A method for preparing nuclear grade hafnium and hafnium alloy single point spectrum standard samples
Through vacuum consumable melting and multiple cold crucible magnetic levitation melting processes, combined with high-purity argon gas introduction and rotating crucible casting, the problem of melting control of low-content elements in nuclear-grade hafnium alloys has been solved, and the uniformity and stability of hafnium alloys have been achieved. Improvement, suitable for the atomic energy industry, promotes the production and research and development of nuclear-grade hafnium alloys.
Patent Information
- Application Number
- CN202111315980.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-11-08
AI Technical Summary
The existing technology is difficult to effectively control the smelting of low-content elements in nuclear-grade hafnium, resulting in poor uniformity and low stability of the prepared hafnium alloy, which limits the production and research and development progress of nuclear-grade hafnium alloys.
Vacuum consumable melting and multiple cold crucible magnetic levitation melting processes are used, combined with high-purity argon gas introduction and rotating crucible casting to ensure the uniformity and stability of the hafnium alloy. The molten metal is evenly stirred through electromagnetic force to form a high-quality single Point spectrum standard sample.
It has improved the uniformity and stability of low-content elements in nuclear-grade hafnium alloys, overcomes analysis errors and stability problems, and is suitable for hafnium control rods and protection devices in the atomic energy industry, promoting the production and production of nuclear-grade hafnium alloys in my country. R&D.
Smart Images

Figure CN114166589B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nuclear-grade hafnium alloy preparation, in particular to a method for preparing nuclear-grade hafnium and hafnium alloy single-point spectrum standard samples. Background Art
[0002] Nuclear-grade hafnium and hafnium alloys are plastic, easy to process, high temperature resistant and corrosion resistant, and are important materials for the atomic energy industry. Hafnium has a large thermal neutron capture cross section and is an ideal neutron absorber. It can be used as a control rod and protection device for atomic reactors. The content of chemical elements in nuclear-grade hafnium and hafnium alloy control rods directly affects the efficiency of their control of the reactor. In order to ensure the consistency and stability of the curve of the detection equipment, the development of nuclear-grade hafnium and hafnium alloy spectral standard samples is a key technical task for nuclear materials, which can ensure that the detection results are more accurate and reliable, and further accelerate the production, research and development, and localization of nuclear-grade hafnium alloy control rods. In the existing technology for preparing nuclear-grade hafnium, it is extremely difficult to carry out smelting control of low-content elements in nuclear-grade hafnium. The low-content elements in the prepared nuclear-grade hafnium have poor uniformity and low stability. In addition, since there is currently no domestic ability to prepare standard samples for single-point spectral analysis of nuclear-grade hafnium and hafnium alloys, the production and research and development progress of nuclear-grade hafnium alloys in my country has been restricted to a certain extent.
[0003] Therefore, the present invention is proposed. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing a single-point spectrum standard sample of nuclear-grade hafnium and hafnium alloy, which can control the smelting of low-content elements in nuclear-grade hafnium, so that the prepared low-content elements in nuclear-grade hafnium have good uniformity and high stability.
[0005] The invention provides a method for preparing a nuclear-grade hafnium and a hafnium alloy single-point spectrum standard sample, comprising: mixing elements according to their mass percentage content: Fe is 0.02% to 0.048%, Cr is 0.0015% to 0.009%, Zr is 0.58% to 0.65%, Al is less than 0.01%, Cu is less than 0.01%, Ni is less than 0.005%, Si is less than 0.01%, and the balance is hafnium to obtain a bulk nuclear-grade sponge hafnium mixed raw material; wherein the hafnium is bulk nuclear-grade sponge hafnium; performing vacuum consumable smelting on the bulk nuclear-grade sponge hafnium mixed raw material to obtain a nuclear-grade hafnium alloy primary ingot; performing cold crucible magnetic suspension smelting on the nuclear-grade hafnium alloy primary ingot for multiple times to obtain a nuclear-grade hafnium alloy ingot; and reprocessing the nuclear-grade hafnium alloy ingot to obtain a nuclear-grade hafnium and a hafnium alloy single-point spectrum standard sample.
[0006] Further, subjecting the primary ingot of nuclear-grade hafnium alloy to multiple cold crucible magnetic suspension smelting to obtain the nuclear-grade hafnium alloy ingot comprises: subjecting the primary ingot of nuclear-grade hafnium alloy to a cold crucible magnetic suspension smelting to obtain a primary ingot of nuclear-grade hafnium alloy; subjecting the primary ingot of nuclear-grade hafnium alloy to a cold crucible magnetic suspension smelting to obtain a secondary ingot of nuclear-grade hafnium alloy;
[0007] Further, the primary ingot of nuclear-grade hafnium alloy is subjected to cold crucible magnetic suspension primary melting to obtain the primary ingot of nuclear-grade hafnium alloy, which comprises: the vacuum degree in the crucible reaches 1.0×10 -2 Under the condition of 2000 MPa, high-purity argon is introduced into the crucible for the primary ingot of nuclear-grade hafnium alloy; the power of the induction coil is controlled to carry out smelting, and the temperature is kept for 10min to 20min; and cooling is carried out to obtain a nuclear-grade hafnium alloy primary ingot.
[0008] Further, controlling the power of the induction coil to perform smelting and keeping warm for 10 minutes to 20 minutes includes: a smelting power of 160KW to 180KW and a keeping warm power of 140KW to 150KW.
[0009] Further, the primary ingot of nuclear-grade hafnium alloy is subjected to cold crucible magnetic suspension secondary melting to obtain the secondary ingot of nuclear-grade hafnium alloy, comprising: the vacuum degree in the crucible reaches 1.0×10 -2 Under the condition of 200 MPa, high-purity argon is introduced into the crucible for the primary ingot of nuclear-grade hafnium alloy; the power of the induction coil is controlled to carry out smelting to obtain a nuclear-grade hafnium alloy solution, and the solution is kept warm for 10 min to 20 min; the nuclear-grade hafnium alloy solution is cast into a mold, and cooled to obtain a secondary ingot of nuclear-grade hafnium alloy.
[0010] Further, controlling the power of the induction coil to carry out smelting and keeping warm for 10 minutes to 20 minutes includes: the secondary smelting power is 260KW to 280KW, and the keeping warm power is 240KW to 250KW.
[0011] Furthermore, subjecting the nuclear-grade hafnium alloy primary ingot to cold crucible magnetic suspension secondary smelting to obtain the nuclear-grade hafnium alloy secondary ingot further comprises: placing the nuclear-grade hafnium alloy primary ingot upside down.
[0012] Furthermore, casting the nuclear-grade hafnium alloy solution into a mold to obtain a nuclear-grade hafnium alloy secondary ingot comprises: direct casting by rotating a crucible.
[0013] Further, the nuclear-grade hafnium alloy ingot is reprocessed to obtain nuclear-grade hafnium and hafnium alloy single-point spectral standard samples, including: initial uniformity inspection: after the surface of the ingot is treated, 100 mm is cut off from the upper and lower ends, and the ingot is subjected to non-destructive testing, and then chip samples are taken from the upper and lower end surfaces and the middle position of the nuclear-grade hafnium alloy ingot to inspect the composition segregation and process the analysis data; processing: the nuclear-grade hafnium alloy ingot that passes the initial uniformity inspection is processed into chip samples with a size of about 3 mm×1 mm×0.2 mm (length×width×thickness); composition uniformity inspection: 3 groups of 15 samples are randomly selected from the uniformly mixed nuclear-grade hafnium alloy chip samples, and the 3 groups of data are inspected on an Agilent inductively coupled plasma emission spectrometer; fixed value: fixed value analysis is performed on the samples that pass the composition uniformity inspection.
[0014] The present invention provides a method for preparing a nuclear-grade hafnium and hafnium alloy single-point spectrum standard sample, which can be used to prepare a spectrum standard sample suitable for nuclear-grade hafnium and hafnium alloy. The nuclear-grade hafnium and hafnium alloy spectrum standard sample prepared by the present invention is mainly aimed at hafnium control rods and protective devices used in the atomic energy industry, which are widely used in China. The present invention purifies the raw materials through a vacuum arc melting, removes volatile elements, and prevents the influence of foreign inclusions, which has a certain uniform effect. Electromagnetic force is used to keep the molten metal and the crucible in a non-contact state for secondary cold crucible magnetic suspension melting to avoid external pollution. During the melting process, the magnetic field acts on the material to make the material more uniform, the surface skin effect is enhanced, the electromagnetic force is increased, and the stirring effect during the capacity process is more obvious, which helps to make the material uniform. After the secondary cold crucible suspension melting, it is cast under vacuum conditions. The casting process is to make the molten metal more fully stirred, the composition is thoroughly uniform, and after molding, the shape is regular and the yield rate is high. The analytical error and stability problems caused by different analytical instruments in different production, research and use units are overcome. The composition design takes into account the application and promotion of a series of products such as hafnium sponge, hafnium rods, hafnium wires, and hafnium plates, which has a positive significance for the development of my country's atomic energy industry. According to the mass percentage of elements: Fe is 0.02% to 0.048%, Cr is 0.0015% to 0.009%, Zr is 0.58% to 0.65%, Al < 0.01%, Cu < 0.01%, Ni < 0.005%, Si < 0.01%, and the remaining mass percentage of hafnium is weighed. The composition design of bulk nuclear-grade hafnium sponge is mixed and prepared to obtain nuclear-grade hafnium and hafnium alloy spectral standard samples, which can meet the analysis requirements of hafnium sponge, hafnium rods, hafnium wires, and hafnium plates. The use of advanced processes such as vacuum arc melting once, cold crucible electromagnetic induction melting twice, casting, and rapid cooling has solved the problem of low-content element melting control and unevenness in nuclear-grade hafnium. The eight qualified laboratories in China have used different principles and reliable analysis methods to collaboratively determine the value, and the determination results are accurate and reliable. The variance method is used for uniformity inspection, and the results show that this single-point standard sample has good uniformity. According to the stability of similar standard samples and the stability of the research and development unit, this single-point standard sample also has good stability.
[0015] Therefore, the method for preparing a single-point spectral standard sample of nuclear-grade hafnium and hafnium alloy provided by the present invention solves the technical problems in the prior art that it is extremely difficult to control the smelting of low-content elements in nuclear-grade hafnium, the low-content elements in the prepared nuclear-grade hafnium have poor uniformity and low stability, and the current domestic lack of the ability to prepare standard samples for single-point spectral analysis of nuclear-grade hafnium and hafnium alloys has restricted the production and research and development progress of nuclear-grade hafnium alloys in my country to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 A schematic flow chart of a method for preparing a single-point spectral standard sample of nuclear-grade hafnium and hafnium alloys according to an embodiment of the present invention;
[0018] Figure 2 The present invention is a flow chart of a method for surface treating, processing and testing a nuclear-grade hafnium alloy ingot to obtain a nuclear-grade hafnium and hafnium alloy single-point spectrum standard sample. DETAILED DESCRIPTION
[0019] In order to make the above and other features and advantages of the present invention more clear, the present invention is further described below in conjunction with the accompanying drawings. It should be understood that the specific embodiments given herein are for the purpose of explaining to those skilled in the art and are only exemplary and not restrictive.
[0020] In the following description, many specific details are set forth to provide a thorough understanding of the present invention. However, it will be apparent to one of ordinary skill in the art that specific details need not be adopted to practice the present invention. In other cases, well-known steps or operations are not described in detail to avoid obscuring the present invention.
[0021] The invention provides a method for preparing a nuclear-grade hafnium and hafnium alloy single-point spectrum standard sample, which can be used to prepare a spectrum standard sample suitable for nuclear-grade hafnium and hafnium alloy. The nuclear-grade hafnium and hafnium alloy spectrum standard sample prepared by the invention is mainly aimed at hafnium control rods and protective devices used in the atomic energy industry, which are widely used in China. The method overcomes the analysis error and stability problems caused by different analytical instruments in different production, research and use units, and the composition design takes into account the application and promotion of a series of products such as hafnium sponge, hafnium rods, hafnium wires, and hafnium plates, which has positive significance for the development of my country's atomic energy industry.
[0022] Embodiment 1
[0023] like Figure 1 As shown, the method includes:
[0024] Step S101, according to the mass percentage of elements: Fe is 0.02% to 0.048%, Cr is 0.0015% to 0.009%, Zr is 0.58% to 0.65%, Al is less than 0.01%, Cu is less than 0.01%, Ni is less than 0.005%, Si is less than 0.01%, and the rest is hafnium, and a bulk nuclear grade sponge hafnium mixed raw material is obtained; wherein the hafnium is bulk sponge hafnium.
[0025] Specifically, the mass percentage content of Fe in the hafnium sponge mixed raw material can be controlled between 0.02% and 0.048%, the mass percentage content of Cr in the hafnium sponge mixed raw material can be controlled between 0.0015% and 0.009%, the mass percentage content of Zr in the hafnium sponge mixed raw material can be controlled between 0.58% and 0.65%, and the contents of other elements are controlled to be Al < 0.01%, Cu < 0.01%, Ni < 0.005%, and Si < 0.01%. The remaining mass percentage content of hafnium can be bulk nuclear grade sponge hafnium. The above raw materials are mixed to obtain a bulk nuclear grade sponge hafnium mixed raw material.
[0026] Step S102, performing vacuum consumable smelting on the bulk nuclear-grade hafnium sponge mixed raw material to obtain a primary ingot of nuclear-grade hafnium alloy;
[0027] After the bulk nuclear-grade hafnium sponge mixed raw material is prepared, the nuclear-grade hafnium sponge mixed raw material can be subjected to vacuum consumable melting, wherein the process of vacuum consumable melting may include: drying, mixing, pressing electrodes, electrode welding, vacuum consumable melting and other steps, and during the melting process, the current is set between 1800A and 2200A, the voltage is set between 28V and 36V, and the vacuum degree is controlled at 0.1Pa to 2Pa. It should be noted that vacuum consumable melting needs to be carried out after the steps of drying, mixing, pressing electrodes, electrode welding and the like are completed.
[0028] Step S103, subjecting the primary nuclear-grade hafnium alloy ingot to multiple cold crucible magnetic suspension melting to obtain a nuclear-grade hafnium alloy ingot;
[0029] Specifically, this solution may include the following steps:
[0030] Step S1031, performing cold crucible magnetic suspension primary melting on the primary ingot of nuclear-grade hafnium alloy to obtain a primary ingot of nuclear-grade hafnium alloy;
[0031] First, the vacuum degree in the crucible reaches 1.0×10 -2MPa, high-purity argon is introduced into the primary ingot of nuclear-grade hafnium alloy in the crucible; then the induction coil power is controlled for smelting and heat preservation for 10min to 20min; wherein, the induction coil power, i.e., the primary smelting power, is controlled between 160KW and 180KW, and the heat preservation power is controlled between 140KW and 150KW; finally, the primary ingot of nuclear-grade hafnium alloy in the crucible is cooled to obtain a primary ingot of nuclear-grade hafnium alloy. It should be noted that the outer wall of the crucible has a certain thickness, and a cooling water flow channel can be set in the outer wall. The cooling water flows through the cooling water flow channel to exchange heat with the inside of the crucible, so as to achieve the purpose of cooling the primary ingot of nuclear-grade hafnium alloy in the crucible.
[0032] Step S1032, performing cold crucible magnetic suspension secondary melting on the nuclear-grade hafnium alloy primary ingot to obtain a nuclear-grade hafnium alloy secondary ingot;
[0033] First, the vacuum degree in the crucible reaches 1.0×10 -2 MPa, high-purity argon is introduced into the crucible to form a primary ingot of nuclear-grade hafnium alloy; then the induction coil power is controlled to carry out smelting to obtain a nuclear-grade hafnium alloy solution, and the solution is kept warm for 10-20 minutes; wherein, the induction coil power, i.e., the secondary smelting power, is controlled between 260KW and 280KW, and the insulation power is between 240KW and 250KW. Finally, the nuclear-grade hafnium alloy solution is cast into a mold, and cooled to obtain a secondary ingot of nuclear-grade hafnium alloy. When the nuclear-grade hafnium alloy solution is cast into the mold, in order to reduce external pollution, it can be directly cast in a magnetic levitation smelting chamber by rotating the crucible, and cooled to obtain a secondary ingot of nuclear-grade hafnium alloy. It should be noted that the placement position of the primary ingot of nuclear-grade hafnium alloy prepared in the previous step is swapped, for example, the primary ingot of nuclear-grade hafnium alloy is placed upside down to improve the effect of its secondary smelting.
[0034] Step S104, as Figure 2 As shown, the nuclear grade hafnium alloy ingot is reprocessed to obtain nuclear grade hafnium and hafnium alloy single point spectrum standard samples.
[0035] Specifically, this solution may also include the following specific steps:
[0036] Step S1041, initial uniformity inspection: after surface treatment of the ingot, 100 mm of the upper and lower ends are cut off, and non-destructive testing is performed on the ingot. Then, chip-like samples are taken from the upper and lower end surfaces and the middle position of the nuclear-grade hafnium alloy ingot to perform component segregation inspection and process the analysis data;
[0037] Step S1042, processing: processing the nuclear-grade hafnium alloy ingot that has passed the initial uniformity inspection into a chip-like sample with a size of about 3 mm×1 mm×0.2 mm (length×width×thickness);
[0038] Step S1043, component uniformity inspection: randomly select 3 groups of uniformly mixed nuclear-grade hafnium alloy chip samples, each with 15 samples, and inspect the 3 groups of data on an Agilent inductively coupled plasma optical emission spectrometer;
[0039] Step S1044, fixed value: perform fixed value analysis on samples that pass the component uniformity inspection.
[0040] Compared with the prior art, this solution purifies the raw materials through a vacuum arc melting, removes volatile elements, and prevents the influence of foreign inclusions, which has a certain uniform effect. Electromagnetic force is used to keep the molten metal and the crucible in a non-contact state for secondary cold crucible magnetic suspension melting to avoid external pollution. The magnetic field acts on the material during the melting process, making the material more uniform, enhancing the surface skin effect, increasing the electromagnetic force, and making the stirring effect more obvious during the capacity process, which helps to make the material uniform. After the secondary cold crucible suspension melting, it is cast under vacuum conditions. The casting process is to make the molten metal more fully stirred, the composition is thoroughly uniform, and after molding, the shape is regular and the yield rate is high.
[0041] Embodiment 2
[0042] In an optional embodiment, the following method may be used to prepare a nuclear grade hafnium and hafnium alloy single point spectrum standard sample:
[0043] Step S201, weighing bulk nuclear grade sponge hafnium according to the element mass percentage content: Fe is 0.045%, Cr is 0.0040%, Zr is 0.62%, and the remainder is hafnium;
[0044] Step S202, the bulk nuclear grade hafnium sponge weighed in step S201 is subjected to vacuum consumable melting once, and the hafnium sponge is subjected to drying, mixing, electrode pressing, electrode welding, and consumable melting once. During the melting process, the current is 1800A to 2200A, the voltage is 28V to 36V, and the vacuum degree is 0.1Pa to 2Pa;
[0045] Step S203, subjecting the nuclear-grade hafnium alloy primary ingot obtained in step S202 to cold crucible magnetic suspension primary melting, and -2 MPa, high-purity argon gas was introduced, the induction coil power was 160KW, smelting was carried out, and the heat preservation power was 140KW. After the heat preservation time was 20min, cooling water was introduced into the crucible for rapid cooling to obtain a nuclear-grade hafnium alloy primary ingot;
[0046] Step S204, subjecting the nuclear-grade hafnium alloy primary ingot obtained in step S203 to cold crucible magnetic suspension secondary melting, and -2MPa, high-purity argon is introduced, the induction coil power is 260KW, smelting is carried out, and the heat preservation power is 240KW. After the heat preservation time is 20min, the nuclear-grade hafnium nuclear-grade solution is cast into a mold with cold water, and rapidly cooled to obtain a nuclear-grade hafnium alloy secondary ingot;
[0047] Step S205, performing surface treatment on the nuclear-grade hafnium alloy secondary ingot obtained in step S204 and then conducting inspection and processing, and obtaining nuclear-grade hafnium and hafnium alloy single-point spectrum standard samples if the ingot is qualified, thereby completing the method.
[0048] The sample number of the standard sample prepared in this example is Hf-1.
[0049] Embodiment 3
[0050] In an optional embodiment, the following method can be used to prepare nuclear grade hafnium and hafnium alloy single point spectrum standard samples:
[0051] Step S301, weighing bulk nuclear grade sponge hafnium according to the element mass percentage content: Fe is 0.033%, Cr is 0.0059%, Zr is 0.60%, and the remainder is hafnium;
[0052] Step S302, the bulk nuclear grade hafnium sponge weighed in step S301 is subjected to vacuum consumable melting once, and the hafnium sponge is subjected to drying, mixing, electrode pressing, electrode welding, and consumable melting once. During the melting process, the current is 1800A to 2200A, the voltage is 28V to 36V, and the vacuum degree is 0.1Pa to 2Pa;
[0053] Step S303, subjecting the nuclear-grade hafnium alloy primary ingot obtained in step S302 to cold crucible magnetic suspension primary melting, and -2 MPa, high-purity argon gas was introduced, the induction coil power was 160KW, smelting was carried out, and the heat preservation power was 140KW. After the heat preservation time was 20min, cooling water was introduced into the crucible for rapid cooling to obtain a nuclear-grade hafnium alloy primary ingot;
[0054] Step S304, subjecting the nuclear-grade hafnium alloy primary ingot obtained in step S303 to cold crucible magnetic suspension secondary melting, and -2 MPa, high-purity argon is introduced, the induction coil power is 260KW, smelting is carried out, and the heat preservation power is 240KW. After the heat preservation time is 20min, the nuclear-grade hafnium nuclear-grade solution is cast into a mold with cold water, and rapidly cooled to obtain a nuclear-grade hafnium alloy secondary ingot;
[0055] Step S305, performing surface treatment on the nuclear-grade hafnium alloy secondary ingot obtained in step S304 and then conducting inspection and processing, and obtaining nuclear-grade hafnium and hafnium alloy single-point spectrum standard samples if the ingot is qualified, thereby completing the method.
[0056] The standard sample number prepared in this example is Hf-2.
[0057] Embodiment 4
[0058] In an optional embodiment, the following method can be used to prepare nuclear grade hafnium and hafnium alloy single point spectrum standard samples:
[0059] Step S401, weighing bulk nuclear grade sponge hafnium according to the element mass percentage content: Fe is 0.021%, Cr is 0.0030%, Zr is 0.64%, and the remainder is hafnium;
[0060] Step S402, the bulk nuclear grade hafnium sponge weighed in step S401 is subjected to vacuum consumable melting once, and the hafnium sponge is subjected to drying, mixing, electrode pressing, electrode welding, and consumable melting once. During the melting process, the current is 1800A to 2200A, the voltage is 28V to 36V, and the vacuum degree is 0.1Pa to 2Pa;
[0061] Step S403, subjecting the nuclear-grade hafnium alloy primary ingot obtained in step S402 to cold crucible magnetic suspension primary melting, and -2 MPa, high-purity argon gas was introduced, the induction coil power was 160KW, smelting was carried out, and the heat preservation power was 140KW. After the heat preservation time was 20min, cooling water was introduced into the crucible for rapid cooling to obtain a nuclear-grade hafnium alloy primary ingot;
[0062] Step S404, subjecting the nuclear-grade hafnium alloy primary ingot obtained in step S403 to cold crucible magnetic suspension secondary melting, and -2 MPa, high-purity argon is introduced, the induction coil power is 260KW, smelting is carried out, and the heat preservation power is 240KW. After the heat preservation time is 20min, the nuclear-grade hafnium nuclear-grade solution is cast into a mold with cold water, and rapidly cooled to obtain a nuclear-grade hafnium alloy secondary ingot;
[0063] Step S405, performing surface treatment on the nuclear-grade hafnium alloy secondary ingot obtained in step S404 and then conducting inspection and processing, and obtaining nuclear-grade hafnium and hafnium alloy single-point spectrum standard samples if the ingot is qualified, thereby completing the method.
[0064] The sample number of the standard sample prepared in this example is Hf-3.
[0065] In order to verify that the low-content elements in the nuclear-grade hafnium prepared by the method for preparing a nuclear-grade hafnium and hafnium alloy single-point spectrum standard sample provided by the present invention have good uniformity and high stability, the following comparative examples 5 to 7 are specially formulated to compare with the above examples 2 to 4.
[0066] Embodiment 5
[0067] Step S501, weighing bulk nuclear grade sponge hafnium according to the mass percentage of the elements: Fe is 0.021%, Cr is 0.0030%, Zr is 0.64%, and the remainder is hafnium;
[0068] Step S502, subjecting the bulk nuclear-grade hafnium sponge weighed in step S501 to cold crucible magnetic suspension primary melting, and subjecting the mixture to a vacuum degree of 1.0×10 -2 MPa, high-purity argon gas was introduced, the induction coil power was 170KW, smelting was carried out, and the heat preservation power was 145KW. After the heat preservation time was 18min, cooling water was introduced into the crucible for rapid cooling to obtain a nuclear-grade hafnium alloy primary ingot;
[0069] Step S503, performing surface treatment on the nuclear-grade hafnium alloy primary ingot obtained in step S502 and then conducting inspection and processing, and obtaining nuclear-grade hafnium and hafnium alloy single-point spectrum standard samples if the ingot is qualified, thereby completing the method.
[0070] Embodiment 6
[0071] Step S601, weighing bulk nuclear grade sponge hafnium according to the mass percentage of the elements: Fe is 0.021%, Cr is 0.0030%, Zr is 0.64%, and the remainder is hafnium;
[0072] Step S602, subjecting the bulk nuclear-grade hafnium sponge weighed in step S601 to cold crucible magnetic suspension primary melting, and -2 MPa, high-purity argon is introduced, the induction coil power is 170KW, smelting is carried out, and the heat preservation power is 146KW, and the heat preservation time is 17min. The nuclear-grade hafnium alloy primary ingot obtained in step 2 is subjected to cold crucible magnetic suspension secondary smelting. Under the condition that the vacuum degree reaches 1.0×10-2MPa, high-purity argon is introduced, the induction coil power is 260KW, smelting is carried out, and the heat preservation power is 240KW. After the heat preservation time is 20min, cold water is introduced into the crucible for rapid cooling to obtain a nuclear-grade hafnium alloy secondary ingot;
[0073] Step S603, performing surface treatment on the nuclear-grade hafnium alloy secondary ingot obtained in step S602 and then conducting inspection and processing, and obtaining a nuclear-grade hafnium and hafnium alloy single-point spectrum standard sample if the ingot passes the inspection.
[0074] Embodiment 7
[0075] Step S701, weighing bulk nuclear grade sponge hafnium according to the mass percentage of the elements: Fe is 0.021%, Cr is 0.0030%, Zr is 0.64%, and the remainder is hafnium;
[0076] Step S702, melting the bulk nuclear-grade hafnium sponge weighed in step S701 in a vacuum consumable arc furnace, the melting times being one time;
[0077] Step S703, performing surface treatment on the nuclear-grade hafnium alloy primary ingot obtained in step S702 and then conducting inspection and processing, and obtaining nuclear-grade hafnium and hafnium alloy single-point spectrum standard samples if the ingot passes the inspection.
[0078] Effect detection
[0079] 1. Initial uniformity inspection: After the surface treatment of the ingot, cut off 100mm from the upper and lower ends, and conduct non-destructive testing on the ingot. Then, take chip-like samples from the upper and lower end surfaces (center, R / 2, R) and the middle of the side wall of the nuclear-grade hafnium alloy ingot to conduct component segregation inspection, and process the analysis data in accordance with the requirements of YS / T 409 "Technical Specifications for Standard Samples for Analysis of Nonferrous Metal Products";
[0080] Example 2 Ingot uniformity
[0081]
[0082]
[0083] Example 3 Ingot Uniformity
[0084] Location Zr element content % Fe content% Cr element content% Upper end face - center 0.5995 0.0331 0.0037 Upper end surface-R / 2 0.5997 0.0329 0.0037 Upper end surface-R 0.5999 0.0328 0.0035 Lower end face - center 0.5997 0.0330 0.0036 Lower end surface-R / 2 0.5998 0.0325 0.0037 Lower end surface-R 0.6002 0.0326 0.0034 Sidewall 0.5998 0.0328 0.0036 average value 0.5998 0.0328 0.0036 Standard DeviationS 0.0002 0.0002 0.0001 1.5S 0.0003 0.0003 0.00015 Repeatability limit 0.05 0.0005 0.0003 in conclusion qualified qualified qualified
[0085] Example 4 Ingot Uniformity
[0086] Location Zr element content % Fe content% Cr element content% Upper end face-center 0.6395 0.0198 0.0025 Upper end surface-R / 2 0.6397 0.0199 0.0027 Upper end surface-R 0.6398 0.0201 0.0029 Lower end face - center 0.6395 0.0197 0.0025 Lower end surface-R / 2 0.6396 0.0199 0.0026 Lower end surface-R 0.6399 0.0200 0.0028 Sidewall 0.6400 0.0196 0.0029 average value 0.6397 0.0198 0.0027 Standard DeviationS 0.0002 0.0002 0.0002 1.5S 0.0003 0.0003 0.0003 Repeatability limit 0.05 0.0005 0.0003 in conclusion qualified qualified qualified
[0087] Example 5 Ingot Uniformity
[0088]
[0089]
[0090] Example 6 Ingot Uniformity
[0091] Location Zr element content % Fe content% Cr element content% Upper end face-center 0.6395 0.0203 0.0028 Upper end surface-R / 2 0.6392 0.0207 0.0026 Upper end surface-R 0.6400 0.0200 0.0026 Lower end face - center 0.6354 0.0183 0.0020 Lower end surface-R / 2 0.6360 0.0180 0.0019 Lower end surface-R 0.6363 0.0187 0.0021 Sidewall 0.6389 0.0200 0.0027 average value 0.6379 0.0194 0.0024 Standard DeviationS 0.0019 0.0011 0.0004 1.5S 0.0028 0.0016 0.0006 Repeatability limit 0.05 0.0005 0.0003 in conclusion qualified Failure Failure
[0092] Example 7 Ingot Uniformity
[0093]
[0094]
[0095] The above experimental data results show that the nuclear-grade hafnium alloy ingot cast by the method of the present invention is qualified and all elements have no segregation phenomenon, which further verifies that the low-content elements in the nuclear-grade hafnium prepared by the method for preparing a nuclear-grade hafnium and hafnium alloy single-point spectrum standard sample provided by the invention have good uniformity and high stability.
[0096] 2. Processing: Process the nuclear-grade hafnium alloy ingot that has passed the initial uniformity inspection into chip-like samples with a size of approximately 3mm×1mm×0.2mm (length×width×thickness);
[0097] 3. Composition uniformity inspection: According to the technical specifications of standard samples, three groups of 15 samples in each group were randomly selected from the uniformly mixed nuclear-grade hafnium alloy chips, numbered in sequence, and the three groups of samples were inspected on the Agilent inductively coupled plasma optical emission spectrometer;
[0098] After inspection, all standard samples are uniform and qualified;
[0099] 4. Fixed value: Samples that have passed the composition uniformity inspection shall be subjected to fixed value analysis in accordance with the requirements of YS / T 409 "Technical Specifications for Standard Samples for Analysis of Nonferrous Metal Products".
[0100] The fixed value analysis selects qualified laboratories, units with both industry representatives and regional representatives to participate in the fixed value analysis, and uses accurate and reliable analysis methods for collaborative customized analysis.
[0101] Data aggregation and processing
[0102] Refer to the data reported by each analytical unit, and check whether there are abnormal values within the group and between units according to the allowable difference of the national standard method. If necessary, the original laboratory can be asked to recheck the suspicious values. Then use the following methods to process the data. Then calculate the standard value and expanded uncertainty of each group of data.
[0103] (1) Normality test: Shapiro-Wilk method
[0104] The original data after removing suspicious values were summarized and the Shapiro-Wilk method was used to conduct a normality test on all the data reported by each collaborative unit.
[0105] Calculation formula:
[0106] Where: k is 1 to h. When the number of measurements n is an even number, h = n / 2. When the number of measurements n is an odd number, h = (n-1) / 2. Coefficient a k It is a specific value related to n and k. If W<W(a,n), it does not obey the normal distribution, otherwise it is normal.
[0107] All data were tested to be normal or nearly normal.
[0108] (2) Outlier test: Grubbs method
[0109] When the data obeys normal distribution or approximate normal distribution, the average value of each group of data is regarded as a single measurement value to form a new group of data. Use Grubbs method to test.
[0110] Here, the significance level α is 0.05 and the critical value is 2.126. Calculate the maximum residual and the minimum residual. If both are less than the critical value, keep them all.
[0111] (3) Equal precision test: Cochran method
[0112] This standard sample uses the Cochrane criterion to test whether the results of each group are of equal precision.
[0113] Cochrane criterion test formula:
[0114] Where: m: number of data sets, n: number of repeated measurements.
[0115] If Cmax≤C(a, m, n), it indicates that each group of data has equal precision.
[0116] If Cmax>C(a, m, n), it indicates that the data set has poor precision.
[0117] The test shows that all data are of equal or approximately equal precision.
[0118] (4) After processing each group of data, calculate the arithmetic mean and single measurement standard deviation of each group of data, and round off the significant figures of the standard value according to GB / T 8170 "Data Rounding Rules".
[0119] (5) Standard value and expanded uncertainty:
[0120] Since the tests are of equal precision, the standard value and expanded uncertainty are calculated using the following method:
[0121] The characteristic quantity of the standard sample is measured, where m is the number of data sets, n is the number of repeated measurements, Determine the average value.
[0122] Arithmetic total mean (standard value)
[0123] Standard deviation of a single measurement
[0124] Standard deviation of the arithmetic mean
[0125] Standard deviation caused by unevenness (unevenness uncertainty) S1:
[0126] When F < 1,
[0127] Combined uncertainty S:
[0128] Expanded uncertainty U:
[0129] Where K is the inclusion factor determined by the confidence probability and the degrees of freedom. Here K is 2.37 (a = 0.05, a is the confidence level; V = 7, V is the degrees of freedom).
[0130] The determination result of this standard sample is expressed by (standard value, expanded uncertainty).
[0131] Example 2 Standard sample number Hf-1 (%)
[0132]
[0133]
[0134] Example 3 Standard sample number Hf-2 (%)
[0135]
[0136] Example 4 Standard sample number Hf-3 (%)
[0137]
[0138] Results of spectral standard samples with sample numbers Hf-1, Hf-2 and Hf-3 (%)
[0139]
[0140] Production Assessment
[0141] This standard sample was analyzed on two inductively coupled plasma emission spectrometers, PE and SPECTRO, and compared with the chemical method. The test results are as follows.
[0142] Production assessment results (%)
[0143]
[0144] After testing with two inductively coupled plasma emission spectrometers, the data obtained were consistent with the chemical test results, indicating that the composition design of the three single-point calibration samples was reasonable, the uniformity was good, and the fixed values were accurate and reliable.
[0145] The various technical features described above can be combined arbitrarily. Although all possible combinations of these technical features are not described, any combination of these technical features should be considered to be covered by this specification as long as there is no contradiction in such combination.
[0146] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing nuclear grade hafnium and hafnium alloy single point spectrum standard samples, characterized in that: The method comprises: According to the mass percentage of the elements: Fe is 0.02% to 0.048%, Cr is 0.0015% to 0.009%, Zr is 0.58% to 0.65%, Al is less than 0.01%, Cu is less than 0.01%, Ni is less than 0.005%, Si is less than 0.01%, and the balance is hafnium, and a bulk nuclear grade hafnium sponge mixed raw material is obtained; wherein the hafnium is bulk nuclear grade hafnium sponge; Vacuum arc melting the bulk nuclear-grade hafnium sponge mixed raw material to obtain a primary ingot of nuclear-grade hafnium alloy; The nuclear-grade hafnium alloy primary ingot is subjected to multiple cold crucible magnetic suspension melting to obtain a nuclear-grade hafnium alloy ingot; this process specifically comprises: The nuclear-grade hafnium alloy primary ingot is subjected to cold crucible magnetic suspension primary melting to obtain a nuclear-grade hafnium alloy primary ingot; The nuclear-grade hafnium alloy primary ingot is subjected to cold crucible magnetic suspension secondary melting to obtain a nuclear-grade hafnium alloy secondary ingot; Specifically, the cold crucible magnetic levitation melting refers to a melting technology that uses electromagnetic force to keep the molten metal and the crucible in a non-contact state; The nuclear-grade hafnium alloy ingot is reprocessed to obtain nuclear-grade hafnium and hafnium alloy single-point spectrum standard samples.
2. The method according to claim 1, characterized in that The step of subjecting the nuclear-grade hafnium alloy primary ingot to cold crucible magnetic suspension primary melting to obtain a nuclear-grade hafnium alloy primary ingot comprises: The vacuum degree in the crucible reaches 1.0×10 -2 Under the condition of MPa, high purity argon gas is introduced into the primary ingot of nuclear grade hafnium alloy in the crucible; Control the power of the induction coil to carry out smelting and keep the temperature for 10 to 20 minutes; The mixture is cooled to obtain a nuclear grade hafnium alloy primary ingot.
3. The method according to claim 2, characterized in that The method of controlling the power of the induction coil to perform smelting and keeping the temperature for 10 to 20 minutes comprises: The primary smelting power is 160KW-180KW, and the heat preservation power is 140KW-150KW.
4. The method according to claim 1, characterized in that: The step of subjecting the nuclear-grade hafnium alloy primary ingot to cold crucible magnetic suspension secondary melting to obtain a nuclear-grade hafnium alloy secondary ingot comprises: The vacuum degree in the crucible reaches 1.0×10 -2 Under the condition of MPa, high purity argon gas is introduced into the primary ingot of nuclear grade hafnium alloy in the crucible; Control the power of the induction coil to perform smelting to obtain a nuclear-grade hafnium alloy solution, and keep the solution warm for 10 to 20 minutes; The nuclear-grade hafnium alloy solution is cast into a mold and cooled to obtain a nuclear-grade hafnium alloy secondary ingot.
5. The method according to claim 4, characterized in that The method of controlling the power of the induction coil to perform smelting and keeping the temperature for 10 to 20 minutes comprises: The secondary smelting power is 260KW-280KW, and the insulation power is 240KW-250KW.
6. The method according to claim 1, characterized in that The nuclear-grade hafnium alloy primary ingot is subjected to cold crucible magnetic suspension secondary melting to obtain a nuclear-grade hafnium alloy secondary ingot, which further comprises: The nuclear-grade hafnium alloy primary ingot is placed upside down.
7. The method according to claim 4, characterized in that The step of casting the nuclear-grade hafnium alloy solution into a mold and cooling the mold to obtain a nuclear-grade hafnium alloy secondary ingot comprises: Direct casting is carried out by rotating the crucible.
8. The method according to claim 1, characterized in that The step of reprocessing the nuclear-grade hafnium alloy ingot to obtain a nuclear-grade hafnium and hafnium alloy single-point spectrum standard sample comprises: Initial uniformity inspection: After the ingot surface is treated, 100mm is cut off from the upper and lower ends, and the ingot is subjected to non-destructive testing. Then, chip-like samples are taken from the upper and lower end surfaces and the middle position of the nuclear-grade hafnium alloy ingot to inspect the component segregation and process the analysis data; Processing: Process the nuclear-grade hafnium alloy ingots that have passed the initial uniformity inspection into chip-like samples with a length × width × thickness of approximately 3mm × 1mm × 0.2mm; Composition uniformity inspection: Randomly select 3 groups of uniformly mixed nuclear-grade hafnium alloy chip samples, each with 15 samples, and inspect the 3 groups of data on the Agilent inductively coupled plasma optical emission spectrometer; Fixed value: Perform fixed value analysis on samples that have passed the component uniformity inspection.
Citation Information
Patent Citations
Uniformity control method for trace element arsenic in cast superalloy standard substance
CN103759991A
Method for measuring content of magnesium in nuclear-level sponge zirconium particles
CN106885799A