Polishing pad, method for manufacturing polishing pad, and polishing method

The design of forming deep grooves and shallow depression patterns on the polishing pad solves the problems of long running time and scratches on the polishing pad, achieving faster running in and more uniform surface roughness, suitable for high-hardness non-foaming polymers body polishing pad.

CN114286737BActive Publication Date: 2024-10-08KURARAY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202080039388.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-06-19
Filing Date
2020-06-04
Publication Date
2024-10-08
Estimated Expiration
2040-06-04

AI Technical Summary

Technical Problem

It is difficult for existing polishing pads to quickly reach a roughness suitable for grinding during the running-in process, resulting in a long running-in time, especially when using polishing pads based on high-hardness non-foaming polymers, and sandpaper polishing may cause scratches. mark.

Method used

Use a polishing pad with a deep groove area and a shallow depression pattern. The depth of the deep groove area is 0.3mm or more, the shallow depression depth is 0.01~0.1mm, and the maximum distance of the island table surface is 8mm or less. It is formed by cutting processing to avoid sandpaper Polished to reduce risk of scratches.

Benefits of technology

It shortens the running-in time of the grinding surface of the polishing pad, improves the uniformity of surface roughness, reduces the time required for running-in, and avoids the scratch problem caused by sandpaper polishing. It is suitable for high-hardness non-foaming polymers. Polishing pad.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114286737B_ABST
    Figure CN114286737B_ABST
Patent Text Reader

Abstract

A polishing pad comprises a polishing layer having a polishing surface, wherein the polishing surface comprises: a deep groove region having a first pattern formed by deep grooves or holes with a depth of 0.3 mm or more; a table region, which is a region other than the deep groove region; the table region having: shallow depressions with a depth of 0.01 to 0.1 mm, which have a second pattern; and a plurality of island-shaped table portions, which are surrounded by the shallow depressions and have a maximum horizontal distance of less than 8 mm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention provides a polishing pad that can be used to shorten the time required for the polishing surface of the polishing pad to have a roughness suitable for polishing. Background Art

[0002] Conventionally, chemical mechanical polishing (CMP) has been used to polish the polished surface while supplying slurry to the polishing surface of a polishing pad in order to perform mirror finishing on glass used as substrate materials such as semiconductors or silicon wafers or materials for hard disks, liquid crystal displays, and lenses, or to flatten the unevenness caused by insulating films or metal films in the manufacturing process of semiconductor devices.

[0003] As the grinding pad for CMP, there are known non-woven type grinding pads, grinding pads with polymer foams having independent bubble structures as the main body, grinding pads with non-foamed polymers as the main body, etc. The grinding pad of the non-woven type has the advantage of good contact with the polished substrate due to its softness, and on the other hand, it has the disadvantage of low flattening property of the polished surface due to its softness. In addition, the grinding pad with polymer foams having independent bubble structures as the main body has the advantage of excellent flattening property compared with the grinding pad of the non-woven type due to its high hardness, and on the other hand, it has the disadvantage of being difficult to achieve high flattening property by further hardening of the grinding layer. On the other hand, the grinding pad with non-foamed polymers as the main body can achieve high flattening property. In addition, the grinding pad with non-foamed polymers as the main body has the advantage of longer life of the grinding pad and the advantage of being difficult to produce the difference in grinding characteristics caused by the change of foaming because the wear resistance is higher than that of the grinding pad with polymer foams as the main body. For example, the following patent document 1 discloses a high hardness grinding pad with non-foamed polyurethane as the main body.

[0004] In CMP, usually, before starting to use a new, unused polishing pad, a pad dresser (also called a dresser) is used to perform a dressing process called running-in for finely roughening the polishing surface of the polishing pad to form a roughness suitable for polishing. Before starting to use an unused polishing pad, the polishing surface is dressed to improve the retention of the slurry on the polishing surface.

[0005] The grinding device cannot be operated during the running-in period of the grinding pad. Therefore, it is required to extend the operating time of the grinding device by shortening the time required for running-in (hereinafter, also referred to as "running-in time"). By extending the operating time of the grinding device, the production cost of semiconductor devices, etc. is reduced.

[0006] Several techniques for shortening the break-in time have been proposed. For example, Patent Document 2 below discloses a polishing pad in which a microstructure having a specific roughness parameter is pre-formed on the polishing surface. Patent Document 2 discloses that such a polishing pad can shorten the break-in time.

[0007] In addition, the following patent document 3 discloses a method for manufacturing a polishing sheet composed of a sheet-like foam body, in which, in the step of adjusting the thickness thereof by sandpaper grinding, the sandpaper grinding of the polishing surface consists of two stages: a first fine grinding and a second fine grinding, the first fine grinding is performed by increasing the grit number of the sandpaper, the grit number of the sandpaper used in the second fine grinding is smaller than the grit number of the sandpaper used at the end of the first fine grinding, and the total grinding amount of the second fine grinding is 10 μm or more and 1000 μm or less. Furthermore, according to the manufacturing method of patent document 3, it is disclosed that a polishing pad having a short time until startup when performing CMP and excellent in-plane uniformity can be obtained.

[0008] In addition, the following patent document 4 discloses a polishing pad for polishing an object to be polished, having a polishing surface pressed against the object to be polished, the undulation period of the polishing surface is 5 mm to 200 mm, the maximum amplitude is 40 μm or less, and the negative Zeta potential of the polishing surface is set to be greater than -50 mV and less than 0 mV. Patent document 4 discloses that according to such a polishing pad, the repulsion between the slurry and the negative polishing particles is suppressed, the fusion of the polishing surface of the polishing pad and the slurry is good, and the running-in time can be shortened.

[0009] In addition, the following patent document 5 discloses a polishing pad for polishing a substrate, the polishing pad having a polishing surface, the polishing surface having: a polishing body having a polishing side opposite to the back surface; and a plurality of cylindrical protrusions continuous with the polishing side of the polishing body. Moreover, patent document 5 records that the height of the cylindrical protrusion is roughly in the range of 0.5 to 1 mm. On the other hand, in patent document 5, there is no mention of shortening the running-in time.

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent Document 1: (Japanese) Patent Publication No. 2014-038916

[0013] Patent Document 2: (Japanese) Patent Publication No. 2002-144220

[0014] Patent Document 3: (Japanese) Patent Publication No. 2010-253665

[0015] Patent Document 4: (Japanese) Patent Publication No. 2012-210709

[0016] Patent Document 5: (Japan) Patent Publication No. 2016-506307 Summary of the invention

[0017] Problems to be solved by the invention

[0018] For example, the grinding pad with the grinding surface containing the microstructure with specific roughness parameter disclosed in patent document 2 can not shorten the running-in time fully sometimes.For example, when forming the concentric or spiral microstructure perpendicularly intersecting with the diameter direction of the grinding pad on the grinding surface by cutting, when using the non-foamed polymer with few surface concave-convex as the grinding layer, because the rotation direction of the grinding pad is consistent with the direction of the groove, water flows in the same direction while rotating and becomes fluid lubrication, and there is the problem that the grinding surface is difficult to be repaired and the running-in time is easy to be lengthened.On the other hand, patent document 3 and patent document 4 propose to provide the scheme of the grinding pad that shortens the running-in time by obtaining a flatter grinding pad.But the grinding pad disclosed in patent document 3 and patent document 4 needs to be manufactured with sandpaper polishing, so it is difficult to be applied to the grinding pad with non-foamed polymer with very high hardness as the main body, and in addition, it is also possible to have residual polishing powder on the grinding surface and easily produce scratches.

[0019] An object of the present invention is to provide a polishing pad capable of shortening the time required for the polishing surface of the polishing pad to have a roughness suitable for polishing.

[0020] Technical solutions to solve problems

[0021] One aspect of the present invention is a polishing pad, which includes a polishing layer having a polishing surface, wherein the polishing surface has: a deep groove area having a first pattern formed by deep grooves or holes with a depth of 0.3 mm or more; a table area, which is an area other than the deep groove area; the table area having: a shallow depression with a depth of 0.01 to 0.1 mm, having a second pattern; and a plurality of island-shaped table portions surrounded by the shallow depressions, and the maximum distance in the horizontal direction is 8 mm or less. The polishing surface refers to a side of the polishing layer on the side that is in contact with the polished surface of the material to be polished during polishing and is provided for polishing. In addition, the horizontal direction of the table portion refers to the surface direction of the polishing surface of the polishing pad. According to such a polishing pad, the running-in time and the running-in polishing time for making the polishing surface of an unused polishing pad into a surface state suitable for polishing can be shortened. In particular, when the maximum distance in the horizontal direction of the table portion is 8 mm or less, the pad dresser is easy to contact each of the table portions surrounded by the shallow depressions, and the time for forming a roughness suitable for polishing can be shortened.

[0022] In addition, the polishing pad of this embodiment can improve the uniformity of the shape and surface roughness of the polishing surface, so it is easy to perform an inspection to check whether the surface shape of the entire surface of the polishing surface is within the specification range. In addition, when the polishing surface is not polished with sandpaper, as described later, a shallow depression can be formed by cutting or the like. When the shallow depression is formed by cutting, it is easy to omit the process of cleaning the polishing powder for suppressing scratches caused by residual polishing powder.

[0023] In addition, in the above-mentioned polishing pad, it is preferred that the second pattern has at least one pattern selected from the group consisting of a triangular lattice, a square lattice, a rectangular lattice, a diamond lattice, and a hexagonal lattice formed on the entire surface of the table area. In the case where the second pattern has such a pattern, the pad dresser can easily contact the multiple island-shaped table parts surrounded by shallow depressions uniformly from all directions, and the time for forming the roughness suitable for grinding can be further shortened, which is preferred from this point of view. In addition, such a pattern can be formed by a combination of linear shallow depressions, and is therefore easy to form by cutting.

[0024] In the above-mentioned polishing pad, it is preferred that the projection area of ​​each land portion is 0.3 to 10 mm. 2 When the projection area of ​​each land portion is within such a range, the pad conditioner can easily contact each land portion surrounded by the shallow recess, and the time for forming the roughness suitable for grinding can be further shortened, which is preferable from this point of view.

[0025] In addition, in the above-mentioned polishing pad, it is preferred that the ratio of the total projection area of ​​the table portion to the total projection area of ​​the table region is 10 to 50%. Here, the ratio of the total projection area of ​​the table portion refers to the ratio of the total projection area of ​​each table portion to the total projection area of ​​the table region when the table region is projected two-dimensionally without considering the concavity and convexity of the polishing surface. When the ratio of the total projection area of ​​the table portion is within such a range, the pad dresser can easily contact each of the table portions surrounded by shallow depressions, and the time for forming a roughness suitable for polishing can be further shortened, which is preferred from this point of view.

[0026] In addition, in the above-mentioned polishing pad, it is preferred that the depth of the shallow depression is 0.02 to 0.06 mm. When the depth of the shallow depression is in such a range, each mesa portion surrounded by the shallow depression wears out in a shorter time during running-in or running-in polishing, so the time for forming a roughness suitable for polishing can be further shortened, which is preferred from this viewpoint.

[0027] In addition, in the above-mentioned polishing pad, from the viewpoint of being able to fully retain the slurry, it is preferred that the ratio of the projection area of ​​the deep groove region to the total projection area of ​​the polishing surface is 5 to 40%, and further, the first pattern has at least one pattern selected from the group consisting of a spiral shape, a concentric circle shape, and a grid shape.

[0028] In the above-mentioned polishing pad, it is preferred that the polishing layer is composed mainly of a sheet containing a non-foamed polymer, from the viewpoint of easily obtaining a high-hardness polishing layer that takes a short time to form a roughness suitable for polishing.

[0029] In the above-mentioned polishing pad, the polishing layer is preferably composed of a thermoplastic polyurethane sheet from the viewpoint of excellent low scratch resistance and easy formation into the polishing layer.

[0030] In addition, another aspect of the present invention is a grinding method, which is used to grind the grinded surface of a semiconductor device in the manufacturing process of the semiconductor device using the above-mentioned grinding pad, and the grinding method has a step of dressing the grinding surface under the dressing conditions that the cumulative dressing time until the average depth of the shallow depression is less than 0.01 mm is within 30 minutes, preferably between 1 and 20 minutes.

[0031] Effects of the Invention

[0032] According to the present invention, the time required for the polishing surface of the polishing pad to have a roughness suitable for polishing can be shortened. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1A It is a schematic diagram for explaining the polishing surface of the polishing pad 10 according to the embodiment.

[0034] Figure 1B It is a schematic cross-sectional view for explaining the polishing surface of the polishing pad 10 according to the embodiment.

[0035] Figure 2 It is a schematic plan view of the polishing surface of the polishing pad 20 for explaining another example of the embodiment.

[0036] Figure 3A It is a partially enlarged schematic diagram of the polishing surface of the polishing pad 30 for explaining another example of the embodiment.

[0037] Figure 3B It is a schematic cross-sectional view of a polishing layer of a polishing pad 30 for explaining another example of the embodiment.

[0038] Figure 4 It is a partially enlarged schematic diagram of the polishing surface of the polishing pad 40 for explaining another example of the embodiment.

[0039] Figure 5 It is an explanatory diagram for explaining the pitch and width of shallow depressions in the form of an equilateral triangle lattice, and the maximum distance in the horizontal direction of a single island-shaped terrace portion.

[0040] Figure 6 It is an explanatory diagram for explaining the pitch and width of the shallow depressions in a square grid pattern and the maximum distance in the horizontal direction of one island-shaped terrace portion.

[0041] Figure 7This is an explanatory diagram for explaining the pitch and width of shallow depressions surrounding circular terrace portions arranged in a regular hexagonal lattice, and the maximum horizontal distance of one island-shaped terrace portion.

[0042] Figure 8 It is an explanatory diagram for explaining the pitch and width of shallow depressions surrounding the terrace portions arranged in a regular hexagonal lattice, and the maximum distance in the horizontal direction of one island-shaped terrace portion.

[0043] Fig. 9 This is an explanatory diagram for explaining CMP.

[0044] Fig. 10A This is an explanatory diagram for explaining changes in the polished surface during running-in.

[0045] Fig. 10B This is an explanatory diagram for explaining changes in the polished surface during running-in.

[0046] Fig.11 This is an enlarged photograph of the polishing surface of the polishing pad obtained in Example 1.

[0047] Fig.12 This is an enlarged photograph showing the state of the polishing surface of the polishing pad obtained in Example 1 during run-in polishing.

[0048] Fig.13 This is an enlarged photograph of the polishing surface of the polishing pad obtained in Comparative Example 1.

[0049] Fig.14 This is an enlarged photograph showing the state of the polishing surface of the polishing pad obtained in Comparative Example 1 during run-in polishing. DETAILED DESCRIPTION

[0050] The polishing pad according to the present embodiment includes a polishing layer having a polishing surface.

[0051] The material forming the grinding layer can use the synthetic or natural polymer material of the manufacture of the existing grinding layer for grinding pad, without special restrictions. As the specific example of the polymer material forming the grinding layer, for example, polyurethane, polyethylene, polypropylene, polybutadiene, ethylene-vinyl acetate copolymer, butyral resin, polystyrene, polyvinyl chloride, acrylic resin, epoxy resin, polyester, polyamide, etc. can be cited. They can be used alone, and two or more combinations can also be used. Among them, from the viewpoint of obtaining a grinding layer with excellent flattening performance and being difficult to produce scratches in addition, it is particularly preferred that the polyurethane obtained by reacting the polyurethane raw material containing polymer diol, organic diisocyanate and chain extender. Below, for the polyurethane used as the material forming the grinding layer, it is described in detail as a representative example.

[0052] Examples of the high molecular weight diol, organic diisocyanate and chain extender as the raw materials of the polyurethane include the following compounds.

[0053] Specific examples of the polymer diol include polyether diols such as polyethylene glycol and polytetramethylene glycol; polyester diols such as poly(nonyl adipate) diol, poly(2-methyl-1,8-octamethylene) diol and poly(3-methyl-1,5-pentylene) diol; polycarbonate diols such as poly(hexamethylene carbonate) diol and poly(3-methyl-1,5-pentylene carbonate) diol, or copolymers thereof, etc. These may be used alone or in combination of two or more.

[0054] In addition, as specific examples of organic diisocyanates, for example, aliphatic or alicyclic diisocyanates such as hexamethylene diisocyanate, isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 1,4-bis(isocyanatomethyl)cyclohexane; aromatic diisocyanates such as 4,4'-diphenylmethane diisocyanate, 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 1,5-naphthalene diisocyanate can be cited. They can be used alone or in combination of two or more. Among them, 4,4'-diphenylmethane diisocyanate is preferred from the viewpoint of excellent wear resistance of the obtained grinding layer.

[0055] In addition, as chain extenders, low molecular weight compounds having a molecular weight of 350 or less and having two or more active hydrogen atoms that can react with isocyanate groups in the molecule can be cited. Specific examples thereof include diols such as ethylene glycol, diethylene glycol, 1,3-propylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, 1,4-bis(β-hydroxyethoxy)benzene, 1,9-nonanediol, and spirodiol; and diamines such as ethylenediamine, tetramethylenediamine, hexamethylenediamine, nonamethylenediamine, hydrazine, xylylenediamine, isophoronediamine, and piperazine. These can be used alone or in combination of two or more. Among them, 1,4-butanediol and / or 1,9-nonanediol are particularly preferred.

[0056] The proportion of each component of the polyurethane raw material can be appropriately adjusted in consideration of the characteristics to be imparted to the polishing layer. Specifically, it is preferred that, for example, the proportion of each component is such that the isocyanate group contained in the organic diisocyanate is 0.95 to 1.3 moles, further 0.96 to 1.1 moles, and particularly 0.97 to 1.05 moles, relative to 1 mole of active hydrogen atoms contained in the polymer diol and the chain extender. When the isocyanate group contained in the organic diisocyanate is too small, the mechanical strength and wear resistance of the obtained polyurethane tend to decrease. In addition, when the isocyanate group contained in the organic diisocyanate is too large, the productivity of the polyurethane or the storage stability of the polyurethane raw material tends to decrease.

[0057] From the viewpoint of obtaining a polishing layer having particularly excellent planarization and low scratch resistance, it is preferred that the ratio of nitrogen atoms from isocyanate groups of organic polyisocyanates in the polyurethane is 4.8 to 7.5% by mass, further 5.0 to 7.3% by mass, and particularly 5.2 to 7.1% by mass. When the ratio of nitrogen atoms from isocyanate groups is too low, the hardness of the polishing layer obtained tends to be low.

[0058] In addition, from the viewpoint of obtaining a grinding layer with excellent flattening property of high hardness, the polyurethane as the material for forming the grinding layer is preferably a thermoplastic polyurethane. It should be noted that thermoplasticity refers to the characteristic that can be melted and formed by heating processes such as extrusion molding, injection molding, calendering molding, 3D printer molding, etc. Such thermoplastic polyurethane uses a polyurethane raw material containing a high molecular weight diol, an organic diisocyanate and a chain extender, and is manufactured using a known polyurethane manufacturing method such as a prepolymer method or a one-step method. In particular, from the viewpoint of excellent productivity, it is preferred that a method of melt-mixing a polyurethane raw material and carrying out melt polymerization in the absence of a solvent in substance, and then using a multi-screw type extruder to carry out a method for continuous melt polymerization.

[0059] The manufacture method of grinding layer is not particularly limited, for example, can enumerate in the polymer material forming the above-mentioned grinding layer, according to need, use known sheeting method, the composition formed by the additive etc. of the grinding layer used in the past, that is, the method for sheeting of the polymer material used for the grinding layer. Specifically, for example, can enumerate and utilize the extruders such as the single screw extruder or the twin screw extruder that T die is installed to melt extrude the polymer material used for the grinding layer and sheeting method. In addition, sheet material can also be made by forming the polymer material used for the above-mentioned grinding layer into block, and the block-shaped body is sliced. The sheet material obtained is processed into desired size, shape by cutting, punching, cutting, etc., or processed into desired thickness by grinding, etc., thereby finished into grinding layer sheet.

[0060] The hardness of the polishing layer D is preferably 45 to 90, more preferably 50 to 88, and particularly preferably 55 to 85, from the viewpoint of achieving an excellent balance between improvement in planarization properties and suppression of scratches on the surface of the polished substrate.

[0061] In addition, the grinding layer is preferably formed by a non-porous sheet with a non-foamed structure, a grinding layer with a non-foamed structure. From the viewpoint of being able to maintain high hardness, showing more excellent flattening, it is preferred to have a grinding layer with a non-foamed structure. In addition, the grinding layer with a non-foamed structure is owing to not exposing pores on its surface, and the abrasive grains in the slurry do not condense or adhere in the pores, so from the viewpoint of being difficult to produce scratches, it is preferred. In addition, the grinding layer with a non-foamed structure is compared with the grinding layer with a foamed structure, because the wear rate of the grinding layer is small, therefore it is preferred from the viewpoint of long life.

[0062] Next, the state of the polishing surface of the polishing layer of the polishing pad according to the present embodiment will be described in detail with reference to the drawings. Figure 1A as well as Figure 1B It is a schematic diagram for explaining the polishing pad 10 of this embodiment. Figure 1A In the figure, (a) is a schematic plan view of the polishing pad 10 observed from the polishing surface P side as one side of the polishing layer, and (b) is a partially enlarged schematic view of the polishing surface P of (a). Figure 1B yes Figure 1A (b) is a schematic cross-sectional view of the II-II' section.

[0063] Figure 1A as well as Figure 1B In the figure, 10 is a circular polishing pad including a polishing layer 5 having a polishing surface P on one side. Figure 1B , the polishing pad 10 has a polishing surface P on one side of a polishing layer 5 and a layer structure in which a buffer layer 7 is bonded via an adhesive layer 6 on the other side.

[0064] The polishing pad of the present embodiment may have a laminated structure of more than two layers, such as a buffer layer 7 laminated on the reverse grinding surface side of the grinding surface P, or laminated other layers such as a support layer on the reverse grinding surface side, as in the polishing pad 10, or may have a single-layer structure consisting only of a grinding layer. It should be noted that, as the polishing pad of the present embodiment, from the viewpoint of more easily improving the grinding uniformity within the surface of the grinding surface, it is particularly preferred to have a laminated structure in which a buffer layer 7 is laminated on the reverse grinding surface side of the grinding layer, such as in the polishing pad 10. In the case where the polishing pad has a laminated structure, a buffer layer or a support layer is laminated on the reverse grinding surface of the grinding layer via a binder or adhesive.

[0065] The C hardness of the buffer layer is preferably 20 to 70. In addition, the material of the buffer layer is not particularly limited. Specifically, for example, a sheet obtained by impregnating a non-woven fabric with a resin, a sheet of an elastomer having a non-foamed structure or a foamed structure, etc. can be cited. More specifically, a composite obtained by impregnating a non-woven fabric with polyurethane; rubbers such as natural rubber, nitrile rubber, polybutadiene rubber, and silicone rubber; thermoplastic elastomers such as polyester thermoplastic elastomers, polyamide thermoplastic elastomers, and fluorine thermoplastic elastomers; foamed plastics; polyurethane and other sheets. Among them, from the viewpoint of easily obtaining preferred softness, a sheet of polyurethane having a foamed structure is particularly preferred.

[0066] Moreover, refer to Figure 1A (b) and Figure 1B The grinding surface P has: a deep groove region G having a first pattern consisting of deep grooves or holes 1 with a depth of 0.3 mm or more; and a terrace region L, which is a region other than the deep groove region G. Figure 1A As shown, in the polishing pad 10, a spiral pattern is formed as a first pattern. The table area L has a shallow depression 2 with a depth of 0.01 to 0.1 mm and a plurality of island-shaped table portions 3 surrounded by the shallow depression 2, and the shallow depression 2 has a second pattern. Here, the island-shaped table portion refers to a convex portion protruding relative to the shallow depression, and is a convex portion having a peripheral edge that is discontinuous and independent from the surrounding table portions. In the polishing pad 10, a triangular lattice pattern is formed as a second pattern. It should be noted that in Figure 1A as well as Figure 1B In the polishing pad 10, the deep groove region G and the shallow depression 2 are formed on the entire polishing surface, but the deep groove region G and the shallow depression 2 are not required to be formed on the entire polishing surface, as long as they are formed at least in the area that contacts the polished substrate.

[0067] Reference Figure 1B , the deep groove or hole 1 forming the deep groove region G is deeper than the shallow depression 2 formed in the terrace region L. Specifically, the depth of the deep groove or hole is 0.3 mm or more, and the depth of the shallow depression is 0.01 to 0.1 mm.

[0068] The deep grooves or holes with a depth of 0.3 mm or more function as a reservoir for holding the slurry during polishing and supplying the slurry to the table area. Such deep grooves or holes with a depth of 0.3 mm or more maintain a sufficient depth to hold the slurry even after a run-in process in which the polishing surface of an unused polishing pad is finely roughened.

[0069] On the other hand, the mesa region having a shallow depression with a depth of 0.01 to 0.1 mm and a plurality of island-shaped mesa portions surrounded by the shallow depressions having a second pattern can shorten the time required for the run-in to finely roughen the grinding surface of an unused grinding pad and the time required for the run-in grinding. Specifically, when the grinding surface is dressed with a pad dresser, the island-shaped mesa portion increases the contact points between the grinding surface and the pad dresser, thereby shortening the time required for the grinding surface to have an appropriate surface roughness.

[0070] The depth of the deep groove or hole formed on the polishing surface is 0.3 mm or more, preferably 0.3 to 3.0 mm, more preferably 0.4 to 2.5 mm, particularly preferably 0.5 to 2.0 mm, and most preferably 0.6 to 1.5 mm. It should be noted that the depth of the deep groove or hole is based on the depth of the deep groove or hole on the surface of the table portion on the polishing surface of the unused polishing pad before the running-in treatment unless otherwise specified.

[0071] When the depth of the deep groove or hole is less than 0.3mm, when the use of the grinding pad is continued, for example, it is easy to wear into a shallow groove or hole less than 0.1mm in a short time of use, so the life of the grinding pad is shortened, or the grinding rate is easy to change. In order to fully keep the slurry, it is preferred to have a depth of at least 0.2mm even at the end of the life of the grinding pad. On the other hand, when the deep groove or hole is too deep, the volume of the deep groove or hole is too large, and it is necessary to supply more slurry when grinding the surface to be ground, so it is not preferred in terms of cost.

[0072] The pattern of the first pattern formed by deep grooves or holes with a depth of 0.3 mm or more is not particularly limited, and may be a regular pattern or an irregular pattern. As a specific example of the pattern of the first pattern, in addition to the spiral pattern, a pattern of grooves or holes for supplying slurry, such as concentric circles, grids, or radial patterns, which are conventionally formed on the polishing surface, may be used without particular limitation. As an example, in Figure 2 , a top view schematically shows a polishing pad 20 having a polishing surface having a deep groove region G formed by concentric deep grooves 11 of a first pattern. The polishing pad 20 is the same as the polishing pad 10 except that the spiral first pattern is changed to a concentric first pattern.

[0073] In addition, the deep groove or hole more than the depth of 0.3mm can be only a deep groove, can be only a hole, and can also be a combination of a deep groove and a hole. In addition, as the shape of the hole, in the grinding surface, shapes such as circle, ellipse, oblong, triangle, quadrilateral can be enumerated.

[0074] In addition, when the polishing pad is a laminated type with a buffer layer, from the viewpoint of easily achieving both polishing uniformity and flattening properties, a deep groove with a depth of preferably 30 to 90% of the thickness of the polishing layer, more preferably 40 to 85%, and particularly preferably 50 to 80% is formed on the polishing surface.

[0075] As the first pattern, from the viewpoint of excellent retention of the slurry and excellent supply of the slurry to the mesa area, a spiral, concentric or lattice pattern is preferred, and a spiral or lattice pattern is particularly preferred. In the case of a spiral, concentric or lattice pattern, there is no particular limitation on the groove pitch and groove width, but from the viewpoint of particularly excellent polishing rate and polishing uniformity, a groove pitch of 1 to 15 mm and a groove width of 0.1 to 4 mm are preferred, a groove pitch of 2 to 12 mm and a groove width of 0.2 to 3 mm are more preferred, and a groove pitch of 3 to 10 mm and a groove width of 0.3 to 2 mm are particularly preferred.

[0076] In addition, refer to Figure 1B In the polishing pad 10, the cross-sectional shape when the deep groove or hole 1 is cut perpendicularly to the length direction is a rectangle. The cross-sectional shape of the deep groove or hole is not particularly limited. Specifically, the cross-sectional shape can be a trapezoid, a triangle, a semicircle, a semi-oblong, etc. in addition to a rectangle.

[0077] From the viewpoint of excellent balance between the retention of the slurry and the grinding rate, the ratio of the projected area of ​​the deep groove area to the total projected area of ​​the grinding surface is preferably 5 to 40%, and more preferably 10 to 30%. Here, the projected area refers to the area when the grinding surface is projected onto a two-dimensional surface. When the ratio of the projected area of ​​the deep groove area to the total projected area of ​​the grinding surface is too low, the retention amount of the slurry decreases during grinding, and there is a tendency for the grinding rate and grinding uniformity to decrease. On the other hand, when the ratio of the projected area of ​​the deep groove area is too high, since the contact area of ​​the table area in contact with the grinding surface being ground during grinding decreases, there is a tendency that the grinding rate is easy to decrease, or the traces of the deep grooves or holes are transferred to the grinding surface and uneven grinding is easy to occur.

[0078] On the other hand, the mesa region L has shallow depressions 2 with a depth of 0.01 to 0.1 mm and a plurality of island-shaped mesa portions 3 surrounded by the shallow depressions 2, wherein the shallow depressions 2 have a second pattern. Figure 1A In the polishing pad 10, shallow depressions 2 having a triangular lattice pattern as a second pattern are formed over the entire surface of the mesa region L. A plurality of island-shaped mesa portions 3 surrounded by the shallow depressions 2 having the second triangular lattice pattern each have a triangle shape, or a shape in which a triangle is divided by deep grooves or holes 1.

[0079] The pattern of the second pattern formed by shallow depressions with a depth of 0.01 to 0.1 mm is not particularly limited, and may be a regular pattern or an irregular pattern. From the viewpoint of excellent productivity and quality management, a regular pattern is preferred. Specific examples of the pattern of the second pattern include, for example, a triangular lattice, an XY lattice, a square lattice, a diamond lattice, a rectangular lattice, a hexagonal lattice, and the like. Among them, in the case where the second pattern has such a pattern, from the viewpoint that the pad dresser can easily and evenly contact the multiple island-shaped table portions surrounded by the shallow depressions from all directions, and the running-in time can be further shortened, a triangular lattice is particularly preferred. In addition, a triangular lattice pattern can be formed by a combination of straight shallow depressions, and is therefore easy to form by cutting, and is preferred from this viewpoint.

[0080] Moreover, the shapes of the multiple island-shaped terrace portions surrounded by shallow depressions are triangles when the second pattern is a triangular lattice, squares when the second pattern is a square lattice, rhombuses when the second pattern is a rhombus lattice, and hexagons when the second pattern is a hexagonal lattice.

[0081] Figure 3A FIG. 1 is a partially enlarged schematic diagram of the polishing surface of the polishing pad 30 according to another example of the present embodiment. Figure 3B 2 is a schematic cross-sectional view of the polishing pad 30. The polishing pad 30 is the same as the polishing pad 10 except that the second pattern in the shape of a triangular lattice is changed to a second pattern in the shape of a square lattice. Figure 3A This is a partially enlarged schematic diagram of the polishing pad 30 when viewed from the polishing surface side as one side of the polishing layer. Figure 3B yes Figure 3A Schematic cross-sectional view of section III-III'.

[0082] The polishing surface of the polishing pad 30 is provided with shallow depressions 12 having a second pattern in a square grid shape. A plurality of island-shaped terrace portions 13 surrounded by the shallow depressions 12 have a square shape or a square shape divided by deep grooves or holes 1 .

[0083] in addition, Figure 4 A partially enlarged schematic diagram of the polishing surface of a polishing pad 40 of another example of the present embodiment is shown. The polishing pad 40 is the same polishing pad as the polishing pad 10 except that the second pattern in the shape of a triangular lattice is changed to a second pattern in the shape of a rhombus lattice. On the polishing surface of the polishing pad 40, shallow depressions 22 having a second pattern in the shape of a rhombus lattice are formed, and a plurality of island-shaped mesa portions 23 surrounded by the shallow depressions 22 have a rhombus shape or a shape in which a rhombus is divided by deep grooves or holes 1.

[0084] The depth of the shallow depression formed in the table area is 0.01 to 0.1 mm, preferably 0.02 to 0.09 mm, more preferably 0.03 to 0.08 mm, and particularly preferably 0.04 to 0.07 mm. The depth of the shallow depression is 0.01 to 0.1 mm, and thus, in the running-in or running-in grinding for making the unused polishing pad become a roughness suitable for grinding, the island-shaped table portion is worn in a short time, thus shortening the time for forming a roughness suitable for grinding. It should be noted that the depth of the shallow depression is also the same, unless otherwise specified, based on the depth of the shallow depression on the surface of the table portion on the grinding surface of the unused polishing pad before the running-in process.

[0085] When the depth of the shallow depression formed in the mesa area exceeds 0.1 mm, the time required for running-in or running-in polishing becomes longer, or the mesa portion remaining after running-in changes the slurry retention or the contact area with the polished surface during polishing, and the polishing characteristics are likely to change over time. In addition, when the depth of the shallow depression is less than 0.01 mm, since the height difference between the mesa portion and the shallow depression is small, the effect of the dresser and the mesa portion in concentrated contact is reduced, and the time required for running-in or running-in polishing becomes longer.

[0086] When the shallow depressions are in a lattice shape such as a triangular lattice shape, a rectangular lattice shape, or a hexagonal lattice shape, there are no particular restrictions on the pitch and width of the shallow depressions. Figure 5 , in the case of a rectangular grid, refer to Figure 6 , in the case of a hexagonal grid, refer to Figure 7 as well as Figure 8 In the case of , the spacing (P1, P2, P3, P4) is preferably 1 to 8 mm, more preferably 2 to 6 mm. In addition, the width (W1, W2, W3, W4) is preferably 0.5 to 4 mm, more preferably 1 to 2 mm. From the perspective of easily forming a table portion that the pad dresser can easily and evenly contact, such a spacing and width are preferred.

[0087] In addition, refer to Figures 5 to 8 The pad dresser can easily and evenly contact each of the table surfaces surrounded by the shallow depressions, and the table surfaces are quickly worn, thereby further shortening the time for forming a roughness suitable for grinding. From this point of view, the maximum distance of a table surface, that is, the maximum distance of the table surface in the horizontal direction (M1, M2, M3, M4) is less than 8 mm, preferably 0.5-6 mm, more preferably 0.7-5 mm, particularly preferably 1-4.5 mm, and most preferably 1.5-4 mm.

[0088] In addition, the projected area of ​​one island-shaped terrace portion is preferably 0.3 mm to 10 mm. 2 , more preferably 0.5 to 9 mm2 , particularly preferably 1 to 7 mm 2 , the most preferred is 1.5 to 5 mm 2 When the projection area of ​​one island-shaped land portion is within such a range, the pad conditioner can easily contact each of the land portions surrounded by the shallow recess, and the running-in time can be further shortened, which is preferable from this point of view.

[0089] If the maximum distance of an island-shaped table portion, i.e., the maximum distance of the table portion in the horizontal direction, exceeds 8 mm, or the projection area of ​​a table portion is too large, it is difficult for the pad dresser to uniformly contact the vicinity of the center of the table portion, and the table portion is easily worn out over time. In addition, if the maximum distance of an island-shaped table portion, i.e., the maximum distance of the table portion in the horizontal direction, is too small, or the projection area of ​​a table portion is too small, there is a tendency that the formation of shallow depressions becomes complicated.

[0090] In addition, the ratio of the total projection area of ​​the table portion to the total projection area of ​​the table region is preferably 10 to 50%, more preferably 15 to 45%, and particularly preferably 20 to 40%. Here, the ratio of the total projection area of ​​the table portion refers to the ratio of the total projection area of ​​each table portion to the total projection area of ​​the table region when the table region is projected two-dimensionally without considering the concavity and convexity of the grinding surface. When the ratio of the total projection area of ​​the table portion is within such a range, the dresser can easily contact each of the table portions surrounded by shallow depressions, and the time for forming a roughness suitable for grinding can be further shortened, which is preferred from this point of view.

[0091] It should be noted that in shallow depressions such as Figure 5 In the case of a triangular lattice shape surrounding an equilateral triangle, the maximum horizontal distance M1 of one island-shaped table portion, the projection area S1 of one island-shaped table portion, and the ratio R1 of the total projection area of ​​the table portions can be calculated by the following formula.

[0092] [Number 1]

[0093] Maximum horizontal distance of the table top

[0094] The projected area of ​​one island-shaped tabletop

[0095] Ratio of the total projected area of ​​the table portion (%) R1 = ((P1-W1) / P1) 3 ×100

[0096] It should be noted that in shallow depressions such as Figure 6When a square grid is shown, the maximum horizontal distance M2 of one island-shaped terrace portion, the projection area S2 of one island-shaped terrace portion, and the ratio R2 of the total projection area of ​​the terrace portions can be calculated by the following formula.

[0097] [Number 2]

[0098] Maximum horizontal distance of the table top

[0099] The projected area of ​​an island-shaped table surface S2 = (P2-W2) 2

[0100] Ratio of the total projected area of ​​the table portion (%) R2 = ((P2-W2) / P2) 2 ×100

[0101] In addition, in Figure 7 When the table portion shown is a circle arranged in a regular hexagonal lattice, the maximum horizontal distance M3 of one island-shaped table portion, the projection area S3 of one island-shaped table portion, and the ratio R3 of the total projection area of ​​the table portion can be calculated by the following formula.

[0102] [Number 3]

[0103] The maximum horizontal distance of the table surface is M3 = P3-W3

[0104] The projected area of ​​one island-shaped table portion S3 = (π / 4) × (P3-W3) 2

[0105] Ratio of the total projected area of ​​the table surface (%)

[0106] In addition, the table surface is as follows Figure 8 When the arrangement is a regular hexagon in a regular hexagonal lattice, the maximum horizontal distance M4 of one island-shaped table portion, the projection area S4 of one island-shaped table portion, and the ratio R4 of the total projection area of ​​the table portions can be calculated by the following formula.

[0107] [Number 4]

[0108] Maximum horizontal distance of the table top

[0109] The projected area of ​​one island-shaped tabletop

[0110] Ratio of the total projected area of ​​the table portion (%) R4 = ((P4-W4) / P4) 2 ×100

[0111] In addition, refer to Figure 1BIn the polishing pad 10, the cross-sectional shape when the shallow depression is cut perpendicularly to the length direction is a rectangle. The cross-sectional shape of the shallow depression of the polishing pad is not particularly limited. Specifically, the cross-sectional shape can be a trapezoid, a triangle, a semicircle, a semi-oblong, a sine curve, etc. in addition to a rectangle.

[0112] The formation method of the deep groove area and the mesa area of ​​the grinding surface of the grinding layer of the grinding pad of the present embodiment is not particularly limited. In addition, the deep groove area and the mesa area can be formed by a separate process respectively, or can be formed simultaneously by a single process. In addition, when formed by a separate process, any one of the deep groove area and the mesa area can also be formed first.

[0113] The method for forming the opening of the first pattern formed by deep grooves or holes of 0.3 mm or more, i.e., the deep groove area, is not particularly limited. Specifically, for example, a method for forming deep grooves or holes by cutting one side of a grinding layer sheet; a method for forming deep grooves or holes by melting or volatilizing a polymer by transfer processing, wherein a heated mold or metal wire is pressed and contacted with one side of a grinding layer sheet; a method for forming deep grooves or holes by decomposing or volatilizing a polymer by laser processing on one side of a grinding layer sheet; a method for forming a grinding layer sheet having a grinding surface with deep grooves or holes by using a mold having a convex portion formed in advance for forming deep grooves or holes, etc.

[0114] In addition, the method for forming the mesa region having a shallow depression with a depth of 0.01 to 0.1 mm and a second pattern formed on the grinding surface of the grinding layer and a plurality of island-shaped mesa portions surrounded by the shallow depression is also not particularly limited. Specifically, for example, a method for forming a shallow depression by cutting one side of a grinding layer sheet along the shape of a specified second pattern; a method for forming a shallow depression by melting or volatilizing a polymer by transfer processing, wherein the heated mold or metal wire is pressed and contacted with one side of a circular polymer sheet forming the grinding layer; a method for forming a shallow depression by laser processing on one side of a polymer sheet forming a circle of the grinding layer to decompose or volatilize the polymer; a method for forming a shallow depression by pre-forming a convex portion for forming a shallow depression on a mold when forming a circular polymer sheet forming a grinding layer, and forming a shallow depression when the polymer sheet is formed, etc. Among them, from the viewpoint of excellent productivity, a method for forming a shallow depression by cutting or a method for forming a shallow depression by transfer processing is preferred, and from the viewpoint of excellent processing accuracy of the shallow depression, a cutting method is particularly preferred.

[0115] It should be noted that as a method for forming shallow depressions by cutting, for example, a method of using a tool such as a turning tool to cut straight shallow depressions with a depth of 0.01 to 0.1 mm on one side of a polymer sheet can be cited, wherein a plurality of straight shallow depressions are combined to form shallow depressions with a depth of 0.01 to 0.1 mm having a second pattern.

[0116] In addition, as a method for forming shallow depressions by transfer processing, for example, the following methods can be cited. (1) A method for forming a sheet for a grinding layer by injection molding a polymer material for forming a grinding layer using a mold, wherein the mold has a shape on the surface of the cavity consisting of convex portions that are the inversion of the shape of the shallow depression having a second pattern; (2) A method for forming a polymer sheet having shallow depressions having a second pattern by melting and extruding the polymer material for forming the grinding layer using an extruder equipped with a T-die and pressing the sheet onto a cooling roller, wherein the cooling roller has a shape on the surface consisting of convex portions that are the inversion of the shape of the shallow depression having the second pattern; (3) A method for forming a polymer sheet having shallow depressions having a second pattern by stamping the heated mold. and contacting with one side of a pre-made grinding layer sheet to melt or volatilize the polymer to form a shallow depression having a second pattern, wherein the mold has a shape on the surface consisting of convex portions that are the inversion of the shape of the shallow depression having the second pattern; (4) using reaction injection molding (RIM), filling uncured resin in the mold and curing it, thereby manufacturing a polymer sheet with a grinding surface in one stage, wherein the grinding surface has a table area consisting of a shallow depression and a plurality of table portions, and the mold has a shape on the cavity surface consisting of convex portions that are the inversion of the shape of the shallow depression having the second pattern.

[0117] The polishing pad of the present embodiment described above is preferably used for CMP. Next, one embodiment of CMP using the polishing pad 10 of the present embodiment will be described.

[0118] In CMP, a CMP apparatus 100 can be used. The CMP apparatus 100 includes: Fig. 9 As shown, there is a circular rotating platform 101, a slurry supply nozzle 102, a carrier 103, and a pad conditioner 104. The polishing pad 10 is attached to the surface of the rotating platform 101 by a double-sided adhesive sheet or the like. In addition, the carrier 103 supports the substrate 50 to be polished.

[0119] In the CMP device 100, the rotating platform 101 is rotated by a motor (not shown), for example, in the direction indicated by the arrow. In addition, the carrier 103 is rotated by a motor (not shown), for example, in the direction indicated by the arrow, while the polished surface of the polished substrate 50 is pressed against the polishing surface of the polishing pad 10. The pad dresser 104 is rotated, for example, in the direction indicated by the arrow. When the diameter of the pad dresser 104 is smaller than the diameter of the polished substrate 50, the pad dresser 104 is swung in the radial direction of the rotating platform 101 in order to make the entire area of ​​the polishing pad in contact with the polished material have a roughness suitable for polishing.

[0120] When an unused polishing pad is used, a dressing process called running-in is usually performed to finely roughen the polishing surface of the polishing pad to a roughness suitable for polishing before the polished substrate is polished. Specifically, while water is passed through the surface of the polishing pad 10 that is fixed on the rotating platform 101 and rotates, a pad dresser 104 for CMP is pressed to dress the surface of the polishing pad 10. As the pad dresser, for example, a pad dresser that fixes diamond particles on the carrier surface by nickel electrodeposition or the like can be used.

[0121] In the case of a polishing pad having a high-hardness polishing layer, there is a problem of the time required for dressing, i.e., running-in, for forming a roughness suitable for grinding on the polishing surface of an unused polishing pad. In addition, in the polishing after running-in, sometimes the running-in polishing before the polishing characteristics are stabilized also requires time. According to the polishing pad of this embodiment, by providing a mesa region having a shallow depression with a depth of 0.01 to 0.1 mm having a second pattern and a plurality of island-shaped mesa portions surrounded by the shallow depression on the polishing surface of the unused polishing pad, the pad dresser can easily contact the plurality of island-shaped mesa portions surrounded by the shallow depression evenly from all directions, thereby shortening the running-in time. Fig. 10A as well as Fig. 10B It is an explanatory diagram for explaining the change of the polishing surface of the polishing pad 10 according to the present embodiment during the running-in. Fig. 10A Shows before trimming, Fig. 10B A portion of the ground surface after trimming is shown. Fig. 10A Before the dressing shown in the figure, the grinding surface P has: a deep groove area G having a first pattern consisting of deep grooves or holes 1 with a depth of 0.3 mm or more; and a mesa area L, which is an area other than the deep groove area G. Moreover, by performing the dressing, the multiple island-shaped mesa portions 3 surrounded by the shallow depressions 2 of the mesa area L are gradually worn, and the shallow depressions 2 gradually become shallower. Moreover, by continuing the dressing, as shown in FIG. Fig. 10B As shown, the island-shaped table portion 3 is worn and becomes lower, and similarly, the shallow depression 2 is also shallower. In the polishing pad of this embodiment, the area that needs to be dressed can be reduced in the polishing surface of the unused polishing pad, and the pad dresser is easy to hang on the periphery of the island-shaped table portion, and the friction force becomes larger, so the running-in time can be shortened.

[0122] There is no particular limitation, but when the average depth of the shallow depression is less than 0.01mm, the effect of the shallow depression is substantially reduced, and the grinding characteristics are stable. The conditions for such dressing are not particularly limited, but from the viewpoint of terminating the startup process of the grinding pad in a short time and stabilizing the grinding characteristics, the type of pad dresser and the dressing load and rotation speed are selected, so that the cumulative dressing time until the average depth of the shallow depression is less than 0.01mm is preferably within 30 minutes, more preferably 1 to 20 minutes, and particularly preferably 2 to 15 minutes. It should be noted that it is also possible to increase the dressing load or rotation speed only during the startup process of the grinding pad to promote the wear of the island-shaped table surface.

[0123] As the type of pad dresser, diamond grain size #60 to #200 is preferred, but it can be appropriately selected according to the resin composition of the grinding layer or the grinding conditions. In addition, as the dressing load, it depends on the diameter of the dresser. In the case of a diameter of less than 150 mm, it is preferably 5 to 50 N, in the case of a diameter of 150 to 250 mm, it is preferably 10 to 250 N, and in the case of a diameter of more than 250 mm, it is preferably about 50 to 300 N. In addition, as the rotation speed, it is preferred that the dresser and the platen are 10 to 200 rpm respectively, but in order to prevent synchronization of rotation, it is preferred that the rotation speeds of the dresser and the platen are different.

[0124] Moreover, after the running-in is completed, the grinding of the polished surface of the polished substrate is started. During the grinding, slurry is supplied to the surface of the rotating polishing pad from the slurry supply nozzle. The slurry contains a liquid medium such as water or oil; an abrasive such as silicon dioxide, aluminum oxide, cerium oxide, zirconium oxide, silicon carbide; an alkali, an acid, a surfactant, an oxidizing agent, a reducing agent, a chelating agent, etc. In addition, when performing CMP, lubricating oil, a coolant, etc. can also be used together with the slurry as needed. Moreover, the polished substrate fixed on the carrier and rotating is pressed against the polishing pad with the slurry spread on the grinding surface. Moreover, the grinding process is continued until a specified flatness or grinding amount is obtained. The processing quality is affected by adjusting the pushing force applied during grinding or the speed of the relative movement of the rotating platform and the carrier.

[0125] The grinding conditions are not particularly limited, but in order to effectively grind, the rotating speed of the preferred platform and the ground substrate is a low rotation of less than 300 rpm. In addition, the pressure applied to the ground substrate for crimping on the grinding pad is preferably set to less than 150 kPa from the viewpoint of not generating damage after grinding. In addition, during grinding, preferably, the slurry is continuously or discontinuously supplied to the grinding pad in such a way that the slurry is spread over the grinding surface.

[0126] After the polishing is completed, the polished substrate is fully cleaned, and then water droplets attached to the polished substrate are shaken off using a spin dryer or the like to dry the substrate. In this way, the polished surface becomes a smooth surface.

[0127] Such a CMP of this embodiment is preferably used for polishing in the manufacturing process of various semiconductor devices, MEMS (MicroElectro Mechanical Systems), etc. Examples of polishing objects include semiconductor substrates such as silicon, silicon carbide, gallium nitride, gallium arsenide, gallium, zinc oxide, sapphire, germanium, diamond, etc.; insulating films such as silicon oxide film, silicon nitride film, low-k film, etc. formed on a wiring board with specified wiring; wiring materials such as copper, aluminum, tungsten, etc.; glass, crystal, optical substrates, hard disks, etc. The polishing pad of this embodiment is particularly preferably used for polishing insulating films or wiring materials formed on semiconductor substrates.

[0128] Example

[0129] Hereinafter, the present invention will be described in more detail by way of examples. It should be noted that the scope of the present invention is not limited to these examples.

[0130] [Manufacturing Example 1]

[0131] Polytetramethylene glycol [abbreviated as PTMG] with a number average molecular weight of 850, polyethylene glycol [abbreviated as PEG] with a number average molecular weight of 600, 1,4-butanediol [abbreviated as BD], and 4,4'-diphenylmethane diisocyanate [abbreviated as MDI] are mixed in a mass ratio of PTMG:PEG:BD:MDI of 24.6:11.6:13.8:50.0, and continuously supplied to a coaxially rotating twin-screw extruder through a metering pump to continuously melt-polymerize thermoplastic polyurethane. Then, the melt of the polymerized thermoplastic polyurethane is continuously extruded into water in the form of strands, and then finely pulverized by a granulator to obtain pellets. After the pellets are dehumidified and dried at 70°C for 20 hours, they are supplied to a single screw extruder and extruded from a T-die to form a sheet with a thickness of 2.0 mm. The surface of the obtained sheet was then ground to form a uniform sheet with a thickness of 1.5 mm, which was then cut into a circular shape with a diameter of 38 cm to obtain a polishing layer sheet. The D hardness of the polishing layer sheet measured at a measurement temperature of 25° C. according to JIS K 7311 was 67.

[0132] [Manufacturing Example 2]

[0133] PTMG, PEG, BD, and MDI are mixed in a ratio of 19.5:9.2:16.4:54.9 of the mass ratio of PTMG:PEG:BD:MDI, and are continuously supplied to a coaxially rotating twin-screw extruder through a metering pump to continuously melt-polymerize thermoplastic polyurethane. Then, the melt of the polymerized thermoplastic polyurethane is continuously extruded into water in the form of strands, and then finely crushed with a granulator to obtain particles. After the particles are dehumidified and dried at 70°C for 20 hours, they are supplied to a single screw extruder and extruded from a T die to form a sheet with a thickness of 2.0 mm. Then, the surface of the obtained sheet is ground to form a uniform sheet with a thickness of 1.5 mm, and then cut into a circular shape with a diameter of 38 cm, thereby obtaining a sheet for a grinding layer. Based on JIS K 7311, the D hardness of the grinding layer sheet measured at a measurement temperature of 25°C is 76.

[0134] [Example 1]

[0135] On the grinding surface of one side of the grinding layer sheet obtained in the manufacturing example 1, the thickness of 1.5mm and the diameter of 38cm, a spiral deep groove with a width of 0.7mm, a depth of 1.0mm and a groove spacing of 9.0mm is formed by cutting. It should be noted that the cross-sectional shape of the deep groove is a rectangle. At this time, the area of ​​the deep groove region is 8% relative to the ratio of the total area of ​​the grinding surface.

[0136] Then, on the grinding surface formed with deep grooves, a triangular grid-shaped shallow depression consisting of multiple straight lines with a width of 1.0 mm, a depth of 0.08 mm, and a spacing of 4.0 mm is formed by cutting. The cross-sectional shape of the shallow depression is also a rectangle. In this way, a plurality of island-shaped mesa portions with a side length of 3.0 mm surrounded by a plurality of shallow depressions are formed. The projected area of ​​an island-shaped mesa portion is 3.9 mm. 2 The maximum horizontal distance of an island-shaped mesa portion is 3.0 mm. In addition, the ratio of the total projection area of ​​the mesa portion to the total projection area of ​​the mesa region is 42%. The enlarged photograph of the polishing surface of the polishing pad obtained is Fig.11 It should be noted that the surface roughness of the terrace region was measured using a surface roughness measuring instrument ("Roughness Tester SJ-210" manufactured by Mitutoyo Co., Ltd.) based on JIS B 0601:2001 and JIS B 0671:2002. The results showed that the arithmetic mean roughness Ra was 9.8 μm, the maximum height Rz was 55.0 μm, and the protruding peak height Rpk was 13.2 μm.

[0137] It should be noted that the depth of the shallow depression and deep groove was measured using a depth gauge "E-DP2J" manufactured by Nakamura Manufacturing Co., Ltd., and the average was taken at 8 points in the part in contact with the wafer. In addition, the projected area of ​​an island-shaped terrace portion and the maximum horizontal distance of an island-shaped terrace portion were measured using a ruler "No. 1983" manufactured by Tokai Sangyo Co., Ltd. Figure 5 P1 and W1 can be obtained from the formula in equation 1.

[0138] Then, a buffer layer was laminated with a double-sided adhesive sheet on the back side of the grinding surface of the grinding layer to make a multilayer grinding pad. As a buffer layer, "POLON H48" made by (company) Inoac Co., Ltd., which is a foamed polyurethane film with a thickness of 0.8 mm, was used. Then, the grinding characteristics of the obtained grinding pad were evaluated by the following evaluation method.

[0139] <Grinding speed and dressing time until shallow pits disappear>

[0140] The obtained polishing pad was mounted on a polishing device "MAT-BC15" manufactured by M.A.T. Then, a slurry having a pH of about 12 was prepared by diluting the slurry "SS-25" manufactured by Robot Microelectronics Co., Ltd. by 2 times, and the slurry was supplied to the polishing surface of the polishing pad at a speed of 120 mL / min while polishing a 4-inch diameter silicon wafer having a silicon oxide film with a film thickness of 1000 nm on the surface for 60 seconds under the conditions of a platen speed of 100 rpm, a head speed of 99 rpm, and a polishing pressure of 41.4 kPa.

[0141] Then, use pad dresser (diamond dresser (diamond grain size #100, base metal diameter 19cm) of (company) ALMT system), under the condition of dresser rotating speed 70rpm, grinding pad rotating speed 100rpm, dresser load 20N, flow pure water with the speed of 150mL / minute, dress the surface of grinding pad for 30 seconds. Then, grind other silicon wafers again, further carry out 30 seconds dressing. Like this, grind 100 silicon wafers. Then, measure the film thickness of silicon oxide film before and after grinding of the silicon wafer that is ground into the 3rd, 5th, 10th, 15th, 25th, 50th, 100th, obtain grinding speed. In addition, every 2 grindings measure the depth of shallow depression, obtain the cumulative dressing time when being less than 0.01mm.

[0142] The results are shown in Table 1. In addition, Fig.12 2 shows an enlarged photograph of the polished surface after polishing 10 silicon wafers using the polishing pad of Example 1. It can be seen that the polished surface is fully mixed with water, the polished surface is finely roughened by the dresser, and the slurry retention is excellent.

[0143] [Table 1]

[0144]

[0145] [Example 2]

[0146] On the grinding surface of one side of the grinding layer sheet with a thickness of 1.5 mm and a diameter of 38 cm obtained in the manufacturing example 1, a spiral deep groove with a width of 0.7 mm, a depth of 1.0 mm and a groove spacing of 4.5 mm is formed by cutting. It should be noted that the cross-sectional shape of the deep groove is a rectangle. At this time, the ratio of the area of ​​the deep groove to the total area of ​​the grinding surface is 16%.

[0147] Then, on the entire surface of the grinding surface formed with deep grooves, a triangular grid-shaped shallow depression consisting of multiple straight lines with a width of 1.0 mm, a depth of 0.04 mm, and a spacing of 3.0 mm is further formed by cutting. The cross-sectional shape of the shallow depression is also a rectangle. In this way, a plurality of island-shaped regular triangle table portions with a side length of 1.9 mm surrounded by a plurality of shallow depressions are formed. The projected area of ​​an island-shaped table portion is 1.5 mm 2 The maximum horizontal distance of an island-shaped mesa portion is 1.9 mm, and the ratio of the total projection area of ​​the mesa portion to the total projection area of ​​the mesa region is 30%.

[0148] Then, using the obtained polishing layer, a polishing pad was prepared in the same manner as in Example 1 and evaluated. The results are shown in Table 1.

[0149] [Example 3]

[0150] Instead of forming shallow depressions in a triangular lattice formed by a plurality of straight lines with a width of 1.0 mm, a depth of 0.04 mm, and a spacing of 3.0 mm on the grinding surface in Example 2, a grinding layer was manufactured in the same manner except that shallow depressions in a triangular lattice formed by a plurality of straight lines with a width of 1.5 mm, a depth of 0.06 mm, and a spacing of 5.5 mm were formed. The cross-sectional shape of the shallow depressions is a rectangle. On the grinding surface, a plurality of island-shaped equilateral triangular table portions with a side length of 3.9 mm surrounded by a plurality of shallow depressions are formed. The projected area of ​​one island-shaped table portion is 6.7 mm. 2 The maximum horizontal distance of an island-shaped table portion is 3.9 mm, and the ratio of the total projection area of ​​the table portion to the total projection area of ​​the table region is 38%. In this way, the polishing layer is manufactured.

[0151] Then, using the obtained polishing layer, a polishing pad was prepared in the same manner as in Example 1 and evaluated. The results are shown in Table 1.

[0152] [Example 4]

[0153] Instead of forming triangular lattice-shaped shallow depressions consisting of a plurality of straight lines with a width of 1.0 mm, a depth of 0.04 mm, and a spacing of 3.0 mm on the grinding surface in Example 2, an XY lattice-shaped shallow depression consisting of a plurality of straight lines with a width of 1.0 mm, a depth of 0.03 mm, and a spacing of 2.5 mm is formed, and the grinding layer is manufactured in the same manner except that. The cross-sectional shape of the shallow depression is a rectangle. On the grinding surface, a plurality of island-shaped square table portions with a side length of 1.5 mm surrounded by a plurality of shallow depressions are formed. The projected area of ​​one island-shaped table portion is 2.3 mm 2 The maximum horizontal distance of an island-shaped mesa portion is 2.1 mm, and the ratio of the total projection area of ​​the mesa portion to the total projection area of ​​the mesa region is 36%. Thus, the polishing layer is manufactured.

[0154] Then, using the obtained polishing layer, a polishing pad was prepared in the same manner as in Example 1 and evaluated. The results are shown in Table 1.

[0155] [Example 5]

[0156] On the grinding surface of one side of the grinding layer sheet obtained in the manufacturing example 1, the thickness of 1.5mm and the diameter of 38cm, a plurality of concentric deep grooves with a width of 0.3mm, a depth of 1.0mm and a groove spacing of 2.5mm are formed by cutting. It should be noted that the cross-sectional shape of the deep groove is a rectangle. At this time, the area of ​​the deep groove is 12% relative to the total area of ​​the grinding surface.

[0157] Then, on the entire surface of the grinding surface formed with deep grooves, a triangular grid-shaped shallow depression consisting of multiple straight lines with a width of 2.0 mm, a depth of 0.05 mm, and a spacing of 4.5 mm is further formed by cutting. The cross-sectional shape of the shallow depression is also a rectangle. In this way, a plurality of island-shaped regular triangle table portions with a side length of 2.2 mm surrounded by a plurality of shallow depressions are formed. The projected area of ​​an island-shaped table portion is 2.0 mm 2 The maximum horizontal distance of an island-shaped mesa portion is 2.2 mm, and the ratio of the total projection area of ​​the mesa portion to the total projection area of ​​the mesa region is 17%.

[0158] Then, using the obtained polishing layer, a polishing pad was prepared in the same manner as in Example 1 and evaluated. The results are shown in Table 1.

[0159] [Example 6]

[0160] Instead of forming shallow depressions in a triangular lattice formed by a plurality of straight lines with a width of 1.0 mm, a depth of 0.04 mm, and a spacing of 3.0 mm on the grinding surface in Example 2, a grinding layer was manufactured in the same manner except that shallow depressions in a triangular lattice formed by a plurality of straight lines with a width of 2.0 mm, a depth of 0.05 mm, and a spacing of 9.0 mm were formed. The cross-sectional shape of the shallow depressions is a rectangle. On the grinding surface, a plurality of island-shaped equilateral triangular table portions with a side length of 7.1 mm surrounded by a plurality of shallow depressions are formed. The projected area of ​​one island-shaped table portion is 22.0 mm 2 The maximum horizontal distance of an island-shaped mesa portion is 7.1 mm, and the ratio of the total projection area of ​​the mesa portion to the total projection area of ​​the mesa region is 47%. Thus, the polishing layer is manufactured.

[0161] Then, using the obtained polishing layer, a polishing pad was prepared in the same manner as in Example 1 and evaluated. The results are shown in Table 1.

[0162] [Example 7]

[0163] Instead of forming triangular lattice-shaped shallow depressions consisting of a plurality of straight lines with a width of 1.0 mm, a depth of 0.04 mm, and a spacing of 3.0 mm on the grinding surface in Example 2, an XY lattice-shaped shallow depression consisting of a plurality of straight lines with a width of 2.0 mm, a depth of 0.05 mm, and a spacing of 7.0 mm is formed, and the grinding layer is manufactured in the same manner except that. The cross-sectional shape of the shallow depression is a rectangle. On the grinding surface, a plurality of island-shaped square table portions with a side length of 5.0 mm surrounded by a plurality of shallow depressions are formed. The projected area of ​​one island-shaped table portion is 25.0 mm. 2 The maximum horizontal distance of an island-shaped mesa portion is 7.1 mm, and the ratio of the total projection area of ​​the mesa portion to the total projection area of ​​the mesa region is 51%.

[0164] Then, using the obtained polishing layer, a polishing pad was prepared in the same manner as in Example 1 and evaluated. The results are shown in Table 1.

[0165] [Embodiment 8]

[0166] On the grinding surface of one side of the grinding layer sheet with a thickness of 1.5 mm and a diameter of 38 cm obtained in the manufacturing example 2, a spiral deep groove with a width of 1.5 mm on the upper surface, a width of 0.5 mm on the bottom surface, a depth of 0.8 mm, and a groove spacing of 7.0 mm is formed by cutting. It should be noted that the cross-sectional shape of the deep groove is a trapezoid. At this time, the area of ​​the deep groove region is 21% relative to the total area of ​​the grinding surface.

[0167] Then, on the entire surface of the grinding surface formed with deep grooves, a triangular grid-shaped shallow depression is formed by cutting, which is composed of multiple straight lines with a width of 1.0 mm on the upper surface, a width of 0.9 mm on the bottom surface, a depth of 0.05 mm, and a spacing of 2.5 mm. The cross-sectional shape of the shallow depression is a trapezoid. In this way, a plurality of island-shaped regular triangle table portions with a side length of 1.3 mm surrounded by a plurality of shallow depressions are formed. The projected area of ​​an island-shaped table portion is 0.8 mm 2 The maximum horizontal distance of an island-shaped mesa portion is 1.3 mm, and the ratio of the total projection area of ​​the mesa portion to the total projection area of ​​the mesa region is 22%.

[0168] Then, using the obtained polishing layer, a polishing pad was prepared in the same manner as in Example 1 and evaluated. The results are shown in Table 1.

[0169] [Example 9]

[0170] Instead of forming shallow depressions in a triangular lattice on the grinding surface consisting of a plurality of straight lines with a width of 1.0 mm on the upper surface, a width of 0.9 mm on the bottom surface, a depth of 0.05 mm, and a spacing of 2.5 mm in Example 8, a grinding layer was manufactured in the same manner except that shallow depressions in a triangular lattice consisting of a plurality of straight lines with a width of 1.5 mm, a depth of 0.03 mm, and a spacing of 6.0 mm were formed. The cross-sectional shape of the shallow depressions is a rectangle. On the grinding surface, a plurality of island-shaped equilateral triangular table portions with a side length of 4.5 mm surrounded by a plurality of shallow depressions are formed. The projected area of ​​one island-shaped table portion is 8.8 mm 2 The maximum horizontal distance of an island-shaped mesa portion is 4.5 mm, and the ratio of the total projection area of ​​the mesa portion to the total projection area of ​​the mesa region is 42%.

[0171] Then, using the obtained polishing layer, a polishing pad was prepared in the same manner as in Example 1 and evaluated. The results are shown in Table 1.

[0172] [Example 10]

[0173] Instead of forming triangular lattice-shaped shallow depressions on the grinding surface consisting of a plurality of straight lines with a width of 1.0 mm on the upper surface, a width of 0.9 mm on the bottom surface, a depth of 0.05 mm, and a spacing of 2.5 mm in Example 8, an XY lattice-shaped shallow depression is formed consisting of a plurality of straight lines with a width of 1.0 mm on the upper surface, a width of 0.9 mm on the bottom surface, a depth of 0.05 mm, and a spacing of 3.0 mm, and the grinding layer is manufactured in the same manner except that the cross-sectional shape of the shallow depression is a trapezoid. On the grinding surface, a plurality of island-shaped square table portions with a side length of 2.0 mm surrounded by a plurality of shallow depressions are formed. The projected area of ​​one island-shaped table portion is 4.0 mm 2The maximum horizontal distance of an island-shaped mesa portion is 2.8 mm, and the ratio of the total projection area of ​​the mesa portion to the total projection area of ​​the mesa region is 44%. Thus, the polishing layer is manufactured.

[0174] Then, using the obtained polishing layer, a polishing pad was prepared in the same manner as in Example 1 and evaluated. The results are shown in Table 1.

[0175] [Example 11]

[0176] At 150°C, a SUS punching plate (hole shape: circle with a diameter of 1.5 mm, hole arrangement: hexagonal grid, hole spacing: 2.5 mm, opening ratio: 33%) was pressed onto the entire surface of the grinding surface of one side of the grinding layer sheet with a thickness of 1.5 mm and a diameter of 38 cm obtained in Manufacturing Example 2 by hot pressing to form shallow depressions. A plurality of island-shaped circular mesa portions with a diameter of 1.5 mm surrounded by a plurality of shallow depressions were formed. The projected area of ​​one island-shaped mesa portion is 1.8 mm 2 The maximum horizontal distance of an island-shaped table portion is 1.5 mm, and the ratio of the total projection area of ​​the table portion to the total projection area of ​​the table region is 33%.

[0177] Then, on the grinding surface, a spiral deep groove with a width of 2.0 mm on the upper surface, a width of 1.0 mm on the bottom surface, a depth of 0.8 mm, and a groove spacing of 7.0 mm is formed by cutting. It should be noted that the cross-sectional shape of the deep groove is a trapezoid. At this time, the area of ​​the deep groove region is 29% relative to the total area of ​​the grinding surface. The grinding layer is manufactured in this way.

[0178] Then, using the obtained polishing layer, a polishing pad was prepared in the same manner as in Example 1 and evaluated. The results are shown in Table 1.

[0179] [Comparative Example 1]

[0180] The polishing layer was manufactured in the same manner as in Example 1 except that the shallow depression was not formed in Example 1. Then, the polishing pad was manufactured in the same manner as in Example 1 using the obtained polishing layer and evaluated. The results are shown in Table 2. The enlarged photograph of the polishing surface of the obtained polishing pad is shown in Table 2. Fig.13 It should be noted that the surface roughness of the table area was measured using a surface roughness measuring instrument ("Roughness Tester JJ-210" manufactured by Mitutoyo Company) based on JIS B 0601:2001 and JIS B 0671:2002. The results showed that the arithmetic mean roughness Ra was 0.2 μm, the maximum height Rz was 1.8 μm, and the protruding peak height Rpk was 0.4 μm. In addition, Fig.142 shows an enlarged photograph of the polishing surface after polishing 10 wafers with the polishing pad of Comparative Example 1. It can be seen that the polishing surface bounces off water and the pad surface does not fully retain the slurry.

[0181] [Table 2]

[0182]

[0183] [Comparative Example 2]

[0184] A polishing layer was produced in the same manner as in Example 1 except that the deep groove was not formed in Example 1. Then, a polishing pad was produced and evaluated in the same manner as in Example 1 using the obtained polishing layer. The results are shown in Table 2.

[0185] [Comparative Example 3]

[0186] Instead of forming shallow depressions in a triangular lattice formed by a plurality of straight lines with a width of 1.0 mm, a depth of 0.04 mm, and a spacing of 3.0 mm on the grinding surface in Example 2, a grinding layer was manufactured in the same manner except that shallow depressions in a triangular lattice formed by a plurality of straight lines with a width of 1.0 mm, a depth of 0.20 mm, and a spacing of 3.0 mm were formed. The cross-sectional shape of the shallow depressions is a rectangle. On the grinding surface, a plurality of island-shaped regular triangular table portions with a side length of 1.9 mm surrounded by a plurality of shallow depressions are formed. The projected area of ​​one island-shaped table portion is 1.5 mm 2 The maximum horizontal distance of an island-shaped mesa portion is 1.9 mm, and the ratio of the total projection area of ​​the mesa portion to the total projection area of ​​the mesa region is 30%.

[0187] Then, using the obtained polishing layer, a polishing pad was prepared in the same manner as in Example 1 and evaluated. The results are shown in Table 2.

[0188] [Comparative Example 4]

[0189] A polishing layer was produced in the same manner as in Example 8 except that the shallow depression was not formed in Example 8. Then, a polishing pad was produced and evaluated in the same manner as in Example 1 using the obtained polishing layer. The results are shown in Table 2.

[0190] [Comparative Example 5]

[0191] Instead of forming triangular lattice-shaped shallow depressions consisting of a plurality of straight lines with a width of 1.5 mm, a depth of 0.03 mm, and a spacing of 6.0 mm on the grinding surface in Example 9, an XY lattice-shaped shallow depression consisting of a plurality of straight lines with a width of 1.0 mm, a depth of 0.20 mm, and a spacing of 3.0 mm is formed, and the grinding layer is manufactured in the same manner except that. The cross-sectional shape of the shallow depression is a rectangle. On the grinding surface, a plurality of island-shaped square table portions with a side length of 2.0 mm surrounded by a plurality of shallow depressions are formed. The projected area of ​​one island-shaped table portion is 4.0 mm. 2 The maximum horizontal distance of an island-shaped mesa portion is 2.8 mm, and the ratio of the total projection area of ​​the mesa portion to the total projection area of ​​the mesa region is 44%. Thus, the polishing layer is manufactured.

[0192] Then, using the obtained polishing layer, a polishing pad was prepared in the same manner as in Example 1 and evaluated. The results are shown in Table 2.

[0193] [Comparative Example 6]

[0194] Instead of forming a triangular lattice-shaped shallow depression consisting of a plurality of straight lines with a width of 1.5 mm, a depth of 0.03 mm, and a spacing of 6.0 mm on the grinding surface in Example 9, a plurality of concentric shallow depressions with a width of 2.0 mm, a depth of 0.04 mm, and a spacing of 4.0 mm were formed, and the grinding layer was manufactured in the same manner. The cross-sectional shape of the shallow depression is a rectangle. The mesa portion between the shallow depressions is continuous in a concentric circle shape instead of an island shape. The total projection area of ​​the mesa portion is 50% relative to the total projection area of ​​the mesa region. The grinding layer was manufactured in this way.

[0195] Then, using the obtained polishing layer, a polishing pad was prepared in the same manner as in Example 1 and evaluated. The results are shown in Table 2.

[0196] [Comparative Example 7]

[0197] Instead of forming the shallow depression formed between the island-shaped circular mesa portions with a diameter of 1.5 mm by hot pressing a punching plate made of SUS by heat pressing in Example 11, the following shallow concave portion was formed, and the polishing layer was manufactured in the same manner as in Example 11. Then, using the obtained polishing layer, a polishing pad was manufactured in the same manner as in Example 1 and evaluated.

[0198] The shallow circular depressions with a diameter of 2 mm and a depth of 0.06 mm were cut into a hexagonal grid shape with a center spacing of 2.5 mm. The cross-sectional shape of the shallow depressions was rectangular. The mesa portion between the shallow depressions was continuous in a hexagonal grid sea shape instead of an island shape. The total projected area of ​​the mesa portion was 42% relative to the total projected area of ​​the mesa region. The results are shown in Table 2.

[0199] The following can be learned from the above results.

[0200] The grinding pads of embodiments 1 to 11 having deep grooves with a depth of more than 0.3 mm, shallow depressions with a depth of 0.01 to 0.1 mm, and multiple island-shaped table portions with a maximum horizontal distance of less than 8 mm surrounded by shallow depressions, compared with the grinding pads of comparative examples 1 and 4 without shallow depressions or the grinding pads of comparative examples 6 and 7 without island-shaped table portions surrounded by shallow depressions, have a shorter time required until the grinding speed is stabilized, and can shorten the time for run-in grinding. It should be noted that the grinding pads of embodiments 1 to 5, 8 to 11 having island-shaped table portions with a maximum horizontal distance of less than 7 mm have a particularly significant effect on shortening the time for run-in grinding. The grinding pads of comparative examples 3 and 5, in which the depth of the shallow depression exceeds 0.1 mm, have a relatively high grinding speed in the initial stage of use, but the grinding speed is difficult to stabilize, and the effect of shortening the time for run-in grinding is small. The grinding pad of comparative example 2 with deep grooves has a low grinding speed.

[0201] The polishing pad of the present invention can be used for polishing semiconductor substrates or glass, etc. It is particularly suitable for chemical mechanical polishing of substrate materials such as semiconductors, hard disks, liquid crystal displays, or optical components such as lenses or reflectors.

[0202] Description of Reference Numerals

[0203] 1 Deep slot or hole

[0204] 2, 12, 22 Shallow depression

[0205] 3.13 Platform

[0206] 5 Grinding layer

[0207] 6 Adhesive layer

[0208] 7 Buffer layer

[0209] 10, 20, 30, 40 polishing pads

[0210] 50 Ground substrate

[0211] G Deep groove area

[0212] L Countertop area

[0213] P Grinding surface

Claims

1. A polishing pad comprising a polishing layer having a polishing surface, in, The grinding surface, before the treatment of the new, unused, worn-in dressing grinding surface, has: a deep groove area having a first pattern formed by deep grooves or holes with a depth of 0.3 mm or more; a mesa area, which is an area other than the deep groove area; The mesa region has: a shallow depression with a depth of 0.01-0.1 mm and a width of 0.5-4 mm, which has a second pattern; and a plurality of island-shaped mesa portions, which are surrounded by the shallow depression and have a maximum horizontal distance of less than 8 mm.

2. The polishing pad according to claim 1, in, The second pattern has at least one pattern selected from the group consisting of a triangular lattice, a rectangular lattice, a diamond lattice, and a hexagonal lattice, which is formed on the entire surface of the mesa region.

3. The polishing pad according to claim 1, in, The second pattern has a square lattice pattern formed on the entire surface of the mesa region.

4. The polishing pad according to any one of claims 1 to 3, in, The projection area of ​​the table portion is 0.3-10 mm 2 range.

5. The polishing pad according to any one of claims 1 to 3, in, The ratio of the total projection area of ​​the table portion to the total projection area of ​​the table area is 10-50%.

6. The polishing pad according to any one of claims 1 to 3, in, The depth of the shallow depression is 0.02-0.06 mm.

7. The polishing pad according to any one of claims 1 to 3, in, The ratio of the projection area of ​​the deep groove region to the total projection area of ​​the grinding surface is 5-40%.

8. The polishing pad according to any one of claims 1 to 3, in, The first pattern has at least one pattern selected from the group consisting of a spiral shape, a concentric circle shape, and a lattice shape.

9. The polishing pad according to any one of claims 1 to 3, in, The polishing layer is composed of a sheet mainly composed of a non-foamed polymer.

10. The polishing pad according to any one of claims 1 to 3, in, The grinding layer includes a thermoplastic polyurethane sheet.

11. A method for manufacturing a polishing pad, comprising: A step of preparing a polymer sheet to be the polishing layer; A step of forming the deep groove region on the side of the polymer sheet that becomes the polished surface; A step of forming the mesa region on the side of the polymer sheet that becomes the polished surface; The shallow depressions forming the mesa region are formed by cutting or transfer processing.

12. A polishing method for polishing a polished surface of a semiconductor device in a manufacturing process of a semiconductor device using the polishing pad according to any one of claims 1 to 10, The method further comprises the step of dressing the polished surface under a dressing condition in which a cumulative dressing time until an average depth of the shallow recesses is less than 0.01 mm is within 30 minutes.

13. The grinding method according to claim 12, in, The cumulative dressing time is 1 to 20 minutes.