Method for manufacturing semiconductor device

Through two etching processes and specific removal methods, the problem of metal particle sputtering in the through-silicon via process is solved, and the withstand voltage performance and test qualification rate of the semiconductor device are improved.

CN114284204BActive Publication Date: 2024-10-18WUHAN XINXIN SEMICON MFG CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202111466636.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-03
Publication Date
2024-10-18
Estimated Expiration
2041-12-03

AI Technical Summary

Technical Problem

In the through-silicon via process, metal particles in the lower wafer metal layer are easily sputtered to the sidewalls of the through-hole, affecting device performance. It is also difficult to effectively remove polymers with existing technology, resulting in failure of the voltage breakdown test.

Method used

A two-step etching process is used. The first etching is to expose the barrier layer and remove the first polymer, and then the second etching is to expose the metal layer at a lower bias power, using dilute hydrofluoric acid and Nitrofluoric acid wet removal removes polymers, combining nitrogen and hydrogen gases to loosen metal particles and reduce the degree of sputtering.

Benefits of technology

It effectively reduces metal particle sputtering and improves the withstand voltage performance of semiconductor devices and the pass rate of voltage breakdown tests.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114284204B_ABST
    Figure CN114284204B_ABST
Patent Text Reader

Abstract

The present invention provides a method for manufacturing a semiconductor device, comprising: providing a substrate, the substrate comprising a substrate and a dielectric layer, a metal layer and a barrier layer being embedded in the dielectric layer; forming an isolation layer; performing a first etching process, etching the isolation layer and the dielectric layer until the barrier layer is exposed, and a first polymer is formed on the sidewall and bottom of the through hole; removing the first polymer; performing a second etching process, etching the barrier layer until the metal layer is exposed. The present invention performs etching in two steps, and removes the first polymer between the two etching processes, thereby avoiding the first polymer and the second polymer generated by the second etching process from being combined together, thereby reducing the difficulty of removing the polymer; and since the second etching only needs to etch the barrier layer, a lower bias power can be used for etching, thereby reducing the degree of metal particle sputtering of the metal layer, improving the withstand voltage performance of the semiconductor device, and improving the pass rate of the voltage breakdown test item.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of integrated circuit manufacturing, and in particular relates to a method for manufacturing a semiconductor device. Background Art

[0002] TSV (Through Silicon Via) technology is a new technology that interconnects chips by creating vertical conductions between chips and between wafers. It can increase the stacking density in three dimensions.

[0003] After the upper wafer and the lower wafer are bonded, an etching process is used to form a through silicon via (TSV). The TSV penetrates the upper wafer and a portion of the thickness of the lower wafer dielectric layer until the metal layer (such as Cu) of the lower wafer is exposed. The interconnect layer is then filled in the TSV, and the interconnect layer is electrically connected to the metal layer of the lower wafer, thereby achieving electrical connection (interconnection) or electrical signal extraction between the bonded upper and lower wafers.

[0004] During the process of forming a TSV to expose the metal layer (eg, Cu) of the lower wafer, metal particles bombarded from the metal layer of the lower wafer are easily sputtered onto the sidewalls of the TSV, affecting the performance of the device composed of the upper wafer and the lower wafer. Summary of the invention

[0005] The purpose of the present invention is to provide a method for manufacturing a semiconductor device, which reduces the difficulty of removing a polymer, reduces the degree of sputtering of metal particles in a metal layer, improves the voltage resistance of the semiconductor device, and improves the pass rate of a voltage breakdown test item.

[0006] The present invention provides a method for manufacturing a semiconductor device, comprising:

[0007] Providing a substrate, the substrate comprising a substrate and a dielectric layer disposed on the substrate, wherein a metal layer is embedded in the dielectric layer and a barrier layer is located between the substrate and the dielectric layer;

[0008] A through hole is formed on a surface of the substrate above the metal layer and away from the dielectric layer, wherein the through hole at least penetrates the substrate and does not expose the barrier layer;

[0009] forming an isolation layer, wherein the isolation layer at least covers the side surface and the bottom surface of the through hole;

[0010] Performing a first etching process to etch the isolation layer and a portion of the dielectric layer between the bottom of the through hole and the barrier layer until the barrier layer is exposed, and a first polymer is formed on the sidewall and bottom of the through hole;

[0011] removing the first polymer;

[0012] A second etching process is performed to etch the barrier layer until the metal layer is exposed.

[0013] Furthermore, the first polymer contains at least C, F, O and Si elements.

[0014] Furthermore, the first polymer is removed by a diluted hydrofluoric acid wet method, and the ratio of the hydrofluoric acid to water is in the range of 1:100 to 1:200.

[0015] Furthermore, an inductively coupled plasma etching machine is used to perform the second etching process, and the bias power of the etching machine is less than 500W.

[0016] Furthermore, during the second etching process, a mixed gas of N2 and H2 is introduced into the etching machine to loosen the metal particles splashed by etching.

[0017] Furthermore, the flow rate of N2 is 100 sccm to 200 sccm, and the flow rate of H2 is 100 sccm to 200 sccm.

[0018] Furthermore, after performing the second etching process, a second polymer is formed on the sidewall and bottom of the through hole.

[0019] Furthermore, an ashing process is used to remove the second polymer, the ashing process comprises a mixed gas of CF4 and O2, the ashing process temperature range is 80°C to 100°C, and the ashing process power range is 250W to 450W.

[0020] Furthermore, the second polymer and the splashed metal particles are removed by a wet method.

[0021] Furthermore, the wet removal uses a mixed solution of sulfuric acid and hydrogen peroxide.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention provides a method for manufacturing a semiconductor device, comprising: providing a substrate, the substrate comprising a substrate and a dielectric layer arranged on the substrate, wherein a metal layer and a barrier layer located between the substrate and the dielectric layer are embedded in the dielectric layer; opening a through hole on a surface of the substrate above the metal layer away from the dielectric layer, wherein the through hole at least penetrates the substrate and does not expose the barrier layer; forming an isolation layer, wherein the isolation layer at least covers the side and bottom surfaces of the through hole; performing a first etching process, etching the isolation layer and a part of the dielectric layer located between the bottom of the through hole and the barrier layer until the barrier layer is exposed, and a first polymer is formed on the sidewall and bottom of the through hole; removing the first polymer; performing a second etching process, etching the barrier layer until the metal layer is exposed.

[0024] The present invention performs etching in two steps and removes the first polymer between the two etching processes, thereby preventing the first polymer from being combined with the second polymer (containing metal) generated by the second etching process, and reducing the difficulty of removing the polymer (containing metal) after the second etching; and because the second etching only needs to etch the barrier layer at the bottom of the through hole, a lower bias power can be used for etching, which greatly reduces the degree of sputtering (splashing) of metal particles in the metal layer, improves the voltage resistance performance of the semiconductor device, and improves the pass rate of the voltage breakdown test item in the wafer acceptability test. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The schematic cross-sectional view of a semiconductor device after an upper wafer isolation layer is formed.

[0026] Figure 2 The schematic diagram is a cross-sectional view of a semiconductor device after exposing the lower wafer metal layer.

[0027] Figure 3 The figure is a flow chart of a method for manufacturing a semiconductor device according to an embodiment of the present invention.

[0028] Figures 4 to 7 Schematic diagram of various steps of a method for forming a semiconductor device according to an embodiment of the present invention.

[0029] Figure 8 FIG. 4 is a schematic diagram of a substrate of a semiconductor device according to another embodiment of the present invention.

[0030] The reference numerals are as follows:

[0031] 10-lower wafer; 101-lower wafer substrate; 102-lower wafer dielectric layer; 103-lower wafer metal layer; 104-lower wafer barrier layer; 105-lower wafer bonding layer; 20-upper wafer; 201-upper wafer substrate; 202-upper wafer bonding layer; A-metal particles; 204-upper wafer isolation layer; 204a-silicon oxide layer; 204b-silicon nitride layer; 204c-silicon oxide layer.

[0032] 30 - first wafer; 301 - first substrate; 302 - first dielectric layer; 303 - first metal layer; 304 - first barrier layer; 305 - first bonding layer;

[0033] 40 - second wafer; 401 - second substrate; 402 - second bonding layer; 403 - second dielectric layer; 404 - isolation layer; 404a - silicon oxide layer; 404b - silicon nitride layer; 404c - silicon oxide layer.

[0034] 50-base; 501-substrate; 502-dielectric layer; 503-metal layer; 504-barrier layer; 505-isolation layer; 505a-silicon oxide layer; 505b-silicon nitride layer; 505c-silicon oxide layer. DETAILED DESCRIPTION

[0035] As described in the background art, after the upper wafer and the lower wafer are bonded, during the process of forming a through hole to expose the metal layer (such as Cu) of the lower wafer, metal particles in the metal layer are easily sputtered onto the side wall of the through hole, affecting the performance of the device formed by the upper wafer and the lower wafer.

[0036] Specifically, Figure 1 As shown, after the upper wafer 20 and the lower wafer 10 are bonded, an etching process is used to form a through hole V1, which passes through the upper wafer substrate 201, the upper wafer bonding layer 202, and a partial thickness of the lower wafer dielectric layer 102 until the lower wafer metal layer 103 (for example, Cu) is exposed. The lower wafer dielectric layer 102 is located on the lower wafer substrate 101, and the lower wafer metal layer 103 is embedded in the lower wafer dielectric layer 102. Then, an upper wafer isolation layer 204 is formed, and the upper wafer isolation layer 204 covers the side and bottom surfaces of the through hole V1. The upper wafer isolation layer 204 can be an ONO film layer structure, including a silicon oxide layer 204a, a silicon nitride layer 204b, and a silicon oxide layer 204c stacked in sequence.

[0037] Then, if Figure 2As shown, the film layer at the bottom of the through hole V1 is etched until the lower wafer metal layer 103 is exposed. Specifically, the upper wafer isolation layer 204, the upper wafer bonding layer 202, the lower wafer bonding layer 105 and the lower wafer dielectric layer 102 with a partial thickness and the lower wafer barrier layer 104 at the bottom of the through hole V1 are sequentially etched until the lower wafer metal layer 103 is exposed. The material of the upper wafer isolation layer 204 includes silicon oxide and / or silicon nitride. The materials of the upper wafer bonding layer 202, the lower wafer bonding layer 105 and the lower wafer dielectric layer 102 with a partial thickness can all include silicon oxide and / or silicon nitride.

[0038] The inventors have discovered that, in the step of etching the film layer at the bottom of the through hole V1 to expose the lower wafer metal layer 103, a first polymer formed by etching the silicon oxide and / or silicon nitride at the bottom (directly below) of the through hole V1 combines with a second polymer produced by etching the lower wafer barrier layer (e.g., tantalum nitride) 104 and the lower wafer metal layer (e.g., Cu) 103 to form a metal compound-containing deposit that is very difficult to remove (clean), and the metal-containing deposit adheres to the side wall surface and then the bottom surface of the through hole V1.

[0039] Due to the high aspect ratio of the through hole V1, the etching process for forming the through hole V1 requires a higher bias power (for example, 1000W~1500W). Under higher bias power, more metal particles in the lower wafer metal layer 103 will be sputtered onto the side wall of the through hole V1 without being cleaned. The material of the lower wafer metal layer 103 is mostly Cu, but because Cu has a very high electron mobility, it is very active. The metal particles (for example, Cu particles) A ​​sputtered onto the side wall of the through hole V1 can easily gradually penetrate into the various layers of the structure penetrated by the through hole in the later process, resulting in a decrease in the withstand voltage of the device composed of the upper wafer 20 and the lower wafer 10, and the failure of the voltage breakdown (VBD, Voltage BreakDown) test in the wafer acceptability test (WAT, Wafer Accept Test).

[0040] Based on the above research, an embodiment of the present invention provides a method for manufacturing a semiconductor device. The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. According to the following description, the advantages and features of the present invention will become clearer. It should be noted that the drawings are all in a very simplified form and use an inaccurate scale, which is only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.

[0041] It should be noted that when two wafers are stacked, there is always one wafer at the top and one wafer at the bottom, but the present invention does not limit which wafer of the first wafer and the second wafer must be placed at the top / bottom, but the positions of the upper and lower wafers can be interchanged. In this article, for the sake of simplicity and convenience, only one position relationship of the two wafers is shown, and those skilled in the art can understand that all technical contents described in this article are also applicable to the situation where the positions of the "first wafer" and the "second wafer" are reversed, and the position relationship of the layers of the stacked semiconductor device is also reversed accordingly.

[0042] The embodiment of the present invention provides a method for manufacturing a semiconductor device, such as Figure 3 As shown, including:

[0043] S1. Provide a substrate, wherein the substrate comprises a substrate and a dielectric layer disposed on the substrate, wherein a metal layer is embedded in the dielectric layer and a barrier layer is located between the substrate and the dielectric layer;

[0044] S2, opening a through hole on a surface of the substrate above the metal layer away from the dielectric layer, wherein the through hole at least penetrates the substrate and does not expose the barrier layer;

[0045] S3, forming an isolation layer, wherein the isolation layer at least covers the side surface and the bottom surface of the through hole;

[0046] S4, performing a first etching process to etch the isolation layer and a portion of the dielectric layer between the bottom of the through hole and the barrier layer until the barrier layer is exposed, and a first polymer is formed on the sidewall and the bottom of the through hole;

[0047] S5, removing the first polymer;

[0048] S6. Perform a second etching process to etch the barrier layer until the metal layer is exposed.

[0049] Combine the following Figures 4 to 7 The steps of a method for manufacturing a semiconductor device according to an embodiment of the present invention are introduced.

[0050] like Figure 4 As shown, in step S1, a base 50 is provided, and the base 50 includes a substrate 501 and a dielectric layer 502 arranged on the substrate 501, a metal layer 503 is embedded in the dielectric layer 502, and a barrier layer 504 is located between the substrate 501 and the dielectric layer 502. In this embodiment, the barrier layer 504 covers the metal layer 503.

[0051] like Figure 8As shown, the base 50 may be a second wafer 40 and a first wafer 30 bonded up and down, the second wafer 40 includes a second substrate 401 and a second bonding layer 402 arranged on one side of the second substrate 401, and the second substrate 401 is further provided with a second dielectric layer 403 on a side away from the second bonding layer 402, and the second dielectric layer 403 is, for example, a high dielectric constant (HK) material layer. The first wafer 30 includes a first substrate 301 and a first dielectric layer 302 disposed on one side of the first substrate 301. A first metal layer 303 and a first barrier layer 304 located between the second substrate 401 and the first dielectric layer 302 are embedded in the first dielectric layer 302. The first barrier layer 304 can cover the first metal layer 303. The first barrier layer 304 is, for example, a tantalum nitride (TaN) layer or a tantalum (Ta) layer, or a stacked layer composed of a tantalum nitride (TaN) layer and a tantalum (Ta) layer. The thickness of the first barrier layer 304 is, for example, 15 angstroms to 60 angstroms. A first bonding layer 305 is also disposed on one side of the first dielectric layer 302 away from the first substrate 301. The second wafer 40 and the first wafer 30 are bonded to each other through the second bonding layer 402 facing the first bonding layer 305. After the two wafers are bonded, the first wafer 30 and / or the second wafer 40 can be thinned as needed.

[0052] Continue as Figure 4 As shown, in step S2 , a through hole V3 is opened on a surface of the substrate 501 above the metal layer 503 away from the dielectric layer 502 , and the through hole V3 at least penetrates the substrate 501 and does not expose the barrier layer 504 .

[0053] In step S3, an isolation layer 505 is formed, and the isolation layer 505 at least covers the side and bottom surfaces of the through hole V3, and may also cover the upper surface of the substrate 501. Exemplarily, the isolation layer 505 includes an ONO film layer structure of a silicon oxide layer 505a, a silicon nitride layer 505b and a silicon oxide layer 505c stacked in sequence.

[0054] like Figure 5As shown, in step S4, the first etching process is performed to etch the isolation layer 505 and the dielectric layer 502 with a partial thickness between the bottom of the through hole and the barrier layer 504 until the barrier layer 504 is exposed, and the sidewall and bottom of the through hole are formed with a first polymer. In this etching step, the outermost silicon oxide layer 505c located on the sidewall of the through hole V3 is etched and lost to a certain extent. The main etching gas used in etching is usually carbon tetrafluoride (CF4), in which the role of fluorine is to react with silicon dioxide or silicon nitride to produce volatile products; the role of carbon is to provide a source of polymers to inhibit the progress of etching, and the generated polymer attached to the sidewall of the through hole V3 can serve as a protective layer to inhibit the influence of isotropic etching. After the first etching process is completed, a certain amount of the first polymer will remain on the sidewall and bottom of the through hole V3, and more first polymer particles B will gather at the bottom of the through hole V3. The remaining polymer is a by-product generated by the first etching process, and the first polymer contains at least C, F, O and Si elements.

[0055] like Figure 6 As shown, in step S5, the first polymer is removed by a diluted hydrofluoric acid wet method, wherein the ratio of the hydrofluoric acid to water is in the range of 1:100 to 1:200.

[0056] like Figure 7 As shown, in step S6, a second etching process is performed to etch the barrier layer 504 until the metal layer 503 is exposed. The second etching process can be performed by using an inductively coupled plasma (ICP) etching machine, and the bias power of the etching machine is less than 500W. The first etching has removed the film structure between the bottom surface of the through hole V3 and the barrier layer 504. The second etching process only needs to etch the barrier layer 504 at the bottom (directly below) of the through hole V3. Therefore, a lower bias power can be used for etching to reduce the degree of metal particle sputtering (splashing) when the metal layer 503 is exposed in the second etching process.

[0057] During the second etching process, a mixed gas of N2 and H2 is introduced into the etching machine to loosen the metal particles splashed by etching. N2 and H2 are used to loosen the sputtered (splashed) metal particles (such as Cu particles or Al particles) so that they can be wet-cleaned more easily later. If the metal particles are wrapped in the first polymer containing C, F, O and Si elements, it is difficult to remove them. Through step S5, the first polymer containing C, F, O and Si elements is removed to prevent the metal particles from being wrapped in the first polymer containing C, F, O and Si elements. The flow rate of N2 is 100sccm~200sccm, and the flow rate of H2 is 100sccm~200sccm. After the second etching process is performed, a second polymer is formed on the sidewalls and bottom of the through hole.

[0058] In one example, the etching gas for the second etching process may be a mixed gas of C4F8, CO and Ar; in another example, the etching gas for the second etching process may be a mixed gas of C4F8, H2 and Ar. During the second etching process, due to the bombardment of plasma in the etching machine, more second polymers are generated, and these second polymers are accumulated around the bottom and sidewalls of the through hole V3.

[0059] In this embodiment, the barrier layer 504 is, for example, a tantalum nitride (TaN) layer or a tantalum (Ta) layer, or may be a stack of a tantalum nitride (TaN) layer and a tantalum (Ta) layer, and the second polymer contains at least Ta, C and O elements.

[0060] In one example, the second polymer can be removed by an ashing process, the ashing process includes a mixed gas of CF4 and O2, the ashing process temperature range is 80°C~100°C, and the ashing process power range is 250W~450W. The loosened metal particles may be wrapped in the second polymer, or attached to the surface of the second polymer, or attached to the surface of the through hole V3. The second polymer and the splashed metal particles can also be removed by a wet method. The wet removal uses a mixed solution of sulfuric acid and hydrogen peroxide. After cleaning the second polymer, an interconnection layer can be formed in the through hole V3, and the interconnection layer fills the through hole V3 and is electrically connected to the metal layer 503. Figures 4 to 7 In the method for manufacturing a semiconductor device of the embodiment described, the through hole eventually exposes the metal layer 503, and the metal layer 503 (electrical signal) on one side (e.g., the lower side) of the substrate 501 in the thickness direction is led out to the other side (e.g., the upper side) in the thickness direction through the interconnection layer filled in the through hole.

[0061] It should be understood that the substrate and the dielectric layer (the dielectric layer having a metal layer and a barrier layer embedded therein) in the present invention may be located in the same wafer; the substrate and the dielectric layer (the dielectric layer having a metal layer and a barrier layer embedded therein) may also be located in different wafers respectively, and the wafer where the substrate is located and the wafer where the dielectric layer (the dielectric layer having a metal layer and a barrier layer embedded therein) are located (for example, by bonding) form a stacked structure.

[0062] It should be understood that, in this article, the numbers such as "first" and "second" are only used to distinguish different components or processes with the same name, and do not mean order or position relationship, etc. In addition, for different components with the same name, such as "first substrate" and "second substrate", "first dielectric layer" and "second dielectric layer", etc., it does not mean that they all have the same structure or components. For example, although not shown in the figure, in most cases, the components formed in the "first substrate" and the "second substrate" are different, and the structure of the substrate may also be different. In some embodiments, the substrate can be a semiconductor substrate, made of any semiconductor material suitable for semiconductor devices (such as Si, SiC, SiGe, etc.). In other embodiments, the substrate can also be various composite substrates such as silicon on insulator (SOI), silicon germanium on insulator, etc. It is understood by those skilled in the art that the substrate is not subject to any restrictions, but can be selected according to actual applications. Various device (not limited to semiconductor devices) components can be formed in the substrate (not shown in the figure). The substrate can also have other layers or components formed, such as: gate structure, contact hole, dielectric layer, metal connection and through hole, etc.

[0063] Figure 1 and Figure 2 In the method for manufacturing the semiconductor device shown, the polymer formed by etching silicon oxide and silicon nitride at the bottom of the through hole V1 and the polymer generated by etching the lower wafer metal layer 103 (eg, Cu) combine to form a metal compound-containing deposit that is very difficult to remove.

[0064] In the method for manufacturing the semiconductor device of this embodiment, etching is performed stepwise in two steps, and a step of removing the first polymer is added in the two etching processes to remove the first polymer (byproduct) generated by the first etching, and the second etching can be etched with a lower bias power, thereby reducing the degree of metal particle sputtering (splashing) of the metal layer 503. Specifically, the first etching process is performed to etch the isolation layer 505 located between the bottom of the through hole V3 and the barrier layer 504; the second etching process is performed to etch the barrier layer 504 located at the bottom (directly below) of the through hole V3 until the metal layer 503 is exposed; between the two etching processes, a step of removing the first polymer is added to first remove the first polymer accumulated in the through hole V3 after the first etching, that is, first remove the first polymer containing C, F, O and Si elements, so as to avoid the first polymer generated by the first etching process and the second polymer (containing metal) generated by the second etching process from being combined together, thereby reducing the difficulty of removing the polymer (containing metal). The etching process is carried out in two steps. The second etching process only needs to etch the barrier layer 504 at the bottom (directly below) of the through hole V3, so a lower bias power can be used for etching, which reduces the degree of metal particle sputtering (splashing) of the metal layer 503. In the absence of the first polymer containing C, F, O and Si elements (removed), nitrogen and hydrogen are used to make the sputtered (splashed) metal particles loose and easier to be wet-cleaned. The second polymer generated by etching the barrier layer 504 and the metal layer 503 is not combined with the first polymer generated by the first etching process, and the second polymer is also easier to be wet-cleaned.

[0065] The second etching process is performed to expose the metal layer 503. After removing the second polymer, an interconnection layer can be formed in the through hole V3, and the interconnection layer fills the through hole V3 and covers the isolation layer 505. Then, a chemical mechanical polishing process is performed to remove the interconnection layer on the surface of the isolation layer 505. The interconnection layer is electrically connected to the metal layer 503 through the through hole V3. The interconnection layer is a conductive material, which can be copper or a copper alloy, such as filling the through hole V3 by electroplating copper.

[0066] In summary, the present invention provides a method for manufacturing a semiconductor device, comprising: providing a substrate, the substrate comprising a substrate and a dielectric layer arranged on the substrate, a metal layer and a barrier layer located between the substrate and the dielectric layer being embedded in the dielectric layer; opening a through hole on a surface of the substrate above the metal layer away from the dielectric layer, the through hole at least passing through the substrate without exposing the barrier layer; forming an isolation layer, the isolation layer at least covering the side and bottom surfaces of the through hole; performing a first etching process, etching the isolation layer and a partial thickness of the dielectric layer between the bottom of the through hole and the barrier layer until the barrier layer is exposed, a first polymer being formed on the sidewalls and the bottom of the through hole; removing the first polymer; performing a second etching process, etching the barrier layer until the metal layer is exposed.

[0067] The present invention performs etching in two steps and removes the first polymer between the two etching processes, thereby preventing the first polymer from being combined with the second polymer (containing metal) generated by the second etching process, and reducing the difficulty of removing the polymer (containing metal) after the second etching; and because the second etching only needs to etch the first barrier layer at the bottom of the through hole, a lower bias power can be used for etching, which greatly reduces the degree of sputtering (splashing) of metal particles in the first metal layer, improves the voltage resistance performance of the semiconductor device, and improves the pass rate of the voltage breakdown test item in the wafer acceptability test.

[0068] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the method disclosed in the embodiment, since it corresponds to the device disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part description.

[0069] The above description is only a description of the preferred embodiment of the present invention, and is not any limitation on the scope of rights of the present invention. Any technical personnel in this field can make possible changes and modifications to the technical solution of the present invention by using the methods and technical contents disclosed above without departing from the spirit and scope of the present invention. Therefore, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the protection scope of the technical solution of the present invention.

Claims

1. A method for manufacturing a semiconductor device, characterized in that: include: Providing a substrate, the substrate comprising a substrate and a dielectric layer disposed on the substrate, wherein a metal layer is embedded in the dielectric layer and a barrier layer is located between the substrate and the dielectric layer; A through hole is formed on a surface of the substrate above the metal layer and away from the dielectric layer, wherein the through hole at least penetrates the substrate and does not expose the barrier layer; forming an isolation layer, wherein the isolation layer at least covers the side surface and the bottom surface of the through hole; Performing a first etching process to etch the isolation layer and a portion of the dielectric layer between the bottom of the through hole and the barrier layer until the barrier layer is exposed, and a first polymer is formed on the sidewall and bottom of the through hole; removing the first polymer; A second etching process is performed to etch the barrier layer until the metal layer is exposed.

2. The method for manufacturing a semiconductor device according to claim 1, wherein: The first polymer contains at least C, F, O and Si elements.

3. The method for manufacturing a semiconductor device according to claim 2, wherein: The first polymer is removed by a diluted hydrofluoric acid wet method, wherein the ratio of the hydrofluoric acid to water is in the range of 1:100 to 1:

200.

4. The method for manufacturing a semiconductor device according to claim 1, wherein: The second etching process is performed using an inductively coupled plasma etching machine, and the bias power of the etching machine is less than 500W.

5. The method for manufacturing a semiconductor device according to claim 4, wherein: During the second etching process, a mixed gas of N2 and H2 is introduced into the etching machine to loosen the metal particles splashed by etching.

6. The method for manufacturing a semiconductor device according to claim 5, wherein: The flow rate of the N2 is 100 sccm to 200 sccm, and the flow rate of the H2 is 100 sccm to 200 sccm.

7. The method for manufacturing a semiconductor device according to claim 5, wherein: After the second etching process is performed, a second polymer is formed on the sidewall and bottom of the through hole.

8. The method for manufacturing a semiconductor device according to claim 7, wherein: The second polymer is removed by an ashing process, wherein the ashing process includes a mixed gas of CF4 and O2, the ashing process temperature ranges from 80°C to 100°C, and the ashing process power ranges from 250W to 450W.

9. The method for manufacturing a semiconductor device according to claim 7, wherein: The second polymer and the splashed metal particles are removed by a wet method.

10. The method for manufacturing a semiconductor device according to claim 9, wherein: The wet removal adopts a mixed solution of sulfuric acid and hydrogen peroxide.

Citation Information

Patent Citations

  • Through silicon via package structure and forming method

    CN103545275A

  • Contact hole etching method

    CN104701242A