A sandwich structure negative electrode sheet, a precursor electrode sheet and its preparation and application

By designing a sandwich-structured precursor anode sheet and performing directional lithiation, the problem of electrical contact failure caused by volume changes in silicon anodes was solved, resulting in a high-performance lithium-ion battery anode that improves the cycle stability and capacity of the battery.

CN114203956BActive Publication Date: 2024-11-22HUNAN CHENYU FUJI NEW ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111508525.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-10
Publication Date
2024-11-22
Estimated Expiration
2041-12-10

AI Technical Summary

Technical Problem

In existing lithium-ion batteries, the silicon anode may detach from the current collector due to volume expansion and contraction during charging and discharging, resulting in loss of electrical contact, capacity decay, and lifespan degradation. Existing solutions are either costly or inefficient.

Method used

The sandwich structure precursor anode sheet includes a core-shell structure active precursor layer and a permanent magnet layer combined with a current collector. Targeted lithiation treatment is used to achieve magnetic correlation between the permanent magnet layer and the converted precursor layer, thereby enhancing the electrical contact between the active material and the current collector.

Benefits of technology

It significantly improves the cycle stability and capacity of lithium-ion batteries, reduces the capacity decay of silicon anodes, and enhances the electrochemical performance of batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003404325300000101
    Figure BDA0003404325300000101
Patent Text Reader

Abstract

The present invention belongs to the technical field of negative electrodes of lithium secondary batteries, and specifically discloses a sandwich structure precursor negative electrode sheet, including a precursor layer, a current collector layer and a permanent magnet layer that are compounded in sequence; the precursor layer contains an active precursor, which includes a core and a shell covering the core, and the core is a magnetic metal element oxide; the shell is an active negative electrode material. The present invention also provides the preparation and application of the precursor electrode sheet, as well as the prepared sandwich negative electrode sheet and battery. The present invention has found that through magnetic constraint, the active material is in more complete contact with the current collector, which significantly reduces the capacity decay of the negative electrode and improves the overall cycle stability and cycle life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of negative electrodes for lithium secondary batteries, and in particular relates to a new high-stability negative electrode sheet preparation technology. Background Art

[0002] Lithium-ion batteries are a type of secondary battery that is widely used in new energy vehicles and electronic consumer products. Compared with other traditional batteries, lithium-ion batteries have advantages such as higher energy density, longer cycle life, and no memory effect. The technological progress of lithium-ion batteries is also very fast, but it still cannot keep up with the requirements of electronic consumer products and new energy vehicles for battery performance, especially the problem of insufficient battery life, which makes consumers still suffer from "insufficient power" and "mileage anxiety". In order to improve the battery life, we can start with the battery structure and battery materials, increase the capacity while reducing the battery weight. Among them, the most fundamental way is to use new electrode materials with high specific capacity.

[0003] Silicon, as a negative electrode material that can be alloyed with lithium, has the highest theoretical specific capacity (~4200mAh / g) and is the most promising next-generation new negative electrode. However, during the actual charging and discharging process, the silicon negative electrode will undergo large volume expansion and contraction as lithium ions are embedded and extracted. Under constant volume changes, the silicon negative electrode will fall off from the current collector. After falling off, the silicon loses electrical contact and will no longer contribute capacity, and the battery will show capacity decay and life decline. The problem of loss of electrical contact caused by volume expansion has prevented silicon negative electrodes from being widely used.

[0004] In order to solve the above problems and improve the performance of silicon negative electrodes, academia and industry have done a lot of work. For example, Zhao Youman et al. (Exploring mechanism of carbon nanotubes as conductive agent for improving performance of a silicon / carbon anode in LIB [J]. Energy Storage Science and Technology, 2021, 10 (01): 118-127.) studied the effect of adding single-walled carbon nanotubes to silicon negative electrode slurry and found that single-walled carbon nanotubes, as a one-dimensional conductive agent, have a large aspect ratio and can be interwoven to form a conductive network. Although it itself cannot inhibit the volume expansion of silicon, it can increase the connection channel between silicon and the current collector, thereby improving the cycle life of the overall electrode. However, single-walled carbon nanotubes are very expensive, and relying on a large number of carbon tubes to connect silicon and the current collector is very inefficient and the cost is unacceptable.

[0005] In addition, Yongxiang Sun et al. (Binary Network of Conductive Elastic Polymer Constraining Nanosilicon for a High Performance Lithium-Ion Battery [J], ACS Nano 2021, 15 (9): 14570-14579) developed a multifunctional conductive polymer as a binder. The binder has strong viscosity and can fix silicon particles on the current collector very well. Its good conductivity also enhances the electrical connection between silicon and the current collector, showing a significant effect in improving the cycle life of silicon negative electrodes. However, the current preparation process of this conductive binder is complex, the cost is high, and it is difficult to prepare on a large scale. Summary of the invention

[0006] In view of the problems existing in the prior art, the first purpose of the present invention is to provide a precursor negative electrode sheet with a sandwich structure, aiming to provide a precursor negative electrode sheet that can be converted into a negative electrode with high electrochemical performance.

[0007] The second object of the present invention is to provide a method for preparing the sandwich structure precursor negative electrode sheet.

[0008] The third object of the present invention is to provide an application method of preparing a negative electrode sheet using the sandwich structure precursor negative electrode sheet.

[0009] The fourth object of the present invention is to provide a sandwich structure negative electrode sheet, aiming to improve the capacity, rate and cycle stability of the negative electrode sheet.

[0010] The fifth object of the present invention is to provide a lithium secondary battery equipped with the sandwich structure negative electrode sheet and its preparation.

[0011] A sandwich structure precursor negative electrode sheet, comprising a precursor layer, a current collector layer and a permanent magnet layer which are compounded in sequence;

[0012] The precursor layer contains an active precursor, which includes a core and a shell covering the core, wherein the core is a magnetic metal element oxide; and the shell is an active negative electrode material.

[0013] The present invention has found that by cooperating the permanent magnet layer and the precursor layer of the core-shell structure with the current collector to construct a hierarchical structure, the permanent magnet layer and the transformed precursor layer can be magnetically associated by in-situ transformation of the precursor layer, thereby facilitating the acquisition of a high-performance negative electrode sheet.

[0014] In the present invention, the precursor negative electrode sheet includes a current collector having two surfaces (divided into surface A and surface B, with surface B located on the back of surface A), a precursor layer composited on surface A, and a permanent magnet layer composited on surface B. In the present invention, the combination of the hierarchical materials and the hierarchical composite structure is the key to improving its electrochemical performance. In addition, the present invention also found that the combination of the precursor composition and the core-shell structure is another key to synergistically improving the electrochemical performance with the permanent magnet layer.

[0015] In the present invention, the magnetic metal element is at least one of iron, cobalt and nickel;

[0016] Preferably, the magnetic metal element oxide is at least one of FeO, Fe2O3, Fe3O4, NiO, and CoO;

[0017] Preferably, the shell is at least one of Si, Ge, and Sn; preferably Si;

[0018] Preferably, in the active precursor, the mass ratio of core to shell is 50-95:5-50;

[0019] Preferably, the D50 of the active precursor is 10-500 nm, more preferably 50-150 nm;

[0020] Preferably, the precursor layer further comprises at least one auxiliary agent selected from the group consisting of a binder and a conductive agent, preferably a binder and a conductive agent;

[0021] The binder may be a component with a bonding effect known in the industry, such as at least one of PVDF, CMC, and PAA;

[0022] The conductive agent may be a carbon material with conductive properties known in the industry, such as at least one of conductive carbon black, acetylene black, and carbon nanotubes.

[0023] Preferably, in the precursor layer, the weight percentage of the active precursor is 70-98%; the balance is an auxiliary agent; preferably, the auxiliary agent includes a binder and a conductive agent, wherein the weight ratio of the two is, for example, 1-3:1-3.

[0024] Preferably, the thickness of the precursor layer can be controlled as required, for example, it can be 1-200 microns, preferably 20-50 microns.

[0025] In the present invention, the permanent magnet is a rigid magnetic material. Preferably, the permanent magnet includes but is not limited to at least one of an aluminum-nickel-cobalt permanent magnet alloy, an iron-chromium-cobalt permanent magnet alloy, and a rare earth permanent magnet;

[0026] Preferably, the permanent magnet is neodymium iron boron powder;

[0027] Preferably, the particle size of the permanent magnet is 1-100 microns, more preferably 30-60 microns;

[0028] Preferably, the magnetic induction intensity of the permanent magnet is 0.05-0.2T;

[0029] Preferably, the thickness of the permanent magnet layer can be controlled as required, for example, it can be 10-500 microns, more preferably 100-300 microns;

[0030] Preferably, the permanent magnet layer further comprises an adhesive;

[0031] The adhesive may be a component with bonding effect known in the industry, such as at least one of PVDF, CMC, PAA, and PVA;

[0032] Preferably, in the permanent magnet layer, the weight percentage of the permanent magnet is 90-99%, and the remainder is other components such as a binder.

[0033] In the present invention, the current collector is at least one of a planar current collector and a 3D current collector; the planar current collector is a metal planar current collector, and the 3D current collector is a 3D metal and its alloy current collector or a carbon-based current collector. Preferably, the current collector is a planar current collector;

[0034] Preferably, the metal element of the planar current collector is at least one of Cu, Fe and Ni;

[0035] Preferably, the thickness of the current collector layer can be controlled as required, for example, it can be 1-50 microns, preferably 10-30 microns.

[0036] The present invention also provides a method for preparing the sandwich structure precursor negative electrode sheet, which is obtained by compounding the active precursor and the permanent magnet on two opposite surfaces of the current collector in any order.

[0037] In the present invention, the active precursor can be prepared based on existing means.

[0038] Preferably, the preparation process of the active precursor is: obtaining the core particles in advance, and then coating the active negative electrode material on the surface of the core particles;

[0039] The core can be a ready-made commercial product, or can be prepared based on existing theories and methods. For example, when the core is ferroferric oxide, it can be prepared by precipitation, microemulsion, emulsification, sol-gel, chemical oxidation, hydrothermal, and high-temperature thermal decomposition. For example, the steps of the precipitation method are as follows: a mixed solution of FeCl2 and FeCl3 is prepared, so that Fe 2+ / Fe3+ The molar ratio is 0.8-1.2:1, heated to 60-80℃ in a water bath, added with ammonia water, adjusted to pH 10-11, precipitated, aged for 20-60min, and then centrifuged to obtain nano-Fe3O4 particles.

[0040] In the present method, the active negative electrode material can be coated on the surface of the core based on existing means, such as CVD, PVD, and evaporation methods;

[0041] For example, silicon can be coated on the surface of the core by a CVD method, the steps are:

[0042] placing the core in a silicon-containing gas source and depositing a silicon layer on the surface of the core at a deposition temperature of 500-600° C.;

[0043] Preferably, the silicon-containing gas source is at least one of silane, trichlorosilane and dichlorosilane;

[0044] Preferably, the CVD deposition time is 1-3 hours.

[0045] In the present invention, the precursor permanent magnet can be compounded on the surface of the current collector by existing means. For example, the precursor layer and the permanent magnet layer can be compounded on the surface of the current collector by solvent slurrying or coating.

[0046] The present invention also provides an application of the sandwich structure precursor negative electrode sheet, and the core of the precursor in the sandwich structure precursor negative electrode sheet is directionally lithified to obtain the sandwich structure negative electrode sheet.

[0047] The directed lithiation of the core described in the present invention refers to inducing metallic lithium to react preferentially with the core. In the present invention, the directed lithiation can be achieved by means of existing means, and the present invention preferably adopts a voltage control method; so that metallic lithium reacts preferentially with the core. For example, in the directed lithiation stage, the lithium insertion voltage of the first cycle is controlled to be between the shell and the core, the subsequent lithium insertion voltage (lithium insertion cut-off voltage) is less than the lithium insertion voltage of the shell, and the deintercalation voltage (deintercalation cut-off voltage) is between the core and shell deintercalation voltages.

[0048] In the present invention, the directional lithiation can be achieved by controlling the lithium insertion voltage with the help of existing electrodeposition means.

[0049] For example, when the core in the precursor is an oxide of a magnetic metal element (labeled as M a O), through the directional lithiation treatment, the metal lithium is induced to react only with the oxide during the first lithium insertion, and the following replacement reaction process is carried out:

[0050] M a O+2Li→M a +Li2O:(M aRefers to magnetic metal elements). (1)

[0051] The generated Ma has stable ferromagnetism, thus building magnetic correlation between layers and improving the performance of the negative electrode.

[0052] The preferred directional lithium insertion process is: preparing the oxide of the magnetic metal (M a O, such as iron, cobalt, nickel oxide) nanoparticles, and then with high capacity negative electrode materials (M b , such as Si, Ge, Sn) are compounded into a core-shell structure to obtain a precursor M a O@M b Then the precursor is coated on one side of the copper foil to form a precursor layer, and the other side is coated with permanent magnet powder to form a permanent magnet layer to obtain the precursor negative electrode sheet. The precursor negative electrode sheet is used as the working electrode, and lithium metal is used as the counter electrode. Based on existing knowledge, a button battery is assembled and charged and discharged once. The lithium insertion voltage is controlled at M a O Lithium insertion voltage (V a1 ) and M b Lithium insertion voltage (V b1 ), that is, V a1 >V 嵌 >V b1 , so that reaction (1) is carried out to obtain M a -Li2O@M b Active material. Subsequent lithium insertion voltage < V b1 The deintercalation voltage is controlled at the oxide lithium intercalation voltage (V a2 ) and high capacity material lithium insertion voltage (V b2 ), that is, V a2 >V 脱 >V b2 , so that the reverse reaction of reaction formula (1) does not occur. Since Ma is a magnetic metal, the active material and the permanent magnet are magnetically adsorbed, thereby enhancing the stability of the active material. In the present invention, the battery after the directional lithiation treatment can be directly subjected to electrochemical cycling.

[0053] For example, when the core of the precursor is ferroferric oxide and its shell is silicon, in the directional lithiation stage, the first cycle of lithium insertion cutoff voltage is 0.25-0.35V, and the subsequent lithium insertion cutoff voltage is less than or equal to 0.1V (preferably 0.02-0.05V); the lithium desorption cutoff voltage is less than or equal to 1.2V, preferably 1-1.2V.

[0054] A typical implementation scheme of the present invention:

[0055] ①Prepare Fe3O4 nanoparticles by precipitation method. Prepare a mixed solution of FeCl2 and FeCl3 so that the molar ratio of Fe2+ / Fe3+ is 0.8-1.2:1, heat it in a water bath to 60-80℃, add ammonia water, adjust the pH to 10-11, and after precipitation, age it for 20-60min, and then centrifuge to obtain nano Fe3O4 particles.

[0056] ② Silicon coating by CVD method. The Si coating layer is made by chemical vapor deposition (CVD) at a certain temperature with a silicon-containing gas source, and the silicon-containing gas source includes: silane, trichlorosilane, and dichlorosilane. Silane gas is preferred, and the deposition temperature is 500-600°C and the time is 1-3h.

[0057] ③ Coating the double-sided pole piece. The back side is coated with NdFeB powder, with a particle size of 1-100 microns and a magnetic induction intensity of 0.05-0.2T. Mix FeNdB magnetic powder and PVA in water at a ratio of 90-95:5-10, stir evenly and apply it on one side of the current collector (copper foil), and dry. Coat the active precursor material on the front side of the pole piece. That is, mix Fe3O4@Si with conductive carbon black and binder CMC in a ratio of 8-9:0.5-1:0.5-1 and dissolve them in water, stir evenly and apply them on the other side of the copper foil.

[0058] ④ Reduce Fe3O4 by controlled voltage method. Use lithium sheet as counter electrode and assemble the above-mentioned electrode sheet into button battery. Charge and discharge the battery once, and control the lithium insertion cutoff voltage to 0.25-0.35V, so that the reaction described in reaction formula (2) occurs, and the active material is converted into Fe-Li2O@Si in situ. The lithium insertion cutoff voltage of subsequent cycles returns to normal, such as 0.05V. Since Fe elemental substance has ferromagnetism, it is magnetized by the permanent magnet on the back and attracts each other, so that Fe-Li2O@Si maintains close electrical contact with the current collector.

[0059] Fe3O4+8Li→3Fe+4Li2O (2)

[0060] ⑤ Control the first and subsequent delithiation cut-off voltages to be lower than 1.2V to ensure that Fe does not undergo phase transformation, thereby maintaining a stable structure and stable magnetic attraction.

[0061] The present invention also provides a sandwich structure negative electrode sheet, which comprises an active layer, a current collector layer and a permanent magnet layer which are compounded in sequence;

[0062] The active layer comprises an active material, which comprises a lithiated core and a coated shell, wherein the lithiated core comprises a magnetic metal element and lithium oxide.

[0063] In the present invention, the magnetic correlation between the active layer and the permanent magnetic layer of the negative electrode sheet, combined with the core-shell structure characteristics of the active layer, helps to synergistically improve the electrochemical performance of the negative electrode sheet, especially the cycle stability.

[0064] In the present invention, the selection range and layer parameters of the current collector layer, permanent magnet layer, magnetic metal elements of the active layer, shell materials in the sandwich structure negative electrode sheet are the same as those of the precursor negative electrode sheet.

[0065] Preferably, the sandwich structure negative electrode sheet is formed by nuclear-directed lithiation of a precursor of the sandwich structure precursor negative electrode sheet.

[0066] In the present invention, the lithium oxide is the product of a replacement reaction between lithium and a core (the magnetic metal element oxide).

[0067] The present invention also provides a lithium secondary battery, comprising the sandwich structure negative electrode sheet.

[0068] The present invention also provides a method for preparing the lithium secondary battery, which comprises assembling a battery with the sandwich structure precursor negative electrode sheet, and directionally lithiating the core of the active precursor in the precursor negative electrode sheet to prepare the lithium secondary battery.

[0069] In the present invention, the precursor negative electrode sheet can be used as a conventional negative electrode sheet for half-cell and full-cell assembly, and then the directional lithiation treatment is performed to convert the precursor negative electrode sheet into a negative electrode sheet in situ in the battery, thereby obtaining the battery.

[0070] For example, after assembling the battery with the precursor negative electrode sheet, the first cycle of lithium insertion voltage is controlled to be between the shell and the core by means of voltage control, the subsequent lithium insertion voltage is less than the shell lithium insertion voltage, and the de-insertion voltage is between the core and shell de-insertion voltages; the lithium secondary battery is obtained after directional lithiation treatment.

[0071] The lithium secondary battery can be a lithium ion battery or a lithium metal battery.

[0072] Beneficial effects:

[0073] 1. The present invention provides a new precursor negative electrode sheet, which combines a permanent magnet layer and the precursor layer of the core-shell structure with a current collector to construct a sandwich hierarchical structure. In this way, the permanent magnet layer and the transformed precursor layer can be magnetically associated by in-situ transformation of the precursor layer, which is conducive to obtaining a high-performance negative electrode sheet.

[0074] 2. The present invention provides a negative electrode sheet with a completely new structure, which can improve the electrochemical performance of the material through the magnetic correlation between the permanent magnetic layer and the active layer;

[0075] 3. The present invention creatively utilizes the controlled voltage method to in situ prepare a stable magnetic active layer, and innovatively utilizes magnetic constraint so that the active negative electrode material (such as silicon) can be firmly adsorbed on the surface of the current collector and maintain good electrical contact with the current collector, which greatly reduces the capacity attenuation of the silicon negative electrode and improves the cycle stability.

[0076] 4. The present invention performs in-situ lithiation of the precursor negative electrode sheet in the battery by a voltage-controlled method, and can construct the magnetically constrained negative electrode in the battery, which helps to improve the performance of the battery. DETAILED DESCRIPTION

[0077] The present invention will be described in detail below with reference to the embodiments, but the present invention is not limited thereto.

[0078] Example 1

[0079] (1) Fe3O4 nanoparticles were prepared by precipitation method. A mixed solution of FeCl2 and FeCl3 was prepared so that Fe 2+ / Fe 3+ The molar ratio of 0.9:1 was set, heated to 80°C in a water bath, ammonia water was added, the pH was adjusted to 10, precipitation was generated, and then aged for 60 minutes, and then centrifuged to obtain nano Fe3O4 particles. After testing, the median particle size D50 of the nano particles was 78.5nm.

[0080] (2) Silicon was coated by CVD method. The silicon source was SiH4 gas, the deposition temperature was 500℃, and the time was 3h. After testing, the thickness of the silicon coating layer was 40.3nm, and Fe3O4@Si active precursor was obtained;

[0081] (3) Coating double-sided pole pieces. NdFeB powder and PVA were mixed in water at a ratio of 95:5, with a D50 particle size of 60 microns and a magnetic induction intensity of 0.2T. The solution was stirred and evenly coated on a 12-micron thick copper foil, and dried to obtain a permanent magnet (thickness of 200 microns). Then, Fe3O4@Si, conductive carbon black and CMC were mixed in water at a ratio of 8:1:1, stirred and evenly coated on the other side of the copper foil, and dried to obtain an active precursor layer (thickness of 20 microns).

[0082] (4) Controlled voltage method for reducing Fe3O4. A lithium sheet is used as a counter electrode, and the above-mentioned electrode sheet is used as a working electrode of a button cell. The electrolyte is 1 mol / L lithium hexafluorophosphate (LiPF6) electrolyte dissolved in ethylene carbonate (EC) and diethyl carbonate (DEC) electrolyte in a volume ratio of 1:1; assembled into a button cell.

[0083] (5): Directed lithium insertion

[0084] The battery was charged and discharged once (directional lithium insertion), and the lithium insertion cutoff voltage was controlled to 0.25 V, so that the reaction described in reaction formula (2) occurred, and the active material was converted into Fe-Li2O@Si in situ, and the subsequent lithium insertion cutoff voltage was restored to the normal 0.05 V. Since Fe elemental substance has ferromagnetism, it is magnetized by the permanent magnet on the back and attracts each other, so that the active material containing silicon maintains electrical contact with the current collector.

[0085] The delithiation cut-off voltage is 1.2V, which ensures that Fe will not undergo phase transformation, thereby maintaining a stable structure and stable magnetic attraction.

[0086] Example 2

[0087] (1) Fe3O4 nanoparticles were prepared by precipitation method. A mixed solution of FeCl2 and FeCl3 was prepared so that the molar ratio of Fe2+ / Fe3+ was 1:1, heated to 70°C in a water bath, and ammonia water was added to adjust the pH to 10.5. After precipitation, the solution was aged for 40 minutes and then centrifuged to obtain nano Fe3O4 particles. The median particle size D50 of the nanoparticles was 59.3 nm.

[0088] (2) Silicon is coated by CVD method. The silicon source is SiH4 gas, the deposition temperature is 550℃, and the time is 2h. After testing, the thickness of the silicon coating layer is 30.2nm.

[0089] (3) Coating double-sided pole pieces. NdFeB powder and PVA were mixed in water at a ratio of 95:5, with a D50 particle size of 50 microns and a magnetic induction intensity of 0.1 T. The solution was stirred and evenly coated on a 12-micron thick copper foil, and dried to obtain a permanent magnet layer (150 microns thick). Then, Fe3O4@Si, conductive carbon black and CMC were mixed in water at a ratio of 8:1:1, stirred and evenly coated on the other side of the copper foil, and dried to obtain an active precursor layer (30 microns thick).

[0090] (4) Controlled voltage method for reducing Fe3O4. A lithium sheet is used as a counter electrode, and the above-mentioned electrode sheet is used as a working electrode of a button cell. The electrolyte is 1 mol / L lithium hexafluorophosphate (LiPF6) electrolyte dissolved in ethylene carbonate (EC) and diethyl carbonate (DEC) electrolyte in a volume ratio of 1:1; assembled into a button cell.

[0091] (5) Directed lithium insertion

[0092] The battery was charged and discharged once (directional lithium insertion), and the lithium insertion cutoff voltage was controlled to 0.3 V, so that the reaction described in reaction formula (2) occurred, and the active material was converted into Fe-Li2O@Si in situ, and the subsequent lithium insertion cutoff voltage was restored to the normal 0.05 V. Since Fe elemental substance has ferromagnetism, it is magnetized by the permanent magnet on the back and attracts each other, so that the active material containing silicon maintains electrical contact with the current collector.

[0093] (6) The delithiation cutoff voltage is 1.2 V, which ensures that Fe does not undergo phase transformation, thereby maintaining a stable structure and stable magnetic attraction.

[0094] Example 3

[0095] (1) Fe3O4 nanoparticles were prepared by precipitation method. A mixed solution of FeCl2 and FeCl3 was prepared so that the molar ratio of Fe2+ / Fe3+ was 1.1:1, heated to 60°C in a water bath, and ammonia water was added to adjust the pH to 11. After precipitation, the solution was aged for 20 minutes and then centrifuged to obtain nano Fe3O4 particles. The median particle size D50 of the nanoparticles was 32.5 nm.

[0096] (2) Silicon was coated by CVD method. The silicon source was SiH4 gas, the deposition temperature was 600℃, and the time was 1h. After testing, the thickness of the silicon coating layer was 23.4nm.

[0097] (3) Coating double-sided pole pieces. NdFeB powder and PVA were mixed and dissolved in water at a ratio of 95:5, with a D50 particle size of 30 microns and a magnetic induction intensity of 0.05T. The solution was stirred and evenly coated on a 12-micron thick copper foil, and dried to obtain a permanent magnet layer (100 microns thick). Then, Fe3O4@Si, conductive carbon black and CMC were mixed and dissolved in water at a ratio of 8:1:1, stirred evenly and coated on the other side of the copper foil, and dried to obtain an active precursor layer (50 microns thick).

[0098] (4) Controlled voltage method for reducing Fe3O4. A lithium sheet is used as a counter electrode, and the above-mentioned electrode sheet is used as a working electrode of a button cell. The electrolyte is 1 mol / L lithium hexafluorophosphate (LiPF6) electrolyte dissolved in ethylene carbonate (EC) and diethyl carbonate (DEC) electrolyte in a volume ratio of 1:1; assembled into a button cell.

[0099] (5) Directed lithium insertion

[0100] The battery was charged and discharged once (directional lithium insertion), and the lithium insertion cutoff voltage was controlled to 0.35 V, so that the reaction described in reaction formula (2) occurred, and the active material was converted into Fe-Li2O@Si in situ, and the subsequent lithium insertion cutoff voltage was restored to the normal 0.05 V. Since Fe elemental substance has ferromagnetism, it is magnetized by the permanent magnet on the back and attracts each other, so that the active material containing silicon maintains electrical contact with the current collector.

[0101] (6) The delithiation cutoff voltage is 1.2 V, which ensures that Fe does not undergo phase transformation, thereby maintaining a stable structure and stable magnetic attraction.

[0102] Comparative Example 1

[0103] Compared with Example 1, the only difference is that no permanent magnet layer is coated on the current collector surface, and only the active precursor layer is coated; other operations and parameters are the same as Example 1.

[0104] Comparative Example 2

[0105] Compared with Example 1, the only difference is that step (5) is not performed, the first cycle voltage control process is not performed, and the subsequent cycle test is directly entered.

[0106] Comparative Example 3

[0107] Compared with Example 1, the only difference is that ferrosoferric oxide and silicon are formed by conventional physical mixing, and the coating structure is not constructed by CVD. Other parameters and operations are the same as in Example 1.

[0108] Cyclic performance measurement

[0109] The battery after directional lithium insertion in each embodiment and comparative example was subjected to cycle performance test. The first charge and discharge was tested at a current density of 0.2C, and the cycle capacity stability was tested at a current of 0.5C. The ratio of the lithium removal capacity at the 100th cycle to the lithium removal capacity at the first cycle was used as the capacity retention index.

[0110] Table 1: Test results of examples and comparative examples

[0111]

[0112] In summary, the material constructed using the method of the present invention has excellent cycle performance.

Claims

1. A sandwich structure precursor negative electrode sheet, characterized in that: It includes a precursor layer, a current collector layer and a permanent magnet layer which are compounded in sequence; The precursor layer contains an active precursor, which includes a core and a shell covering the core, wherein the core is a magnetic metal element oxide; and the shell is an active negative electrode material of at least one of Si, Ge and Sn.

2. The sandwich structure precursor negative electrode sheet according to claim 1, characterized in that: The magnetic metal element is at least one of iron, cobalt and nickel.

3. The sandwich structure precursor negative electrode sheet according to claim 1, characterized in that: The magnetic metal element oxide is at least one of FeO, Fe2O3, Fe3O4, NiO and CoO.

4. The sandwich structure precursor negative electrode sheet according to claim 1, characterized in that: The shell is Si.

5. The sandwich structure precursor negative electrode sheet according to claim 1, characterized in that: In the active precursor, the mass ratio of core to shell is 50-95:5~50.

6. The sandwich structure precursor negative electrode sheet according to claim 1, characterized in that: The D50 of the active precursor is 10-500nm.

7. The sandwich structure precursor negative electrode sheet according to claim 1, characterized in that: The precursor layer further comprises at least one auxiliary agent selected from the group consisting of a binder and a conductive agent.

8. The sandwich structure precursor negative electrode sheet according to claim 7, characterized in that: In the precursor layer, the weight percentage of the active precursor is 70-98%; the remainder is an auxiliary agent.

9. The sandwich structure precursor negative electrode sheet according to claim 1, characterized in that: The thickness of the precursor layer is 1~200 microns.

10. The sandwich structure precursor negative electrode sheet according to claim 1, characterized in that: The permanent magnet is at least one of an aluminum-nickel-cobalt permanent magnet alloy, an iron-chromium-cobalt permanent magnet alloy, and a rare earth permanent magnet.

11. The sandwich structure precursor negative electrode sheet according to claim 10, characterized in that: The permanent magnet is neodymium iron boron powder.

12. The sandwich structure precursor negative electrode sheet according to claim 10, characterized in that: The particle size of permanent magnets is 1-100 microns.

13. The sandwich structure precursor negative electrode sheet according to claim 10, characterized in that: The magnetic induction intensity of the permanent magnet is 0.05-0.2T.

14. The sandwich structure precursor negative electrode sheet according to claim 1, characterized in that: The thickness of the permanent magnet layer is 10~500 microns.

15. The sandwich structure precursor negative electrode sheet according to claim 1, characterized in that: The permanent magnet layer further includes a binder.

16. The sandwich structure precursor negative electrode sheet according to claim 15, characterized in that: In the permanent magnet layer, the weight percentage of permanent magnets is 90-99%.

17. The sandwich structure precursor negative electrode sheet according to claim 1, characterized in that: The current collector is at least one of a planar current collector and a 3D current collector.

18. The sandwich structure precursor negative electrode sheet according to claim 17, characterized in that: The metal element of the planar current collector is at least one of Cu, Fe and Ni.

19. The sandwich structure precursor negative electrode sheet according to claim 1, characterized in that: The thickness of the current collector layer is 1 to 50 microns.

20. A method for preparing a sandwich structure precursor negative electrode sheet according to any one of claims 1 to 19, characterized in that: The active precursor and the permanent magnet are compounded on two opposite surfaces of the current collector in any order to obtain the product.

21. The method for preparing a sandwich structure precursor negative electrode sheet according to claim 20, characterized in that: The preparation process of the active precursor is: obtaining the core particles in advance, and then coating the active negative electrode material on the surface of the core particles.

22. The method for preparing a sandwich structure precursor negative electrode sheet according to claim 21, characterized in that: The active negative electrode material is coated on the surface of the core by chemical vapor deposition, physical vapor deposition and evaporation method.

23. The method for preparing a sandwich structure precursor negative electrode sheet according to claim 21, characterized in that: Silicon is coated on the surface of the core by chemical vapor deposition method, the steps are as follows: The core is placed in a silicon-containing gas source, and a silicon layer is deposited on the surface of the core at a deposition temperature of 500-600°C.

24. The method for preparing a sandwich structure precursor negative electrode sheet according to claim 23, characterized in that: The silicon-containing gas source is at least one of silane, trichlorosilane and dichlorosilane.

25. The method for preparing a sandwich structure precursor negative electrode sheet according to claim 23, characterized in that: The chemical vapor deposition deposition time is 1-3 hours.

26. The method for preparing a sandwich structure precursor negative electrode sheet according to claim 1, characterized in that: The precursor layer and the permanent magnet layer are compounded on the surface of the current collector by means of solvent slurrying and coating.

27. An application of the sandwich structure precursor negative electrode sheet according to any one of claims 1 to 19, characterized in that: The core of the precursor in the sandwich structure precursor negative electrode sheet is directionally lithified to obtain the sandwich structure negative electrode sheet.

28. The use according to claim 27, characterized in that Directed lithiation is carried out by a voltage control method, the steps of which are: controlling the lithium insertion voltage of the first cycle to be between the lithium insertion voltage of the shell and the lithium insertion voltage of the core, the subsequent lithium insertion voltage is less than the lithium insertion voltage of the shell, and the de-insertion voltage is between the core and shell de-insertion voltages.

29. The use according to claim 28, characterized in that When the core of the precursor is ferroferric oxide and the shell is silicon, in the directional lithiation stage, the first lithium insertion voltage is 0.25-0.35V, and the subsequent lithium insertion voltage is less than or equal to 0.1V; The de-embedding voltage is less than or equal to 1.2V.

30. A sandwich structure negative electrode sheet, characterized in that: It is formed by the core-oriented lithiation of the precursor of the sandwich structure precursor negative electrode sheet according to any one of claims 1 to 19.

31. A lithium secondary battery, characterized in that: A sandwich structure negative electrode sheet comprising the method of claim 30.

32. A method for preparing a lithium secondary battery according to claim 31, characterized in that: The sandwich structure precursor negative electrode sheet described in any one of claims 1 to 19 is used to assemble a battery, and the lithium insertion voltage of the charge and discharge process is controlled to be greater than the lithium insertion voltage of the shell of the precursor and less than the lithium insertion voltage of the core, and the core of the active precursor in the precursor negative electrode sheet is directionally lithified to obtain the lithium secondary battery.