A method for preparing polymer microspheres with controllable surface roughness

By dispersing and emulsifying under ultrasonic conditions, surface functionalized porous polymer microspheres without solvent extraction are prepared, which solves the problems of high cost and metal residue in the existing technology, and achieves efficient and low-cost microsphere preparation. , and can control surface roughness.

CN114213595BActive Publication Date: 2024-10-18ANHUI ZHONGKE YUANZHEN TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202111361042.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-17
Publication Date
2024-10-18
Estimated Expiration
2041-11-17

AI Technical Summary

Technical Problem

The existing preparation method of polymer microspheres requires solvent extraction to obtain a porous structure, which increases the cost and production cycle, and the use of CuCl2 may cause metal residues, limiting its application in the biomedical field.

Method used

A method for preparing polymer microspheres with controllable surface roughness is adopted, by dispersing olefin monomers, initiators and dispersants under ultrasonic conditions, and then adding emulsifiers and cross-linking agents for constant temperature reaction, washing and drying. , avoiding the use of solvent extraction and metal polymerization inhibitors, and regulating the surface roughness of microspheres.

Benefits of technology

It realizes the preparation of surface functionalized porous polymer microspheres without solvent extraction, reduces production costs and time, avoids the problem of metal residues, and freely controls the surface roughness of the microspheres.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114213595B_ABST
    Figure CN114213595B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing polymer microspheres with controllable surface roughness, and the preparation method comprises the following steps: taking a number of olefin monomers, at a certain temperature. Mixing a polymer seed ball solution with a swelling agent solution to obtain a primary reaction solution; then adding a portion of a solution containing an olefin monomer and a cross-linking agent, swelling, and isothermal reaction to obtain a secondary reaction solution; finally adding a solution containing an olefin monomer, a functional group monomer, and a cross-linking agent, swelling, isothermal reaction, and then solid-liquid separation to obtain surface functionalized porous polymer microspheres. The present invention prepares surface functionalized porous polymer microspheres without solvent extraction to form pores, avoids the use of porogens and metal inhibitors, saves production time, reduces costs, solves the problem of metal residues, and further increases the surface roughness of the polymer microspheres by increasing the ratio of the cross-linking agent to the olefin monomer in the solution, thereby achieving surface roughness control.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, and in particular to a method for preparing polymer microspheres with controllable surface roughness. Background Art

[0002] Polymer microspheres can be used in related high-tech fields such as standard measurement, drug delivery, chromatographic separation, liquid crystal spacing control, catalytic carriers and electronic packaging. Related polymer microsphere products have the advantages of controllable particle size, monodispersity, high mechanical strength, etc., and can be used as basic materials to prepare metal-plated microspheres, catalysts and drug carriers, liquid chromatography fillers and photonic crystals.

[0003] After studying the existing technical literature, it was found that Sun Kang proposed in his invention patent with Chinese publication number CN101045755A, entitled "Method for preparing surface functionalized non-porous or porous polymer microspheres", to prepare seed balls by dispersion polymerization, then obtain non-porous polymer microspheres by seed swelling method, and finally use organic solvent extraction to obtain surface functionalized porous polymer microspheres.

[0004] However, this method has the following problems: porous polymer microspheres need to be obtained through solvent extraction, which increases costs and has a long production cycle. The use of CuCl2 in the synthesis process easily causes metal residues, which limits the application of this material in the biomedical field. Summary of the invention

[0005] The purpose of the present invention is to solve the shortcomings of the prior art and to propose a method for preparing polymer microspheres with controllable surface roughness.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] A method for preparing polymer microspheres with controllable surface roughness, the method comprising the following steps:

[0008] S01: taking some olefin monomers and distilling them under reduced pressure at a certain temperature before use;

[0009] S02: adding 0.1%-1.0% initiator by mass into olefin monomers, dispersing the solution in a continuous phase solvent with a polymer having a molecular weight of 20,000 to 54,000 as a dispersant, dispersing completely under ultrasound, reacting at a constant temperature, washing and drying to obtain polymer pellets;

[0010] S03: Wetting the prepared polymer bulbs and adding them into an emulsifier solution with a mass fraction of 1.0%-10.0% to prepare a bulb solution;

[0011] The swelling agent is added into an emulsifier solution having a mass fraction of 1.0% to 10.0% and then emulsified to obtain a swelling liquid;

[0012] The swelling liquid is added into the bulb solution and stirred and activated at room temperature to obtain a primary reaction liquid;

[0013] S04: mixing the crosslinking agent and the olefin monomer with the initiator in different proportions, adding the emulsifier solution with a mass fraction of 1.0%-10.0% and emulsifying for 10 minutes to obtain a prepolymer solution;

[0014] Add olefin monomers and functional group-containing monomers into an emulsifier solution with a mass fraction of 1.0%-10.0% and emulsify for 10 minutes to obtain a shell liquid;

[0015] The prepolymer liquid is stirred and the temperature is adjusted to 20-35°C. After isothermal reaction for 3-5 hours, it is cooled to room temperature. Then, the shell liquid and a dispersant solution with a mass fraction of 5.0-10.0% are added, stirred and reacted at a constant temperature for 10-12 hours. After washing and drying, rough polymer microspheres are obtained. The surface roughness of the polymer microspheres is increased by increasing the ratio of the crosslinking agent to the olefin monomer in the solution.

[0016] Preferably, the olefin monomer in step S01 is one or a combination of styrene, vinyl halide, acrylic acid and propylene, including but not limited to the above substances.

[0017] Preferably, the initiator in step S02 refers to an initiator soluble in an organic solvent including one or a combination of azobisisobutyronitrile, dimethyl azobisisobutyrate, lauroyl peroxide, dicyclohexyl peroxydicarbonate, and benzoyl peroxide, including but not limited to the above substances.

[0018] Preferably, the dispersant in steps S02 and S04 refers to a water-soluble high molecular polymer including one or a combination of polyvinyl alcohol, polyvinyl pyrrolidone, polyacrylamide, hydroxypropyl cellulose, etc., including but not limited to the above substances.

[0019] Preferably, the swelling agent in step S03 includes one or a combination of toluene, ethylbenzene, dichloromethane, and dibutyl phthalate, including but not limited to the above substances.

[0020] Preferably, the alcohol solvent in steps S03 and S04 includes one or a combination of methanol, ethanol, n-propanol, isopropanol, including but not limited to the above substances.

[0021] Preferably, the cross-linking agent in step S04 includes one or a combination of polyethylene glycol dimethacrylate, divinylbenzene, and methylenebisacrylamide, including but not limited to the above substances.

[0022] Preferably, the functional group-containing monomer in step S04 includes one or a combination of methacrylic acid, methacrylamide, and N,N′-methylenebisacrylamide, including but not limited to the above substances.

[0023] Compared with the prior art, the present invention has the following beneficial effects: when the present invention prepares surface functionalized porous polymer microspheres, no solvent extraction is required to form pores, thus avoiding the use of porogens and metal inhibitors, saving production time, reducing costs, and solving the problem of metal residues. In addition, the surface roughness of the polymer microspheres is increased by increasing the ratio of the crosslinking agent to the olefin monomer in the solution, and the surface roughness can be freely adjusted. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more specifically and intuitively illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art are briefly introduced below.

[0025] Figure 1 Electron microscopic images of polymer microspheres prepared with increasing ratios of cross-linker to olefin monomers. DETAILED DESCRIPTION

[0026] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0027] Example 1

[0028] Reference Figure 1 , a method for preparing polymer microspheres with controllable surface roughness, the preparation method comprising the following steps:

[0029] S01: Take 500g of styrene monomer and use it after vacuum distillation at 40°C;

[0030] S02: Add 1g of initiator azobisisobutyronitrile into the prepared 20g of styrene, and then disperse the solution in 80g of ethanol solvent containing 5g of polyvinyl pyrrolidone as a dispersant, disperse under ultrasound for 20 minutes, react at 100r / min, 70°C for 12h, wash and dry to obtain polymer pellets;

[0031] S03: Wetting 2 g of the prepared bulbs with 1 g of ethanol solvent and adding them to 10 g of a 1.0% sodium dodecyl sulfate solution to prepare a bulb solution;

[0032] 2 g of dibutyl phthalate was added into 10 g of 1.0% sodium dodecyl sulfate solution and emulsified to obtain a swelling solution;

[0033] Add the swelling solution to the bulb solution and emulsify for 10 minutes to obtain the primary reaction solution. Stir and activate at 30°C for 12 hours;

[0034] S04: 2 g of divinylbenzene, 2 g of styrene, and 0.1 g of azobisisobutyronitrile were added to 40 g of a 1% sodium dodecyl sulfate solution and emulsified for 10 min to obtain a prepolymer solution;

[0035] 2 g of styrene, 2 g of methacrylic acid and 1 g of divinylbenzene were added to 40 g of 1.0% sodium dodecyl sulfate solution and emulsified for 10 min to prepare a shell liquid;

[0036] The prepolymer solution was stirred and heated to 70°C for reaction for 3 hours, then cooled to room temperature, and then the shell liquid and 5.0% dispersant solution were added, stirred and heated to 70°C, and the reaction was continued for 10 hours. After washing and drying, smooth polymer microspheres were obtained.

[0037] Example 2

[0038] Reference Figure 1 , a method for preparing polymer microspheres with controllable surface roughness, the preparation method comprising the following steps:

[0039] S01: Take 500g of styrene monomer and use it after vacuum distillation at 40°C;

[0040] S02: Add 1g of initiator benzoyl peroxide to the prepared 20g of styrene, and then disperse the solution in 80g of methanol solvent containing 5g of polyvinyl alcohol as a dispersant, disperse under ultrasound for 20 minutes, react at 100r / min, 70°C for 12h, wash and dry to obtain polymer pellets;

[0041] S03: Wetting 2 g of the prepared bulbs with 1 g of ethanol solvent and adding them to 10 g of a 1.0% sodium dodecyl sulfate solution to prepare a bulb solution;

[0042] 2 g of toluene was added into 10 g of 1.0% sodium dodecyl sulfate solution and emulsified to obtain a swelling solution;

[0043] Add the swelling solution to the bulb solution and emulsify for 10 minutes to obtain the primary reaction solution. Stir and activate at 30°C for 12 hours;

[0044] S04: 2 g of divinylbenzene, 2 g of styrene, and 0.1 g of benzoyl peroxide were added to 40 g of 1.0% sodium dodecyl sulfate solution and emulsified for 10 min to prepare a prepolymer solution;

[0045] 2 g of styrene, 2 g of methacrylic acid and 2 g of divinylbenzene were added to 40 g of 1.0% sodium dodecyl sulfate solution and emulsified for 10 min to prepare a shell liquid;

[0046] The prepolymer solution was stirred and heated to 70°C for reaction for 3 hours and then cooled to room temperature. Then, the shell liquid and 5% by mass dispersant solution were added and stirred and heated to 70°C. The reaction was continued for 10 hours. After washing and drying, rough non-porous polymer microspheres were obtained.

[0047] Example 3

[0048] Reference Figure 1 , a method for preparing polymer microspheres with controllable surface roughness, the preparation method comprising the following steps:

[0049] S01: Take 500g of styrene monomer and use it after vacuum distillation at 40°C;

[0050] S02: Add 1g of initiator benzoyl peroxide to the prepared 20g of styrene, and then disperse the solution in 80g of methanol solvent containing 5g of polyvinyl alcohol as a dispersant, disperse under ultrasound for 20 minutes, react at 100r / min, 70°C for 12h, wash and dry to obtain polymer pellets;

[0051] S03: Wetting 2 g of the prepared bulbs with 1 g of ethanol solvent and adding them to 10 g of a 1.0% sodium dodecyl sulfate solution to prepare a bulb solution;

[0052] 2 g of dichloromethane was added to 10 g of 1.0% sodium dodecyl sulfate solution and emulsified to obtain a swelling solution;

[0053] Add the swelling solution to the bulb solution and emulsify for 10 minutes to obtain the primary reaction solution. Stir and activate at 35°C for 12 hours;

[0054] S04: 2 g of divinylbenzene, 2 g of styrene, and 0.1 g of azobisisobutyronitrile were added to 40 g of a 1% sodium dodecyl sulfate solution and emulsified for 10 min to obtain a prepolymer solution;

[0055] 2 g of styrene, 2 g of methacrylic acid and 6 g of divinylbenzene were added to 40 g of 1.0% sodium dodecyl sulfate solution and emulsified for 10 min to prepare a shell liquid;

[0056] The prepolymer solution was stirred and heated to 70°C for reaction for 3 hours and then cooled to room temperature. Then, the shell liquid and 5% by mass dispersant solution were added and stirred and heated to 70°C. The reaction was continued for 10 hours. After washing and drying, rough fine-porous polymer microspheres were obtained.

[0057] Example 4

[0058] Reference Figure 1 , a method for preparing polymer microspheres with controllable surface roughness, the preparation method comprising the following steps:

[0059] S01: Take 500g of halogenated styrene monomer and use it after vacuum distillation at 40°C;

[0060] S02: Add 1g of initiator benzoyl peroxide to the prepared 20g of styrene, and then disperse the solution in 80g of methanol solvent containing 5g of polyvinyl alcohol as a dispersant, disperse under ultrasound for 20 minutes, react at 100r / min, 70°C for 12h, wash and dry to obtain polymer pellets;

[0061] S03: Wetting 2 g of the prepared bulbs with 1 g of ethanol solvent and adding them to 10 g of a 1.0% sodium dodecyl sulfate solution to prepare a bulb solution;

[0062] 2 g of dibutyl phthalate was added into 10 g of 1.0% sodium dodecyl sulfate solution and emulsified to obtain a swelling solution;

[0063] Add the swelling solution to the bulb solution and emulsify for 10 minutes to obtain the primary reaction solution. Stir and activate at 30°C for 12 hours;

[0064] S04: 2 g of divinylbenzene, 2 g of halogenated styrene, and 0.1 g of azobisisobutyronitrile were added to 40 g of a 1% sodium dodecyl sulfate solution and emulsified for 10 min to obtain a prepolymer solution;

[0065] 2 g of halogenated styrene, 2 g of methacrylic acid and 6 g of divinylbenzene were added to 40 g of 1.0% sodium dodecyl sulfate solution and emulsified for 10 min to prepare a shell liquid;

[0066] The prepolymer solution was stirred and heated to 70°C for reaction for 3 hours, then cooled to room temperature, and then the shell liquid and 5.0% dispersant solution were added, stirred and heated to 70°C, and the reaction was continued for 10 hours. After washing and drying, coarse-porous polymer microspheres were obtained.

[0067] In step S01, the olefin monomer is one or a combination of styrene, vinyl halide, acrylic acid and propylene, including but not limited to the above substances.

[0068] The initiator in step S02 refers to an organic solvent-soluble initiator including azobisisobutyronitrile, dimethyl azobisisobutyrate, lauroyl peroxide, dicyclohexyl peroxydicarbonate, benzoyl peroxide, or a combination thereof, including but not limited to the above substances.

[0069] The dispersant in steps S02 and S04 refers to a water-soluble high molecular polymer including one or a combination of polyvinyl alcohol, polyvinyl pyrrolidone, polyacrylamide, hydroxypropyl cellulose, etc., including but not limited to the above substances.

[0070] The swelling agent in step S03 includes one or a combination of toluene, ethylbenzene, dichloromethane, and dibutyl phthalate, including but not limited to the above substances.

[0071] The alcohol solvent in steps S03 and S04 includes one or a combination of methanol, ethanol, n-propanol, and isopropanol, including but not limited to the above substances.

[0072] In step S04, the cross-linking agent includes one or a combination of polyethylene glycol dimethacrylate, divinylbenzene, and methylenebisacrylamide, including but not limited to the above substances.

[0073] The functional group-containing monomer in step S04 includes one or a combination of methacrylic acid, methacrylamide, and N,N′-methylenebisacrylamide, including but not limited to the above substances.

[0074] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing polymer microspheres with controllable surface roughness, characterized in that: The preparation method comprises the following steps: S01: taking some olefin monomers and distilling them under reduced pressure at a certain temperature before use; S02: adding 0.1%-1.0% initiator by mass into olefin monomers, dispersing the solution in a continuous phase solvent with a polymer having a molecular weight of 20,000-54,000 as a dispersant, and after complete dispersion under ultrasonic conditions, reacting at a constant temperature, washing and drying to obtain polymer pellets; S03: adding the prepared polymer bulbs to an emulsifier solution having a mass fraction of 1.0%-10.0% to prepare a bulb solution; The swelling agent is added into an emulsifier solution having a mass fraction of 1.0% to 10.0% and then emulsified to obtain a swelling liquid; The swelling liquid is added into the bulb solution and stirred and activated at room temperature to obtain a primary reaction liquid; S04: mixing the crosslinking agent and the olefin monomer with the initiator in different proportions, adding the emulsifier solution with a mass fraction of 1%-10% and emulsifying for 10 minutes to obtain a prepolymer solution; Add olefin monomers and functional group-containing monomers into an emulsifier solution with a mass fraction of 1.0%-10.0% and emulsify for 10 minutes to obtain a shell liquid; The prepolymer liquid is stirred and the temperature is adjusted to 20-35°C. After isothermal reaction for 3-5 hours, it is cooled to room temperature. Then, the shell liquid and a dispersant solution with a mass fraction of 5.0-10.0% are added, stirred and reacted at a constant temperature for 10-12 hours. After washing and drying, rough polymer microspheres are obtained. The surface roughness of the polymer microspheres is increased by increasing the ratio of the crosslinking agent to the olefin monomer in the solution.

2. The method for preparing polymer microspheres with controllable surface roughness according to claim 1, characterized in that: In the step S01, the olefin monomer is one or a combination of styrene, vinyl halide, acrylic acid and propylene, including but not limited to the above substances.

3. The method for preparing polymer microspheres with controllable surface roughness according to claim 2, characterized in that: The initiator in step S02 refers to an initiator soluble in an organic solvent, including azobisisobutyronitrile, dimethyl azobisisobutyrate, lauroyl peroxide, dicyclohexyl peroxydicarbonate, benzoyl peroxide, or a combination thereof, including but not limited to the above substances.

4. The method for preparing polymer microspheres with controllable surface roughness according to claim 3, characterized in that: The dispersant in steps S02 and S04 refers to a water-soluble high molecular polymer including one or a combination of polyvinyl alcohol, polyvinyl pyrrolidone, polyacrylamide, hydroxypropyl cellulose, etc., including but not limited to the above substances.

5. The method for preparing polymer microspheres with controllable surface roughness according to claim 4, characterized in that: The swelling agent in step S03 includes one or a combination of toluene, ethylbenzene, dichloromethane, and dibutyl phthalate, including but not limited to the above substances.

6. The method for preparing polymer microspheres with controllable surface roughness according to claim 1, characterized in that: The crosslinking agent in step S04 includes one or a combination of polyethylene glycol dimethacrylate, divinylbenzene, and methylenebisacrylamide, including but not limited to the above substances.

7. The method for preparing polymer microspheres with controllable surface roughness according to claim 1, characterized in that: The functional group-containing monomer in step S04 includes one or a combination of methacrylic acid and methacrylamide, including but not limited to the above substances.

Citation Information

Patent Citations

  • Preparation method of non-porous or porous polymer microsphere of surface function

    CN101045755A

  • Preparation method of polymer particles

    CN102603929A

  • Method for Preparing Monodisperse Macro-Porous PolymerParticle

    KR1020040071431A