A forging method for improving the flaw detection level of high-temperature alloy free forgings

By adjusting the heating temperature and the amount of hole expansion deformation, using high-temperature liquid materials and horse frame hole expansion methods, the problems of narrow temperature and poor plasticity in the forging of GH9105 material are solved, the flaw detection level and forging quality are improved, and the scrap rate and energy consumption are reduced. .

CN114289676BActive Publication Date: 2024-10-25SHAANXI HONGYUAN AVIATION FORGING
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202111533913.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-15
Publication Date
2024-10-25
Estimated Expiration
2041-12-15

AI Technical Summary

Technical Problem

During the forging process of GH9105 material, the temperature range is narrow, the plasticity is poor, and it is easy to crack, resulting in unqualified flaw detection, high scrap rate, and large waste of energy, making it difficult to meet the requirements of high flaw detection level.

Method used

By adjusting the heating temperature of the billet, increasing the hammering force, shortening the forging time, increasing the amount of hole expansion deformation, and using special high-temperature liquid material surface treatment, horse frame hole expansion and flat end face forging methods, we can control the development of cracks and optimize the forging process.

Benefits of technology

It improves the flaw detection level of forgings, reduces the scrap rate and energy consumption, ensures the uniform structure and surface quality of forgings, and solves the problems of narrow forging temperature range and serious cracks.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention belongs to the technical field of forging, and relates to a forging method for improving the flaw detection level of high-temperature alloy free forgings. The method comprises: using a special high-temperature liquid material for heat preservation feeding, and performing surface treatment on the blanking raw material during horse reaming and hole reaming; placing the treated raw material in a natural gas furnace for heating, and the heating requirements are: entering the furnace at 700°C, preheating 700°C to 950°C×1.1~1.5min / mm, and then heating and controlling the temperature to a high temperature of 1109°C to 1150°C×1.0~1.5min / mm; punching through holes on the heated raw material, and machining through holes; and performing horse frame reaming and hole reaming on the raw material after the through holes are machined.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of forging, and relates to a forging method for improving the flaw detection level of high-temperature alloy free forgings. Background Art

[0002] Usually, the forging of GH9105 material adopts the forging method of multiple fires and small deformation to solve the problems of narrow forging temperature range, poor plasticity, and easy cracking at the corners during forging. However, it is difficult to meet the requirements under the premise of high flaw detection level for forgings. Multiple fire heating and small forging deformation will make the forging grains coarse, resulting in final flaw detection failure, high scrap rate, and large energy waste. It is difficult for manufacturers to ensure quality and quantity and deliver on time. Summary of the invention

[0003] The purpose of the present invention is to track and control the crack development process on the basis of conventional forging, and effectively solve the heating problem, narrow forging temperature range, fast cooling, severe cracks, high scrap rate and other problems in the forging process of GH105 ring parts by adjusting the heating temperature of the blank, increasing the hammer impact force, shortening the forging time, and improving the hole expansion deformation.

[0004] Technical solution:

[0005] A forging method for improving the flaw detection level of a high-temperature alloy free forging, comprising:

[0006] Use special high-temperature liquid material for heat preservation feeding, and perform surface treatment on the blanking materials during reaming and hole expansion;

[0007] The treated raw material is placed in a natural gas furnace for heating. The heating requirements are: put into the furnace at 700℃, preheat at 700℃~950℃×1.1~1.5min / mm, then increase the temperature and control it to a high temperature of 1109℃~1150℃×1.0~1.5min / mm;

[0008] Punching through holes in the heated raw material and machining the through holes;

[0009] The raw material after machined through holes is expanded by horse rack and reamer. The deformation amount of each time of horse rack expansion is set as: △Φ horse inner ≥ 35%; the deformation amount of each time of reamer expansion is set as: △Φ expansion inner ≥ 25%.

[0010] The raw material after the through hole is machined is expanded by a rack, including:

[0011] Odd-numbered fires: expand the through-hole horse rack;

[0012] Even-numbered fire: Use the free forging method to flatten the end surface of the rough material after the horse hole;

[0013] The total number of fires is 4.

[0014] The deformation of the horse frame hole expansion per fire △Φ ≥ 40mm, and the deformation of the flat end surface of the hammer per fire △h ≥ 10mm.

[0015] The raw material after the through hole is expanded by horse frame and expansion machine, and also includes:

[0016] After the blank is expanded, it is heated according to the above heating requirements and then rolled. The deformation of each fire is significantly increased. The deformation increases △Φ 内扩max ≥90mm, minimum deformation increase △Φ 内扩min ≥35mm, fire number is N 扩 =2 times; the forging temperature is controlled at 1109℃~1150℃ to ensure the last deformation △Φ 外 ≥75mm; until the hole is expanded and formed.

[0017] Before the raw material after the through-hole is expanded by a horse frame and an expansion machine, the method further comprises:

[0018] Surface defect treatment is performed on the rough material with machined through holes.

[0019] Cooling method: windproof pile cooling.

[0020] Beneficial effects: 1. Usually, heating is done after the jacket is produced. To solve the cumbersome process of the jacket, the billet is directly heated in the furnace after being fed with a special high-temperature liquid for protection. 2. The heating temperature is adjusted, and refractory bricks are used to pad the forgings during the heating process to ensure that the forgings are heated evenly. 3. The forging method of horse rack expansion and large deformation of the flat end surface is adopted to ensure the uniform internal structure of the forgings. Reduce the number of production fires and increase the deformation rate. 4. Solve the problems of long production cycle, large grinding volume and poor crack control of GH105 forging with multiple fires. DETAILED DESCRIPTION

[0021] The present invention provides a forging method for improving the flaw detection level of a high-temperature alloy free forging, comprising:

[0022] 1. Design the forging steps and required materials, and determine the cutting specifications and cutting length.

[0023] 2. Use special high-temperature liquid material for heat preservation feeding, and carry out surface treatment of blanking raw materials during reaming and hole expansion.

[0024] 3. The billet is heated in a natural gas furnace, the heating temperature range is 700℃ into the furnace, preheated at 700℃~950℃×1.1~1.5min / mm, and heated to a high temperature of 1109℃~1150℃×1.0~1.5min / mm;

[0025] 4. Surface defects can be treated by machining, sand blasting, grinding and other methods; production can only be carried out after cleaning.

[0026] 5. The deformation amount of each fire of the horse frame hole expansion is set as follows: △Φ horse inner ≥ 35%; the deformation amount of each fire of the hole expansion machine hole expansion is set as follows: △Φ expansion inner ≥ 25%; finally reach the forging size; no visible cracks on the surface.

[0027] 6. Cooling method: windproof pile cooling.

[0028] Specific examples:

[0029] Material: GH105 Forging size: φ638±5×564±5×56±4 Cutting specification: φ360×60, Features: This forging is a ring with a thin wall thickness: α 较薄 =37mm; lower height: h 高度 =60mm; height and thickness ratio β 高径比 ≈1.62, it is not easy to roll directly. It must be rolled immediately to ensure the final deformation β 最终变形量 Hole expansion can only be carried out when the diameter is ≥25%.

[0030] 1. The steel bars cut according to the specifications are heated in a natural gas furnace with a fire sleeve. According to the alloy phase diagram, the heating specification is: 700℃ loading, 12 pieces are loaded according to the furnace area and operation level, preheat at 700℃; keep warm for 80 minutes, then heat up to 1150℃ with the furnace and keep warm for 95 minutes. Forging is carried out.

[0031] 2. Punch a through hole as large as φ130 on a 3-ton free forging equipment, and the punching core material is φ130×35.

[0032] 3. Machined inner hole: Because the quality of the inner hole after punching is poor and there are visible cracks on the surface, machining is used to eliminate the defects. The single-sided machining amount is 5mm; the inner hole is machined to φinside = 130mm; the upper and lower end faces of the inner hole are chamfered R15.

[0033] 4. Sand blasting and grinding inspection:

[0034] After sandblasting and grinding twice, the technical and inspection personnel will conduct a surface quality inspection once; the width-to-depth ratio is set to 1:6 during grinding to remove flaws, and the horse frame hole expansion process can only be carried out after checking that there are no obvious visible cracks on the surface of the forging.

[0035] 5. Horse frame expansion and flat end surface

[0036] 5.1 Heat the cleaned blank in the same way as above and then proceed with the horse frame expansion and flat end surface process.

[0037] 5.11, No. 1 fire horse expansion: φ412±5×280±5×70±4;

[0038] 5.12, 2nd fire flat end face: 3 tons of free forging to flatten the end face: the flat end face height H1 = 55mm;

[0039] 5.13, the third fire horse expansion: φ500±5×395±5×70±4;

[0040] 5.14. 4th fire flat end face: 3 tons of free forging for flat end face: flat end face height H1 = 55mm.

[0041] The actual production number is N = 4 times. 马扩 =2 fire, hammer flat end surface P 平 = 2 fires, that is, the horse frame expansion fire is followed by the flat end face fire, and the deformation of the horse frame expansion per fire is △ Φ内 ≥40mm, the deformation of the flat end surface on the hammer for each fire △h≥10mm, due to the hole expansion on the hammer frame, the final expanded size of the ring blank should be controlled at φ520±5×φ395±5×52 before hole expansion can be carried out.

[0042] 5.2, Φ1200mm hole expansion by rolling; hole expansion machine for 2 times.

[0043] After the blank is expanded, it is heated as mentioned above and then rolled. The deformation of each fire increases significantly. The deformation increases △Φ 内扩max ≥90mm, minimum deformation increase △Φ 内扩min ≥35mm, fire number is N 扩 =2 times; the forging temperature can be reduced to 1000℃ to ensure the last deformation △Φ 外 ≥75mm; to expand the hole.

[0044] The actual expansion hole size is: φ638±5×564±5×56±4

[0045] 6. If the forging is warped or has a large height increase during the intermediate fire, add a 3-ton free forging hammer or a 630KJ counter-blow hammer to flatten the end surface. 平 =56±4 mm, heating is carried out according to the above requirements. The flat end surface should be sandblasted and polished for inspection before forging. The method is the same as above;

[0046] According to the technical requirements of forgings Q / 16GJX0-348-2000 forging acceptance standards, heat treatment and final forging rough machining were carried out after flaw detection. According to the AA level (water immersion method) of standard HB / Z59-1997, the inspection was qualified. The size, surface quality and hardness all met the requirements of the drawings.

Claims

1. A forging method for improving the flaw detection level of high-temperature alloy free forgings, characterized in that: include: Use special high-temperature liquid material insulation coating to carry out surface treatment on the blank raw materials when expanding holes in horse racks and expanding holes in expanding machines; The treated raw material is placed in a natural gas furnace for heating. The heating requirements are: put into the furnace at 700℃, preheat at 700℃~950℃×1.1~1.5min / mm, then increase the temperature and control it to a high temperature of 1109℃~1150℃×1.0~1.5min / mm; Punching through holes in the heated raw material and machining the through holes; The raw material after the through hole is machined is expanded by horse frame and expansion machine; The raw material after the through hole is machined is expanded by a rack, including: Odd-numbered fires: expand the through-hole horse rack; Even-numbered fire: Use the free forging method to flatten the end surface of the raw material after the horse frame is expanded; The total number of fires is 4; The raw material after the through hole is expanded by horse frame and expansion machine, and also includes: The blank after the hole expansion of the horse frame is heated according to the above heating requirements and then rolled. The deformation of each fire is significantly increased. The deformation increases △Φ 内扩max =90mm, the deformation increases to the minimum △Φ 内扩min =35mm, fire number is N 扩 =2 times; the forging temperature is controlled at 1109℃~1150℃ to ensure the last deformation △Φ 外 ≥75mm to expand the hole; The deformation amount of each fire of the frame expansion hole is set as follows: △Φ horse inner ≥ 35%; The deformation setting of each hole expansion by the hole expander is: △Φ expansion ≥ 25%.

2. The method according to claim 1, characterized in that Before the raw material after the through-hole is expanded by a horse frame and an expansion machine, the method further comprises: Perform surface defect treatment on rough materials with machined through holes.

Citation Information

Patent Citations

  • Forging method of circular GH105 high-temperature alloy forging

    CN103706740A

  • GH4169 alloy annular forge piece forming method

    CN107913963A

  • Forming method of GH141 alloy forging

    CN110976746A

  • Forging method for improving grain size of GH4099 high-temperature alloy thin-wall ring piece

    CN111215567A

  • Molding method of Waspaloy thin-walled ring forging pieces

    CN112589020A