Method for producing a casting mold and a casting mold produced using the method

By decomposing the casting mold into multiple laminates and assembling it into stacks, the problems of high production costs and long time in the prior art are solved, and low-cost and high-efficiency casting mold manufacturing is realized, which is suitable for a variety of casting processes .

CN114286727BInactive Publication Date: 2024-11-15FRAUNHOFER GESELLSCHAFT ZUR FORDERUNG DER ANGEWANDTEN FORSCHUNG EV
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202080045643.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-06-21
Filing Date
2020-06-19
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art has high cost and long production time when producing complex casting molds, making it difficult to achieve simple and low-cost casting mold manufacturing.

Method used

The decomposed casting mold model is used to form multiple laminates, and they are separately produced and assembled into stacks through different methods to form a complex casting structure, including the use of alignment bodies, magnetic bonding, welding and other connection methods.

Benefits of technology

It realizes the production of complex casting molds in a short time and economical manner, suitable for large and small components, reduces production costs, and improves the flexibility and efficiency of the casting process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114286727B_ABST
    Figure CN114286727B_ABST
Patent Text Reader

Abstract

The invention relates to a method for producing a casting mold (201, 204), according to which at least three, in particular at least four, five, more than five or more than ten sandwich elements (300, 301, 302, 400, 401) of the casting mold are first produced separately from each other and then combined into one or more stacks (1100) to form the casting mold.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The invention belongs to the field of mechanics, mechanical engineering and casting technology. The invention can be used particularly advantageously for the production of casting molds, the use of which in large casting molds (for example in the construction of houses, parts of houses or other large parts) is just as conceivable as in casting molds for small parts. Furthermore, the casting molds produced can be used for casting processes for a large number of different casting materials.

[0002] Basically, so-called lost molds and permanent molds with and without cores are referred to as casting molds for producing castings. Based on the stripping molding process (which is based on the destruction of the mold), the lost mold can be used to produce particularly complex casting products. The internal structure of the casting mold can be realized using a core that defines the cavity during the casting process, and the internal structure of the casting mold can be destroyed and removed using various methods after the casting material solidifies. The corresponding casting molds and cores can be produced using, for example, a sand casting molding process (in which sand is mixed with a binder and shaped with the help of a tool).

[0003] It is also known that casting molds can be produced using additive manufacturing processes, which in a layered structure allow the molding of complex bodies with great design freedom. In this process, particles are applied in layers to a platform and selectively solidified, for example, by targeted addition of binder materials or by laser sintering. Disadvantages of this method for producing casting molds are high costs and long production times.

[0004] Against the background of the prior art, the object of the present invention is to develop a method for producing a casting mold and a casting mold which is as simple, labor-saving and cost-effective as possible in structure, thereby making it possible to produce complex casting molds.

[0005] This object is achieved by a method for producing a casting mold having the features of claim 1. Claims 2 to 14 show embodiments of this method. Claim 15 relates to a casting mold produced according to this method.

[0006] Accordingly, the invention relates to a method for producing a casting mold, wherein at least three, in particular at least four, five, more than five or more than ten laminates of the casting mold are first produced separately from one another and then joined together to form one or more stacks to form the casting mold.

[0007] The method described above also enables the production of complex casting moulds which may consist of layered laminates, the individual laminates being able to be produced without difficulty in different ways.

[0008] The model of the casting mold can therefore first be broken down into layers, and the laminates forming the individual layers can be produced individually and separately from one another. The laminates are then assembled so that the cavities of each of the individual laminates share an interior, i.e., a cavity defining the mold to be filled with casting material. By dividing the casting mold into a plurality of laminates, complex casting molds can also be assembled from laminates, each having a cavity or opening of a simple design.

[0009] The individual laminates are joined together to form a stack to form a casting mold. The stacking direction is the direction in which the stack grows by adding more laminates. The direction perpendicular to the boundary surfaces between the individual laminates joined together can also be referred to as the stacking direction.

[0010] The casting mould can be assembled from a single stack of individual laminates, but multiple stacks of individual laminates can also be cast or connected into a casting mould, wherein different stacks can be arranged, for example, adjacent to each other, one behind the other, one on top of the other, or a stack can also be arranged in the cavity of another stack.

[0011] One embodiment of the present invention can be provided as follows: after being assembled into a casting mold, a plurality of laminates, in particular each laminate except the end laminates of the stack, each surrounds the cavity of the casting mold to be filled with the casting material in an annular manner. For example, a casting mold for a ball can be assembled from a plurality of laminates so that the outer contour of the casting mold is designed to be in the shape of a cube, and each layer of the cube has a circular through groove and a groove that jointly defines a spherical cavity after the casting mold is assembled. In each laminate, the circular groove is surrounded by an annular wall and a straight boundary wall on the outside, and the annular wall has an approximately cylindrical profile inside it. The end laminates of the stack that define the mold do not have through holes, but only have dome-shaped depressions that define the spherical cavity.

[0012] Another possible embodiment of the method can be arranged that: a plurality of laminates, in particular each laminate, except for the end laminates of the stack, each has / has at least one opening, the opening completely penetrates the laminate and is surrounded by a circumferential laminate wall. Depending on the shape of the individual laminates and the shape of the cavity for actual casting, the laminate wall has a thickness that varies along the circumferential direction. For example, the laminate can be in the form of a cuboid or a flat plate or a curved plate, and the plate can be designed, for example, as a circle, square, rectangular or polygon.

[0013] The method can also be designed so that the laminates are aligned when they are joined together to form a stack on a common alignment body or by interlocking protrusions and grooves provided on each of the laminates. This design of the laminates and optionally of the alignment body can ensure that the laminates and their grooves are positioned relative to each other so that the grooves as a whole define the casting mold, that is, define the mold cavity to be filled with the casting material.

[0014] The alignment body can be formed, for example, by a straight rod or a plate, on which the outer contour of the laminate is arranged. The laminate can also have, for example, a through hole, through which the alignment body can be inserted. The ridges and grooves on the laminate can be designed, for example, as grooves and ribs or holes and pegs, in order to align adjacent laminates with each other.

[0015] Another embodiment of the method can be arranged that when the laminates are joined together to form a stack, the laminates are connected to each other on adjacent boundary surfaces and the laminates have the same layer thickness or different layer thicknesses in the stacking direction. Since the laminates are produced separately from each other, they must be connected to each other after production, unlike known additive production processes. In some cases, a form-fit connection with an alignment body is sufficient, while in other cases, the laminates are glued or welded to each other. Magnetic bonding or other known joining techniques between the laminates are also conceivable. Finally, the laminates can also be clamped to each other by springs or clamps so as to be connected to each other in this way in a force-locking manner.

[0016] The laminates can each have the same thickness, which is advantageous for mass production of laminates. However, it may also be useful to process different laminates or groups of laminates with different layer thicknesses in a stack within a mold, so as to set the correct size of the mold or mold parts in this way. For example, it is useful to form certain parts of the mold with as few laminates as possible, while other parts / parts of the mold are composed of a large number of laminates with smaller layer thicknesses. This may be the case, for example, if the size of the mold in the stacking direction varies greatly in some parts, but varies little in other parts.

[0017] For example, the method can also provide that the laminates are connected to one another when they are joined together by gluing, welding or by a force-fitting or form-fitting connection.

[0018] It can also be provided that the laminate is produced by an extrusion process, a rolling process, a casting process, a core shot process or an additive manufacturing process.

[0019] For example, it may be provided that the laminate is produced as a solid body and then a groove penetrating the laminate is formed in a plurality of laminates, in particular in each laminate.

[0020] In principle, all machinable materials can be considered as materials for the laminate. For example, the laminate can be produced from plastic, metal or also from bonded sand materials, as is customary for producing lost casting molds. Depending on the materials used, the machining methods used are suitable for producing recesses in the laminate, which then each form part of a mold / cavity for casting the material.

[0021] For this purpose, it can be provided, for example, that grooves penetrating the laminate are formed in the laminate by a subtractive process, in particular by a cutting process, punching, laser cutting, water jet cutting or by a chemical process. In addition to sawing, for example milling can also be used as a processing method. Processing by drilling, grinding, planing, flame cutting, compressed air jets, sandblasting or etching is also possible. If the bonding forces of the laminate particles are appropriately adjusted, parts of the laminate can also be removed by negative pressure / suction. When magnetic particles are used as the base material for the laminate, targeted demagnetization can at least promote the subtractive processing process.

[0022] With regard to the shape of the laminate and / or the laminate stack, it can be provided that the laminate is designed in the form of a disc or a plane-parallel plate.

[0023] It can also be provided that the surfaces of the laminates of stacks of adjacent laminates are coplanar.

[0024] The maximum angle that two mutually opposing boundary surfaces of a laminate form with one another should be limited and less than 30°, in particular less than 10°, more particularly less than 1°, so that the stacking direction or the alignment of the individual laminates over the height of the stack does not vary too much and the joining of the laminates can be achieved in a simple manner. In some constellations, it may be advantageous to provide a plurality of wedge-shaped laminates which follow one another in the stack with opposite wedge directions or alternating wedge directions.

[0025] The method can also be arranged such that each laminate has no undercuts in the stacking direction. In this way, the production of the individual laminates is facilitated, since, for example, the laminate can be processed in a simple manner from one side. If undercuts are to be provided in the cavity of the casting mold in the stacking direction, these can be realized at least partially by the interfaces of the laminates.

[0026] In the method, it can be provided, for example, that the laminates are designed and joined together such that in the stacking direction at least one undercut is provided in the cavity of the casting mold to be filled with casting material and is formed by the interface of the laminates.

[0027] In addition to the method steps directly used to produce laminates and casting molds, the method can also include a planning step, which is based on the model of the casting mold and the model is temporarily divided into one or more stacks of laminates in multiple stacking directions. The stacking direction and the layer thickness of the laminate can be selected according to a variety of optimization criteria. For example, the number of laminates in the casting mold can be minimized, or the unevenness caused by the interface between the laminates in the casting mold can be minimized. The undercut position in the casting mold can also be optimized in this way.

[0028] It can be provided, for example, that the model of the casting mold is divided into layers in succession according to different stacking directions and that the stacking direction with the least number of undercuts is selected, in particular the layer thickness of the laminate is divided so that all undercuts at the interface are located between every two layers. If it is not reasonable or impossible to locate all undercuts at the interface between two different laminates, the goal can at least be to locate as many undercuts as possible at the interface so that undercuts only need to be produced in a few laminates.

[0029] Finally, the invention relates not only to a method for producing a casting mould, but also to a casting mould produced using this method.

[0030] In the following, the invention is shown based on an embodiment in the drawings and explained below. It is shown:

[0031] Figure 1 It is a three-dimensional image of the casting;

[0032] Figure 2 is a schematic diagram showing the Figure 1 A cross-sectional view of a casting mold of a casting component;

[0033] Figure 3 is similar to Figure 2 The casting mold shown is a cross-sectional view of a casting mold formed by stacking a plurality of laminates;

[0034] Figure 4 is a cross-sectional view of a casting mold formed from a laminate having variable layer thickness;

[0035] Figure 5 is a laminate having two recesses, each of which forms a part of a cavity to be filled with casting material after the casting mould is assembled;

[0036] Figure 6 a) is a cross-sectional view of a laminate, schematically showing a groove to be made therein;

[0037] Figure 6 b) is a cross-sectional view of the laminate, in which the milling cutter is schematically shown in the direction of the milling axis perpendicular to the boundary surface of the laminate;

[0038] Figure 6 c) in the figure shows Figure 6 b) with an inclined milling cutter;

[0039] Figure 6 d) in the figure shows Figure 6 c) in which two milling cutters are shown, which produce grooves in the laminate in a stepped manner from both sides without an inclined position;

[0040] Figure 7 a) is a diagram of producing a laminate by a rolling process;

[0041] Figure 7 b) Figure 7 c) is a diagram of producing a laminate in a pressing or core shooting process;

[0042] Figure 8 It is a diagram of the different layers being joined and pressed together;

[0043] Fig. 9 is a diagram of a casting process in which the laminate stack is held together by weight;

[0044] Fig.10 is a diagram of a casting process in which the laminates of the stack are clamped together;

[0045] Fig.11 is a diagram of a casting mold consisting of different stacks of various laminates;

[0046] Fig.12 is similar to Figure 3 A view of the casting mold shown, but with the stacking direction of the laminate rotated 90°;

[0047] Fig.13 is a cross-sectional view of a laminate stack having a plurality of wedge-shaped laminates;

[0048] Fig.14 is a cross-sectional view of a laminate stack having grooves for alignment bodies;

[0049] Fig.15 is a perspective view of a laminate having ridges for interlocking with adjacent laminates.

[0050] In the following, various methods for producing molds for components produced by casting are described using a layer-by-layer build-up process, in which a layer is prepared in each case in the form of a laminate, into which a cavity is introduced according to the casting cross section, and the individual laminates produced in this way are stacked until the desired shape is completely stacked. This provides a casting mold building process that is also possible without tools and enables the economical production of larger series of components.

[0051] exist Figure 1 A typical component 100 that can be produced as a casting is depicted in a perspective view. The casting molds produced by the method are suitable for small components with a volume of several liters as well as for large components. The casting material is not limited and can be from metals, ceramics, polymers, natural substances and mixtures thereof.

[0052] The component 100 produced by molding by means of the method according to the invention corresponds in one embodiment to the unprocessed green casting known in the prior art. In this case, they represent an intermediate state and usually have to be completed by further processing steps, such as milling or grinding on the functional surface.

[0053] The object of the present invention is to provide a method for producing a mold which makes it possible to produce a cast component 100 in a short time, in particular without tools, economically and with few restrictions in terms of shaping.

[0054] The casting mold produced by the method according to the invention can be widely used in the industrial field. The application range ranges from the casting of large individual parts to large-scale production in the automotive industry.

[0055] Metals can be poured in liquid form, as can materials such as plastics, concrete or ceramic slurries.

[0056] Casting processes can be very different: The pressure can be caused by the weight of the melt, as in gravity casting. However, there are also processes in use that facilitate mold filling by significantly increased pressure. This is the case, for example, with die casting when particularly thin wall thicknesses are to be achieved.

[0057] In all casting processes, it is important to use tools in the form of molds, such as Figure 2 as shown in the example. Figure 2 The casting mold shown can be used to produce, for example Figure 1The casting mold including molds 201, 204 (outer contour) and core 202 can be used for single use (lost foam) or multiple castings (permanent mold). In addition to the mold cavity 200, a cavity for accommodating the casting material, a pouring basin and a pouring system 203 must also be provided in the casting mold.

[0058] The method according to the invention is a layered construction method which provides a casting mold 201, 204 and optionally one or more cores for a casting method. Figure 3 As shown, each laminate 300 is prepared separately and stacked one on top of another. In one embodiment, the method according to the present invention has the following steps:

[0059] In a first step, the cast component 100 to be produced is virtually placed in the installation space. In doing so, the construction position that can be optimally mapped using the method is determined. The component 100 is then temporarily divided into possible laminates 300 by the program, and a processing image is generated for each laminate 300 according to the layer generation mechanism and the stacking direction. The calculation method used minimizes the generation of artifacts through digitalization and reduces their influence on the desired mold shape. The stacking direction corresponds to the direction in which the laminates are arranged one above the other. The stacking direction can also be defined as the direction perpendicular to the interface between the laminates, or, for example, if some wedge-shaped laminates are provided, the average direction of all perpendicular lines on the interface between adjacent laminates.

[0060] After the mold is divided, laminates 300 are produced. These laminates are closed plates made of molding material that is compatible with the planned casting material. The result of this process step is a compressed plate of molding material.

[0061] These compressed sheets are processed in a further step and the contour of the component at the corresponding cutting height is introduced in the form of a groove into the corresponding laminate at which the corresponding laminate is positioned in the mold. This can be done in Figure 5 Clearly seen in.

[0062] The casting mold 201 , 204 is now completed by stacking and connecting the individual laminates and can be used in a conventional casting process.

[0063] The starting point of the method according to the invention is a component 100 having a casting structure that can be used for a casting process. This structure generally provides a gating system, air channels, a feeder and a system for pouring liquids. According to the prior art, such a system is determined and tested by simulation before the production of the mold 201, 204.

[0064] In the method according to the invention, this virtual structure is analyzed in an automated way in a data processing device and tested in simulation. This takes into account the following characteristics of the method: during subsequent use, the layers are not produced where they are to be placed, as in conventional 3D printing processes, but are prepared as laminates outside the actual installation space of the machine and then transferred to the installation space. The algorithm optimizes the individual layers so that no loose layer parts occur. Secondly, the algorithm can prioritize certain construction locations that reduce delamination in the relevant area.

[0065] This optimization cannot occur based solely on the rotation of the stacking direction relative to the component 100. Figure 4 As shown, different layer thicknesses can also be used in the stack, i.e., laminates of different heights can be used. In this way, areas requiring high resolution due to strong curvatures of the mold can be imaged with thin laminates 300, 400, 401, for example. The program can also make recommendations to the user, which reflect the trade-offs between production time, component quality, and resource consumption.

[0066] In component 100, as Fig.11 As shown, the digital generation of layers can produce multiple areas with different stacking directions. These areas can be in the shape of cubes or spatulas. The stack 1100 itself can have different stacking directions to reduce the negative impact of the stacking direction on the surface of the part to be cast. The stacking direction of the internal stack 1100 is Fig.11 The inner portion is indicated by 1100a, and the stacking direction of the outer stacking body is indicated by 300a.

[0067] The laminate 300, 400, 401 itself must be transportable in order to be relocated to the installation space. In the known molding materials for various casting processes, layers thicker than 1 mm can be considered for this in many cases. The thickness of the layer has no upper limit and is actually only set by the layer processing method.

[0068] The method is based on laminates made of shaped materials. The laminates can be produced in advance for the method, but they can also be produced individually on a production line by the method steps required for the method. The layer generation can be carried out in a highly parallel and highly automated manner, thus achieving a high throughput.

[0069] The material of the laminate depends on the desired casting process: for example, sawdust is a simple material and a cheap waste material. Sawdust can be used in forms 201 for processes with low heat build-up. Other materials, such as plastic waste, straw, paper scraps or wood chips, can also be considered for such applications. If higher requirements are placed on the molding material, other materials can be used; for example, metal powder or metal granules can be used as molding material. Depending on the casting material, each has advantages and disadvantages. When temperature influences are strong, such as in iron and steel casting, molding sand, ceramic sand and special molding materials are used. Graphite can also be used for materials with a high melting point.

[0070] The shape of the particles can vary from a free particle distribution to geometrically defined particles. One extreme is a natural bed in a molding material layer, which consists of a mixture of particles with a specific particle size distribution. The other extreme is a laminate of puzzle-like elements that can be connected to each other.

[0071] The individual laminates can be produced individually or as a strand. The strand can run on a conveyor belt and be processed or cut to length or into a specified format with the aid of a so-called flying tool.

[0072] The laminate 300 itself can be composed of a loose, moldable molding material and a bonding system. The bonding system can be based on different mechanisms: for example, sand can be mixed with a clay-containing adhesive that can swell in water. Such a system can form a load-bearing laminate 300 by pure mechanical compression. Compaction can be considered by tamping, blowing or rolling. Chemical adhesives can also be known from metal casting technology. These adhesives are added to the sand and hardened by polymerization. Molding material adhesives are also known in this article, which are physically hardened by drying. The adhesive system can be mixed by a mechanical mixer before being formed into a board. Adhesives can also be applied over a large area using a spraying system or an inkjet printhead. Special forms of bonding are magnetic particles or mechanical connections that have been described above by specific particle geometries. Based on the moisture content, it may be useful to produce the laminate 300 by pouring liquid molding materials.

[0073] Figure 7 a) to Figure 7 c) schematically shows various methods of producing blanks for laminates.

[0074] Figure 7 A) in FIG. 7 shows a rolling method in which the material emerges from the spray nozzles 701 and is guided past the rollers 700 so that a smooth layer is present behind the rollers.

[0075] Figure 7 b) in the figure shows a pressing method, in which the material is pressed into a plate shape by force under a press 704.

[0076] Figure 7 Figure c) shows an injection method, where compressed air and molding material 707 are injected into the box through an injection nozzle 705 below a striker plate 706 to form a board in the box. The compressed air 708 can escape through an exhaust port.

[0077] When preparing for a processing method for a single laminate, it may be desirable to provide a structure in the laminate 300 so that the laminate can be transferred and handled, wherein the processing may result in loose or free areas that are not directly associated with the respective laminate, but should be retained by the laminate and positioned in the mold. Such a structure may be, for example, a mesh or filament that is inserted into the laminate 300 during the manufacturing process. Depending on the processing method for the laminate 300, it may be useful to position such a mesh or filament in the middle of the laminate 300 or at the edge of the laminate 300.

[0078] The mesh / wires can be made of different materials. For example, the mesh or wires can be designed so that they form a unit with the casting material, because they consist of the same material or a similar composition as the cast part to be produced. However, it is also conceivable that the mesh or structure consists of a material that strengthens or hardens the casting body.

[0079] The laminate formed in this way is plate-shaped and has vertical or inclined edges depending on the position and use in the installation space.

[0080] In the next step, a mold cavity 200 is produced in the corresponding laminate 300. For this purpose, a subtractive method is used, as described in reference Figure 6 a) to Figure 6 d) in the example. The method removes individual regions from the prefabricated laminate 300. Advantageously, the laminate has no undercuts when viewed in the stacking direction or in another direction in which the laminate can be processed, for example using a milling cutter.

[0081] All conceivable processes which remove the molding material and can be controlled automatically at the same time are suitable for machining. Milling is an example of such a process. In this context, the molding material can be machined after hardening, ie, molding material having a high strength.

[0082] In the region of the casting mold, ie in the region of the recesses, the laminate can have structural features, such as notches and draft angles, so that the cast body produced can be removed reliably from the mold even with difficult material pairings.

[0083] The laminate 300 is exemplified in Figure 6In a), a portion of the mold cavity depicted by the dashed line is to be produced. Figure 6 As shown in b) in FIG. 1 , milling can be performed vertically using a cylindrical end mill 600. As a result, layers can thus be produced which correspond substantially to the prismatic extrusion in the direction of the stacking direction.

[0084] Vertical milling slot Figure 6 In order to obtain a better inclined surface on the final casting, according to the present invention, as Figure 6 It is also advantageous to tilt the milling cutter 600 relative to the vertical direction as shown in c).

[0085] Inclined slot milling Figure 6 c) in FIG. 2 is indicated by 603. The chamfer on the mold cavity 200 reproduces the component contour better than a contour generated in steps using a straight milling cutter. This effect can be further improved if the laminate 300 is processed from above and from below.

[0086] Figure 6 d) in FIG. 4 shows the processing of the laminate from above and below by means of a vertical milling cutter, by means of which a stepped profile 604 can be produced. The profile cutter represents a further improvement. Three-dimensional path control of the milling cutter 600 is also possible in order to reproduce the shape profile more accurately, but this path control is more laborious.

[0087] As well as milling, other methods known from metal cutting and forming can be used. These include drilling, sawing, grinding, planing, laser cutting, flame cutting, water jet cutting, compressed air jetting, sandblasting or etching. For thin and solid sheets of forming material, the mold cavity can also be produced by punching or fine blanking. For very loose or not yet hardened forming material, unbound material can also be sucked away in a targeted manner. Likewise, in the case of mechanical bonding mechanisms, negative pressure can be used to easily remove the forming material parts. Targeted demagnetization is advantageous when using magnetic base materials for ablation or supporting ablation.

[0088] In addition to using mesh structures or wires inside layer 300, it can be advantageous to introduce structures that additionally increase the structural strength of the layer 300. An example can be a mesh, grid, rod or other reinforcement of a special shape. This is especially necessary for large layers and molds weighing hundreds of kilograms or tons. It is also useful to provide transportation assistance for the layer. These assistances can be in the form of small holes or forklift bags (forklift pocket). Honeycomb structures or bags can reduce weight and can be implemented in the laminate 300 outside the region of the mold cavity 200.

[0089] After producing them, the produced laminates are stacked into a casting mold 201. The laminates are placed face to face in the correct order to perform this operation. The stacking can preferably be carried out perpendicular to the direction of gravity, so that the stacking direction extends parallel to the effective direction of gravity. However, stacking at any desired angle to the direction of gravity is also possible. Fig.11 As shown, the package 1100 having a layer stack can also be inserted into another layer stacked package having a different layer stacking direction.

[0090] A variety of mechanisms can be used to join together the laminates to form the mold 201. The simplest method is to place one layer on top of another and use gravity as the joining force. Depending on the density of the molding material and the casting medium, it may be necessary to hold down the mold 201 with a weight 900 prior to casting, such as Fig. 9 After weighing, the liquid casting material / melt 902 can be poured into the mold through a ladle 901 via a pouring system.

[0091] Likewise, if Figure 8 As shown, the compacted laminates 300, 401 may be pressed against each other or together on a support plate / substrate 800 and thus bonded together. Here, for example, expandable bonding clay on the surface of the laminates 300, 401 or an adhesive may be used.

[0092] Fibers may also be used on the surface of the laminate 300, 401 in the sense of a Velcro fastener system.

[0093] Such a system may be attached to the top and bottom of the laminate 300, 401 during the laminate production process.

[0094] The laminates can also be connected by physical and chemical adhesives. As with the bonding of molding materials, many systems are known in this context and can be borrowed, for example, from metal casting technology. An example can be resin-coated sand, the shell of which melts when heated. The laminates 300, 401 to be joined are heated flat on their bottom and immediately pressed together with the laminates 300, 401 located below them. When the resin coating cools, the laminates are connected. Similarly, the laminates can also be sprayed with a chemically hardening adhesive, thereby producing a layered composite.

[0095] You can also Fig.10 The use of a low tensioner 1000 to clamp each laminate is shown. This can be done in layers or for a large number of laminates. The entire layer package or the entire mold 201 can be connected in this way. The holes in the laminates can also accommodate screws or bolts that can enter special pins or threaded holes in the top and bottom laminates to enable screwing to the mold.

[0096] Similar to the layer encapsulation, during the layer stacking process the laminate can be placed in the resulting mold 201. These can be various reinforcements, inserted castings or cores, functional elements (e.g. controllers, actuators), fibers, pre-processing structures, cooling irons, castings or piping systems.

[0097] A mold such as Fig.12 As shown, the stacking direction is perpendicular to Fig. 9 In addition, Fig.12 Layer 1200 is depicted for vertical mounting of the laminate as an alignment body.

[0098] Fig.13 The cross section of the casting mold is shown, which has two wedge-shaped laminates 301, 302 in addition to a plurality of plate-shaped laminates 300. The wedge-shaped laminates 301, 302 define an undercut 303 in the casting mold by their interface. Another undercut surface 304 is formed by the planar laminate 300. The stacking direction is Fig.14 Indicated by 300a.

[0099] Fig.14 A casting mould with a frustoconical mould cavity is shown.The laminates 300 each have two through holes 305, 306 which are aligned with each other and on peg-shaped alignment bodies 307, 308, wherein the alignment bodies are inserted into the holes.

[0100] Fig.15 A perspective view of a laminate 300 is shown having a groove and a surrounding laminate wall with two peg-shaped protuberances 309, 310 thereon for interlocking with an adjacent laminate having a corresponding groove.

[0101] The mold of a large casting can be post-processed to improve the surface. For example, this can be done by grinding away the gradation that appears on the mold. The mold 201 can also be smoothed on the inside using a sandblasting medium.

[0102] The casting molds produced in this way can be used for all known casting processes. For example, this process includes the use of gravity casting of metals. Metals such as aluminum, iron or steel can be processed here. However, it is also possible to cast concrete parts or use them in the area of ​​plastic parts.

[0103] Application Examples

[0104] The geometry of a bridge over a pond is required for a garden project. The treads should be realized with the help of wooden boards. The left and right edges of the steps are realized by a topologically optimized lightweight structure, the different parts are connected to each other by individual supporting struts. The installation space of this structure is 900×600×600mm 3The design of the bridge was calculated using a mathematical optimization algorithm and did not exist in the form of a physical model 201.

[0105] For aesthetic reasons, the bridge structure was to be made of bronze. Casting was chosen as the manufacturing process due to the high complexity of the supporting structure. The foundry commissioned for the project saw the high level of complexity and chose the above method based on a favorable cost structure.

[0106] In preparation for production of the mould, the bridge geometry is placed in a virtual installation space and automatically rotated so that when the geometry is broken down into the individual layers, all laminates are free of undercuts and the laminates each form a coherent body. The laminates are automatically arranged to be as thick as possible and as thin as necessary. The rotation angle and inclination of the component 100 in the installation space are taken from the foundry's program so that the casting system can be designed and simulated for this geometry. The boundary conditions of the undercut-free laminates with the overall model of the designed gating system are checked again and the representation of the individual layers is exported as a .dxf file.

[0107] The installation space required for the rotation of the component 100 was also calculated and the casting system designed. This resulted in an installation space of 1200×800×800 mm 3 The result of the component 100 is a vertical layer division with 21 layers. Each laminate 300 is uniquely identified in the form of a layer number 201. The bridge system is cast upright, cut from the inside and fed in.

[0108] For logistical reasons, the digital representation of the laminate is clustered according to the number of layers and sent to the production system. Each of the seven layers forms a cluster and is placed one after another for the manufacturing process according to increasing layer height.

[0109] Quartz sand is used as the basic molding material. The connection between the sand grains is ensured by a self-hardening chemical system based on furan resins. The standard size of the laminate 300 is 1200 mm × 800 mm as the basic size, the height is individualized according to the calculated height of the individual laminate. The production system can produce laminates up to 10 cm in an endless process. The loose base molding material, the particles of which have been coated with a chemical adhesive, is placed on a conveyor belt and pre-smoothed using a scraper.

[0110] The rollers 700 compact the molding material layer 300 and simultaneously produce the required layer height. Excess material may fall to the left and right of the conveyor belt. Directly behind the rollers 700, the endless belt of molding material is cut at the edge by a band saw to a width of 800 mm for the installation space. Once the required length is reached, the conveyor stops and the laminate 300 is cut to the appropriate size using a movable saw. This process sequence is intermittently run in layers.

[0111] The laminates of the cluster are actually classified from the smallest layer thickness to the largest layer thickness and are produced according to the smallest layer thickness to the largest layer thickness. The layer height transition between the two layers is achieved using a linear method in the vertical direction of the roller 700. Therefore, when there is a transition between the two layer thicknesses / laminate heights, the thickness of the blank increases linearly. The laminate is hardened to solid within a running meter on the conveyor belt, so it can be mechanically handled without damaging the laminate.

[0112] While the blank layer is still being produced on the material input side of the production machine, the endless layer is separated into individual layers of 1200 mm length on the output side of the machine using a movable band saw. The wedge-shaped connections between two laminates with different layer heights are also separated by the movable saw system.

[0113] There is now a laminate with a basic size of 1200 mm x 800 mm, with different layer heights between the laminates 300. The conveyor belt pushes the laminate onto a roller conveyor arranged at right angles to the first belt. The separated layer transition is discharged to the side in front of the roller conveyor and fed back into the regeneration cycle.

[0114] While the laminates on the first conveyor are still sorted according to increasing layer height, when they are placed on the roller conveyor they are now sorted directly according to their respective number of layers and position in the final casting mold. This can be achieved by shifting the laminates already on the roller conveyor. For example, if laminates with layer numbers 3 and 7 are already placed on the roller conveyor, layer number 6 will be placed directly between these two already placed laminates, while layer number 1 will be placed to the left of layer number 3.

[0115] The individual laminates are now placed on the roller conveyor in standardized basic dimensions and at individual heights, in increasing numbers of layers / positions from left to right.

[0116] A computer-controlled milling machine is installed to the left of the roller conveyor, which allows milling of 2D geometries and, as an additional degree of freedom, can also rotate the milling head with the end mill 600. The laminate is positioned on the milling table according to the number of layers and individual milling of the required cavities / recesses in the laminate 300 present in each case is carried out. The molding material dust after demoulding is discharged directly from above and below, and burrs are removed directly from the edges of the laminate by means of trailing chains. As a result, no further cleaning work is required for the laminate 300 and, after a successful milling process, the laminate can be lifted by a robot using pneumatic suction grippers. Each of the seven laminates is bundled on a Euro pallet as a package and forms a shipping unit.

[0117] Molding material remaining as waste from the manufacturing process and molding material residues from the blank manufacturing process are directly shredded and recycled.

[0118] The twenty-one laminates are delivered to the customer foundry on three Euro pallets 201, which can use its in-house crane to stack the laminates directly one on top of the other and add weight. The subsequent casting process does not differ from the conventional sand casting process.

[0119] The aspects of the present invention are as follows, each of which may represent an independent invention on its own, but may also represent an independent invention together with the patent claims of this application, either individually or in groups.

[0120] Aspect 1: A method for producing an article by a casting process, characterized in that the casting mold consists of multiple layers, which are produced and structured outside the space in which they are assembled to form the casting mold.

[0121] Aspect 2: A method for producing an article by a casting method according to aspect 1, characterized in that the layer is constructed using a subtractive method.

[0122] Aspect 3: A method for producing an article by a casting process according to aspect 1 or 2, characterized in that the layers have substantially no undercuts perpendicular to their extension planes.

[0123] Aspect 4: A method for producing an article by a casting process according to aspect 1, 2 or 3, characterized in that layers of different thicknesses can be used to produce the casting mold.

[0124] Aspect 5: A method for producing products through a casting process according to aspects 1 to 4, characterized in that processing is carried out through mechanical processing methods, such as milling, drilling, sawing, corrosion, ultrasonic processing, laser cutting, plasma cutting, water jet cutting, stamping, and precision cutting.

[0125] Aspect 6: A method for producing an article by a casting process according to any one of Aspects 1 to 5, characterized in that processing is performed in a still unbonded state by suction, scraping, milling or similar processes.

[0126] Aspect 7: A method for producing an article by a casting process according to any one of Aspects 1 to 6, characterized in that the layer is composed of metal, ceramic, plastic or natural material.

[0127] Aspect 8: A method for producing an article by a casting process according to any one of Aspects 1 to 7, characterized in that the layer is formed by a solid, a particulate material, a suspension, an emulsion, a dispersion, a slip, or an aerosol.

[0128] Aspect 9: A method for producing an article by a casting process according to any one of Aspects 1 to 8, characterized in that quartz sand, artificial sand, mullite, rutile sand, chrome ore sand, kerphalites, cerabeads, glass beads, ceramic particles, ceramic powder, steel particles, aluminum particles, copper particles, particles made of copper alloys, metal particles, plastic particles or granules, or natural material particles or granules are used as granular materials.

[0129] Aspect 10: A method for producing an article by a casting process according to any one of Aspects 1 to 9, characterized in that the particles are combined into layers by a bonding force including chemical bonding, physical drying, magnetic interaction, electrostatic interaction or gravity.

[0130] Aspect 11: A method for producing an article by a casting process according to any one of Aspects 1 to 10, characterized in that bonding clay, furan resin adhesive, cold box adhesive, water glass-based adhesive, phenolic resin-based adhesive, PEP SET adhesive, molding material or kernel oil, acrylic resin adhesive or other bonding systems are used as adhesives.

[0131] Aspect 12: An apparatus for performing the method according to any one of aspects 1 to 11.

[0132] Aspect 13: A mold for casting a component, produced according to the method according to any one of aspects 1 to 11.

[0133] Reference Number

[0134] 100 Components / Castings

[0135] 200 mold cavities

[0136] 201 mold (upper box)

[0137] 202 cores

[0138] 203 Pouring basin and pouring spout

[0139] 204 mold (lower box)

[0140] 300th floor

[0141] 400 layers (changed layer thickness)

[0142] 401 layers (thick layer thickness)

[0143] 600 Milling Cutter

[0144] 601 Vertical Slot Milling

[0145] 602 angled milling cutter

[0146] 603 Angle Milling

[0147] 604 Milling slot with steps in one layer

[0148] 605 Milling cutter for bottom machining

[0149] 700 Smooth Roller

[0150] 701 Spray Nozzle

[0151] 702 Smoothing Layer

[0152] 704 Press for compacting layers

[0153] 705 Spray Nozzle

[0154] 706 Pressure Plate

[0155] 707 Compressed air and molding materials

[0156] 708 Sand-free air escapes through the nozzle

[0157] 800 substrate

[0158] 900 weights

[0159] 901 Ladle

[0160] 902 Melt

[0161] 1000 Low Tensioner

[0162] 1100 Layers with different orientations

[0163] 1200 Layers for vertical installation

Claims

1. A method for producing a casting mold (201, 204), the method comprising: First, at least four laminates of the casting mold are produced separately from each other, wherein, after the pattern of the casting mold (201, 204) is divided into laminates in different stacking directions (300a, 1100a) in sequence and the stacking direction with the least number of undercuts is selected, the layer thickness of the laminates is divided so that at least one undercut is formed by the interface of the laminates, The laminates are then joined together to form one or more stacks (1100) along a selected stacking direction to form the casting mold.

2. The method according to claim 1, characterized in that The laminated bodies are formed such that, after being assembled into the casting mold (201, 204), a plurality of the laminated bodies surround in an annular manner a cavity (200) of the casting mold to be filled with casting material.

3. The method according to claim 1 or 2, characterized in that: The laminate is formed such that a plurality of the laminates each have at least one opening (311) that completely penetrates the laminate and is surrounded by a circumferential laminate wall (312).

4. The method according to claim 1, 2 or 3, characterized in that: The laminates are aligned when they are joined together to form a stack either on a common alignment feature (307, 308, 1200) or by interlocking projections (309, 310) and grooves provided on each of the laminates.

5. The method according to any one of claims 1 to 4, characterized in that When the laminates are assembled into a stack (1100), the laminates are connected to each other at adjacent boundary surfaces, and the laminates have the same layer thickness or different layer thicknesses in the stacking direction (300a, 1100a).

6. The method according to claim 5, characterized in that The laminates are connected to one another when they are joined together by gluing, welding or by a force-fitting or form-fitting connection.

7. The method according to any one of claims 1 to 6, characterized in that The laminate is produced by an extrusion process, a rolling process, a casting process or an additive manufacturing process.

8. The method according to any one of claims 1 to 7, characterized in that The laminate is produced as a solid body, and grooves (311) penetrating the laminate are made in a plurality of the laminates.

9. The method according to any one of claims 1 to 8, characterized in that A groove (311) penetrating the laminate is formed in the laminate by a subtractive process.

10. The method according to any one of claims 1 to 8, characterized in that A groove (311) penetrating the laminate is formed in the laminate by a cutting process, punching or by a chemical process.

11. The method according to claim 10, wherein: The cutting process is laser cutting or water jet cutting.

12. The method according to claim 1, wherein: The five laminates of the casting mold are first produced separately from one another and then the laminates are joined together.

13. The method according to claim 1, wherein: The more than five laminates of the casting mould are first produced separately from one another and then the laminates are joined together.

14. The method according to claim 1, wherein: More than ten laminates of the casting mould are first produced separately from one another and then the laminates are joined together.

15. The method according to any one of claims 1 to 14, characterized in that The laminate is designed in the form of a disc.

16. The method according to any one of claims 1 to 14, characterized in that The laminate is designed in the form of a plane-parallel plate.

17. The method according to any one of claims 1 to 16, characterized in that The surfaces of the laminates of a stack are coplanar, the stack being a stack abutting adjacent laminates.

18. The method according to any one of claims 1 to 17, characterized in that Each of the laminates has no undercut in the stacking direction (300a, 1100a).

19. The method according to claim 18, characterized in that The laminates are designed and joined together such that in the stacking direction (300a, 1100a), at least one undercut is provided in the cavity (200) of the casting mold (201, 204) to be filled with casting material and is formed by the interface of the laminates.

20. The method according to any one of claims 1 to 19, characterized in that After the model of the casting mold (201, 204) is divided into the laminates in turn according to different stacking directions (300a, 1100a) and the stacking direction with the least number of undercuts is selected, the layer thickness of the laminate is divided so that all undercuts (303, 304) at the interface are located between every two laminates.

21. A casting mold consisting of a plurality of laminated bodies, the casting mold being produced by the method according to any one of claims 1 to 20, wherein: One stack is arranged in the cavity of another stack.

Citation Information

Patent Citations

  • Production method with vacuum sand mould

    CN108067607A

  • Metal gravity casting die

    CN202239496U

  • Molding tool used for casting metal comprises several parallel layers each having raised sections and / or recesses or forming a layer-like section of a molded section

    DE102005059486A1

  • Producing mold or mold part for casting, comprises placing molding box with its frame around model of casting, filling molding material in interior of molding box, and curing molding material and separating the model from the molding box

    DE102010060868A1

  • Process for casting a component with a complex geometry using a segmental mold

    DE102016202657A1