Electrode, electrode group, secondary battery, battery pack and vehicle

By using titanium-containing oxides and carbon nanotubes with a particle size of 0.1 μm to 3 μm in the electrode, the peeling strength of the electrode and the current collector is controlled, the problem of electrode cracking at the bending part is solved, and the capacity and capacity of the secondary battery are improved. performance.

CN114203980BActive Publication Date: 2024-10-29KK TOSHIBA
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202110212424.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-02-25
Publication Date
2024-10-29
Estimated Expiration
2041-02-25

AI Technical Summary

Technical Problem

In the wound electrode group of non-aqueous electrolyte batteries, the electrodes are easily broken at the bending parts, resulting in capacity loss and short circuit. It is difficult to effectively prevent this problem with existing technology.

Method used

An electrode containing titanium-containing oxide particles and carbon nanotubes with an average particle size of 0.1 μm or more and 3 μm or less is used, and the peeling strength between the current collector and the active material-containing layer is controlled to be 0.2 kN/m or more and 0.7 kN/m or less to ensure The active material-containing layer of the negative electrode is in a non-bonded state around the winding body to prevent the electrode from cracking.

Benefits of technology

It effectively suppresses cracks and short circuits around the electrode in the winding body, improves the capacity and performance of the secondary battery, and ensures the charge and discharge stability of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114203980B_ABST
    Figure CN114203980B_ABST
Patent Text Reader

Abstract

Embodiments of the present invention relate to electrodes, electrode groups, secondary batteries, battery packs and vehicles. The present invention provides electrodes and electrode groups capable of improving the capacity of secondary batteries, secondary batteries and battery packs with improved capacity, and vehicles equipped with the battery packs. According to an embodiment, an electrode having a current collector and an active material layer in contact with the current collector is provided. The active material layer contains titanium oxide particles and carbon nanotubes having an average particle size of 0.1 μm or more and 3 μm or less. The peel strength between the current collector and the active material layer is 0.2 kN / m or more and 0.7 kN / m or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] Embodiments of the present invention relate to an electrode, an electrode group, a secondary battery, a battery pack, and a vehicle. Background Art

[0002] In the structure of the electrode group contained in the secondary battery such as the non-aqueous electrolyte battery, as general examples, there are a stack structure formed by stacking electrodes and a winding structure in which the winding body of the electrode is stored in an outer packaging container. In the winding structure, when winding a hard electrode, the electrode sometimes breaks at the bending part of the innermost circumference where the stress is added. If the electrode is completely cut, it will not help charge and discharge, and it may not be possible to obtain the specified battery capacity. Summary of the invention

[0003] An object of the present invention is to provide an electrode and an electrode group capable of improving the capacity of a secondary battery, a secondary battery and a battery pack having improved capacity, and a vehicle including the battery pack.

[0004] According to an embodiment, an electrode is provided, which includes a current collector and an active material layer in contact with the current collector. The active material layer contains titanium oxide particles and carbon nanotubes having an average particle size of 0.1 μm or more and 3 μm or less. The peel strength between the current collector and the active material layer is 0.2 kN / m or more and 0.7 kN / m or less.

[0005] According to another embodiment, an electrode group having a positive electrode and a negative electrode is provided. The negative electrode contains the electrode according to the above embodiment. The electrode group has a flat winding structure in which a stacked body including a positive electrode and a negative electrode is wound in a manner that is located at the center along a first direction. At the first bend along the winding direction from the end located at the innermost periphery and along the first direction in the winding structure, that is, the innermost bend, a portion of the active material layer of the negative electrode is in a non-bonded state relative to the current collector.

[0006] According to still another embodiment, there is provided a secondary battery including the electrode group according to the above embodiment and an electrolyte.

[0007] According to still another embodiment, there is provided a battery pack including the secondary battery according to the above embodiment.

[0008] According to still another embodiment, a vehicle including the battery pack according to the above embodiment is provided.

[0009] According to the above configuration, it is possible to provide an electrode and an electrode group capable of improving the capacity of a secondary battery, a secondary battery and a battery pack having improved capacity, and a vehicle including the battery pack. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1It is a cross-sectional view schematically showing an example of an electrode according to an embodiment.

[0011] Figure 2 It is a cross-sectional view schematically showing an example of an electrode group according to an embodiment.

[0012] Figure 3 It is along Figure 2 A schematic cross-sectional view of an imaginary plane III is shown.

[0013] Figure 4 yes Figure 3 An enlarged cross-sectional view of portion A of the electrode assembly is shown.

[0014] Figure 5 It is a cross-sectional view schematically showing an example of a secondary battery according to an embodiment.

[0015] Figure 6 yes Figure 5 An enlarged cross-sectional view of portion B of the secondary battery shown.

[0016] Figure 7 It is a perspective view schematically showing an example of a battery assembly according to an embodiment.

[0017] Figure 8 It is an exploded perspective view schematically showing an example of a battery pack according to an embodiment.

[0018] Fig. 9 Yes means Figure 8 A block diagram of an example of a circuit of a battery pack is shown.

[0019] Fig.10 This is a partial perspective view schematically showing an example of a vehicle according to the embodiment.

[0020] Fig.11 This is a diagram schematically showing an example of a control system related to an electrical system in a vehicle according to an embodiment.

[0021] Explanation of symbols

[0022] 1-electrode group, 2-outer packaging member, 3-negative electrode, 3a-negative electrode collector, 3b-containing negative electrode active material layer, 3c-fold, 3d-gap, 4-separator, 5-positive electrode, 5a-positive electrode collector, 5b-containing positive electrode active material layer, 6-negative electrode terminal, 7-positive electrode terminal, 9-space, 11-first direction, 12a-first curved surface, 12b-second curved surface, 13-flat portion, 14-end, 15-innermost circumferential bend, 21-mother 1-1, 2-2, 3-4, 5-6, 7-8, 9-10, 11-12, 13-14, 15-16, 17-18, 19-20, 21-22, 23-24, 25-26, 27-28, 29-30, 31-32, 33-34, 35-36, 37-38, 39-40, 41-42, 43-44, 45-46, 47-48, 49-50, 51-52, 53-54, 55-56, 57-58, 59-60, 61-61, 62-63, 64-65, 67-68, 69-71, 72-73, 74-75, 76-77, 78-79, 80-80, 81-82, 82-83, 84-85, 86-87, 88-89, 90-91, 91-92, 93-94, 95-96, 97-98, 99-10 , 200b - battery pack, 200c - battery pack, 300 - battery pack, 300a - battery pack, 300b - battery pack, 300c - battery pack, 301a - battery pack monitoring device, 301b - battery pack monitoring device, 301c - battery pack monitoring device, 342 - positive side connector, 343 - negative side connector, 342a - wiring, 343a - wiring, 345 - thermistor, 346 - protection circuit, 348a - positive side Wiring, 348b - negative electrode side wiring, 350 - external terminal for power supply, 352 - positive side terminal, 353 - negative side terminal, 400 - vehicle, 411 - battery management device, 412 - communication bus, 413 - positive terminal, 414 - negative terminal, 415 - switching device, 416 - current detection unit, 417 - negative electrode input terminal, 418 - positive electrode input terminal, C - winding axis, L1 - connecting wire, L2 - connecting wire, W - driving wheel. DETAILED DESCRIPTION

[0023] In an electrode having a composite layer formed by bonding particles of a few μm in diameter as an active material with a resin component, there is a tendency for the composite layer to harden. The oxide-based active material commonly used in the composite layer of the negative electrode tends to have low electronic conductivity, and is preferably micronized to reduce charge resistance. For example, with respect to a negative electrode containing a titanium-containing oxide-based active material, active material particles having a primary particle size of from 0.1 μm to 10 μm are sometimes used, or active material secondary particles having a secondary particle size of from 1 μm to 30 μm obtained by increasing the particle size of the primary particles are used. In addition, in order to obtain good battery performance, a particle size of less than 10 μm is preferred. If active material particles with a particle size in such a range are used, there is a tendency for the electrode to harden.

[0024] As an electrode structure, a structure in which a composite layer containing an active material, that is, a layer containing an active material, is supported on a conductive substrate such as a metal foil is widely used. As a means of improving battery performance, it is known to control the peel strength of the composite layer relative to a substrate such as a collector. For example, by making the peel strength of the negative electrode composite layer containing an oxide-based active material that expands and contracts due to charging and discharging to be above 1.1 kN / m and below 20 kN / m, an electrode structure with sufficient adhesion is formed, thereby preventing the composite layer from peeling off from the collector foil, and it is expected to suppress resistance increase, etc. However, in electrodes with higher peel strength, when used in a wound electrode group, there is a tendency for the electrode to easily break at the inner periphery of the winding body, and there is a concern that the inner periphery cannot contribute to the battery reaction.

[0025] Hereinafter, the embodiments will be described with reference to the accompanying drawings as appropriate. In addition, the same symbols are used to mark the common components throughout the embodiments, and repeated descriptions are omitted. In addition, each figure is a schematic diagram for facilitating the description and understanding of the embodiments, and its shape, size, proportion, etc. are different from the actual device, but they can be appropriately changed in design by referring to the following description and known technologies.

[0026] [First embodiment]

[0027] According to a first embodiment, an electrode having a current collector and an active material-containing layer is provided. The active material-containing layer is in contact with the current collector. The active material-containing layer contains particles containing titanium oxide and carbon nanotubes. The particles containing titanium oxide have an average particle size of 0.1 μm or more and 3 μm or less. The peel strength between the current collector and the active material-containing layer is in the range of 0.2 kN / m or more and 0.7 kN / m or less.

[0028] The electrode may be a battery electrode. The electrode used as the battery electrode may be, for example, a negative electrode for a secondary battery. The secondary battery mentioned here includes, for example, a lithium ion secondary battery and a non-aqueous electrolyte battery.

[0029] The current collector may be, for example, a strip-shaped metal foil or alloy foil.

[0030] The active material-containing layer may be formed on one surface or both surfaces of the current collector. The active material-containing layer contains titanium oxide as an active material and carbon nanotubes as a conductive agent. The active material-containing layer may further contain a binder.

[0031] In the electrode used in the electrode group having a wound structure, the portion located at the inner circumference of the wound body can be bent at an angle close to 180°. In particular, in the case of making an electrode group with a flat wound structure, although the wound body can be pressurized, the portion on the inner circumference can be bent to an angle of about 180° during the pressurization. As a result, cracks may occur in the inner circumference of the electrode wound body, which may become the main cause of battery performance loss and short circuit in the inner circumference. For example, due to cracks in the electrode in the inner circumference of the wound body, a portion that does not contribute to charging and discharging may be generated, thereby damaging the actual capacity of the battery. The occurrence of these failures becomes particularly significant when the battery is enlarged. The electrode involved in the embodiment can suppress the above-mentioned cracks through the above-mentioned structure.

[0032] Specifically, if the peel strength of the current collector and the active material layer is within the range of 0.2kN / m or more and 0.7kN / m or less, at the portion where the electrode is bent at an angle close to 180° in the inner periphery of the winding body, a portion of the active material layer is peeled off from the current collector, and a non-bonded state can be formed. Thus, the electrode thickness is locally thinned at the bent portion. Therefore, the electrode will not be broken starting from the most stressed area near the outermost surface of the active material layer, and the electrode can be prevented from breaking at the inner periphery of the winding body. By making the peel strength above 0.2kN / m, the peeling of the active material layer on the electrode containing the bent portion can be appropriately suppressed, and the occurrence of micro-short circuits caused by the fragments of the peeled active material layer can be suppressed. By keeping the peel strength below 0.7kN / m, the above-mentioned effect of preventing fracture by forming a non-bonded state in the bent portion of the active material layer can be exerted. The above-mentioned peel strength is preferably above 0.3kN / m.

[0033] When the active material-containing layer is provided on both sides of the current collector, the peel strength on each side is made the same. For example, as long as the peel strength is reduced on the inner peripheral side facing the inner side of the winding body, the cracks of the electrode starting from the inner peripheral side can be suppressed. However, when the peel strength of the active material-containing layer is different from that of the outer peripheral surface and the inner peripheral surface of the current collector, the electrode composition is changed on each side, which becomes the cause of electrode deformation during the electrode pressurization and winding process. In addition, the battery performance is different on each side of the electrode. In order to avoid such an undesirable situation, it is preferred to set the peel strength on each side in the same way. Specifically, on each side of the current collector, the design of the composition and thickness of the active material-containing layer is unified. Between each surface, a range of errors in manufacturing is allowed.

[0034] The peel strength in the electrode is affected by the particle size of the titanium oxide and the composition of the secondary components such as the conductive agent and the binder. For example, with the change of the particle size of the titanium oxide and the content of the binder, the following tendency can be seen. On the one hand, as long as the binder coats the surface of the particles, there is a tendency that the more particles the peel strength is improved. On the other hand, when the binder amount is insufficient relative to the surface area increase accompanying the micronization, a decrease in the peel strength occurs.

[0035] In this electrode, the average particle size of the titanium oxide particles is within the range of 0.1 μm or more and 3.0 μm or less. The average particle size mentioned here refers to the average diameter of the secondary particles. From the viewpoint of taking into account the input and output performance and life performance of the battery, the average particle size in this range is preferred. By setting the average particle size to a size greater than 0.1 μm, even if a large amount of conductive agent is not contained, the conductive permeation between the particles formed by the conductive agent can be maintained, thereby maintaining a high energy density. By making the average particle size as small as 3.0 μm or less, the occurrence of cracks inside the particles when the active material expands and contracts during repeated charge and discharge can be reduced, thereby suppressing the increase in resistance of the active material.

[0036] The composition of auxiliary components such as conductive agent and adhesive agent affects the occurrence of electrode peeling and cutting at the bent part. There is a tendency that the increase of conductive agent leads to a decrease in peel strength. On the other hand, the increase of adhesive agent is related to the improvement of peel strength. However, the increase of adhesive agent makes the electrode harder, so be careful.

[0037] The peel strength in the electrode is not only affected by the composition of the active material and the auxiliary components in the active material layer, but also by the manufacturing conditions. As described later, the active material, the conductive agent and the binder are dispersed in a solvent, the obtained slurry is applied to the collector, and the slurry coating is dried to make the electrode. In the production of the electrode, when the slurry is dried quickly, there is a tendency to reduce the peel strength due to the movement of the binder during drying. Therefore, the peel strength is easily reduced when the drying temperature is high.

[0038] The active material-containing layer contains a titanium-containing oxide as an active material. As the active material, the titanium-containing oxide may be contained alone, or two or more titanium-containing oxides may be contained. In addition, a mixture of one or two or more titanium-containing oxides and one or two or more other active materials may be contained.

[0039] Examples of titanium-containing oxides include lithium titanate (e.g., Li 2+y Ti3O7, 0≤y≤3), lithium titanate with spinel structure (such as Li 4+x Ti5O 12, 0≤x≤3), monoclinic titanium dioxide (TiO2), anatase titanium dioxide, rutile titanium dioxide, alkali pyrolusite titanium composite oxide, orthorhombic titanium composite oxide and monoclinic niobium titanium composite oxide.

[0040] Examples of the orthorhombic titanium-containing composite oxide include Li 2+a Mα 2-b Ti 6-c Mβ d O 14+σ A compound represented by . Here, Mα is at least one selected from Sr, Ba, Ca, Mg, Na, Cs, Rb and K. Mβ is at least one selected from Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni and Al. Each subscript in the composition formula is 0≤a≤6, 0≤b<2, 0≤c<6, 0≤d≤6, -0.5≤σ≤0.5.

[0041] Specific examples of orthorhombic titanium-containing composite oxides include those having the general formula Li 2+a’ Na 2-v Mα' w Ti 6-c’-d’ Nb c’ Mβ' d’ O 14+σ The orthorhombic niobium-titanium composite oxide containing Na is represented by: wherein Mα' is one or more selected from Cs, K, Sr, Ba and Ca. Mβ' is one or more selected from Zr, Sn, V, Ta, Mo, W, Fe, Co, Mn and Al. The subscripts in the composition formula are 0≤a'≤4, 0<v<2, 0≤w<2, 0<c'<6, 0≤d'<3, c'+d'<6, -0.5≤σ≤0.5. As a more specific example, Li 2+a Na2Ti6O 14 (0≤a≤6).

[0042] Examples of the monoclinic niobium-titanium composite oxide include Li x Ti 1-y M1 y+z Nb 2-z O 7-δ Here, M1 is at least one selected from Mg, Fe, Ni, Co, W, Ta and Mo. Each subscript in the composition formula is 0≤x≤5, 0≤y<1, 0≤z<2, -0.3≤δ≤0.3.

[0043] Other examples of monoclinic niobium-titanium composite oxides include Li x Ti 1-y M2y Nb 2-z M3 z O 7+δ Here, M2 is at least one selected from Zr, Si and Sn. M3 is at least one selected from V, Ta and Bi. The subscripts in the composition formula are 0≤x≤5, 0≤y<1, 0≤z<2, -0.3≤δ≤0.3. As specific examples of monoclinic niobium titanium composite oxides, Li x Nb2TiO7(0≤x≤5).

[0044] Specific examples of monoclinic niobium titanium composite oxides include Nb2TiO7, Nb2Ti2O9, Nb 10 TiO 29 , Nb 14 TiO 37 and Nb 24 TiO 62 The monoclinic niobium-titanium composite oxide may also be a substituted niobium-titanium composite oxide in which at least a portion of Nb and / or Ti is substituted with a different element. Examples of the substituted element are Na, K, Ca, Co, Ni, Si, P, V, Cr, Mo, Ta, Zr, Mn, Fe, Mg, B, Pb, and Al. The substituted niobium-titanium composite oxide may contain one substituted element or two or more substituted elements.

[0045] The conductive agent is formulated to improve the current collection performance and suppress the contact resistance between the active material and the collector. The active material layer contains carbon nanotubes as a conductive agent. Carbon nanotubes include, for example, single-walled carbon nanotubes (SWCNT) and multi-walled carbon nanotubes (MWCNT). By containing single-walled or multi-walled carbon nanotubes as a conductive agent, powder loss when the electrode is bent can be suppressed. Therefore, excessive peeling of the active material layer can be suppressed at the inner periphery of the wound electrode group.

[0046] The active material-containing layer may further contain other conductive agents together with the carbon nanotubes. Examples of other conductive agents include carbon black such as vapor grown carbon fiber (VGCF), acetylene black (AB), and carbonaceous materials such as graphite. One of them may be used as the other conductive agent, or two or more thereof may be combined and used as the other conductive agent. Alternatively, instead of using other conductive agents, the surface of the active material particles may be coated with carbon and an electronically conductive inorganic material.

[0047] The binder is used to fill the gaps between the dispersed active materials and to bind the active materials to the current collector. Examples of binders include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine rubber, styrene-butadiene rubber (SBR), polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC) and salts of CMC. One of these can be used as a binder, or two or more can be used in combination as a binder.

[0048] The proportion of the active material, the conductive agent and the binder in the active material layer can be changed appropriately according to the purpose of the electrode, but for example, it is set to the following proportion. The active material layer preferably contains active material, conductive agent and binder in a ratio of 70% by mass or more and 96% by mass or less, 2% by mass or more and 28% by mass or less, and 2% by mass or more and 10% by mass or less. By setting the amount of the conductive agent to more than 2% by mass, the current collection performance of the active material layer can be improved. In addition, by setting the amount of the binder to more than 2% by mass, the binding property of the active material layer and the collector becomes sufficient, and excellent cycle performance can be expected. On the other hand, it is preferred to set the conductive agent and the binder to less than 28% by mass and less than 10% by mass, respectively, in order to achieve high capacity.

[0049] In addition, by appropriately reducing the content of the conductive agent, excessive peeling of the active material layer can be suppressed around the bent portion. As for the binder, by appropriately reducing the content, it is possible to avoid electrode hardening associated with electrode cutting and avoid the inability to release stress during bending due to excessive adhesion of the collector.

[0050] As the current collector, a material that is electrochemically stable at the potential at which lithium (Li) is inserted and released in the active material can be used. The potential at which lithium (Li) is inserted and released in the active material is, for example, higher than 1.0 V (vs. Li / Li + ) high (expensive) potential. For example, when the electrode according to the embodiment functions as a negative electrode, the current collector is preferably made of copper, nickel, stainless steel or aluminum, or an aluminum alloy containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu and Si. The thickness of the current collector is preferably not less than 5 μm and not more than 20 μm. A current collector having such a thickness can achieve a balance between the strength and lightness of the electrode.

[0051] Furthermore, the current collector may include a portion on the surface of which the active material-containing layer is not formed and does not overlap with the active material-containing layer in a non-bound state. This portion can function as a current collector tab.

[0052] The density of the active material layer (excluding the current collector) is preferably 2.0 g / cm 3 Above and 3.0g / cm 3 The following range. The density of the active material layer can also be referred to as the electrode density. If the electrode density is within this range, the active material particles and the conductive agent are appropriately adhered, so the balance between the formation of the electronic conductive path in the electrode and the permeability of the liquid electrolyte becomes good, and the rapid charge and discharge performance and life performance are improved. When the electrode density is high, there is a tendency for the electrode to harden easily. Therefore, from the viewpoint of avoiding electrode cutting at the bending part of the winding body, it is preferred that the electrode density is not too high.

[0053] The electrode can be made, for example, by the following method. First, an active material, a conductive agent, and a binder are suspended in a solvent to prepare a slurry. The slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate containing an active material layer and a current collector. Then, the laminate is pressurized. In this way, an electrode is made.

[0054] By adjusting the drying speed and drying temperature when the slurry is dried, the peel strength of the current collector and the active material layer can be controlled. As mentioned above, if the slurry dries quickly, the peel strength may decrease due to the movement of the binder during drying. Therefore, be careful not to increase the drying temperature too much. On the contrary, when the drying temperature is too low, there is a concern that the smoothness of the electrode surface may be damaged or the residual solvent may increase. Therefore, the drying temperature should be appropriately set according to the solvent used in the slurry.

[0055] The electrode density can be controlled by adjusting the pressing conditions.

[0056] <Measurement method>

[0057] Various measurement methods for electrodes are described below. Specifically, a method for measuring the peel strength between a current collector and an active material-containing layer of an electrode and a method for confirming the active material contained in the electrode are described.

[0058] When the electrode to be measured is incorporated in a secondary battery, for example, the electrode taken out by disassembling the battery as described below can be used as a measurement sample.

[0059] First, after the battery is completely discharged, it is disassembled in an inactive atmosphere, the electrode group is taken out, and the electrode is cut into a specified size. The taken-out electrode is washed with a non-aqueous solvent to remove the electrolyte remaining in the electrode, and it is dried under reduced pressure to form a sample. As the non-aqueous solvent, a chain carbonate such as diethyl carbonate and ethyl methyl carbonate, a cyclic carbonate such as propylene carbonate and ethylene carbonate, etc. can be used.

[0060] (Determination of peel strength)

[0061] The peel strength can be measured by a surface-interface cutting method using a cutting strength measuring apparatus such as SAICAS (Surface And Interfacial Cutting Analysis System) (registered trademark). The surface-interface cutting method is also called a SAICAS method.

[0062] As a measuring device of SAICAS, for example, DN-GS manufactured by Daipla-Wintest Co., Ltd. can be used. As a cutting edge, a ceramic edge made of cubic boron carbide with an edge width of 2.0 mm is used.

[0063] The measurement conditions are as follows. The blade angle is set to 20 degrees for the front angle and 10 degrees for the back angle. Cutting is performed in the vertical direction with a vertical load of 1N until the interface between the current collector and the active material layer is reached. Then, the cutting in the vertical direction is stopped and cutting is performed in the horizontal direction at a horizontal speed of 2μm / second. The horizontal force (horizontal load) required to continue the horizontal speed is measured to obtain the peel strength.

[0064] (Method for confirming active substances)

[0065] Using the electrode obtained according to the above steps as a sample, the composition of the active material contained in the active material layer can be confirmed by combining elemental analysis based on a scanning electron microscope (Scanning Electron Microscope-Energy Dispersive X-rayspectrometry: SEM-EDX) equipped with an energy dispersive X-ray analyzer, X-ray diffraction (XRD) measurement and inductively coupled plasma (ICP) emission spectrometry. Through SEM-EDX analysis, the shape of the components contained in the active material layer and the composition of the components contained in the active material layer (elements B to U in the periodic table) can be understood. Through ICP measurement, the elements in the active material layer can be quantified. Moreover, the crystal structure of the material contained in the active material layer can be confirmed by XRD measurement.

[0066] The cross section of the electrode taken out as above was cut out by Ar ion milling. The cut cross section was observed by SEM. The sampling of the sample was carried out in an inactive atmosphere such as argon and nitrogen in order to avoid contact with the atmosphere. Several particles were selected by SEM observation at 3000 times. At this time, the selected particles were selected in a manner that the particle size distribution was as wide as possible.

[0067] Next, elemental analysis is performed on each selected particle using EDX, thereby enabling the type and amount of elements other than Li contained in each selected particle to be identified.

[0068] Regarding Li, information on the Li content in the entire active material can be obtained by ICP emission spectroscopy. ICP emission spectroscopy is performed in the following steps.

[0069] Prepare a powder sample from a dried electrode in the following manner. Peel off the active material layer from the current collector and grind it in a mortar. Dissolve the ground sample in an acid to prepare a liquid sample. In this case, hydrochloric acid, nitric acid, sulfuric acid, hydrogen fluoride, etc. can be used as the acid. By subjecting the liquid sample to ICP emission spectrometry analysis, the concentration of the element contained in the active material to be measured can be obtained.

[0070] The crystal structure of the compound contained in each particle selected by SEM can be determined by XRD measurement. XRD measurement is performed with CuKα rays as the line source within the measurement range of 2θ=5° to 90°. This measurement can obtain the X-ray diffraction pattern of the compound contained in the selected particle.

[0071] As an apparatus for XRD measurement, SmartLab manufactured by Rigaku Corporation was used. The measurement conditions were defined as follows:

[0072] X-ray source: Cu target

[0073] Power: 45kV 200mA

[0074] Sola slit: Both incident and received light are 5°

[0075] Step amplitude (2θ): 0.02deg

[0076] Scanning speed: 20 degrees per minute

[0077] Semiconductor detector: D / teX Ultra 250

[0078] Sample plate holder: Flat glass sample plate holder (thickness 0.5 mm)

[0079] Measurement range: 5°≤2θ≤90°.

[0080] When using other devices, perform measurements using powder X-ray diffraction using standard Si powder, find conditions that can produce measurement results of peak intensity, half-value width and diffraction angle equivalent to those obtained using the above-mentioned device, and measure the sample under these conditions.

[0081] The conditions for XRD measurement are defined as those that allow the acquisition of an XRD pattern that can be used in Rietveld analysis. To collect data for Rietveld analysis, the measurement time or X-ray intensity is appropriately adjusted so that the step width is 1 / 3 to 1 / 5 of the minimum half-value width of the diffraction peak and the intensity at the strongest reflection peak position is 5000 cps or more.

[0082] The XRD pattern obtained above is analyzed by the Rietveld method. In the Rietveld method, the diffraction pattern is calculated by a pre-estimated crystal structure model. The estimation of the crystal structure model here is based on the analysis results of EDX and ICP. By making the calculated value and the measured value fully fit, the parameters related to the crystal structure (lattice constant, atomic coordinates, occupancy, etc.) can be accurately analyzed.

[0083] XRD measurement can be carried out by directly mounting the electrode sample on the glass holder of the wide-angle X-ray diffraction device for measurement. At this time, the XRD spectrum is measured in advance according to the type of metal foil of the electrode collector, and the peak from the collector is grasped. In addition, the presence or absence of peaks of mixtures such as conductive agents and binders is also grasped in advance. When the peak of the collector overlaps with the peak of the active material, it is preferred to peel off the active material-containing layer from the collector for measurement. This is to separate the overlapping peaks when quantitatively measuring the peak intensity. Of course, if these are grasped in advance, this operation can also be omitted.

[0084] The above-mentioned electrode is specifically described with reference to the accompanying drawings. As a specific example of the electrode, Figure 1 The form as a negative electrode is shown in FIG. Figure 1 It is a cross-sectional view schematically showing an example of an electrode according to an embodiment.

[0085] Figure 1 The negative electrode 3 shown includes a negative electrode current collector 3 a and negative electrode active material containing layers 3 b formed on both surfaces thereof.

[0086] The negative electrode current collector 3a is, for example, Figure 1 The two ends are omitted and it can be a strip of metal or alloy foil.

[0087] The negative electrode active material containing layer 3b is carried on the negative electrode current collector 3a. In the example shown in the figure, the negative electrode active material containing layer 3b is carried on both the front and back main surfaces of the negative electrode current collector 3a, but the negative electrode active material containing layer 3b may be carried on only one main surface of the negative electrode current collector 3a.

[0088] The negative electrode current collector 3a may include a portion (not shown) on both sides of which the negative electrode active material layer 3b is not supported, that is, a negative electrode current collector tab.

[0089] The electrode involved in the first embodiment comprises a current collector and an active material layer. The active material layer is in contact with the current collector and contains titanium oxide particles and carbon nanotubes having an average particle size of 0.1 μm or more and 3 μm or less. The peel strength of the active material layer relative to the current collector is in the range of 0.2 kN / m or more and 0.7 kN / m or less. The electrode can suppress cracks in the inner circumference of a wound electrode group. Thus, it is possible to prevent the occurrence of failures caused by cracks in the inner circumference, and it is possible to exert the original battery performance, thereby improving the capacity of a secondary battery having a wound electrode group.

[0090] [Second embodiment]

[0091] According to a second embodiment, an electrode group having a positive electrode and a negative electrode is provided. The negative electrode includes the electrode according to the first embodiment. The electrode group has a flat winding structure in which a stack including a positive electrode and a negative electrode is wound in a manner that is centered along a first direction. In the innermost circumferential bend in the winding structure, a portion of the active material-containing layer of the negative electrode is in a non-bonded state relative to the current collector. The innermost circumferential bend is the first bend along the winding direction from the end portion located at the innermost circumference of the winding structure and along the first direction.

[0092] The electrode group may be a battery electrode group. The battery mentioned here includes, for example, a lithium ion secondary battery and a non-aqueous electrolyte battery. By using the electrode group, the capacity of the secondary battery can be ensured.

[0093] The electrode group includes one or more positive electrodes and one or more negative electrodes.

[0094] The electrode group may further include a separator disposed between the positive electrode and the negative electrode. The electrode group may include one or more separators.

[0095] Reference Figure 2 to Figure 4 The electrode group according to the embodiment will be described. Figure 2 It is a perspective view schematically showing an example of an electrode group according to an embodiment. Figure 3 It is along Figure 2 A schematic cross-sectional view of an imaginary plane III is shown. Figure 4 yes Figure 3An enlarged cross-sectional view of part A of the electrode assembly is shown.

[0096] The electrode group 1 shown in the figure is Figure 2 As shown in FIG. 1 , the flat winding structure is wound around an imaginary winding axis C along the first direction 11. Figure 3 and Figure 4 As shown in the figure, the wound structure is a structure in which a stacked body including a negative electrode 3, a positive electrode 5, and a separator 4 provided between the negative electrode 3 and the positive electrode 5 is wound into a flat shape. The negative electrode 3, the positive electrode 5, and the separator 4 each include a plurality of windings, and are repeatedly arranged in the order of -negative electrode 3, separator 4, positive electrode 5, separator 4, negative electrode 3, separator 4, positive electrode 5, separator 4- in the electrode group 1. There is a space 9 around the winding axis C. In the example shown in the figure, the wound structure has a space 9 in the center, but the electrode group 1 may also have a structure without a space 9.

[0097] The negative electrode 3 includes a negative electrode current collector 3a and negative electrode active material containing layers 3b disposed on both surfaces thereof. The positive electrode 5 includes a positive electrode current collector 5a and positive electrode active material containing layers 5b formed on both surfaces thereof.

[0098] Figure 3 The winding cross section of the electrode group 1 perpendicular to the first direction 11 is shown. Figure 3 The dot-dash line 10 shown in the figure indicates the position along the longest straight line from one end to the other end of the electrode group 1 on the winding cross section. The electrode group 1 includes a first curved surface portion 12a and a second curved surface portion 12b at both ends along the longest straight line, where the negative electrode 3, the separator 4, and the positive electrode 5 are bent into a curved surface, and a flat portion 13 where the negative electrode 3, the separator 4, and the positive electrode 5 are flat or substantially flat is provided therebetween. In the first curved surface portion 12a and the second curved surface portion 12b, the negative electrode 3, the separator 4, and the positive electrode 5 each include a plurality of bent portions.

[0099] Figure 41 is an enlarged cross-sectional view showing a portion of the first curved surface 12a including the innermost circumferential bend 15 and its surroundings in the electrode group 1. The innermost circumferential bend 15 is the first bend from the innermost end 14 of the winding structure of the electrode group 1 toward the winding direction. The innermost end 14 mentioned here is the end along the first direction 11 of the stack of the negative electrode 3, the separator 4 and the positive electrode 5 constituting the electrode group 1, and is the end of the winding head on the inner circumference of the winding structure. As shown in the figure, at the portion of the negative electrode 3 located at the innermost circumferential bend 15, a portion of the negative electrode active material layer 3b is not bonded to the negative electrode collector 3a. In other words, at the innermost circumferential bend 15, the negative electrode active material layer 3b is peeled off from the negative electrode collector 3a. In addition, at the innermost circumferential bend 15, a fold 3c along the first direction 11 is generated on the negative electrode collector 3a. In the example shown in the figure, a gap 3d is formed between the negative electrode collector 3a and the negative electrode active material containing layer 3b, but such a gap 3d may not be present. For example, in the portion of the negative electrode 3 included in the innermost folded portion 15, the negative electrode collector 3a and the negative electrode active material containing layer 3b may be in surface contact with each other although they are in a non-bonded state. In addition, the fold 3c on the negative electrode collector 3a is not necessarily formed.

[0100] In the electrode group 1, the non-bonding rate of the negative electrode active material containing layer 3b in the innermost circumferential bend portion 15 is preferably 1% or more and 20% or less per unit area. In other words, in the portion included in the innermost circumferential bend portion 15 of the negative electrode 3, the negative electrode active material containing layer 3b is not bonded to the negative electrode current collector 3a in a portion of 1% or more and 20% or less per unit area of ​​the negative electrode 3. The non-bonding rate of the negative electrode active material containing layer 3b indicates the extent of the amount of peeling of the negative electrode active material containing layer 3b from the negative electrode current collector 3a.

[0101] In the electrode group 1, since the negative electrode current collector 3a and the negative electrode active material layer 3b are not bonded at the innermost fold 15, stress is not concentrated at this part. Therefore, the cutting, cracking and breaking of the negative electrode 3 are suppressed. For example, when the negative electrode 3 is included and the electrode is cut in the winding structure, a part that does not contribute to charging and discharging due to the cutting is generated, but by suppressing the cutting of the electrode, such an undesirable situation can be avoided. Therefore, in the secondary battery equipped with the electrode group 1, undesirable situations such as capacity reduction can be reduced.

[0102] Hereinafter, the negative electrode, the positive electrode, and the separator will be described in detail.

[0103] (1) Negative electrode

[0104] The negative electrode may include a negative electrode current collector and a negative electrode active material containing layer. The negative electrode current collector and the negative electrode active material containing layer may be the current collector and the active material containing layer that can be included in the electrode according to the first embodiment, respectively.

[0105] That is, the electrode group may include the electrode involved in the first embodiment as a negative electrode. The negative electrode may be, for example, the electrode described in the first embodiment. The active material-containing layer included in the electrode may be a negative electrode active material-containing layer. The active material included in the electrode may be a negative electrode active material.

[0106] When the electrode group includes a plurality of negative electrodes, at least one of the plurality of negative electrodes is the electrode involved in the first embodiment. For example, all negative electrodes may be the electrodes involved in the first embodiment. Alternatively, one of the plurality of negative electrodes may be the electrode involved in the first embodiment. Among the plurality of negative electrodes, the negative electrode at least a portion of which is located at the innermost circumference of the wound structure of the electrode group is preferably the electrode involved in the first embodiment.

[0107] The details of the negative electrode overlap with those described in the first embodiment and thus will be omitted.

[0108] (2) Positive electrode

[0109] The positive electrode may include a positive electrode current collector and a positive electrode active material-containing layer. The positive electrode active material-containing layer may be formed on one side or both sides of the positive electrode current collector. The positive electrode active material-containing layer may contain a positive electrode active material and any conductive agent and binder.

[0110] As the positive electrode active material, for example, an oxide or a sulfide can be used. The positive electrode can contain one compound alone as the positive electrode active material, or can also contain two or more compounds in combination. As examples of oxides and sulfides, compounds that can embed and de-embed Li or Li ions can be cited.

[0111] Examples of such compounds include manganese dioxide (MnO2), iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide (e.g., Li x Mn2O4 or Li x MnO2, 0<x≤1), lithium nickel composite oxide (such as Li x NiO2, 0<x≤1), lithium cobalt composite oxide (such as Li x CoO2, 0<x≤1), lithium nickel cobalt composite oxide (such as Li x Ni 1-y Co y O2, 0<x≤1, 0<y<1), lithium manganese cobalt composite oxide (such as Li x Mn y Co 1-y O2, 0<x≤1, 0<y<1), lithium manganese nickel composite oxide with spinel structure (such as Li x Mn 2-y Ni y O4, 0<x≤1, 0<y<2), lithium phosphate with olivine structure (such as Lix FePO4, 0<x≤1, Li x Fe 1-y Mn y PO4, 0<x≤1, 0<y<1, Li x CoPO4, 0<x≤1), iron sulfate (Fe2(SO4)3), vanadium oxide (such as V2O5) and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2, 0<x≤1, 0<y<1, 0<z<1, y+z<1).

[0112] Among the above, examples of more preferred compounds as positive electrode active materials include: lithium manganese composite oxides having a spinel structure (e.g., Li x Mn2O4, 0<x≤1), lithium nickel composite oxide (such as Li x NiO2, 0<x≤1), lithium cobalt composite oxide (such as Li x CoO2, 0<x≤1), lithium nickel cobalt composite oxide (such as Li x Ni 1-y Co y O2, 0<x≤1, 0<y<1), lithium manganese nickel composite oxide with spinel structure (such as Li x Mn 2-y Ni y O4, 0<x≤1, 0<y<2), lithium manganese cobalt composite oxide (such as Li x Mn y Co 1-y O2, 0<x≤1, 0<y<1), lithium iron phosphate (such as Li x FePO4, 0<x≤1) and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2, 0<x≤1, 0<y<1, 0<z<1, y+z<1). If these compounds are used in the positive electrode active material, the positive electrode potential can be increased.

[0113] When a room temperature molten salt containing lithium iron phosphate, Li x Positive electrode active materials of VPO4F (0≤x≤1), lithium manganese composite oxide, lithium nickel composite oxide, lithium nickel cobalt composite oxide or mixtures thereof. These compounds can improve cycle life due to their low reactivity with room temperature molten salts. Details of room temperature molten salts will be described later.

[0114] The primary particle size of the positive electrode active material is preferably 100 nm or more and 1 μm or less. Positive electrode active materials with a primary particle size of 100 nm or more are easy to handle in industrial production. Positive electrode active materials with a primary particle size of 1 μm or less can smoothly perform solid diffusion of lithium ions.

[0115] The specific surface area of ​​the positive electrode active material is preferably 0.1 m 2 / g or more and 10m 2 / g or less. With 0.1m 2 / g or more of the positive electrode active material can fully secure the insertion and extraction sites of Li ions. 2 A positive electrode active material having a specific surface area of ​​100 Å / g or less is easy to handle in industrial production and can ensure good charge and discharge cycle performance.

[0116] The binder is used to fill the gaps between the dispersed positive electrode active materials and to bind the positive electrode active materials to the positive electrode collector. Examples of binders include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose (CMC) and salts of CMC. One of these can be used as a binder, or two or more can be combined and used as a binder.

[0117] The conductive agent is added to improve the current collection performance and suppress the contact resistance between the positive electrode active material and the positive electrode collector. Examples of conductive agents include carbon black such as vapor grown carbon fiber (VGCF), acetylene black, and carbonaceous materials such as graphite. One of them can be used as the conductive agent, or two or more can be combined and used as the conductive agent. In addition, the conductive agent can also be omitted.

[0118] In the positive electrode active material containing layer, the positive electrode active material and the binder are preferably blended in a ratio of 80 mass % to 98 mass % and 2 mass % to 20 mass %, respectively.

[0119] By making the amount of the binder more than 2% by mass, sufficient electrode strength can be obtained. In addition, the binder can function as an insulator. Therefore, if the amount of the binder is less than 20% by mass, the internal resistance can be reduced due to the reduction in the amount of the insulator contained in the electrode.

[0120] When a conductive agent is added, the positive electrode active material, the binder and the conductive agent are preferably blended in a ratio of 77 mass % to 95 mass %, 2 mass % to 20 mass % and 3 mass % to 15 mass %, respectively.

[0121] By making the amount of the conductive agent more than 3% by mass, the above-mentioned effect can be exerted. In addition, by making the amount of the conductive agent less than 15% by mass, the proportion of the conductive agent in contact with the electrolyte can be reduced. If this proportion is low, the decomposition of the electrolyte can be reduced under high temperature storage.

[0122] The positive electrode current collector is preferably an aluminum foil or an aluminum alloy foil containing one or more elements selected from Mg, Ti, Zn, Ni, Cr, Mn, Fe, Cu and Si.

[0123] The thickness of the aluminum foil or aluminum alloy foil is preferably 5 μm or more and 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99% by mass or more. The content of transition metals such as iron, copper, nickel and chromium contained in the aluminum foil or aluminum alloy foil is preferably 1% by mass or less.

[0124] Furthermore, the positive electrode current collector may include a portion on the surface of which the positive electrode active material-containing layer is not formed. This portion may function as a positive electrode current collector tab.

[0125] The positive electrode can be made, for example, by the following method. First, an active material (positive electrode active material), a conductive agent, and a binder are suspended in a solvent to prepare a slurry. The slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate containing an active material layer and a current collector. Then, pressure is applied to the laminate. In this way, a positive electrode is made.

[0126] Alternatively, the positive electrode can also be prepared by the following method. First, an active material (positive electrode active material), a conductive agent and a binder are mixed to obtain a mixture. Next, the mixture is formed into particles. Then, the particles are arranged on a current collector to obtain a positive electrode.

[0127] (3) Diaphragm

[0128] The separator can be formed of a porous film or a synthetic resin nonwoven fabric containing polyethylene (PE), polypropylene (PP), cellulose or polyvinylidene fluoride (PVdF). From the perspective of safety, it is preferred to use a porous film formed of polyethylene or polypropylene. This is because these porous films melt at a certain temperature and can cut off the current.

[0129] <Measurement method>

[0130] Various measurement methods for the electrode group are described below. Specifically, a method for measuring the non-binding rate of the active material-containing layer with respect to the current collector in the electrode included in the electrode group and a method for measuring the effective electrode area ratio of the electrode are described.

[0131] When the electrode assembly to be measured is incorporated in a secondary battery, the battery may be disassembled, for example, in the following manner, and the electrode assembly taken out may be used as a measurement sample.

[0132] First, after the battery is completely discharged, it is disassembled in an inactive atmosphere and the electrode group is taken out. The electrode group taken out is cleaned with a non-aqueous solvent, the electrolyte remaining in the electrode is removed, and it is dried under reduced pressure to form a sample. Alternatively, according to the measurement to be implemented, the electrode is cut into a specified size from the electrode group, the cut electrode is cleaned with a non-aqueous solvent, the electrolyte remaining in the electrode is removed, and it is dried under reduced pressure to form a sample. As non-aqueous solvents, chain carbonates such as diethyl carbonate and ethyl methyl carbonate and cyclic carbonates such as propylene carbonate and ethylene carbonate can be used.

[0133] (Determination of non-bonding rate)

[0134] The non-binding ratio of the active material-containing layer to the current collector in the innermost folded portion of the electrode group can be quantified by the measurement method described below.

[0135] From the electrode group taken out by disassembling the battery, the electrode was cut into a square shape with a width of 5 cm and a height of 5 cm with the bent portion as the center. The cut electrode sheet was cleaned with a solvent and vacuum dried. Then, the electrode sheet was pressed with a load of 20 kN for 30 seconds, and the active material-containing layer not bonded to the collector was blown off with a hair dryer to obtain a flat sample.

[0136] By performing binary analysis on the image data of the obtained planar sample, the non-bonding rate is calculated. The area equivalent to 1 cm wide and 5 cm high with the bending part as the center in the winding structure is used as the measurement site. Here, the direction of "5 cm high" of the size of the measurement site is consistent with the direction along the first direction (winding axis direction) when winding in the sample. When binarized, for example, image analysis software such as Image J (Dr. Michael et al., Image Processing with Image J, Reprinted from the July 2004 issue of Biophotonics International copyrighted by Laurin Publishing Co. INC.) can be used. Furthermore, as image data, it is preferred to obtain an image under conditions such as the contrast between the substrate, i.e., the current collector, and the active material layer. The central value of the peak of the hue from the substrate and the active material layer is set as a threshold by Image J to binarize the image data. For the obtained binary image, the ratio of the area of ​​the non-bonded part containing the active material layer to the total area of ​​the region subjected to the binary analysis is calculated as the non-bonding rate. In addition, the current collector is exposed on the non-bonded portion of the active material layer because the portion of the active material layer not bonded to the current collector is blown away by a hair dryer. When the electrode is coated on both sides, both sides are measured and the average value is taken as the non-bonding rate.

[0137] The image analysis software Image J is a public domain software, and the version of Image J used was 1.52a.

[0138] <Effective Electrode Area Ratio>

[0139] The ratio of the portion not contributing to charge and discharge that may be generated in the inner circumference of the wound electrode group due to cutting of the electrode and the presence of a non-binding portion in the active material-containing layer was determined as follows and was taken as the effective electrode area ratio.

[0140] First, after the electrode group taken out by disassembling the battery is washed and dried under reduced pressure, the electrode group is unwound and the winding is opened. Confirm the length of the insulated portion of the electrode contained in the electrode group. Specifically, the physically cut, non-conductive portion is regarded as the insulated portion, and the electrode length is regarded as the insulated electrode length. The insulated electrode length and the total electrode length are measured, and the effective electrode area ratio can be calculated by their ratio. Here, the measured electrode length is, for example, defined as the length along the winding direction when in the wound state, that is, the length intersecting the first direction.

[0141] The electrode group involved in the second embodiment includes a positive electrode and a negative electrode, and has a flat winding structure in which a stack including these positive electrodes and negative electrodes is wound in a manner that is located at the center along the first direction. The electrode group includes the electrode involved in the first embodiment as a negative electrode. In the innermost circumferential bend in the winding structure, the active material-containing layer of the negative electrode is partially peeled off from the collector and is in a non-bonded state relative to the collector. The innermost circumferential bend mentioned here is the initial bend from the end located at the innermost circumference of the winding structure toward the winding direction. The end located at the innermost circumference is the end along the first direction. The electrode group can provide a secondary battery with improved capacity.

[0142] [Third Embodiment]

[0143] According to a third embodiment, a secondary battery including an electrode group and an electrolyte is provided. The electrode group included in the secondary battery is the electrode group according to the second embodiment. The electrolyte may be retained in the electrode group.

[0144] In addition, the secondary battery according to the third embodiment may further include an outer packaging member for housing the electrode group and the electrolyte.

[0145] In addition, the secondary battery according to the third embodiment may further include a negative electrode terminal electrically connected to the negative electrode and a positive electrode terminal electrically connected to the positive electrode.

[0146] The secondary battery according to the third embodiment may be, for example, a lithium secondary battery. The secondary battery includes a nonaqueous electrolyte secondary battery containing a nonaqueous electrolyte.

[0147] Hereinafter, the electrolyte, the outer casing member, the negative electrode terminal, and the positive electrode terminal will be described in detail.

[0148] I. Electrolytes

[0149] As the electrolyte, for example, a liquid nonaqueous electrolyte or a gel nonaqueous electrolyte can be used. The liquid nonaqueous electrolyte can be prepared by dissolving an electrolyte salt as a solute in an organic solvent. The concentration of the electrolyte salt is preferably 0.5 mol / L or more and 2.5 mol / L or less.

[0150] Examples of electrolyte salts include lithium salts such as lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3) and bistrifluoromethanesulfonyl imide (LiN(CF3SO2)2) and mixtures thereof. The electrolyte salt is preferably one that is difficult to oxidize even at high potentials, and LiPF6 is most preferred.

[0151] Examples of organic solvents include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methylethyl carbonate (MEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyltetrahydrofuran (2MeTHF), and dioxolane (DOX); chain ethers such as dimethoxyethane (DME) and diethoxyethane (DEE); γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These organic solvents may be used alone or as a mixed solvent.

[0152] The gel nonaqueous electrolyte can be prepared by compounding a liquid nonaqueous electrolyte with a polymer material. Examples of the polymer material include polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyethylene oxide (PEO), or a mixture thereof.

[0153] Alternatively, as the nonaqueous electrolyte, besides a liquid nonaqueous electrolyte and a gel nonaqueous electrolyte, a room-temperature molten salt (ionic melt) containing lithium ions, a polymer solid electrolyte, an inorganic solid electrolyte, or the like may be used.

[0154] As a room temperature molten salt (ionic melt), in an organic salt composed of a combination of organic cations and anions, it refers to a compound that can exist as a liquid at room temperature (above 15°C and below 25°C). Room temperature molten salts include: room temperature molten salts in which the monomer exists as a liquid, room temperature molten salts that become liquid by mixing with electrolyte salts, room temperature molten salts that become liquid by dissolving in an organic solvent, or mixtures of these room temperature molten salts. Generally speaking, the melting point of the room temperature molten salt used in secondary batteries is below 25°C. In addition, the organic cation usually has a quaternary ammonium skeleton.

[0155] A polymer solid electrolyte can be prepared by dissolving an electrolyte salt in a polymer material and solidifying it.

[0156] The inorganic solid electrolyte is a solid substance having Li ion conductivity.

[0157] II. Outer packaging components

[0158] As the outer packaging member, for example, a container formed of a laminated film or a metal container can be used.

[0159] The thickness of the laminate film is, for example, 0.5 mm or less, or preferably 0.2 mm or less.

[0160] As the laminated film, a multilayer film including a plurality of resin layers and a metal layer sandwiched between the resin layers can be used. The resin layer contains, for example, a polymer material such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably formed of aluminum foil or aluminum alloy foil for light weight. The laminated film can be sealed by hot melt bonding and molded into the shape of an outer packaging member.

[0161] The thickness of the wall of the metal container is, for example, preferably 1 mm or less, more preferably 0.5 mm or less, and further preferably 0.2 mm or less.

[0162] The metal container can be made of, for example, aluminum or an aluminum alloy. Preferably, the aluminum alloy contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains transition metals such as iron, copper, nickel, and chromium, the content thereof is preferably 100 mass ppm or less.

[0163] The shape of the outer packaging member is not particularly limited. The shape of the outer packaging member may be, for example, flat (thin), square, cylindrical, coin-shaped, or button-shaped. The outer packaging member may be appropriately selected according to the battery size and the purpose of the battery.

[0164] III. Negative terminal

[0165] The negative terminal can be formed of a material that is electrochemically stable and conductive at the Li insertion and extraction potential of the above-mentioned negative electrode active material. Specifically, as the material of the negative terminal, copper, nickel, stainless steel or aluminum, or an aluminum alloy containing at least one element selected from Mg, Ti, Zn, Mn, Fe, Cu and Si can be listed. As the material of the negative terminal, aluminum or an aluminum alloy is preferably used. In order to reduce the contact resistance with the negative electrode collector, the negative terminal is preferably formed of the same material as the negative electrode collector.

[0166] IV. Positive terminal

[0167] The positive terminal can be formed by a potential range of 3V or more and 4.5V or less relative to the redox potential of lithium (vs. Li / Li + ) is formed of a material that is electrically stable and conductive. Examples of the material of the positive terminal include aluminum or an aluminum alloy containing at least one element selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si. The positive terminal is preferably formed of the same material as the positive electrode collector in order to reduce the contact resistance with the positive electrode collector.

[0168] Next, a secondary battery according to a third embodiment will be described in more detail with reference to the drawings.

[0169] Figure 5 It is a cross-sectional view schematically showing an example of a secondary battery according to a third embodiment. Figure 6 yes Figure 5 An enlarged cross-sectional view of portion B of the secondary battery shown.

[0170] Figure 5 and Figure 6 The secondary battery 100 shown has: Figure 5 The bag-shaped outer packaging member 2 shown, Figure 5 and Figure 6 The electrode group 1 shown and the electrolyte (not shown) are accommodated in a bag-shaped outer packaging member 2. The electrolyte (not shown) is retained in the electrode group 1.

[0171] The bag-like outer package member 2 is formed of a laminated film including two resin layers and a metal layer sandwiched therebetween.

[0172] like Figure 5 As shown in FIG. 1 , the electrode group 1 is a flat, wound electrode group. Figure 6 As shown, the negative electrode 3, the separator 4 and the positive electrode 5 are included. The separator 4 is interposed between the negative electrode 3 and the positive electrode 5.

[0173] The negative electrode 3 includes a negative electrode current collector 3a and a negative electrode active material layer 3b. Figure 6 As shown, the negative electrode active material containing layer 3b is formed only on the inner surface side of the negative electrode current collector 3a. In the other parts of the negative electrode 3, the negative electrode active material containing layer 3b is formed on both surfaces of the negative electrode current collector 3a.

[0174] The positive electrode 5 includes a positive electrode current collector 5 a and positive electrode active material-containing layers 5 b formed on both surfaces thereof.

[0175] like Figure 5As shown, the negative terminal 6 and the positive terminal 7 are located near the outer peripheral end of the wound electrode group 1. The negative terminal 6 is connected to the outermost portion of the negative electrode collector 3a. In addition, the positive terminal 7 is connected to the outermost portion of the positive electrode collector 5a. These negative terminals 6 and positive terminals 7 extend to the outside from the opening of the bag-like outer packaging member 2. A thermoplastic resin layer is provided on the inner surface of the bag-like outer packaging member 2, and the opening is sealed by heat-melting bonding.

[0176] The secondary battery according to the third embodiment includes the electrode group according to the second embodiment. Therefore, the secondary battery has a high capacity.

[0177] [Fourth embodiment]

[0178] According to a fourth embodiment, a battery pack is provided. The battery pack according to the fourth embodiment includes a plurality of secondary batteries according to the third embodiment.

[0179] In the assembled battery according to the fourth embodiment, the individual cells may be arranged by being electrically connected in series or in parallel, or may be arranged by combining series connection and parallel connection.

[0180] Next, an example of a battery assembly according to a fourth embodiment will be described with reference to the drawings.

[0181] Figure 7 It is a perspective view schematically showing an example of a battery assembly according to a fourth embodiment. Figure 7 The illustrated assembled battery 200 includes five cells 100 a to 100 e , four bus bars 21 , a positive electrode lead 22 , and a negative electrode lead 23 . The five cells 100 a to 100 e are each a secondary battery according to the third embodiment.

[0182] The bus bar 21 connects, for example, the negative terminal 6 of one cell 100a and the positive terminal 7 of the adjacent cell 100b. In this way, five cells 100 are connected in series via four bus bars 21. That is, Figure 7 The assembled battery 200 is a battery assembly of five connected in series. Although not shown in the figure, in an assembled battery including a plurality of cells electrically connected in parallel, the plurality of cells can be electrically connected by, for example, connecting a plurality of negative terminals with a bus bar and connecting a plurality of positive terminals with a bus bar.

[0183] The positive electrode terminal 7 of at least one of the five cells 100a to 100e is electrically connected to the positive electrode lead 22 for external connection. The negative electrode terminal 6 of at least one of the five cells 100a to 100e is electrically connected to the negative electrode lead 23 for external connection.

[0184] The assembled battery according to the fourth embodiment includes the secondary battery according to the third embodiment. Therefore, the assembled battery exhibits a high capacity.

[0185] [Fifth embodiment]

[0186] According to a fifth embodiment, a battery pack is provided. The battery pack includes the assembled battery according to the fourth embodiment. The battery pack may include a single secondary battery according to the third embodiment instead of the assembled battery according to the fourth embodiment.

[0187] The battery pack according to the fifth embodiment may further include a protection circuit. The protection circuit has a function of controlling the charge and discharge of the secondary battery. Alternatively, a circuit included in a device (such as an electronic device, a car, etc.) that uses the battery pack as a power source may be used as the protection circuit of the battery pack.

[0188] In addition, the battery pack involved in the fifth embodiment may further include an external terminal for power supply. The external terminal for power supply is used to output the current from the secondary battery to the outside and / or input the current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, the current is supplied to the outside through the external terminal for power supply. In addition, when the battery pack is charged, the charging current (including the regenerative energy of the power of the car, etc.) is supplied to the battery pack through the external terminal for power supply.

[0189] Next, an example of a battery pack according to a fifth embodiment will be described with reference to the drawings.

[0190] Figure 8 It is an exploded perspective view schematically showing an example of a battery pack according to a fifth embodiment. Fig. 9 Yes means Figure 8 A block diagram of an example of a circuit of a battery pack is shown.

[0191] Figure 8 and Fig. 9 The battery pack 300 shown includes a storage container 31 , a cover 32 , a protective sheet 33 , the battery module 200 , a printed wiring board 34 , wirings 35 , and an insulating plate (not shown).

[0192] Figure 8 The storage container 31 shown is a bottomed square container having a rectangular bottom surface. The storage container 31 is configured to accommodate a protective sheet 33, a battery pack 200, a printed wiring substrate 34, and wiring 35. The cover 32 has a rectangular shape. The cover 32 accommodates the battery pack 200 and the like by covering the storage container 31. Although not shown in the figure, the storage container 31 and the cover 32 are also provided with an opening or a connection terminal for connection with an external device and the like.

[0193] The assembled battery 200 includes a plurality of unit cells 100 , a positive electrode lead 22 , a negative electrode lead 23 , and an adhesive tape 24 .

[0194] At least one of the plurality of cells 100 is a secondary battery according to the third embodiment. Fig. 9 The plurality of cells 100 may be electrically connected in parallel, or in a combination of series and parallel. If the plurality of cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.

[0195] The adhesive tape 24 bundles the plurality of cells 100. A heat shrink tape may be used instead of the adhesive tape 24 to fix the plurality of cells 100. In this case, the protective sheet 33 is disposed on both sides of the battery pack 200, and after the heat shrink tape is wrapped around, the heat shrink tape is thermally shrunk to bundle the plurality of cells 100.

[0196] One end of the positive electrode lead 22 is connected to the assembled battery 200. One end of the positive electrode lead 22 is electrically connected to the positive electrode of one or more cells 100. One end of the negative electrode lead 23 is connected to the assembled battery 200. One end of the negative electrode lead 23 is electrically connected to the negative electrode of one or more cells 100.

[0197] The printed wiring board 34 is provided on a surface along one short side of the inner side surface of the storage container 31. The printed wiring board 34 includes a positive side connector 342, a negative side connector 343, a thermistor 345, a protection circuit 346, wirings 342a and 343a, an external terminal 350 for power supply, a positive side wiring (positive side wiring) 348a, and a negative side wiring (negative side wiring) 348b. One main surface of the printed wiring board 34 faces one side surface of the battery pack 200. An insulating plate (not shown) is sandwiched between the printed wiring board 34 and the battery pack 200.

[0198] The other end 22 a of the positive electrode lead 22 is electrically connected to the positive electrode connector 342 . The other end 23 a of the negative electrode lead 23 is electrically connected to the negative electrode connector 343 .

[0199] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each unit cell 100 and sends the detection signal to the protection circuit 346.

[0200] The external terminals 350 for power supply are fixed to the other main surface of the printed wiring board 34. The external terminals 350 for power supply are electrically connected to a device existing outside the battery pack 300. The external terminals 350 for power supply include a positive terminal 352 and a negative terminal 353.

[0201] The protection circuit 346 is fixed to the other main surface of the printed wiring substrate 34. The protection circuit 346 is connected to the positive terminal 352 via the positive side wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via the negative side wiring 348b. In addition, the protection circuit 346 is electrically connected to the positive side connector 342 via the wiring 342a. The protection circuit 346 is electrically connected to the negative side connector 343 via the wiring 343a. In addition, the protection circuit 346 is electrically connected to the plurality of cells 100 via the wiring 35.

[0202] The protection sheet 33 is disposed on both inner side surfaces in the longitudinal direction of the storage container 31 and on the inner side surface in the transverse direction facing the printed wiring board 34 via the battery module 200. The protection sheet 33 is formed of, for example, resin or rubber.

[0203] The protection circuit 346 controls the charge and discharge of the plurality of cells 100. In addition, based on a detection signal sent from the thermistor 345 or a detection signal sent from each cell 100 or the assembled battery 200, the protection circuit 346 blocks the electrical connection between the protection circuit 346 and the external terminal 350 (positive terminal 352, negative terminal 353) for powering an external device.

[0204] As the detection signal sent from the thermistor 345, for example, a signal for detecting that the temperature of the single cell 100 is above a predetermined temperature can be cited. As the detection signal sent from each single cell 100 or the assembled battery 200, for example, a signal for detecting overcharge, overdischarge, and overcurrent of the single cell 100 can be cited. When detecting overcharge, etc. of each single cell 100, the battery voltage can be detected, or the positive electrode potential or the negative electrode potential can be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each single cell 100.

[0205] Alternatively, as the protection circuit 346 , a circuit included in a device (eg, electronic equipment, automobile, etc.) that uses the battery pack 300 as a power source may be used.

[0206] In addition, the battery pack 300 has the external terminal 350 for power supply as described above. Therefore, the battery pack 300 can output the current from the assembled battery 200 to the external device via the external terminal 350 for power supply, and can input the current from the external device to the assembled battery 200. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 can be supplied to the external device through the external terminal 350 for power supply. In addition, when charging the battery pack 300, the charging current from the external device can be supplied to the battery pack 300 through the external terminal 350 for power supply. When the battery pack 300 is used as a vehicle-mounted battery, the regenerative energy of the power of the vehicle can be used as the charging current from the external device.

[0207] In addition, the battery pack 300 may also include a plurality of battery assemblies 200. In this case, the plurality of battery assemblies 200 may be connected in series, in parallel, or in a combination of series and parallel. In addition, the printed wiring substrate 34 and the wiring 35 may be omitted. In this case, the positive electrode side lead 22 and the negative electrode side lead 23 may be used as the positive side terminal 352 and the negative side terminal 353 of the external terminal 350 for power supply, respectively.

[0208] Such a battery pack can be used, for example, for applications requiring excellent cycle performance when a large current is taken out. Specifically, the battery pack can be used, for example, as a power source for electronic equipment, a stationary battery, or a vehicle-mounted battery for various vehicles. Examples of electronic equipment include digital cameras. The battery pack is particularly suitable for use as a vehicle-mounted battery.

[0209] The battery pack according to the fifth embodiment includes the secondary battery according to the third embodiment or the assembled battery according to the fourth embodiment. Therefore, the battery pack has a high capacity.

[0210] [Sixth embodiment]

[0211] According to a sixth embodiment, a vehicle is provided. The vehicle is equipped with the battery pack according to the fifth embodiment.

[0212] In the vehicle according to the sixth embodiment, the battery pack can recover regenerative energy of the power of the vehicle, for example. The vehicle may include a mechanism (Regenerator) that converts the kinetic energy of the vehicle into regenerative energy.

[0213] Examples of the vehicle according to the sixth embodiment include a two-wheeled to four-wheeled hybrid electric vehicle, a two-wheeled to four-wheeled electric vehicle, an assist bicycle, and a railway vehicle.

[0214] The mounting position of the battery pack in the vehicle according to the sixth embodiment is not particularly limited. For example, when the battery pack is mounted in a car, the battery pack may be mounted in the engine room of the vehicle, behind the vehicle body, or under a seat.

[0215] The vehicle involved in the sixth embodiment may also be equipped with multiple battery packs. In this case, the batteries contained in each battery pack may be electrically connected to each other in series, in parallel, or in a combination of series connection and parallel connection. For example, when each battery pack contains a battery pack, the battery packs may be electrically connected to each other in series, in parallel, or in a combination of series connection and parallel connection. Alternatively, when each battery pack contains a single battery, the batteries may be electrically connected to each other in series, in parallel, or in a combination of series connection and parallel connection.

[0216] Next, an example of a vehicle according to a sixth embodiment will be described with reference to the drawings.

[0217] Fig.10 This is a partial perspective view schematically showing an example of a vehicle according to the sixth embodiment.

[0218] Fig.10 The vehicle 400 shown includes a vehicle body 40 and a battery pack 300 according to the fifth embodiment. Fig.10 In the example shown, the vehicle 400 is a four-wheeled automobile.

[0219] The vehicle 400 may also be equipped with a plurality of battery packs 300. In this case, the batteries (eg, single batteries or battery packs) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series connection and parallel connection.

[0220] Fig.10 The middle figure shows an example in which the battery pack 300 is mounted in the engine room located in front of the vehicle body 40. As described above, the battery pack 300 may be mounted, for example, behind the vehicle body 40 or under a seat. The battery pack 300 can be used as a power source for the vehicle 400. In addition, the battery pack 300 can recover the regenerative energy of the power of the vehicle 400.

[0221] Next, refer to Fig.11 An embodiment of a vehicle according to a sixth embodiment will be described.

[0222] Fig.11 This is a diagram schematically showing an example of a control system related to an electrical system in a vehicle according to the sixth embodiment. Fig.11 The illustrated vehicle 400 is an electric vehicle.

[0223] Fig.11 The vehicle 400 shown includes a vehicle body 40 , a vehicle power supply 41 , a vehicle ECU (Electric Control Unit) 42 which is a superior control device of the vehicle power supply 41 , an external terminal (a terminal for connecting to an external power supply) 43 , an inverter 44 and a drive motor 45 .

[0224] The vehicle 400 has a vehicle power supply 41 mounted in, for example, an engine room, a rear part of a vehicle body, or under a seat. Fig.11 In the illustrated vehicle 400 , a mounting location of a vehicle power supply 41 is schematically shown.

[0225] The vehicle power supply 41 includes a plurality of (eg, three) battery packs 300 a , 300 b , and 300 c , a battery management unit (BMU) 411 , and a communication bus 412 .

[0226] The battery pack 300a includes a battery pack 200a and a battery pack monitoring device 301a (e.g., VTM: Voltage Temperature Monitoring). The battery pack 300b includes a battery pack 200b and a battery pack monitoring device 301b. The battery pack 300c includes a battery pack 200c and a battery pack monitoring device 301c. The battery packs 300a to 300c are the same battery packs as the above-mentioned battery pack 300, and the battery packs 200a to 200c are the same battery packs as the above-mentioned battery pack 200. The battery packs 200a to 200c are electrically connected in series. The battery packs 300a, 300b, and 300c can be independently removed and exchanged with other battery packs 300.

[0227] Each of the assembled batteries 200a to 200c includes a plurality of cells connected in series. At least one of the plurality of cells is a secondary battery according to the third embodiment. Each of the assembled batteries 200a to 200c is charged and discharged via a positive electrode terminal 413 and a negative electrode terminal 414.

[0228] The battery management device 411 communicates with the assembled battery monitoring devices 301a to 301c to collect information on voltage and temperature of each cell 100 included in the assembled batteries 200a to 200c of the vehicle power supply 41. Thus, the battery management device 411 collects information on maintenance of the vehicle power supply 41.

[0229] The battery management device 411 and the assembled battery monitoring devices 301a to 301c are connected via a communication bus 412. In the communication bus 412, a plurality of nodes (the battery management device 411 and one or more assembled battery monitoring devices 301a to 301c) share a set of communication lines. The communication bus 412 is, for example, a communication bus configured based on the CAN (Control Area Network) standard.

[0230] The assembled battery monitoring devices 301a to 301c measure the voltage and temperature of each cell constituting the assembled batteries 200a to 200c based on the communication command from the battery management device 411. The temperature may be measured at only a few locations in one assembled battery, and the temperature of all cells may not be measured.

[0231] The vehicle power supply 41 may further include an electromagnetic contactor (eg, Fig.11 The switch device 415 is shown in the figure. The switch device 415 includes a pre-charge switch (not shown) that is turned on when charging the assembled batteries 200a to 200c and a main switch (not shown) that is turned on when the output from the assembled batteries 200a to 200c is supplied to the load. The pre-charge switch and the main switch each include a relay circuit (not shown) that is switched on or off by a signal supplied to a coil disposed near the switch element. The electromagnetic contactor such as the switch device 415 is controlled based on a control signal from the vehicle ECU 42 that controls the operation of the battery management device 411 or the entire vehicle 400.

[0232] The inverter 44 converts the input DC voltage into a three-phase AC high voltage for motor driving. The three-phase output terminals of the inverter 44 are connected to the three-phase input terminals of the drive motor 45. The inverter 44 is controlled based on a control signal from the vehicle ECU 42 that controls the battery management device 411 or the overall operation of the vehicle. The output voltage from the inverter 44 is adjusted by controlling the inverter 44.

[0233] The drive motor 45 is rotated by the electric power supplied from the inverter 44. The driving force generated by the rotation of the drive motor 45 is transmitted to the axle and the drive wheel W through, for example, a differential transmission.

[0234] In addition, although not shown, the vehicle 400 is provided with a regenerative braking mechanism (regenerator). The regenerative braking mechanism rotates the drive motor 45 when braking the vehicle 400, converting kinetic energy into regenerative energy as electrical energy. The regenerative energy recovered by the regenerative braking mechanism is input to the inverter 44 and converted into a direct current. The converted direct current is input to the vehicle power supply 41.

[0235] One terminal of the connection line L1 is connected to the negative terminal 414 of the vehicle power supply 41. The other terminal of the connection line L1 is connected to the negative input terminal 417 of the inverter 44. On the connection line L1, a current detection unit (current detection circuit) 416 in the battery management device 411 is provided between the negative terminal 414 and the negative input terminal 417.

[0236] One terminal of the connection line L2 is connected to the positive terminal 413 of the vehicle power supply 41. The other terminal of the connection line L2 is connected to the positive input terminal 418 of the inverter 44. A switch device 415 is provided between the positive terminal 413 and the positive input terminal 418 on the connection line L2.

[0237] The external terminal 43 is connected to the battery management device 411. The external terminal 43 can be connected to an external power source, for example.

[0238] The vehicle ECU 42 responds to the operation input of the operator, etc., and coordinates and controls the vehicle power supply 41, the switch device 415, the inverter 44, etc. together with other management devices and control devices including the battery management device 411. Through the coordinated control of the vehicle ECU 42, etc., the output of the power from the vehicle power supply 41 and the charging of the vehicle power supply 41 are controlled, and the entire vehicle 400 is managed. Data related to the maintenance of the vehicle power supply 41, such as the remaining capacity of the vehicle power supply 41, is transmitted between the battery management device 411 and the vehicle ECU 42 through the communication line.

[0239] The vehicle according to the sixth embodiment is equipped with the battery pack according to the fifth embodiment. Therefore, a high-performance vehicle can be provided.

[0240] [Example]

[0241] Although examples are described below, the embodiment is not limited to the examples described below.

[0242] (Example 1)

[0243] <Electrode Production>

[0244] First, for the positive electrode, 90% by mass of LiMn2O4 powder, 5% by mass of acetylene black and 5% by mass of polyvinylidene fluoride (PVdF) were added to N-methylpyrrolidone (NMP) and mixed to prepare a slurry. For the negative electrode, Li4Ti5O 12 90 parts by weight of acetylene black, 5 parts by weight of multi-walled carbon nanotubes, and 3 parts by weight of PVdF were added to N-methylpyrrolidone and mixed to prepare a slurry. 2The coating amount was applied on both sides of the current collector formed by aluminum foil with a thickness of 15 μm, and after the slurry coating was dried, the positive and negative electrodes were made by pressing. In addition, the positive and negative electrodes were dried by blowing hot air at 130°C from the top and bottom of the substrate.

[0245] <Production of laminated batteries>

[0246] After the positive electrode, the separator formed by a polyethylene porous film with a thickness of 25 μm, the negative electrode and the separator are stacked in this order, they are wound into a spiral shape. The obtained winding body is pressurized at 40 kN for 10 seconds at room temperature (25°C) to produce a flat electrode group with a width of 30 mm, a height of 65 mm and a thickness of 6.0 mm. The obtained electrode group is placed in a pack formed by a laminated film and vacuum dried at 80°C for 24 hours. The laminated film can be formed by forming a polypropylene layer on both sides of an aluminum foil with a thickness of 40 μm, and the overall thickness is 0.1 mm. In a mixed solution containing propylene carbonate (PC), diethyl carbonate (DEC) and methyl ethyl carbonate (MEC) in a volume ratio of 1:1:1, LiPF6 is dissolved at a concentration of 1.0 M to prepare a liquid electrolyte. A liquid nonaqueous electrolyte (1.0 M LiPF6, PC:DEC:MEC=1:1:1 (vol%)) was injected into the bag of laminated film containing the electrode group. Then, the bag was completely sealed by heat sealing to produce a 5Ah nonaqueous electrolyte battery (laminated battery) with a width of 35 mm and a thickness of 6.2 mm.

[0247] (Example 2)

[0248] In addition to being used as a negative electrode active material to replace Li4Ti5O 12 A nonaqueous electrolyte battery was manufactured by the same procedure as in Example 1 except that TiNb2O7 having an average particle size of 2.0 μm was used.

[0249] (Example 3)

[0250] In addition to being used as a negative electrode active material to replace Li4Ti5O 12 TiNb2O7 with an average particle size of 2.0 μm is used, 1.5 parts by mass of carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) are used instead of PVdF, water is used as the slurry solvent instead of NMP, the drying temperature of the electrode is changed to 110°C, and a non-aqueous electrolyte battery is manufactured according to the same steps as in Example 1.

[0251] (Example 4)

[0252] In addition to being used as a negative electrode active material to replace Li4Ti5O 12 A nonaqueous electrolyte battery was manufactured by the same procedure as in Example 1 except that TiNb2O7 having an average particle size of 0.5 μm was used.

[0253] (Example 5)

[0254] In addition to being used as a negative electrode active material to replace Li4Ti5O 12 A nonaqueous electrolyte battery was manufactured by the same procedure as in Example 1 except that TiNb2O7 having an average particle size of 3.0 μm was used.

[0255] (Example 6)

[0256] A nonaqueous electrolyte battery was manufactured in the same manner as in Example 2 except that the winding body was pressed at 80° C. instead of at room temperature.

[0257] (Comparative Example 1)

[0258] In addition to changing the negative electrode slurry composition to Li4Ti5O with an average particle size of 3.0 μm 12 A nonaqueous electrolyte battery was produced in the same manner as in Example 1 except for 90 parts by mass of MgSO4, 2 parts by mass of acetylene black, and 8 parts by mass of PVdF.

[0259] (Comparative Example 2)

[0260] In addition to changing the negative electrode slurry composition to Li4Ti5O with an average particle size of 3.0 μm 12 A nonaqueous electrolyte battery was produced in the same manner as in Example 1 except for 90 parts by mass of MgSO4, 8 parts by mass of acetylene black, and 2 parts by mass of PVdF.

[0261] (Comparative Example 3)

[0262] A nonaqueous electrolyte battery was manufactured by the same steps as in Example 1, except that the slurry composition of the negative electrode was changed to 90 parts by mass of TiNb2O7 with an average particle size of 2.0 μm, 7 parts by mass of acetylene black, 1.5 parts by mass each of CMC and SBR, water was used as the slurry solvent instead of NMP, and the drying temperature of the electrode was changed to 110°C.

[0263] (Comparative Example 4)

[0264] A nonaqueous electrolyte battery was manufactured by the same steps as in Example 1, except that the slurry composition of the negative electrode was changed to 90 parts by mass of TiNb2O7 with an average particle size of 2.0 μm, 4 parts by mass of acetylene black, 2 parts by mass of multilayer carbon nanotubes, 2 parts by mass of CMC and 2 parts by mass of SBR, water was used as the slurry solvent instead of NMP, and the drying temperature of the electrode was changed to 110°C.

[0265] (Comparative Example 5)

[0266] A nonaqueous electrolyte battery was produced in the same manner as in Example 4 except that the drying temperature of the electrode was changed to 200°C.

[0267] Tables 1 and 2 summarize the details of the manufacture of the laminated batteries in Examples 1 to 6 and Comparative Examples 1 to 5. Specifically, Table 1 summarizes the details of the negative electrode, and Table 2 summarizes the manufacturing conditions of the electrode group. Regarding the details of the negative electrode in Table 1, the composition, average particle size and content of the negative electrode active material, the material type and content of the conductive agent, the material type and content of the binder, and the drying temperature of the slurry are shown. In addition, in Table 1, for the conductive agent, acetylene black and multilayer carbon nanotubes are marked as "AB" and "MWCNT", respectively. In addition, for the binder, polyvinylidene fluoride, carboxymethyl cellulose and styrene butadiene rubber are marked as "PVdF", "CMC" and "SBR", respectively. Regarding the manufacturing conditions of the electrode group in Table 2, the pressing temperature, load during pressing and pressing time of the winding body including the negative electrode, the positive electrode and the separator are shown.

[0268] Table 1

[0269]

[0270] Table 2

[0271]

[0272] <Confirmation of effective electrode area ratio>

[0273] The laminated battery was disassembled and the electrode group was taken out. After washing with a mixed solvent of diethyl carbonate and propylene carbonate and drying under reduced pressure, the electrode group of the wound structure was unwound to confirm the electrode cutting at the innermost part of the negative electrode and the peeling of the active material layer. In the case of electrode cutting or peeling of the active material layer, the ratio of the effective electrode area that can contribute to charging and discharging to the effective electrode area when the negative electrode was made was calculated as the effective electrode area ratio using the above method.

[0274] <Peel Strength Test>

[0275] Separate the negative electrode from the unwound electrode group. Cut a 5 cm square test piece from the negative electrode from the flat part of the electrode group in the wound state. Immerse the test piece cut from the negative electrode in a mixed solvent of diethyl carbonate and propylene carbonate for 5 minutes, and then vacuum dry it for about 10 minutes under a pressure of -96 kPa. Press the plane with a load of 20 kN for 30 seconds in a direction perpendicular to the test piece, blow off the peeled part containing the active material layer with a hair dryer, and prepare the sample.

[0276] The obtained samples were used to measure the peel strength between the current collector and the active material-containing layer by the surface-interface cutting method (SAICAS method) described above.

[0277] <Confirmation of non-bonding rate>

[0278] From the separated negative electrode, in the wound state, a 5 cm square test piece was cut with the bend closest to the end portion corresponding to the innermost circumference of the electrode group as the center. The test piece cut from the negative electrode was immersed in a mixed solvent of diethyl carbonate and propylene carbonate for 5 minutes, and then vacuum dried for about 10 minutes under a pressure of -96 kPa. A plane was pressed with a load of 20 kN in a direction perpendicular to the test piece for 30 seconds, and the peeled portion containing the active material layer was blown off with a hair dryer to prepare the sample.

[0279] Using the obtained sample, the image of the innermost folded portion of the negative electrode was binarized by image J according to the above method using the average value of each surface of the negative electrode produced by double-sided coating, thereby determining the non-binding rate.

[0280] <Charge and discharge test>

[0281] Each of the manufactured nonaqueous electrolyte batteries was charged at a current value of 0.5 A, under the termination conditions of an upper limit voltage of 2.7 V and a charging time of 20 hours. Then, it was discharged at 0.5 A. The ratio of the actual capacity obtained to the designed capacity of the battery was calculated.

[0282] Table 3 summarizes the results of various measurements performed on the laminated batteries involved in Examples 1 to 6 and Comparative Examples 1 to 5. Specifically, the peel strength of the current collector and the active material layer in the negative electrode, the non-bonding rate on the innermost folded portion in the negative electrode, the effective electrode area rate in the negative electrode, the state of the negative electrode, and the ratio of the actual capacity of the laminated battery to the designed capacity are shown. Regarding the state of the negative electrode, the point is marked when a part of the active material layer is confirmed to be in a non-bonded state. When the state of the negative electrode is marked as "inner peripheral part cut", it means that it is in the following state: in the electrode group in the wound state, from the end side located at the innermost circumference to the initial bend part, the current collector and the active material layer are contained, the negative electrode is cut, and the part between the innermost folded portion and the innermost circumference end is separated from the other parts. In addition, when the negative electrode is cut, although the part of the active material layer that becomes non-bonded is also confirmed, the negative electrode is cut first and marked as "inner peripheral part cut".

[0283] Table 3

[0284]

[0285] As shown in Table 3, in Examples 1 to 6, the peel strength in the negative electrode is within the range of 0.2 kN / m or more and 0.7 kN / m or less. In the laminated batteries using these negative electrodes, the non-bonding rate of the active material-containing layer on the innermost folded portion of the negative electrode is within the range of 1% or more and 20% or less. In addition, in the laminated batteries of Examples 1 to 6, the effective electrode area ratio of the negative electrode is higher than that of the laminated batteries of Comparative Examples 1 to 5, and the actual capacity relative to the designed capacity is also higher.

[0286] In Comparative Example 1, the inner peripheral portion of the negative electrode was cut, resulting in a low effective electrode area of ​​the negative electrode and a low actual capacity of the battery. In Comparative Example 1, the peel strength in the negative electrode was high, and carbon nanotubes were not contained as a conductive agent. Therefore, in Comparative Example 1, it is presumed that the hard negative electrode active material-containing layer could not be peeled off from the current collector, causing the negative electrode to break.

[0287] In Comparative Examples 2 and 3, although no electrode cut-off occurs, the negative electrode active material layer is more peeled off from the negative electrode current collector, resulting in a slightly lower effective electrode area of ​​the negative electrode and the actual capacity of the battery. In either Comparative Examples 2 or 3, the peel strength in the negative electrode is about the same as that in Examples 1-6. Nevertheless, it is speculated that the reason for the increased peeling of the active material layer in Comparative Examples 2 and 3 is that the active material layer does not contain carbon nanotubes and cannot impart flexibility.

[0288] In Comparative Example 4, the inner peripheral portion of the negative electrode was cut, resulting in a low effective electrode area of ​​the negative electrode and a low actual capacity of the battery. In Comparative Example 4, although the active material-containing layer contained carbon nanotubes, the peel strength of the active material-containing layer relative to the current collector was high. In Comparative Example 4, it is presumed that the hard negative electrode active material-containing layer could not be peeled off from the current collector, causing the negative electrode to break.

[0289] In Comparative Example 5, the effective electrode area of ​​the negative electrode is low, and the actual capacity of the battery is slightly low. In Comparative Example 5, on the one hand, the peel strength in the negative electrode is low, and on the other hand, although the non-bonding rate of the active material-containing layer in the innermost circumferential bend of the negative electrode is slightly increased, it is within the range of 1% to 20%. Although the non-bonding rate in the innermost circumferential bend of the negative electrode is low, the reason why the actual capacity of the laminated battery involved in Comparative Example 5 is reduced is presumed to be that the peel strength of the entire negative electrode is low, and the active material-containing layer is peeled off in places other than the innermost circumferential part and the bend part of the negative electrode.

[0290] According to one or more of the embodiments and examples described above, an electrode is provided. The electrode comprises a current collector and an active material layer connected to the current collector. The active material layer comprises titanium oxide as an active material and carbon nanotubes as a conductive agent. The titanium oxide has the form of particles with an average particle size of 0.1 μm or more and 3 μm or less. The peel strength of the active material layer relative to the current collector is in the range of 0.2 kN / m or more and 0.7 kN / m or less. When the above-mentioned electrode is used in a wound electrode group, it is possible to suppress the cutting and cracking of the electrode in the inner peripheral part of the electrode group. The electrode can prevent the battery performance from being reduced due to such cutting and cracking, thereby exerting the original battery performance in a secondary battery having a wound electrode group, and can improve the battery capacity. In addition, the electrode can provide an electrode group capable of improving the capacity of a secondary battery, a secondary battery and a battery pack with improved capacity, and a vehicle equipped with the battery pack.

[0291] Furthermore, the above-mentioned implementation modes can be summarized into the following technical solutions.

[0292] (Technical Solution 1)

[0293] An electrode comprising a current collector and an active material layer, wherein the active material layer is in contact with the current collector and contains titanium oxide particles and carbon nanotubes having an average particle size of not less than 0.1 μm and not more than 3 μm, and the peel strength between the current collector and the active material layer is not less than 0.2 kN / m and not more than 0.7 kN / m.

[0294] (Technical Solution 2)

[0295] According to the above technical solution 1, the titanium-containing oxide contains lithium titanate with a spinel structure, monoclinic titanium dioxide, Li 2+a Mα 2-b Ti 6-c Mβ d O 14+σ The orthorhombic titanium-containing composite oxide represented by Li x Ti 1- y M1 y+z Nb 2-z O 7-δAt least one of the monoclinic niobium-titanium composite oxides represented by the present invention, wherein Mα is at least one selected from Sr, Ba, Ca, Mg, Na, Cs, Rb and K, Mβ is at least one selected from Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni and Al, 0≤a≤6, 0≤b<2, 0≤c<6, 0≤d<6, -0.5≤σ≤0.5; M1 is at least one selected from Mg, Fe, Ni, Co, W, Ta and Mo, 0≤x≤5, 0≤y<1, 0≤z<2, -0.3≤δ≤0.3. .

[0296] (Technical Solution 3)

[0297] An electrode group comprising a positive electrode and a negative electrode, wherein the negative electrode comprises the electrode of technical solution 1 or 2, and the stack comprising the positive electrode and the negative electrode has a flat winding structure wound in a manner centered along a first direction, and at the first bending portion along the winding direction from the end portion located at the innermost periphery and along the first direction in the winding structure, i.e., the innermost bending portion, a portion of the active material-containing layer of the negative electrode is in a non-bonded state relative to the collector.

[0298] (Technical Solution 4)

[0299] According to the third aspect, the non-bonding rate of the active material containing layer in the innermost circumferential bent portion is 1% to 20% per unit area.

[0300] (Technical Solution 5)

[0301] A secondary battery comprises the electrode group according to claim 3 or 4 and an electrolyte.

[0302] (Technical Solution 6)

[0303] A battery pack comprises the secondary battery of the above-mentioned technical solution 5.

[0304] (Technical Solution 7)

[0305] According to the above-mentioned technical solution 6, it further comprises an external terminal for power supply and a protection circuit.

[0306] (Technical Solution 8)

[0307] According to the above technical solution 6 or 7, there are a plurality of the above-mentioned secondary batteries, and the above-mentioned secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.

[0308] (Technical Solution 9)

[0309] A vehicle comprises a battery pack according to any one of technical solutions 6 to 8.

[0310] (Technical Solution 10)

[0311] According to the above-mentioned technical solution 9, it includes a mechanism for converting the kinetic energy of the above-mentioned vehicle into regenerative energy.

[0312] Several embodiments of the present invention have been described, but these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other ways, and various omissions, substitutions, and changes can be made without departing from the scope of the subject matter of the invention. These embodiments and their variations are included in the scope and subject matter of the invention, and are also included in the invention described in the claims and their equivalents.

Claims

1. An electrode group, comprising: Positive electrode, and negative electrode, The negative electrode has: current collector, and An active material layer disposed on both the front and back surfaces of the current collector and containing titanium oxide-containing particles having an average particle size of 0.1 μm or more and 3 μm or less and carbon nanotubes; The peel strength between the current collector and the active material-containing layer is 0.2 kN / m or more and 0.7 kN / m or less, The negative electrode is an electrode having the same peel strength on each surface of the current collector, The stack including the positive electrode and the negative electrode has a flat wound structure wound in a manner such that the positive electrode and the negative electrode are centered along a first direction. At the first bend along the winding direction from the innermost end of the wound structure along the first direction, that is, the innermost bend, a portion of the active material containing layer of the negative electrode is in a non-bonded state with respect to the current collector.

2. The electrode assembly according to claim 1, wherein The titanium-containing oxide contains lithium titanate having a spinel structure, monoclinic titanium dioxide, 2+a Mα 2-b Ti 6-c Mβ d O 14+σ The orthorhombic titanium-containing composite oxide represented by Li x Ti 1-y M1 y+z Nb 2-z O 7-δ One or more of the monoclinic niobium-titanium composite oxides represented by wherein Mα is at least one selected from Sr, Ba, Ca, Mg, Na, Cs, Rb and K, Mβ is at least one selected from Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni and Al, 0≤a≤6, 0≤b<2, 0≤c<6, 0≤d<6, −0.5≤σ≤0.5; M1 is at least one selected from the group consisting of Mg, Fe, Ni, Co, W, Ta and Mo, 0≤x≤5, 0≤y<1, 0≤z<2, and -0.3≤δ≤0.

3.

3. The electrode assembly according to claim 1, wherein The non-bonding rate of the active material-containing layer in the innermost circumferential bent portion is 1% to 20% per unit area.

4. A secondary battery comprising: The electrode group according to any one of claims 1 to 3, and Electrolytes. 5 . A battery pack comprising the secondary battery according to claim 4 .

6. The battery pack according to claim 5, wherein: Further possesses: External terminals for power supply, and Protection circuit.

7. The battery pack according to claim 5 or 6, wherein: A plurality of the secondary batteries are provided, The secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel. 8 . A vehicle comprising the battery pack according to claim 5 .

9. The vehicle according to claim 8, wherein: A mechanism is included for converting the kinetic energy of the vehicle into regenerative energy.

Citation Information

Patent Citations

  • Nonaqueous electrolyte secondary battery and battery pack

    CN104466261A

  • Nonaqueous electrolyte battery, battery pack and vehicle

    CN107863549A

  • Nonaqueous electrolyte secondary battery

    JP2008091054A