening treatment: roughening the inner wall of the substrate; ③ Drying: Dry the pipe thoroughly to prevent moisture from affecting the later sintering effect; 2) Lining preparation: Mixing: Mix the materials for lining preparation; 3) Coating treatment: The detailed process of coating treatment includes the following: Pipe preheating: Before coating, the stainless steel pipe is preheated to improve the adhesion and drying efficiency of the ceramic slurry; Initial coating: Use coating equipment to evenly coat the ceramic slurry on the inner wall of the stainless steel pipe; Layer-by-layer coating: For pipes that require a thicker lining layer, coating should be done layer by layer. After each layer is coated, it is necessary to wait for it to dry to a certain degree (usually surface dry) before coating the next layer; Inspection and repair: After each layer is applied, carefully check whether there are bubbles, cracks or uncovered areas in the coating layer, and repair them in time; 4) Drying and curing: Allow the coating to dry naturally at room temperature; 5) Sintering treatment: Sinter the dried and solidified substrate to ensure that the ceramic lining layer is dense, defect-free and tightly bonded to the stainless steel substrate; 6) Quality inspection: Appearance inspection: Check whether the coating layer is flat, smooth, free of cracks, bubbles and other defects; Performance test: Conduct corrosion resistance and strength performance tests on the coated pipes; In this embodiment, other additives include dispersants, thickeners, defoamers, preservatives, pH regulators, and leveling agents.

[0016] In this embodiment, the stirring furnace needs to be heated when the lining materials are mixed, and the detailed processing parameters are as follows: Stirring time: 30-50min; Stirring speed: 500-800n / min; Stirring temperature: 20-35℃; Stir until the slurry has no obvious particles, lumps, or bubbles.

[0017] In this embodiment, the substrate is roughened by sandblasting or chemical etching.

[0018] Preferably, the equipment required for sintering is a high temperature furnace, and the sintering parameters of the high temperature furnace are as follows: Sintering time: 1.5-2h; Sintering temperature: 1300-1450℃.

[0019] In this embodiment, during the initial coating, it is necessary to ensure that there are no bubbles or gaps on the surface.

[0020] In this embodiment, in the drying process step proposed in step 4), accelerated drying is required when the following conditions are encountered: ①. Time constraints: There are strict time limits for production or repair tasks; ②. Unfavorable environmental conditions: If the production environment has high humidity, low temperature or poor ventilation; ③. The coating thickness is large: When the coated silicon nitride ceramic slurry layer is thicker, it takes longer for natural drying to ensure that the moisture and solvent inside the coating are completely volatilized; ④. Improve production efficiency: In large-scale production, in order to improve production efficiency and output, accelerated drying is often used to shorten the production cycle of each batch of products; The methods for accelerating drying include heating drying, vacuum drying and forced ventilation drying; Among them: the heating and drying uses a hot air circulation oven, the hot air temperature is 240-320℃, the hot air time is 1.5-2h, and the wind speed is 2-3.5m / s; Among them: vacuum drying uses a vacuum oven, the vacuum atmospheric pressure is 110-133Pa, the vacuum temperature is 340-460℃, and the time is 1.5-2h; Among them: forced ventilation drying requires the use of a forced ventilation dryer, with a temperature of 65-125°C, a time of 35-85 minutes, a wind speed of 5-6.3m / s, and a humidity of 10%-15%. In this embodiment, during and after sintering, the following should be noted: ①. Insulation: A insulation stage is set during the sintering process to keep the material at the set temperature for a certain period of time to ensure that the material is fully sintered and achieves the required performance; Among them: the insulation time is 15-20min, and the insulation triggering condition is that the furnace body rises 300-350℃ every time as one cycle.

[0021] ② Heating rate: Control the heating rate to avoid excessive thermal stress inside the material due to rapid heating, which may cause cracking or deformation; Among them: the heating rate does not exceed 8-9℃ / min; ③. Cooling rate: Control the cooling rate to avoid excessive cooling, which may cause residual stress inside the material and affect the performance and service life of the material; Among them: the cooling rate is 5-6.5℃ / min.

[0022] ④. After sintering is completed, the material is cooled to room temperature by natural cooling.

[0023] Embodiment 2: Compared with Example 1, all parameters in Example 2 are within the range described in Example 1, such as Figure 1 As shown, a method for preparing a high-corrosion-resistant and high-strength precision pipeline, wherein the preparation materials include a substrate and a lining, wherein the substrate is 316 stainless steel, and the preparation materials of the lining include the following: Ceramic powder: 70%, made of silicon nitride; Silicon nitride is an important structural ceramic material. It is a superhard material that is lubricating and wear-resistant. It is an atomic crystal and resistant to oxidation at high temperatures. It can also resist thermal shocks. It will not break even if it is heated to over 1000°C in air, cooled rapidly, and then heated rapidly. It is an excellent material for making linings. Water: 20%; Water is the most easily available material with low cost. Silicon nitride powder is insoluble in water and forms a suspension after stirring. Silicon nitride powder is evenly dispersed in water, which is conducive to subsequent coating. That is, silicon nitride powder will not gather in one place with the flow of water, causing uneven coating. Binder: 5%; The binder is a non-metallic medium material that can tightly connect one object to another. The binders used include but are not limited to organic binder epoxy resin, which can be evenly mixed with ceramic powder to form a stable suspension and can form a strong adhesion layer on the stainless steel surface; inorganic binder phosphate binder, which has high high temperature resistance and can form a strong chemical bond with the stainless steel surface to improve the adhesion strength; Total amount of other additives 5%; Other additives include dispersants, thickeners, defoamers, preservatives, pH adjusters, and leveling agents, which are added in the ratio of 1:1:1:1:1:1; Dispersant, to prevent the aggregation of ceramic powder in the formed suspension, improve the stability and fluidity of the suspension, using cationic polyacrylamide, the cationic groups on the molecular chain can interact with the negative charges on the surface of the ceramic powder to form a stable dispersion system; Thickeners increase the viscosity of the suspension, making it easier to apply and disperse. Cellulose thickeners, such as sodium carboxymethyl cellulose, are used. They have good water solubility and form a network structure in the liquid through their long-chain molecular structure, effectively dispersing and stabilizing the ceramic particles. Defoaming agent, a chemical substance that can reduce the surface tension of water, solutions, suspensions, etc., prevent the formation of foam, or reduce or even eliminate the original foam. The defoaming agents used include but are not limited to polyether-modified polysiloxane defoaming agents, which can make the silicon nitride suspension free of gas. After the coating is completed, heating is required, and the gas in the foam will expand and overflow, affecting the uniform distribution of the ceramic powder; Preservatives, the ceramic powder suspension produced is a system with high humidity. At the same time, the thickener added is a cellulose thickener, which provides a potential carbon source and is conducive to the growth and reproduction of microorganisms. Preservatives are used to inhibit the growth of microorganisms. When microorganisms grow and aggregate into groups, they form extracellular polymers. Extracellular polymers have a three-dimensional spatial structure and have an aggregation effect on the ceramic powder in the ceramic powder suspension, causing the ceramic powder to aggregate and disperse unevenly. In actual production, ceramic powder suspensions are produced in large quantities and need to be stored for a long time. Preservatives inhibiting the growth of microorganisms are beneficial to maintaining the stability of the ceramic powder suspension and help to store it for a long time. pH adjuster: pH value will affect the effect of dispersant and thickener. Cationic polyacrylamide is a cationic dispersant, which is more effective in alkaline volume. Under alkaline conditions, the extension of the molecular chain of sodium carboxymethyl cellulose increases, and the biological activity is better exerted. Therefore, pH adjuster is used to adjust the pH value of the suspension system to between 9.2 and 9.8. Leveling agent, which helps the coating to form a flat, smooth and uniform coating during the drying process. Acrylic leveling agent is used to promote the uniform distribution of ceramic powder in the coating, thereby improving the overall performance of the coating. The preparation method includes the following: 1) Matrix pretreatment: S1. Matrix inspection: Check whether there are cracks on the surface of the pipeline; Pipes with cracks are defective raw materials, and the finished products made from them are not of good quality. S2. Matrix treatment: ①. Cleaning: Clean the pipes to remove impurities such as oil, rust, etc. to ensure that the surface is clean and pollution-free; Not only can new 316 stainless steel pipes be used as the substrate, but also the structure of the 316 stainless steel pipes in use can be strengthened. There may be impurities such as oil and rust on the surface of the pipes in use, which need to be cleaned to facilitate subsequent operations. Use hydrochloric acid to remove rust, and use detergent to remove oil. The removal method is to dissolve the impurities and the detergent, and then use a high-pressure water gun to rinse the surface to ensure the surface is clean; ② Roughening treatment: roughening the inner wall of the substrate; The roughening of the inner wall of the substrate is conducive to the adhesion of the ceramic slurry, while the smooth surface easily causes the ceramic slurry to flow under the action of gravity, resulting in uneven coating of the ceramic slurry on the inner wall; ③ Drying: Dry the pipe thoroughly to prevent moisture from affecting the later sintering effect; 2) Lining preparation: Mixing: Mixing the materials for preparing the lining to form a ceramic slurry; 3) Coating treatment: The detailed process of coating treatment includes the following: Pipe preheating: Before coating, the stainless steel pipe is preheated to improve the adhesion and drying efficiency of the ceramic slurry; Initial coating: Use a pipe lining coating machine to evenly coat the ceramic slurry on the inner wall of the stainless steel pipe; Layer-by-layer coating: For pipes that require a thicker lining layer, coating should be done layer by layer. After each layer is coated, it is necessary to wait for it to dry to a certain degree (usually surface dry) before coating the next layer; When the surface is dry, the surface of the coated ceramic slurry solidifies, but still retains the adhesion it had when the slurry was in liquid state. When the next layer is coated, the solidified surface of the previous layer is used as the base, and the new ceramic slurry is evenly attached to it.

[0024] Inspection and repair: After each layer is applied, carefully check whether there are bubbles, cracks or uncovered areas in the coating layer, and repair them in time; If bubbles, cracks and uncovered areas are not repaired in time, they may expand or cause more serious problems in future use, such as coating shedding, accelerated corrosion, etc. By checking the coating for bubbles, cracks or uncovered areas, problems in the coating process can be discovered and corrected in time, thereby ensuring the integrity and uniformity of the coating, which is the basis for ensuring the ultimate performance and quality of the coating.

[0025] 4) Drying and curing: Allow the coating to dry naturally at room temperature; Natural drying is suitable for large-scale operations. When a large number of pipe inner walls are coated with ceramic slurry, natural drying can be carried out, that is, within the natural drying time, as many pipes as possible can be prepared and processed, reducing energy consumption during machine drying, which is in line with environmental protection policies; 5) Sintering treatment: Sinter the dried and solidified substrate to ensure that the ceramic lining layer is dense, defect-free and tightly bonded to the stainless steel substrate; 6) Quality inspection: Appearance inspection: Check whether the coating layer is flat, smooth, free of cracks, bubbles and other defects; Performance test: Conduct corrosion resistance and strength performance tests on the coated pipes; Strength performance test items include tensile strength and yield strength tests; In this embodiment, the stirring furnace needs to be heated when the lining materials are mixed, and the detailed processing parameters are as follows: Stirring time: 40min; Stirring speed: 800n / min; Stirring temperature: 35°C; Stir until the slurry has no obvious particles, lumps, or bubbles.

[0026] In this embodiment, the substrate is roughened by sandblasting or chemical etching.

[0027] The equipment required for sintering is a high temperature furnace. The sintering parameters of the high temperature furnace are as follows: Sintering time: 1.5h; Sintering temperature: 1400℃.

[0028] In this embodiment, during the initial coating, it is necessary to ensure that there are no bubbles or gaps on the surface.

[0029] In this embodiment, in the drying process step proposed in step 4), accelerated drying is required when the following conditions are encountered: ①. Time constraints: There are strict time limits for production or repair tasks; ②. Unfavorable environmental conditions: If the production environment has high humidity, low temperature or poor ventilation; ③. The coating thickness is large: When the coated silicon nitride ceramic slurry layer is thicker, it takes longer for natural drying to ensure that the moisture and solvent inside the coating are completely volatilized; ④. Improve production efficiency: In large-scale production, in order to improve production efficiency and output, accelerated drying is often used to shorten the production cycle of each batch of products; The methods for accelerating drying include heating drying, vacuum drying and forced ventilation drying; Among them: the heating and drying uses a hot air circulation oven, the hot air temperature is 300℃, the hot air time is 1.5h, and the wind speed is 3m / s; Among them: vacuum drying uses a vacuum oven, the vacuum atmospheric pressure is 120Pa, the vacuum temperature is 400℃, and the time is 2h; Among them: forced ventilation drying requires the use of a forced ventilation dryer, with a temperature of 90°C, a time of 85 minutes, a wind speed of 6m / s, and a humidity of 12%; In this embodiment, during and after sintering, the following should be noted: ①. Insulation: A insulation stage is set during the sintering process to keep the material at the set temperature for a certain period of time to ensure that the material is fully sintered and achieves the required performance; Among them: the insulation time is 20 minutes, and the insulation trigger condition is that every time the furnace body rises 300℃, it is a cycle, that is, after the furnace body rises 300℃, it maintains the current temperature for 20 minutes before continuing to heat up.

[0030] ② Heating rate: Control the heating rate to avoid excessive thermal stress inside the material due to rapid heating, which may cause cracking or deformation; Among them: the heating rate is 7℃ / min; ③. Cooling rate: Control the cooling rate to avoid excessive cooling, which may cause residual stress inside the material and affect the performance and service life of the material; Among them: the cooling rate is 6℃ / min.

[0031] ④. After sintering is completed, the material is cooled to room temperature by natural cooling.

[0032] Example 3 Compared with Example 2, the only difference in Example 3 is that the proportions of the materials used in preparing the lining are different: Ceramic powder: 80%, made of silicon nitride; Water: 15%; Binder: 2%; The total amount of other additives is 3%; The preparation method and other parameters of this embodiment are consistent with those of embodiment 2.

[0033] Example 4 Compared with Example 2 and Example 3, the only difference in Example 4 is that the proportion of each material in the lining preparation material is different. Compared with Example 1, the only difference in Example 4 is that the proportion of ceramic powder in the lining preparation material is not within the range described in Example 1: Ceramic powder: 65%, made of silicon nitride; Water: 20%; Binder: 10%; Total amount of other additives 5%; The preparation method and other parameters of this embodiment are consistent with those of embodiment 2.

[0034] Comparative Example 1: Pipes made of 304 stainless steel, which contains ≈18% chromium, 8% nickel; Comparative Example 2: Pipes made of Q235B carbon steel; Table 1 Comparison of basic physical properties of finished products As can be seen from the above table, the pipeline made of 316 stainless steel base pipeline plus silicon nitride lining proposed in this application is generally superior to 304 stainless steel and carbon steel pipelines in terms of strength and corrosion resistance. This combination not only improves the overall performance of the pipeline, but also extends the service life of the pipeline and reduces maintenance costs.

[0035] It can be seen from the above table that the pipe made of 316 stainless steel base pipe plus silicon nitride lining proposed in this application is generally superior to 304 stainless steel and carbon steel pipes in terms of strength and corrosion resistance. According to the parameter range described in Example 1, the pipe made of 316 stainless steel base pipe plus silicon nitride lining has excellent performance as a whole. Example 2 and Example 3 are better examples within the parameter range of Example 1, and Example 4 is a better example outside the parameter range of Example 1. Through the data results, it is obtained that the combination described in Example 1 not only improves the overall performance of the pipe, but also extends the service life of the pipe and reduces the maintenance cost.

[0036] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a high-corrosion-resistant and high-strength precision pipeline, characterized in that: The preparation materials include a substrate and a lining. The substrate is 316 stainless steel, and the preparation materials of the lining include the following: Ceramic powder: 70%-80%, made of silicon nitride; Water: 10%-20%; Binder: 1%-10%; Total amount of other additives: 1%-5%; The preparation method includes the following: 1) Matrix pretreatment: S1. Matrix inspection: Check whether there are cracks on the surface of the pipeline; S2. Matrix treatment: ①. Cleaning: Clean the pipes to remove impurities such as oil, rust, etc. to ensure that the surface is clean and pollution-free; ② Roughening treatment: Roughening the inner wall of the substrate; ③ Drying: Dry the pipe thoroughly to prevent moisture from affecting the later sintering effect; 2) Lining preparation: Mixing: Mix the materials for lining preparation; 3) Coating treatment: The detailed process of coating treatment includes the following: Pipe preheating: Before coating, the stainless steel pipe is preheated to improve the adhesion and drying efficiency of the ceramic slurry; Initial coating: Use coating equipment to evenly coat the ceramic slurry on the inner wall of the stainless steel pipe; Layer-by-layer coating: For pipes that require a thicker lining layer, coating should be done layer by layer. After each layer is coated, it is necessary to wait for it to dry to a certain degree (usually surface dry) before coating the next layer; Inspection and repair: After each layer is applied, carefully check whether there are bubbles, cracks or uncovered areas in the coating layer, and repair them in time; 4) Drying and curing: Allow the coating to dry naturally at room temperature; 5) Sintering treatment: Sinter the dried and solidified substrate to ensure that the ceramic lining layer is dense, defect-free and tightly bonded to the stainless steel substrate; 6) Quality inspection: Appearance inspection: Check whether the coating layer is flat, smooth, free of cracks, bubbles and other defects; Performance test: Conduct corrosion resistance and strength performance tests on the coated pipes.

2. The method for preparing a high-corrosion-resistant and high-strength precision pipeline according to claim 1, characterized in that: Other additives include dispersants, thickeners, defoamers, preservatives, pH adjusters, and leveling agents.

3. The method for preparing a high-corrosion-resistant and high-strength precision pipeline according to claim 1, characterized in that: The mixing furnace needs to be heated when the lining materials are mixed. The detailed processing parameters are as follows: Stirring time: 30-50min; Stirring speed: 500-800n / min; Stirring temperature: 20-35℃; Stir until the slurry has no obvious particles, lumps, or bubbles.

4. The method for preparing a high-corrosion-resistant and high-strength precision pipeline according to claim 1, characterized in that: The substrate is roughened by sandblasting or chemical etching.

5. The method for preparing a high-corrosion-resistant and high-strength precision pipeline according to claim 1, characterized in that: The equipment required for sintering is a high temperature furnace. The sintering parameters of the high temperature furnace are as follows: Sintering time: 1.5-2h; Sintering temperature: 1300-1450℃.

6. The method for preparing a high-corrosion-resistant and high-strength precision pipeline according to claim 1, characterized in that: When applying for the first time, make sure there are no bubbles or gaps on the surface.

7. The method for preparing a high-corrosion-resistant and high-strength precision pipeline according to claim 1, characterized in that: According to the drying process proposed in step 4), accelerated drying is required when the following situations occur: ①. Time constraints: There are strict time limits for production or repair tasks; ②. Unfavorable environmental conditions: If the production environment has high humidity, low temperature or poor ventilation; ③. The coating thickness is large: When the coated silicon nitride ceramic slurry layer is thicker, it takes longer for natural drying to ensure that the moisture and solvent inside the coating are completely volatilized; ④. Improve production efficiency: In large-scale production, in order to improve production efficiency and output, accelerated drying is often used to shorten the production cycle of each batch of products; The methods for accelerating drying include heating drying, vacuum drying and forced ventilation drying; Among them: the heating and drying uses a hot air circulation oven, the hot air temperature is 240-320℃, the hot air time is 1.5-2h, and the wind speed is 2-3.5m / s; Among them: vacuum drying uses a vacuum oven, the vacuum atmospheric pressure is 110-133Pa, the vacuum temperature is 340-460℃, and the time is 1.5-2h; Among them: forced ventilation drying requires the use of a forced ventilation dryer, with a temperature of 65-125°C, a time of 35-85 minutes, a wind speed of 5-6.3m / s, and a humidity of 10%-15%.

8. The method for preparing a high corrosion-resistant and high-strength precision pipeline according to claim 1, characterized in that: During and after sintering, the following should be noted: ①. Insulation: A insulation stage is set during the sintering process to keep the material at the set temperature for a certain period of time to ensure that the material is fully sintered and achieves the required performance; Among them: the insulation time is 15-20min, and the insulation triggering condition is that the furnace body rises 300-350℃ every time as one cycle; ② Heating rate: Control the heating rate to avoid excessive thermal stress inside the material due to rapid heating, which may cause cracking or deformation; Among them: the heating rate does not exceed 8-9℃ / min; ③. Cooling rate: Control the cooling rate to avoid excessive cooling, which may cause residual stress inside the material and affect the performance and service life of the material; Wherein: the cooling rate is 5-6.5℃ / min; ④. After sintering is completed, the material is cooled to room temperature by natural cooling.

Citation Information

Patent Citations

  • Preparation method for metal-ceramic composite tube

    CN101576178A

  • Method for preparing silicon dioxide hydrogen-resistant coatings on inner walls of 316L stainless steel pipelines

    CN112756238A

Cited By

  • A process for the machining of a crystalline silicon component and the assembly of the same with a metal fitting