A CCM preparation method for water electrolysis hydrogen production, CCM and membrane electrode

Through ultrasonic atomization treatment and tension fixation technology, combined with heating and catalyst formulation adjustment, the proton exchange membrane swelling problem in hydrogen production by water electrolysis is solved, and high-efficiency and low-cost membrane electrode preparation is achieved, simplifying the process flow and improving membrane electrode Performance and water electrolytic efficiency.

CN114220978BActive Publication Date: 2024-11-05SINOHYKEY TECHNOLOGY FOSHAN CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202111564295.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-20
Publication Date
2024-11-05
Estimated Expiration
2041-12-20

AI Technical Summary

Technical Problem

In the existing water electrolysis hydrogen production technology, proton exchange membranes are prone to swelling and deformation during coating, resulting in a decrease in the performance of membrane electrodes. The preparation method is complex and costly, making it difficult to achieve large-scale production.

Method used

Ultrasonic atomization treatment and tension fixation technology are used to pretreat the proton exchange membrane, combined with heating and adjustment of the catalyst slurry formula, reduce the degree of swelling, and double-side direct coating is used to simplify the process flow.

Benefits of technology

It effectively avoids swelling and deformation of the proton exchange membrane, improves production speed and yield, reduces costs, simplifies operating steps, and improves the performance of the membrane electrode and water electrolytic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114220978B_ABST
    Figure CN114220978B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of fuel cell preparation, and more specifically, to a CCM preparation method, CCM and membrane electrode for water electrolysis hydrogen production, wherein the preparation method is to ultrasonically atomize a thick proton exchange membrane, fix the proton exchange membrane with tension, and then apply catalyst slurry to both sides of the proton exchange membrane under heating conditions and dry it to form a catalytic layer on both sides of the proton exchange membrane. The present invention can avoid swelling and deformation of the proton exchange membrane during the coating process, and can use ordinary slit coating equipment to prepare CCM for water electrolysis hydrogen production on a large scale, greatly reducing production costs while ensuring product quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of fuel cell preparation, and more specifically, to a CCM preparation method for producing hydrogen by water electrolysis, a CCM and a membrane electrode. Background Art

[0002] As a green energy with a wide range of sources, zero pollution and zero carbon emissions, hydrogen energy is an ideal energy source to promote the clean utilization of traditional fossil energy and promote the large-scale development of renewable energy. In the future, hydrogen energy will play an important role in the process of carbon reduction in my country's industrial sector.

[0003] Depending on the hydrogen production method, hydrogen can be gray hydrogen, blue hydrogen and green hydrogen. Among them, gray hydrogen refers to hydrogen produced by carbon-based energy such as coal, and the production process will emit carbon dioxide; blue hydrogen refers to the use of "carbon-free" technical means such as capturing carbon dioxide in the production process of gray hydrogen; green hydrogen is hydrogen that truly achieves zero carbon emissions during the production process. Based on the original intention of the development of the hydrogen energy industry to achieve zero or low carbon emissions, green hydrogen will become the development direction of the future energy industry. The main methods of green hydrogen production are solar photocatalytic water decomposition and water electrolysis. The proton exchange membrane water electrolysis hydrogen production technology has the advantages of high energy efficiency, high purity of hydrogen production, good high-voltage tolerance, compact structure and strong adaptability to input power fluctuations. It is especially suitable for renewable energy power electrolysis hydrogen production and is considered to be very suitable as the next generation of large-scale hydrogen production technology. At this stage, this field has also made great progress, and market demand has exploded.

[0004] At present, the domestic proton exchange membrane water electrolysis hydrogen production technology is still in the early stages of development, and there are problems that restrict its application and development, such as small-scale preparation of key materials, high unit cost, and insufficient life of electrolyzers. Therefore, it is of great significance to carry out the design of key materials for low-cost water electrolysis hydrogen production and conduct research on batch preparation technology for the industrial development and promotion of water electrolysis hydrogen production.

[0005] In conventional fuel cell CCMs, the proton exchange membranes used are ultra-thin reinforced proton exchange membranes, which are generally only 8 to 15 μm thick, and the reinforcing material can alleviate the swelling of the proton exchange membrane surface caused by the solvent when the slurry is applied. However, the proton exchange membranes used in the current water electrolysis hydrogen production CCMs are relatively thick. When the slurry is directly applied on the surface of the proton exchange membrane, the solvent will cause the proton exchange membrane to swell and wrinkle or curl, resulting in a decrease in the performance of the prepared membrane electrode. When the degree of wrinkling or curling is high, it is even impossible to make a membrane electrode. Therefore, the current preparation of CCMs for water electrolysis hydrogen production generally adopts methods such as electrochemical deposition, ultrasonic spraying or transfer printing to avoid large amounts of direct contact between the catalyst slurry and the proton exchange membrane. However, these schemes are complicated to operate, take a long time to prepare, and are costly. Summary of the invention

[0006] The present invention aims to overcome at least one defect (shortcoming) of the above-mentioned prior art and provides a CCM preparation method, CCM and membrane electrode for water electrolysis hydrogen production, which can avoid swelling and deformation of the proton exchange membrane during the coating process. CCM for water electrolysis hydrogen production can be prepared on a large scale using ordinary slit coating equipment, which greatly reduces production costs while ensuring product quality.

[0007] The technical solution adopted by the present invention is a CCM preparation method for hydrogen production by water electrolysis. After ultrasonic atomization treatment is performed on a thick proton exchange membrane, the proton exchange membrane is fixed with tension, and then catalyst slurry is coated on both sides of the proton exchange membrane under heating conditions and dried to form a catalytic layer on both sides of the proton exchange membrane.

[0008] Since the catalyst slurry contains organic solvents, the proton exchange membrane is prone to swelling and obvious wrinkles when the organic solvent contacts the surface of the proton exchange membrane, which affects the morphology and performance of the prepared CCM. In this technical solution, the proton exchange membrane is first subjected to ultrasonic atomization treatment to reduce the swelling degree of the proton exchange membrane in the subsequent coating process and avoid wrinkles in the proton exchange membrane. After the ultrasonic atomization treatment, the proton exchange membrane is continuously heated during the coating process to evaporate the solvent in the slurry on the surface of the proton exchange membrane, reduce contact with the surface of the proton exchange membrane, and thus reduce the swelling degree. The use of tension to fix the proton exchange membrane can make the proton exchange membrane evenly stressed when it swells. After a variety of treatment methods are combined, the slurry can be directly applied to the surface of the proton exchange membrane using slit coating, which has lower equipment requirements, higher yield, faster manufacturing speed, and lower cost.

[0009] Furthermore, the preparation method specifically comprises the following steps:

[0010] S1 ultrasonic atomization treatment: ultrasonic atomization spraying treatment is performed on the surface of the proton exchange membrane with water under heating conditions;

[0011] S2: preparing an anode catalyst layer: preparing an anode catalyst slurry, fixing the proton exchange membrane treated in step S1 with a certain tension, applying the anode catalyst slurry on one side of the proton exchange membrane under heating, and drying to form an anode catalyst layer;

[0012] S3: preparing a cathode catalyst layer: preparing a cathode catalyst slurry, fixing the proton exchange membrane treated in step S2 with a certain tension, applying the cathode catalyst slurry to the other side of the proton exchange membrane under heating, and drying to form a cathode catalyst layer, thereby obtaining the CCM for hydrogen production by water electrolysis;

[0013] The order of step S2 and step S3 can be swapped.

[0014] Preferably, in step S1, the heating temperature is 80-120°C.

[0015] In the present technical solution, in step S1, water is sprayed by heating and ultrasonic atomization to pre-expand the proton exchange membrane, so that the swelling degree of the proton exchange membrane is reduced during the coating process. At the same time, the surface of the proton exchange membrane is atomized by water, which can improve the surface properties of the proton exchange membrane, improve the interaction between the catalyst slurry and the proton exchange membrane, and further avoid excessive swelling of the proton exchange membrane to produce wrinkles.

[0016] Preferably, the proton exchange membrane is a reinforced or non-reinforced proton exchange membrane, and its thickness is 50-200 μm.

[0017] The proton exchange membranes used in water electrolysis are basically thicker proton exchange membranes. Currently, non-enhanced proton exchange membranes are generally used, while enhanced proton exchange membranes have not yet been promoted. Although enhanced proton exchange membranes have added reinforcing materials, due to their large thickness, the catalyst slurry will actually cause swelling on their surfaces during direct coating. Therefore, in this technical solution, ultrasonic atomization pretreatment is performed on thicker enhanced or non-enhanced proton exchange membranes, and heating and fixing treatment is performed during coating, which can further alleviate or even avoid their swelling phenomenon, making them directly applicable to double-sided direct coating.

[0018] More preferably, the proton exchange membrane is a non-reinforced proton exchange membrane with a thickness of 125 to 175 μm.

[0019] More preferably, the proton exchange membrane is a proton exchange membrane Nafion 117 membrane or a Nafion 115 membrane.

[0020] Preferably, in step S2 and step S3, the temperature of the heating condition is 70-90° C., and the tension is 0.01 MPa to 0.05 MPa.

[0021] In the present technical solution, when the proton exchange membrane contacts the catalyst slurry, the solvent easily causes the proton exchange membrane to swell. Therefore, the proton exchange membrane is continuously heated to a certain temperature during the coating process to allow the solvent of the slurry on the surface of the proton exchange membrane to evaporate quickly, reducing contact with the surface of the proton exchange membrane, thereby reducing the degree of swelling. At the same time, if the fixing tension is too small during the coating process, the proton exchange membrane will move during the coating process and cannot be coated. If the fixing tension is too large, the proton exchange membrane will be stretched directly, causing the thickness and mechanical properties of the membrane to change, and may even cause the proton exchange membrane to rupture. Therefore, a certain tension is used to fix the proton exchange membrane so that it is evenly stressed when swelling occurs, preventing the proton exchange membrane from wrinkling or curling due to swelling during direct coating. At the same time, the proton exchange membrane will not deform and cause performance degradation. The direct coating method can also make the surface of the prepared CCM smooth, thereby improving the yield rate and product quality.

[0022] Furthermore, in step S2, the method for preparing the anode catalyst slurry is to mix and evenly disperse the anode catalyst, resin solution, alcohol solvent and water; in step S3, the method for preparing the cathode catalyst slurry is to mix and evenly disperse the cathode catalyst, resin solution, alcohol solvent and water.

[0023] Preferably, the active component loading in the anode catalyst is 0.3-2.0 mg / cm 2 The anode catalyst is at least one of the following: a. Ir, IrO 2 or RuO 2 ; b. Loaded IrO 2 , the metal loading is in terms of Ir, wherein the carrier is a mixture of one or more of titanium oxide, tantalum pentoxide, tin dioxide or niobium oxide; c. an oxide of Mn, Fe or Co; d. the perovskite metal oxide is A x A' 1-x B y B' 1-y O 3 , wherein A and A' are one of Sm, Ba, Sr, Co, La, Bi, and Ce, and A and A' are the same or different, B and B' are one of Co, Ni, and Fe, and B and B' are the same or different; and / or, the noble metal loading in the cathode catalyst is 0.05 to 0.6 mg / cm 2 , the cathode catalyst is Pt / C.

[0024] In the present technical solution, since the anode is in a strongly oxidizing environment, it is more easily polarized, so antioxidant and corrosion-resistant Ir and its oxide, Ru are selected as catalysts to make the anode more stable, and the amount of Pt is reduced, thereby reducing costs; using a carrier or a non-precious metal catalyst can reduce the amount of precious metals, increase the active specific surface area of ​​the catalyst, and improve the mechanical strength and chemical stability of the catalyst.

[0025] More preferably, in the method for preparing the anode catalyst slurry, the alcohol solvent is isopropanol; in the method for preparing the cathode catalyst slurry, the alcohol solvent is isopropanol.

[0026] More preferably, the resin solution is a Nafion solution, specifically a perfluorosulfonic acid resin solution from Chemours.

[0027] More preferably, the weight ratio of the anode catalyst, resin solution, alcohol solvent and water is (7-9):(1-3):(3-54):(6-72), and / or the weight ratio of the cathode catalyst, resin solution, alcohol solvent and water is (2.5-6):(4-7.5):(6-54):(12-72).

[0028] In the present technical solution, a highly volatile solvent is used. During the coating process, the solvent can evaporate quickly at a higher temperature, and the formula of the slurry is adjusted so that the distribution ratio of each component of the slurry is more suitable for the coating of proton exchange membranes with thicker thickness, thereby reducing the swelling effect of the catalyst slurry on it, so that the proton exchange membrane can be directly coated with the slurry by direct coating methods such as slit coating without generating wrinkles.

[0029] The present invention also provides a CCM for producing hydrogen by water electrolysis, which is prepared by the above-mentioned CCM preparation method for producing hydrogen by water electrolysis.

[0030] The present invention also provides a membrane electrode, comprising an anode diffusion layer, the above-mentioned CCM for producing hydrogen by water electrolysis and a cathode diffusion layer stacked in sequence, wherein the anode diffusion layer is opposite to the anode catalyst layer, and the cathode diffusion layer is opposite to the cathode catalyst layer.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] (1) The present invention performs ultrasonic atomization treatment on the proton exchange membrane before coating, heats the proton exchange membrane during the coating process and fixes the proton exchange membrane with a certain tension, and adjusts the component ratio of the slurry. The swelling degree of the proton exchange membrane during the coating process is effectively reduced by combining multiple technical means, thereby avoiding wrinkles or curling of thick proton exchange membranes, improving production speed and yield rate, and reducing costs;

[0033] (2) During the coating process of the proton exchange membrane, the degree of swelling is low and the deformation is small. The catalyst slurry can be directly coated by methods such as slit coating. The coating method is simple, the equipment requirements are low, the operation steps are simple, and it effectively improves the utilization rate of the catalyst, improves the performance of the membrane electrode, and increases the efficiency of water electrolysis. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 This is a photograph of the catalyst layer surface of Example 1.

[0035] Figure 2 This is a photograph of the catalyst layer surface of Comparative Example 1.

[0036] Figure 3 This is a photograph of the catalyst layer surface of Comparative Example 2.

[0037] Figure 4 This is a photograph of the catalyst layer surface of Comparative Example 3.

[0038] Figure 5 This is a photograph of the catalyst layer surface of Comparative Example 4.

[0039] Figure 6 This is a photograph of the catalyst layer surface of Comparative Example 5.

[0040] Figure 7 It is a schematic diagram of the structure of the membrane electrode of the present invention.

[0041] Figure 8 These are the performance test curves of Example 1 and Comparative Example 7.

[0042] The markings in the attached figure are: 1-proton exchange membrane; 2-anode catalyst layer; 3-cathode catalyst layer; 4-anode diffusion layer; 5-cathode diffusion layer. DETAILED DESCRIPTION

[0043] Hydrogen production by water electrolysis refers to the dissociation of water molecules into oxygen and hydrogen under the action of direct current, which are precipitated from the anode and cathode of the electrolyzer respectively. According to the different materials of the electrolyzer diaphragm, hydrogen production by water electrolysis is usually divided into alkaline water electrolysis (AE), proton exchange membrane (PEM) water electrolysis and high-temperature solid oxide water electrolysis (SOEC). Proton exchange membrane water electrolysis uses perfluorosulfonic acid proton exchange membrane. Compared with other methods, it has good chemical stability, proton conductivity and gas separation, and is a water electrolysis hydrogen production technology with great development prospects.

[0044] The core component of the proton exchange membrane water electrolyzer is the catalyst membrane (CCM), and its low-cost industrialization research is of great significance. There are three main CCM preparation processes that have been widely recognized and can be scaled up: electrochemical deposition, ultrasonic spraying, and transfer printing. Among them, the electrochemical deposition method has the advantages of strong bonding between the catalyst layer and the proton exchange membrane, low interface resistance, and low precious metal loading, but the catalyst deposited particles are of different sizes, large and unevenly distributed, and the water electrolysis efficiency is low; the ultrasonic spraying method can solve this problem well and save catalysts, but the method has high energy consumption; the biggest advantage of the transfer method is that it can avoid problems such as swelling and wrinkling of the proton exchange membrane, but the catalyst utilization rate is low. These methods have their own shortcomings, and the operation is complicated and the preparation time is long, resulting in low production efficiency and high cost.

[0045] At present, fuel cell CCM widely uses direct coating of both anode and cathode. The slurry is directly coated on the surface of the proton exchange membrane by slit coating, etc., and the preparation is completed. It has high production efficiency and greatly reduces production costs. However, this double-sided direct coating process cannot be applied to the catalytic membrane for water electrolysis to produce hydrogen. The reason is that the proton exchange membrane used for water electrolysis to produce hydrogen is relatively thick. When the slurry is directly coated on the surface of the proton exchange membrane, the solvent will cause the proton exchange membrane to swell and wrinkle or curl, resulting in a decrease in the performance of the prepared membrane electrode. When the degree of wrinkling or curling is high, it is even impossible to make a membrane electrode. Therefore, if the double-sided direct coating process is simply used for the catalytic membrane for water electrolysis to produce hydrogen, the preparation time will be longer and the yield rate will be lower.

[0046] In order to overcome the above technical problems, the present invention chooses to perform ultrasonic atomization treatment on the proton exchange membrane, and cooperates with the temperature, fixed tension and adjusted catalyst slurry formula during the coating process to reduce the swelling degree of the proton exchange membrane, so that it can be suitable for double-sided direct coating process, improve production efficiency and yield rate, and reduce costs.

[0047] Regarding the treatment of the proton exchange membrane during the coating process, Chinese patent CN101276919A discloses placing the proton exchange membrane on a carrier plate, heating it, and then spraying the catalyst slurry. However, since the proton exchange membrane is only heated, the proton exchange membrane will still swell to a certain extent. Therefore, it is still necessary to use a spraying method to control the amount of catalyst slurry, and the production efficiency is still not improved.

[0048] The preparation method of the present invention cooperates with a variety of means to enable the double-sided direct coating process to be applied to thicker reinforced or non-reinforced proton exchange membranes. The coating can be completed using a common slit coating process, and the production efficiency can be improved. In the actual slit coating production of CCM, the current maximum production speed can reach 3 meters / minute. During this process, the swelling degree of the proton exchange membrane is extremely low, the product quality is improved, the yield is greater than 90%, and the cost can be effectively reduced.

[0049] In order to allow those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with specific embodiments. In the following embodiments, the methods used are all prior art unless otherwise specified; the materials used are all commercial materials well known to those skilled in the art unless otherwise specified.

[0050] Example 1

[0051] This embodiment provides a CCM for producing hydrogen by water electrolysis, which uses a Nafion 117 proton exchange membrane and is specifically prepared by the following preparation method, including the following steps:

[0052] S1 ultrasonic atomization treatment: heating the proton exchange membrane to 90° C. and ultrasonically atomizing water and spraying it on the surface of the proton exchange membrane;

[0053] S2 Preparation of anode catalyst layer: 10g IrO 2 Anode catalyst, 15g 20% ​​D2020 Nafion solution, 11g isopropanol and 17g water are mixed, dispersed evenly using a high-speed shear disperser, and deaerated to obtain an anode catalyst slurry; the proton exchange membrane treated in step S1 is heated to 90°C and fixed with a tension of 0.02MPa, and then the anode catalyst slurry is directly coated on one side of the proton exchange membrane in a heated state, and dried at 90°C to form an anode catalyst layer on one side of the proton exchange membrane;

[0054] S3: preparing a cathode catalyst layer: mixing 10 g of a Pt / C cathode catalyst, 18 g of a 20% D2020 Nafion solution, 10 g of n-propanol and 54 g of water, dispersing the mixture using an ultrasonic crusher, and performing a degassing treatment to obtain a cathode catalyst slurry; heating the proton exchange membrane treated in step S1 to 90° C. and fixing the membrane with a tension of 0.02 MPa, directly coating the cathode catalyst slurry on the other side of the proton exchange membrane treated in step S2 under heating, and drying the membrane at 90° C. to form a cathode catalyst layer on one side of the proton exchange membrane, thereby obtaining the CCM for producing hydrogen by water electrolysis;

[0055] The order of step S2 and step S3 can be swapped.

[0056] In this embodiment, the surface of the prepared CCM is as follows: Figure 1 As shown in the figure, it can be seen that even if the double-sided direct coating method is used to coat the surface of a non-reinforced membrane with a larger thickness, the swelling degree of the proton exchange membrane is low, the surface of the CCM is flat, without wrinkles or curling, and the quality is better.

[0057] like Figure 7 As shown, the CCM can be further made into a membrane electrode, which includes an anode diffusion layer, the CCM prepared in this embodiment and a cathode diffusion layer stacked in sequence, the anode diffusion layer is opposite to the anode catalyst layer, and the cathode diffusion layer is opposite to the cathode catalyst layer. In this embodiment, the anode diffusion layer is titanium felt, and the cathode diffusion layer is carbon paper.

[0058] The preparation method of the membrane electrode is: placing an anode diffusion layer on one side of the CCM anode catalyst layer, placing a cathode diffusion layer on one side of the CCM cathode catalyst layer, and then pressing them together by mechanical pressing to obtain the membrane electrode.

[0059] Comparative Example 1

[0060] This comparative example provides a CCM using a Nafion 117 proton exchange membrane, which is substantially the same as Example 1, except that the proton exchange membrane is not subjected to ultrasonic atomization treatment and is not heated during the coating process. It is specifically prepared by the following preparation method, comprising the following steps:

[0061] S1 Preparation of anode catalyst layer: 10g IrO 2 An anode catalyst, 15 g of 20% D2020 Nafion solution, 11 g of isopropanol and 17 g of water were mixed, dispersed evenly using a high-speed shear disperser, and deaerated to obtain an anode catalyst slurry; the proton exchange membrane was fixed with a tension of 0.01 MPa, and the anode catalyst slurry was directly coated on one side of the proton exchange membrane, and dried at 90° C. to form an anode catalyst layer on one side of the proton exchange membrane;

[0062] In this comparative example, since the Nafion 117 proton exchange membrane was not subjected to ultrasonic atomization treatment, the proton exchange membrane swelled severely when the anode catalyst slurry was applied. Figure 2 As shown, the surface of the proton exchange membrane after coating has obvious wrinkles and curling, and the next step of coating to prepare CCM cannot be carried out.

[0063] Comparative Example 2

[0064] This comparative example provides a CCM using a Nafion 117 proton exchange membrane, which is substantially the same as Example 1, except that the proton exchange membrane is not subjected to ultrasonic atomization treatment and is not heated during the coating process. It is specifically prepared by the following preparation method, comprising the following steps:

[0065] S1 Preparation of anode catalyst layer: 10g IrO 2An anode catalyst, 15 g of 20% D2020 Nafion solution, 11 g of isopropanol and 17 g of water were mixed, dispersed evenly using a high-speed shear disperser, and deaerated to obtain an anode catalyst slurry; the proton exchange membrane was fixed with a tension of 0.02 MPa, and the anode catalyst slurry was directly coated on one side of the proton exchange membrane, and dried at 90° C. to form an anode catalyst layer on one side of the proton exchange membrane;

[0066] In this comparative example, although a certain tension was used to fix the proton exchange membrane during the coating process, it was not subjected to ultrasonic atomization treatment and was not heated during the coating process. The solvent of the catalyst slurry could not evaporate quickly, and the severe swelling of the proton exchange membrane during the coating of the anode catalyst slurry could not be alleviated by only fixing the tension. Figure 3 As shown, the surface of the proton exchange membrane after coating still swells and has a large number of wrinkles and curls, making it impossible to proceed to the next step of coating to prepare CCM.

[0067] Comparative Example 3

[0068] This comparative example provides a CCM using Nafion 117 proton exchange membrane, which is basically the same as Example 1, except that the fixing tension during the coating process is smaller. It is specifically prepared by the following preparation method, including the following steps:

[0069] S1 ultrasonic atomization treatment: heating the proton exchange membrane to 90° C. and ultrasonically atomizing water and spraying it on the surface of the proton exchange membrane;

[0070] S2 Preparation of anode catalyst layer: 10g IrO 2 The anode catalyst, 15 g of 20% D2020 Nafion solution, 11 g of isopropanol and 17 g of water were mixed, dispersed evenly using a high-speed shear disperser, and deaerated to obtain an anode catalyst slurry; the proton exchange membrane treated in step S1 was heated to 90°C and fixed with a tension of 0.005 MPa, and then the anode catalyst slurry was directly coated on one side of the surface under heating, and dried at 90°C to form an anode catalyst layer on one side of the proton exchange membrane.

[0071] In this comparative example, the proton exchange membrane was subjected to ultrasonic atomization treatment and was also heated during the coating process. However, the fixing tension during the coating process was small, and when the proton exchange membrane began to swell, the internal force was uneven, so a serious swelling phenomenon still occurred, such as Figure 4 As shown, the proton exchange membrane after coating had a lot of wrinkles and curling, and it was impossible to proceed to the next step of coating to prepare CCM.

[0072] Comparative Example 4

[0073] This comparative example provides a CCM using a Nafion 117 proton exchange membrane, which is basically the same as Example 1, except that the proton exchange membrane is not subjected to ultrasonic atomization treatment. It is specifically prepared by the following preparation method, including the following steps:

[0074] S1 Preparation of anode catalyst layer: 10g IrO 2 The anode catalyst, 15 g of 20% D2020 Nafion solution, 11 g of isopropanol and 17 g of water were mixed, dispersed evenly using a high-speed shear disperser, and degassing was performed to obtain an anode catalyst slurry; the proton exchange membrane was heated to 90°C and fixed with a tension of 0.02 MPa, and then the anode catalyst slurry was directly coated on one side of the proton exchange membrane in a heated state, and dried at 90°C to form an anode catalyst layer on one side of the proton exchange membrane.

[0075] In this comparative example, the proton exchange membrane was not subjected to ultrasonic atomization treatment. Therefore, although the proton exchange membrane was heated and fixed with a certain tension during the coating process, the swelling degree of the proton exchange membrane was still relatively high at this time, and it would still swell rapidly when in contact with the catalyst slurry. Figure 5 As shown, the proton exchange membrane after coating still has a certain degree of swelling and has obvious wrinkles and curling, and it is impossible to proceed to the next step of coating to prepare CCM.

[0076] Comparative Example 5

[0077] This comparative example provides a CCM using Nafion 117 proton exchange membrane, which is basically the same as Example 1, except that no heating is performed during the coating process. It is specifically prepared by the following preparation method, including the following steps:

[0078] S1 ultrasonic atomization treatment: heating the proton exchange membrane to 90° C. and ultrasonically atomizing water and spraying it on the surface of the proton exchange membrane;

[0079] S2 Preparation of anode catalyst layer: 10g IrO 2 The anode catalyst, 15 g of 20% D2020 Nafion solution, 11 g of isopropanol and 17 g of water were mixed, dispersed evenly using a high-speed shear disperser, and deaerated to obtain an anode catalyst slurry; the proton exchange membrane treated in step S1 was fixed with a tension of 0.01 MPa, and the anode catalyst slurry was directly coated on one side of the proton exchange membrane, and dried at 90°C to form an anode catalyst layer on one side of the proton exchange membrane.

[0080] In this comparative example, the proton exchange membrane was subjected to ultrasonic atomization treatment, which reduced its swelling degree during the coating process, and then reduced the degree of swelling. A certain fixed tension was used to balance the force on the proton exchange membrane, which could further alleviate the swelling. However, the proton exchange membrane was not heated during the coating process in this comparative example, and the alcohol solvent in the catalyst slurry was in contact with the surface of the proton exchange membrane for a long time, which aggravated the swelling. Figure 6 As shown, the proton exchange membrane after coating in this comparative example still has a certain degree of swelling and has obvious wrinkles and curling, and cannot be used for the next step of coating to prepare CCM.

[0081] Comparative Example 6

[0082] This comparative example provides a CCM using Nafion 117 proton exchange membrane, which is basically the same as Example 1, except that the fixing tension is larger during the coating process. It is specifically prepared by the following preparation method, including the following steps:

[0083] S1 ultrasonic atomization treatment: heating the proton exchange membrane to 90° C. and ultrasonically atomizing water and spraying it on the surface of the proton exchange membrane;

[0084] S2 Preparation of anode catalyst layer: 10g IrO 2 The anode catalyst, 15 g of 20% D2020 Nafion solution, 11 g of isopropanol and 17 g of water were mixed, dispersed evenly using a high-speed shear disperser, and degassing was performed to obtain an anode catalyst slurry; the proton exchange membrane treated in step S1 was heated to 90°C and fixed with a tension of 0.08 MPa, and then the anode catalyst slurry was directly coated on one side of the surface under heating, and dried at 90°C to form an anode catalyst layer on one side of the proton exchange membrane.

[0085] In this comparative example, the proton exchange membrane was subjected to ultrasonic atomization treatment, but the fixed tension during coating was relatively large, causing the proton membrane to be significantly deformed, making it impossible to proceed to the next step of coating to prepare CCM.

[0086] Comparative Example 7

[0087] This comparative example provides a CCM using Nafion 117 proton exchange membrane, which is basically the same as Example 1, except that it is prepared by transfer printing. It is prepared by the following preparation method, including the following steps:

[0088] S1 Preparation of anode catalyst layer: 10g IrO 2An anode catalyst, 15 g of 20% D2020 Nafion solution, 11 g of isopropanol and 17 g of water were mixed, dispersed evenly using a high-speed shear disperser, and deaerated to obtain an anode catalyst slurry; the anode catalyst slurry was coated on a PTFE transfer membrane and dried at 90° C. to form an anode catalyst layer on the surface of the PTFE transfer membrane;

[0089] S2: preparing a cathode catalyst layer: mixing 10 g of a Pt / C cathode catalyst, 18 g of a 20% D2020 Nafion solution, 10 g of n-propanol and 54 g of water, dispersing the mixture using an ultrasonic crusher, and performing a degassing treatment to obtain a cathode catalyst slurry; coating the cathode catalyst slurry on a PTFE transfer membrane, and drying the mixture at 90° C. to form a cathode catalyst layer on the surface of the PTFE transfer membrane;

[0090] S3: transferring the anode catalyst layer prepared in step S1 and the cathode catalyst layer prepared in step S2 to the surfaces of both sides of the proton exchange membrane by hot pressing, respectively, to obtain the CCM for producing hydrogen by water electrolysis;

[0091] The order of step S1 and step S2 can be swapped.

[0092] This comparative example uses the transfer method, and the proton exchange membrane will not have the problem of swelling and wrinkling. However, the operation steps are complicated and the production efficiency is low. At present, its maximum production speed can only reach 1 meter / minute, and multiple PTFE transfer membranes are required, resulting in a high cost for a single CCM.

[0093] The CCM can be further made into a membrane electrode, which includes an anode diffusion layer, the CCM prepared in this embodiment and a cathode diffusion layer stacked in sequence, the anode diffusion layer is opposite to the anode catalyst layer, and the cathode diffusion layer is opposite to the cathode catalyst layer. In this comparative example, the anode diffusion layer is titanium felt, and the cathode diffusion layer is carbon paper.

[0094] The preparation method of the membrane electrode is: placing an anode diffusion layer on one side of the CCM anode catalyst layer, placing a cathode diffusion layer on one side of the CCM cathode catalyst layer, and then pressing them together by mechanical pressing to obtain the membrane electrode.

[0095] The membrane electrodes prepared in Example 1 and Comparative Example 7 were supported by titanium mesh, respectively, and then assembled with the cathode and anode plates and the cathode and anode end plates to form an electrolytic cell. The electrolytic cell was heated to 80°C, and after the membrane electrodes were activated, a polarization curve test was performed, specifically, the current density-voltage curve was plotted after testing and recording the voltage of the electrolytic cell at different current densities. The test results are shown in FIG. Figure 8It can be seen that the performance of the membrane electrode of Example 1 is not much different from that of the membrane electrode of Comparative Example 6. It can be seen that the preparation method of the present invention can be quickly coated using ordinary direct coating equipment, effectively avoiding swelling of the proton exchange membrane, simplifying the preparation steps, and significantly improving the manufacturing speed. At the same time, it can ensure the quality and performance of CCM, thereby greatly reducing the manufacturing cost.

[0096] Obviously, the above embodiments of the present invention are merely examples for clearly illustrating the technical solution of the present invention, and are not intended to limit the specific implementation methods of the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the claims of the present invention shall be included in the protection scope of the claims of the present invention.

Claims

1. A method for preparing CCM for hydrogen production by water electrolysis, characterized in that: After ultrasonic atomization treatment of a thick proton exchange membrane, the proton exchange membrane is fixed by tension, and then catalyst slurry is coated on both sides of the proton exchange membrane under heating conditions and dried to form a catalytic layer on both sides of the proton exchange membrane; the thickness of the proton exchange membrane is 50 to 200 μm; The preparation method specifically comprises the following steps: S1 ultrasonic atomization treatment: ultrasonic atomization spraying treatment of the surface of the proton exchange membrane with water under heating conditions; S2: preparing an anode catalyst layer: preparing an anode catalyst slurry, fixing the proton exchange membrane treated in step S1 with a certain tension, applying the anode catalyst slurry on one side of the proton exchange membrane under heating, and drying to form an anode catalyst layer; S3: preparing a cathode catalyst layer: preparing a cathode catalyst slurry, fixing the proton exchange membrane treated in step S2 with a certain tension, applying the cathode catalyst slurry to the other side of the proton exchange membrane under heating, and drying to form a cathode catalyst layer, thereby obtaining the CCM for hydrogen production by water electrolysis; The order of step S2 and step S3 can be exchanged; in step S2 and step S3, the temperature of the heating condition is 70-90° C., and the tension is 0.01 MPa-0.05 MPa.

2. The method for preparing CCM for producing hydrogen by water electrolysis according to claim 1, characterized in that: In step S1, the heating temperature is 80-120°C.

3. The method for preparing CCM for producing hydrogen by water electrolysis according to claim 1, characterized in that: The proton exchange membrane is an enhanced or non-enhanced proton exchange membrane.

4. The method for preparing CCM for producing hydrogen by water electrolysis according to claim 1, characterized in that: In step S2, the method for preparing the anode catalyst slurry is to mix and evenly disperse the anode catalyst, resin solution, alcohol solvent and water; in step S3, the method for preparing the cathode catalyst slurry is to mix and evenly disperse the cathode catalyst, resin solution, alcohol solvent and water.

5. The method for preparing CCM for producing hydrogen by water electrolysis according to claim 4, characterized in that: The active component loading in the anode catalyst is 0.3-2.0 mg / cm 2 , the anode catalyst is at least one of the following: a. Ir, IrO2 or RuO2; b. supported IrO2, metal loading in terms of Ir, wherein the carrier is at least one of titanium oxide, tantalum pentoxide, tin dioxide or niobium oxide; c. oxides of Mn, Fe or Co; d. a perovskite metal oxide solid solution, wherein the perovskite metal oxide is A x A' 1-x B y B' 1-y O3, wherein A and A' are one of Sm, Ba, Sr, Co, La, Bi, Ce, A and A' are the same or different, B and B' are one of Co, Ni, Fe, B and B' are the same or different; and / or the noble metal loading in the cathode catalyst is 0.05-0.6 mg / cm 2 , the cathode catalyst is Pt / C.

6. The method for preparing CCM for producing hydrogen by water electrolysis according to claim 4, characterized in that: The weight ratio of the anode catalyst, resin solution, alcohol solvent and water is (7-9):(1-3):(3-54):(6-72), and / or the weight ratio of the cathode catalyst, resin solution, alcohol solvent and water is (2.5-6):(4-7.5):(6-54):(12-72).

7. A CCM for producing hydrogen by water electrolysis, characterized in that: The method is prepared by the CCM preparation method for producing hydrogen by water electrolysis as claimed in any one of claims 1 to 6.

8. A membrane electrode, characterized in that: The invention comprises an anode diffusion layer, a CCM for producing hydrogen by water electrolysis as claimed in claim 7 and a cathode diffusion layer which are stacked in sequence, wherein the anode diffusion layer is opposite to the anode catalyst layer, and the cathode diffusion layer is opposite to the cathode catalyst layer.

Citation Information

Patent Citations

  • Preparation technique for membrane electrode of proton exchange film fuel cell

    CN101276919A

  • Method for preparing membrane electrode of fuel batter with proton exchange film

    CN101355166A

  • Preparation method of proton exchange membrane fuel cell membrane electrode (CCM)

    CN106684413A

  • Preparation method of fuel cell membrane electrode

    CN110459774A

  • Medium-temperature proton exchange membrane fuel cell membrane electrode and preparation method thereof

    CN111490277A