Alumina carrier and preparation method thereof, hydrorefining catalyst and preparation method thereof
Through the combination of mesoporous δ-Al2O3 support and highly active metal components, the lack of catalyst activity and mesoporous alumina synthesis problems in the existing hydrorefining technology are solved, and efficient ultra-deep desulfurization and nitrogen removal of diesel are achieved, satisfying the High-quality clean diesel standards and reduce production costs and environmental impacts.
Patent Information
- Application Number
- CN202011030849.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2020-09-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-09-27
AI Technical Summary
The existing hydrogenation refining technology is difficult to meet the standards of high-quality clean diesel, especially in the case of high sulfur content and large nitrogen and aromatic content in FCC diesel, the activity of traditional catalysts is insufficient, and the synthesis method of mesoporous alumina is immature. Causes high costs and environmental protection issues.
Mesoporous δ-Al2O3 is used as a carrier, with organic molecules as template agents, inorganic aluminum salt aluminum chloride as aluminum source, and ammonia water as precipitant, and high-active hydrogenation is developed based on it. Refining the catalyst, combining Group VIB metals and Group VIII metals as active components, optimizes the structure and performance of the catalyst.
It has achieved ultra-deep desulfurization and nitrogen removal of FCC diesel, with a sulfur content of less than 10ppm, comply with the "National VI" standard, improves the activity and diffusion performance of the catalyst, reduces costs, and is environmentally friendly.
Smart Images

Figure CN114308000B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of petroleum refining, and in particular to an alumina carrier and a preparation method thereof, a hydrorefining catalyst and a preparation method thereof. The hydrorefining catalyst is particularly suitable for ultra-deep desulfurization of diesel. Background Art
[0002] With the widespread popularity of automobiles, the environmental pollution caused by automobiles has become increasingly prominent, which has brought pressure and challenges to the petrochemical industry. Diesel vehicles have the advantages of low fuel consumption, good economy, sufficient power, and long life. They will be one of the main directions of automobile development in the future. The pollution caused by the huge increase in the number of motor vehicles will cause urban pollution in my country to show the characteristics of motor vehicle exhaust pollution. At present, my country's annual diesel consumption has reached 125 million tons, and the annual growth rate has reached 5-7%. The pollutants produced by diesel combustion account for more than 40% of the total atmospheric pollutants. The sulfide in diesel not only corrodes the engine, but also causes the activity of automobile exhaust conversion catalyst to decrease or even poison and deactivate. The SOx released into the atmosphere is easy to form acid rain, thereby causing a series of more serious environmental pollution problems and endangering human health. Therefore, countries around the world have formulated strict environmental protection regulations and fuel quality standards. The diesel sulfur content index is a key factor in improving the quality of diesel oil.
[0003] At present, among the many methods for producing clean diesel, hydrofining technology is a relatively effective method. In the existing diesel hydrofining unit, it is hoped that the minimum cost will be spent on the minimum modification of the unit, and the product quality and production volume will be improved by optimizing the operation and improving the configuration. However, the traditional hydrofining process and catalyst are widely used in refineries at present. After processing FCC diesel feedstock, the sulfur content of the product is generally 100-200ppm, which obviously cannot meet the current production requirements of high-quality clean diesel standards. Therefore, my country's diesel hydrofining faces severe challenges.
[0004] For hydrorefining technology, the core and fundamental of its technological upgrade lies in the development of highly active ultra-deep hydrodesulfurization catalysts, which can not only reduce the severity of process operations, but also reduce the investment in industrial equipment, while also improving product quality. In hydrodesulfurization catalysts, the role of the carrier is very important. A carrier with excellent physical and chemical properties is not only conducive to the dispersion of additives and active metals in the catalyst, but also can adjust the interaction between the active metals and the carrier; and suitable acidity and pore structure are conducive to improving the composition distribution of its products, and can enhance the activity of the hydrodesulfurization reaction and improve the quality of the final product.
[0005] At present, mesoporous alumina has potential application value in many fields, but the synthesis method of mesoporous alumina is immature, which limits the practical application of mesoporous alumina. Among them, alumina prepared by the surfactant template method has the advantages of adjustable pore size and large specific surface area, but this preparation method still has some defects: the surfactant template method requires the use of aluminum alkoxides to be synthesized in an alcohol solution. However, aluminum alkoxides are easily hydrolyzed in the aqueous phase, but in order to inhibit hydrolysis, they must be carried out in organic solvents. The use of aluminum alkoxides increases costs, and the organic solvents used are toxic, as well as the cumbersome synthesis conditions, which make the synthesis of mesoporous alumina difficult to mass produce at present. Therefore, the development of alumina carrier materials with suitable pore structure, low price and environmental protection has important theoretical research value and practical application significance for the research and development of diesel ultra-deep desulfurization catalysts.
[0006] CN104117362A discloses a method for preparing a diesel hydrorefining catalyst. The alumina used in the method is γ-Al2O3, which is prepared by roasting pseudo-boehmite. The invention believes that the catalyst prepared from the carrier is suitable for diesel hydrorefining reaction.
[0007] CN104923244A discloses a method for preparing a diesel hydrotreating catalyst. The carrier used in the method is a composite oxide carrier of SiO2 and γ-Al2O3. According to the description of the invention, the carrier has the characteristics of a large specific surface area, which is conducive to the dispersion of active metals and has excellent catalytic activity in diesel hydrotreating reactions.
[0008] From the above literature research, it can be found that in the prior art, γ-Al2O3 has always been used as the main carrier material of hydrofining catalysts, while there are few reports on the application of δ-Al2O3 in the field of FCC diesel hydrofining. In addition, there are few reports on the investigation of templates in the synthesis process of δ-Al2O3 and the catalysts prepared as carriers.
[0009] One third of my country's diesel comes from catalytic cracking, which is characterized by high sulfur, high nitrogen, and high aromatics. Therefore, it is very important to improve the quality of inferior diesel to prevent the generation of NO after combustion. x 、SO x and excessive particulate matter, which threaten the ecological environment and human health. Faced with increasingly stringent environmental regulations and diesel quality standards, traditional hydrotreating technology is currently facing severe challenges. Therefore, it is of far-reaching significance to develop new high-efficiency hydrotreating catalysts to achieve clean production of diesel with ultra-low sulfur content. Summary of the invention
[0010] In view of the above problems in the prior art, the purpose of the present invention is to provide an Al2O3 carrier and a preparation method thereof, as well as a hydrorefining catalyst with mesoporous δ-Al2O3 as a carrier and a preparation method thereof. The hydrorefining catalyst can be applied to FCC diesel desulfurization, especially deep desulfurization, so that the yield of FCC diesel is higher than 99%, the sulfur content is lower than 10ppm, and it meets the "National VI" standard.
[0011] In order to achieve the above-mentioned object, the present invention provides an Al2O3 carrier, which is a mesoporous δ-Al2O3. When preparing the mesoporous δ-Al2O3, an organic molecule is used as an organic template, an inorganic aluminum salt aluminum chloride is used as an aluminum source, and ammonia water is used as a precipitant, and the mesoporous δ-Al2O3 is prepared by high-temperature calcination at 800-900°C; the X-ray diffraction spectrum of the mesoporous δ-Al2O3 shows that it is a delta phase, with characteristic peaks at 33°, 38°, 45° and 67°, and a specific surface area of 90-200m 2 ·g -1 , pore diameter is 10-20nm, pore volume is 0.6-1.0cm 3 ·g -1 , preferably 0.32-1.0cm 3 ·g -1 .
[0012] The Al2O3 carrier provided by the present invention has a specific surface area of 90-200m 2 ·g -1 , pore diameter is 10-20nm, pore volume is 0.32-1.0cm 3 ·g -1 . It can be seen that the mesoporous δ-Al2O3 provided by the present invention has a moderate pore size and a relatively concentrated pore size distribution, and the reactants can effectively diffuse in its open pore structure. At the same time, the hydroxyl groups on the surface of δ-Al2O3 are reduced after high-temperature calcination, which weakens the interaction between the metal and the carrier, and is more conducive to the formation of a highly active type II active phase. The hydrogenation refining performance of the catalyst prepared therefrom can be further improved.
[0013] In the mesoporous δ-Al2O3 of the present invention, it is preferred that the organic molecule is selected from at least one of ethanol, PEG, sucrose and glucose, and PEG is further preferred. Since the present invention uses PEG, ethanol, sucrose and glucose as templates, not only good effects are achieved, but also the selected templates are inexpensive and pollution-free, so that the cost of the alumina carrier is greatly reduced and environmentally friendly.
[0014] To achieve the above object, the present invention also provides a method for preparing a mesoporous δ-Al2O3 carrier, which is the method for preparing the above-mentioned mesoporous δ-Al2O3 carrier, comprising the following steps:
[0015] Step 1: Use AlCl3·6H2O as aluminum source, add organic template as pore-enlarging agent, and stir for 30 to 60 minutes;
[0016] Step 2: Slowly add NH3·H2O solution to the above solution system, stir for 6 to 24 hours, and then filter;
[0017] Step 3: After washing, drying and high temperature calcination at 800-900°C, mesoporous δ-Al2O3 is obtained.
[0018] The preparation method of the mesoporous δ-Al2O3 carrier provided by the present invention has the following characteristics:
[0019] (1) The synthesis is carried out using a low-cost and environmentally optimized template agent, and the average pore size is greatly increased compared with similar γ-Al2O3 materials. The larger pore size is beneficial to improving the diffusion performance of the corresponding catalyst.
[0020] (2) Compared with γ-Al2O3, the δ-Al2O3 prepared by the present invention has a reduced number of surface hydroxyl groups during the calcination process, and the interaction force between the metal and the carrier is weakened, thereby avoiding the formation of a NiAl2O4 spinel structure due to excessive interaction force, which is conducive to the formation of a more active type II active phase.
[0021] (3) δ-Al2O3 has a more suitable acidity than γ-Al2O3, which is conducive to the hydrogenation refining reaction.
[0022] In the method for preparing mesoporous δ-Al2O3 of the present invention, it is preferred that in step 1 and step 2, the stirring temperature is independently 30-80°C; in step 3, the drying temperature is 80-120°C.
[0023] In the method for preparing mesoporous δ-Al2O3 of the present invention, in step 2, preferably, the pH value of the solution system is maintained at 7-10 during the dropwise addition of the NH3·H2O solution.
[0024] To achieve the above object, the present invention also provides a hydrotreating catalyst, which uses the above mesoporous δ-Al2O3 as a carrier, Group VIB metals and Group VIII metals as active components, and the content of the active components is 15-25wt%.
[0025] The hydrorefining catalyst prepared with the mesoporous delta-Al2O3 as a carrier can achieve hydrodesulfurization and denitrification rates of 99.1% and 99.3% for FCC diesel.
[0026] In the hydrotreating catalyst of the present invention, it is preferred that the Group VIB metal element is Mo, the Group VIII metal is Ni, and the molar ratio of Ni to Mo is Ni / (Ni+Mo)=0.1-0.9:1, and more preferably 0.2-0.5:1.
[0027] To achieve the above object, the present invention also provides a method for preparing a hydrotreating catalyst, which is the above method for preparing a hydrotreating catalyst, comprising the following steps: (1) impregnating an active component on a carrier, and then drying and calcining to obtain a supported catalyst.
[0028] The method for preparing a hydrorefining catalyst using mesoporous δ-Al2O3 as a carrier provided by the present invention has the following characteristics:
[0029] The hydrorefining catalyst prepared with δ-Al2O3 as the carrier has outstanding performance. The evaluation results of the hydrorefining of Hohhot FCC diesel using the catalyst and the supporting process technology show that the desulfurization and denitrification rates of the hydrorefining catalyst prepared with PEG as the template agent reached 99.1% and 99.3%.
[0030] In the method for preparing the hydrotreating catalyst of the present invention, it is preferred that the impregnation is a step-by-step impregnation, first impregnating the Group VIB metal and then the Group VIII metal, and ultrasonic dispersion is preferably performed during the impregnation.
[0031] The method for preparing the hydrotreating catalyst of the present invention is preferably that the impregnation solution contains a Ni source and a Mo source respectively, the Ni source is selected from at least one of nickel nitrate, nickel sulfate, nickel acetate and nickel acetylacetonate, and nickel nitrate is further preferred; the Mo source is selected from at least one of ammonium dimolybdate, ammonium tetramolybdate, ammonium heptamolybdate and ammonium octamolybdate, and ammonium heptamolybdate is further preferred.
[0032] In the method for preparing the hydrotreating catalyst of the present invention, it is preferred that the drying temperature is 80-120° C. and the time is 4-24 hours; and the calcination temperature is 400-580° C. and the time is 4-12 hours.
[0033] The method for preparing the hydrotreating catalyst of the present invention preferably further comprises the following steps: (2) introducing an organic complexing agent into the supported catalyst, followed by drying and calcining to obtain the hydrotreating catalyst.
[0034] Since there is a strong interaction between the alumina carrier and the active metal, the activity of the catalyst will be seriously hindered. The present invention coordinates the interaction between the carrier and the active metal and improves the dispersibility of the active metal by adding a complexing agent; it not only ensures that the catalyst has good metal dispersibility, but also makes the interaction between the active metal and the carrier moderate. In addition, the introduction of the complexing agent can make the active metal on the surface of the catalyst "secondary dissolution" and "secondary dispersion", and the phenomenon of partial agglomeration of active metals (such as Ni, Mo) can be improved, thereby further dispersing the active metal. In addition, due to the use of δ-Al2O3 as a carrier, compared with the traditional γ-Al2O3, the pore size is increased, the diffusion performance is increased, and at the same time, the interaction between the metal and the carrier is weakened, which is conducive to the formation of a highly active NiMoS-Ⅱ type active phase. Therefore, the obtained alumina-based hydrorefining catalyst has a more superior performance than the traditional catalyst with γ-Al2O3 as a carrier.
[0035] The method for preparing the hydrotreating catalyst of the present invention is preferably that the organic complexing agent is ethylenediaminetetraacetic acid, aminotriacetic acid, acetylacetone, oxalic acid and citric acid, and ethylenediaminetetraacetic acid EDTA is further preferred; the molar ratio of the complexing agent to the active component is 1-5:1, and more preferably 1-2:1.
[0036] In the method for preparing the hydrotreating catalyst of the present invention, in step (2), preferably, the drying temperature is 80-120° C. and the time is 4-24 h; the calcination temperature is 400-580° C. and the time is 4-12 h.
[0037] The present invention also provides the use of the hydrofining catalyst in the hydrofining of Hohhot diesel oil products. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 The wide-angle XRD spectra of mesoporous δ-Al2O3 prepared in Examples 1-1 to 1-4 and Comparative Example 1;
[0039] Figure 2 The N2 adsorption-desorption isotherms of the mesoporous δ-Al2O3 prepared in Examples 1-1 to 1-4 and Comparative Example 1;
[0040] Figure 3 The pore size distribution diagram of mesoporous δ-Al2O3 prepared in Examples 1-1 to 1-4 and Comparative Example 1;
[0041] Figure 4 It is the Raman spectrum of the δ-Al2O3-supported NiMo catalyst prepared in Examples 2-1 to 2-4 and Comparative Example 2. DETAILED DESCRIPTION
[0042] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.
[0043] Example 1-1
[0044] The synthesis scheme of mesoporous δ-Al2O3 in this embodiment includes the following steps:
[0045] (1) Weigh 6 g of AlCl3·6H2O and 5 g of organic template ethanol and add them to 82.8 mL of deionized water. Stir evenly at 35°C until a transparent solution is formed.
[0046] (2) After heating the solution to 40°C, slowly add NH3·H2O solution dropwise until the pH value of the solution reaches 9. Stir for 12 hours, then take out and filter.
[0047] (3) After the filtration is completed, the filter cake is washed with deionized water and anhydrous ethanol respectively and then placed in a 100°C oven to dry.
[0048] (4) The dried filter cake was heated to 900°C in air at a heating rate of 2°C / min and then calcined for 6 h.
[0049] The mesoporous δ-Al2O3 prepared above was tested and analyzed, and its wide-angle XRD results are as follows: Figure 1 The N2 adsorption and desorption results are shown in Figure 2 Its pore size distribution is shown as Figure 3 Its pore structure parameters and nomenclature are shown in Table 1.
[0050] Example 1-2
[0051] The synthesis scheme of mesoporous δ-Al2O3 in this embodiment includes the following steps:
[0052] (1) Weigh 6 g AlCl3·6H2O and 5 g organic template glucose into 82.8 mL deionized water and stir at 35 °C until a transparent solution is formed.
[0053] (2) After heating the solution to 40°C, slowly add NH3·H2O solution dropwise until the pH value of the solution reaches 9. Stir for 12 hours, then take out and filter.
[0054] (3) After the filtration is completed, the filter cake is washed with deionized water and anhydrous ethanol respectively and then placed in a 100°C oven to dry.
[0055] (4) The dried filter cake was heated to 900°C in air at a heating rate of 2°C / min and then calcined for 6 h.
[0056] The mesoporous δ-Al2O3 prepared above was tested and analyzed, and its wide-angle XRD results are as follows: Figure 1 The N2 adsorption and desorption results are shown in Figure 2 Its pore size distribution is shown as Figure 3 Its pore structure parameters and nomenclature are shown in Table 1.
[0057] Examples 1-3
[0058] The synthesis scheme of mesoporous δ-Al2O3 in this embodiment includes the following steps:
[0059] (1) Weigh 6 g of AlCl3·6H2O and 5 g of organic template PEG and add them to 82.8 mL of deionized water. Stir evenly at 35°C until a transparent solution is formed.
[0060] (2) After heating the solution to 40°C, slowly add NH3·H2O solution dropwise until the pH value of the solution reaches 9. Stir for 12 hours, then take out and filter.
[0061] (3) After the filtration is completed, the filter cake is washed with deionized water and anhydrous ethanol respectively and then placed in a 100°C oven to dry.
[0062] (4) The dried filter cake was heated to 900°C in air at a heating rate of 2°C / min and then calcined for 6 h.
[0063] The mesoporous δ-Al2O3 prepared above was tested and analyzed, and its wide-angle XRD results are as follows: Figure 1 The N2 adsorption and desorption results are shown in Figure 2 Its pore size distribution is shown as Figure 3 Its pore structure parameters and nomenclature are shown in Table 1.
[0064] Examples 1-4
[0065] The synthesis scheme of mesoporous δ-Al2O3 in this embodiment includes the following steps:
[0066] (1) Weigh 6 g of AlCl3·6H2O and 5 g of organic template sucrose and add them to 82.8 mL of deionized water. Stir evenly at 35°C until a transparent solution is formed.
[0067] (2) After heating the solution to 40°C, slowly add NH3·H2O solution dropwise until the pH value of the solution reaches 9. Stir for 12 hours, then take out and filter.
[0068] (3) After the filtration is completed, the filter cake is washed with deionized water and anhydrous ethanol respectively and then placed in a 100°C oven to dry.
[0069] (4) The dried solid was heated to 900°C in air at a heating rate of 2°C / min and then calcined for 6 h.
[0070] The mesoporous δ-Al2O3 prepared above was tested and analyzed, and its wide-angle XRD results are as follows: Figure 1 The N2 adsorption and desorption results are shown in Figure 2 Its pore size distribution is shown as Figure 3 Its pore structure parameters and nomenclature are shown in Table 1.
[0071] Comparative Example 1
[0072] The synthesis scheme of mesoporous δ-Al2O3 in this embodiment includes the following steps:
[0073] (1) Weigh 6 g of AlCl3·6H2O and 5 g of organic template CTAB (expensive and toxic) and add them to 82.8 mL of deionized water. Stir evenly at 35 °C until a transparent solution is formed.
[0074] (2) After heating the solution to 40°C, slowly add NH3·H2O solution dropwise until the pH value of the solution reaches 9. Stir for 12 hours, then take out and filter.
[0075] (3) After the filtration is completed, the filter cake is washed with deionized water and anhydrous ethanol respectively and then placed in a 100°C oven to dry.
[0076] (4) The dried solid was heated to 900°C in air at a heating rate of 2°C / min and then calcined for 6 h.
[0077] The mesoporous δ-Al2O3 prepared above was tested and analyzed, and its wide-angle XRD results are as follows: Figure 1 The N2 adsorption and desorption results are shown in Figure 2 Its pore size distribution is shown as Figure 3 Its pore structure parameters and nomenclature are shown in Table 1.
[0078] Table 1
[0079]
[0080] Depend on Figures 1 to 3 As shown in Table 1, the mesoporous δ-Al2O3 prepared in Examples 1-1 to 1-4 of the present invention is a delta phase with characteristic peaks at 33°, 38°, 45° and 67° and a specific surface area of 90-200 m 2 ·g -1, pore diameter is 10-20nm, pore volume is 0.6-1.0cm 3 ·g -1 .
[0081] Among them, the δ-crystalline alumina material prepared with the template agent PEG has the best pore expansion effect, and the material has the largest specific surface area, pore volume, and pore diameter, reaching 195m 2 ·g -1 、0.89cm 3 ·g -1 The pore expansion effect of the δ-crystalline alumina material prepared with the template agent CTAB is also good, and the pore volume and pore size of the material are large, reaching 0.47cm 3 ·g -1 and 14.5nm, the pore size distribution is more concentrated, and its specific surface area is slightly increased to 120m 2 ·g -1 The specific surface area, pore volume and pore size of the δ-crystalline alumina materials prepared by other template agents such as glucose, ethanol and sucrose are not much different from those prepared without template agents, but their pore size distribution is very concentrated. The above data show that the template agents PEG and CTAB play a good role in expanding the pores in the process of synthesizing δ-crystalline alumina materials, thereby improving the physical and chemical properties of the materials.
[0082] Example 2-1
[0083] The preparation method of the hydrotreating catalyst of this embodiment comprises the following steps:
[0084] Step 1: Dissolve 6.09 g of ammonium molybdate in deionized water to prepare a solution, use the solution to impregnate the mesoporous δ-Al2O3 carrier (5 g) prepared in Example 1-1, and disperse it by ultrasonic for 15 minutes, stir for 3 minutes, dry at 100°C for 5 hours, calcine at 550°C for 6 hours, and cool to room temperature to obtain Mo / δ-Al2O3 loaded with molybdenum;
[0085] Step 2: Dissolve 0.81 g of nickel nitrate in deionized water to prepare a solution, use the solution to impregnate the Mo / δ-Al2O3 carrier, and disperse it ultrasonically for 15 minutes. Stir for 3 minutes, dry at 100°C for 5 hours, calcine at 550°C for 6 hours, and cool to room temperature to obtain a hydrorefining catalyst loaded with molybdenum and nickel;
[0086] According to the test, in the above hydrotreating catalyst, the mass fraction of Mo calculated as MoO3 is 12%; the mass fraction of Ni calculated as NiO is 3.5%.
[0087] The above prepared δ-Al2O3 supported NiMo catalyst was tested and analyzed, and its Raman results are as follows Figure 4 shown.
[0088] Example 2-2
[0089] The preparation method of the hydrotreating catalyst of this embodiment comprises the following steps:
[0090] Step 1: Dissolve 6.09 g of ammonium molybdate in deionized water to prepare a solution, use the solution to impregnate the mesoporous δ-Al2O3 carrier (5 g) prepared in Example 1-2, and disperse it by ultrasonic for 15 minutes. After stirring for 3 minutes, dry it at 100°C for 5 hours, calcine it at 550°C for 6 hours, and cool it to room temperature to obtain Mo / δ-Al2O3 loaded with molybdenum;
[0091] Step 2: Dissolve 0.81 g of nickel nitrate in deionized water to prepare a solution, use the solution to impregnate the Mo / δ-Al2O3 carrier, and disperse it ultrasonically for 15 minutes. Stir for 3 minutes, dry at 100°C for 5 hours, calcine at 550°C for 6 hours, and cool to room temperature to obtain a hydrorefining catalyst loaded with molybdenum and nickel;
[0092] According to the test, in the above hydrotreating catalyst, the mass fraction of Mo calculated as MoO3 is 12%; the mass fraction of Ni calculated as NiO is 3.5%.
[0093] The above prepared δ-Al2O3 supported NiMo catalyst was tested and analyzed, and its Raman results are as follows Figure 4 shown.
[0094] Example 2-3
[0095] The preparation method of the hydrotreating catalyst of this embodiment comprises the following steps:
[0096] Step 1: Dissolve 6.09 g of ammonium molybdate in deionized water to prepare a solution, use the solution to impregnate the mesoporous δ-Al2O3 carrier (5 g) prepared in Example 1-3, and disperse it by ultrasonic for 15 minutes. After stirring for 3 minutes, dry it at 100°C for 5 hours, calcine it at 550°C for 6 hours, and cool it to room temperature to obtain Mo / δ-Al2O3 loaded with molybdenum;
[0097] Step 2: Dissolve 0.81 g of nickel nitrate in deionized water to prepare a solution, use the solution to impregnate the Mo / δ-Al2O3 carrier, and disperse it ultrasonically for 15 minutes. Stir for 3 minutes, dry at 100°C for 5 hours, calcine at 550°C for 6 hours, and cool to room temperature to obtain a hydrorefining catalyst loaded with molybdenum and nickel;
[0098] According to the test, in the above hydrotreating catalyst, the mass fraction of Mo calculated as MoO3 is 12%; the mass fraction of Ni calculated as NiO is 3.5%.
[0099] The above prepared δ-Al2O3 supported NiMo catalyst was tested and analyzed, and its Raman results are as follows Figure 4 shown.
[0100] Embodiment 2-4
[0101] The preparation method of the hydrotreating catalyst of this embodiment comprises the following steps:
[0102] Step 1: Dissolve 6.09 g of ammonium molybdate in deionized water to prepare a solution, use the solution to impregnate the mesoporous δ-Al2O3 carrier (5 g) prepared in Example 1-4, and disperse it by ultrasonic for 15 minutes, stir for 3 minutes, dry at 100°C for 5 hours, calcine at 550°C for 6 hours, and cool to room temperature to obtain Mo / δ-Al2O3 loaded with molybdenum;
[0103] Step 2: Dissolve 0.81 g of nickel nitrate in deionized water to prepare a solution, use the solution to impregnate the Mo / δ-Al2O3 carrier, and disperse it ultrasonically for 15 minutes. Stir for 3 minutes, dry at 100°C for 5 hours, calcine at 550°C for 6 hours, and cool to room temperature to obtain a hydrorefining catalyst loaded with molybdenum and nickel;
[0104] According to the test, in the above hydrotreating catalyst, the mass fraction of Mo calculated as MoO3 is 12%; the mass fraction of Ni calculated as NiO is 3.5%.
[0105] The above prepared δ-Al2O3 supported NiMo catalyst was tested and analyzed, and its Raman results are as follows Figure 4 shown.
[0106] Comparative Example 2
[0107] The preparation method of the hydrotreating catalyst of this embodiment comprises the following steps:
[0108] Step 1: Dissolve 6.09 g of ammonium molybdate in deionized water to prepare a solution, use the solution to impregnate the mesoporous δ-Al2O3 carrier (5 g) prepared in Comparative Example 1, and disperse it by ultrasonic for 15 minutes, stir for 3 minutes, dry at 100°C for 5 hours, calcine at 550°C for 6 hours, and cool to room temperature to obtain Mo / δ-Al2O3 loaded with molybdenum;
[0109] Step 2: Dissolve 0.81 g of nickel nitrate in deionized water to prepare a solution, use the solution to impregnate the Mo / δ-Al2O3 carrier, and disperse it ultrasonically for 15 minutes. Stir for 3 minutes, dry at 100°C for 5 hours, calcine at 550°C for 6 hours, and cool to room temperature to obtain a hydrorefining catalyst loaded with molybdenum and nickel;
[0110] According to the test, in the above hydrotreating catalyst, the mass fraction of Mo calculated as MoO3 is 12%; the mass fraction of Ni calculated as NiO is 3.5%.
[0111] The above prepared δ-Al2O3 supported NiMo catalyst was tested and analyzed, and its Raman results are as follows Figure 4 shown.
[0112] Figure 4 The main characteristic peak of the Raman spectrum is 250 cm -1 、331cm -1 、564cm -1 、839cm -1 、818cm -1 and 961cm -1 , of which 331cm -1 and 838cm -1 The vibration peaks on the left and right are attributed to the tetrahedral coordination of MoO4 2- Bending vibration of terminal Mo=O bond, 961cm -1 The vibration peaks on the left and right are attributed to the two-dimensional poly-Mo species Mo7O 24 6- Mo=O stretching vibration in. Figure 4 You can see the 564cm -1 The characteristic peak of the two-dimensional molybdenum polymer at 960cm -1 The peak intensities of the left and right characteristic peaks have a good linear relationship with the activity of the catalyst HDS. From the Raman spectrum, it can be seen that the materials prepared with the template PEG and CTAB have a peak intensity of 960 cm -1 A strong spectral peak is shown near it, that is, the catalyst prepared with PEG and CTAB as templates should have good hydrodesulfurization activity.
[0113] Example 3-1
[0114] The preparation method of the hydrotreating catalyst treated with an organic complexing agent provided in this embodiment comprises the following steps:
[0115] Step 1: Dissolve 1.6 g of EDTA in 10.6 g of an ammonia solution having a pH of 9 to obtain solution a;
[0116] Step 2: Use solution a to impregnate the NiMo / δ-Al2O3 catalyst prepared in Example 2-1, and then dry it at 120°C for 4h.
[0117] Example 3-2
[0118] The preparation method of the hydrotreating catalyst treated with an organic complexing agent provided in this embodiment comprises the following steps:
[0119] Step 1: Dissolve 1.6 g of EDTA in 10.6 g of an ammonia solution having a pH of 9 to obtain solution a;
[0120] Step 2: Use solution a to impregnate the NiMo / δ-Al2O3 catalyst prepared in Example 2-2, and then dry it at 120°C for 4h.
[0121] Example 3-3
[0122] The preparation method of the hydrotreating catalyst treated with an organic complexing agent provided in this embodiment comprises the following steps:
[0123] Step 1: Dissolve 1.6 g of EDTA in 10.6 g of an ammonia solution having a pH of 9 to obtain solution a;
[0124] Step 2: Use solution a to impregnate the NiMo / δ-Al2O3 catalyst prepared in Example 2-3, and then dry it at 120°C for 4h.
[0125] Embodiment 3-4
[0126] The preparation method of the hydrotreating catalyst treated with an organic complexing agent provided in this embodiment comprises the following steps:
[0127] Step 1: Dissolve 1.6 g of EDTA in 10.6 g of an ammonia solution having a pH of 9 to obtain solution a;
[0128] Step 2: Use solution a to impregnate the NiMo / δ-Al2O3 catalyst prepared in Example 2-4, and then dry it at 120°C for 4h.
[0129] Comparative Example 3
[0130] The preparation method of the hydrotreating catalyst treated with an organic complexing agent provided in this embodiment comprises the following steps:
[0131] Step 1: Dissolve 1.6 g of EDTA in 10.6 g of an ammonia solution having a pH of 9 to obtain solution a;
[0132] Step 2: The NiMo / δ-Al2O3 catalyst prepared in Comparative Example 2 was impregnated with solution a, and then dried at 120°C for 4h.
[0133] Test Case
[0134] This test example is based on the application of the hydrotreating catalyst prepared in Examples 3-1 to 3-4 and Comparative Example 3 in the hydrotreating reaction of Hohhot FCC diesel.
[0135] The properties of the reaction materials are shown in Table 2.
[0136] Table 2
[0137] parameter Hohhot FCC Diesel <![CDATA[Density (20 °C), g / cm 3 > 0.869 Saturation (v%) 39.3 Aromatics (v%) 49.0 Olefins (v%) 11.7 Cetane number 37.7 Sulfur content (μg / g) 1013.0 Nitrogen content (μg / g) 640.3
[0138] Hohhot FCC diesel was used as feedstock, and the catalyst of the present invention was used as a refining catalyst to carry out a hydrorefining reaction. The hydrodesulfurization rate and denitrification rate of the feedstock were investigated. The naming and evaluation results of the catalysts are shown in Table 3.
[0139] The specific test methods for the catalyst are as follows:
[0140] (1) Catalyst loading: quartz wool + quartz sand (20-40 mesh) 6.5 mL + quartz wool + 2 g of hydrogenation refining agent (40-60 mesh) + quartz wool + quartz sand 3.5 mL + quartz wool;
[0141] (2) Pre-sulfidation process conditions: temperature 320 °C, pressure 4 MPa, sulfidation liquid flow rate 2.5 mL / L; stable for 4 h;
[0142] (3) Evaluation process reaction conditions: reaction temperature 350°C, pressure 5 MPa, space velocity 1.0 h -1 , hydrogen to oil ratio 600.
[0143] Table 3
[0144]
[0145] It can be seen from Table 1 that δ3 using PEG as the template has the largest specific surface area, pore volume and pore size, reaching 195m 2 / g, 0.89cm 3 / g and 16.5nm, which are significantly better than other templates. Compared with CTAB, the specific surface area, pore volume and pore size of the three templates of ethanol, glucose and sucrose have decreased to a certain extent. Combined with the evaluation results in Table 3, compared with the expensive and toxic CTAB, although the catalyst activity of ethanol, glucose and sucrose as templates has decreased, they still have good hydrodesulfurization and denitrification effects, with a desulfurization rate of more than 97% and a denitrification rate of more than 95%. Compared with the catalyst NiMo / δ5 with CTAB as the template, the catalyst NiMo / δ3 with cheap PEG as the template has better hydrodesulfurization and denitrification effects, with a desulfurization rate of 99.1% and a denitrification rate of 99.3%. Taking into account the activity, cost and environmental protection issues, non-toxic and cheap PEG is preferred as the template.
[0146] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.
Claims
1. Application of a catalyst in a hydrofining reaction, characterized in that: The preparation method of the catalyst comprises the following steps: (1) impregnating the active component on the carrier, followed by drying and calcining; The carrier is mesoporous δ-Al2O3. When preparing the mesoporous δ-Al2O3, organic molecules are used as organic templates, inorganic aluminum salt aluminum chloride is used as aluminum source, and ammonia water is used as precipitation agent. The mesoporous δ-Al2O3 is prepared by high-temperature calcination at 800-900°C. The X-ray diffraction spectrum of the mesoporous δ-Al2O3 shows that it is a delta phase with characteristic peaks at 33°, 38°, 45° and 67°, and a specific surface area of 90-200 m 2 •g -1 , pore diameter is 10-20 nm, pore volume is 0.32-1.0 cm 3 ·g -1 ; The organic molecule is selected from at least one of ethanol, PEG, sucrose and glucose.
2. The use according to claim 1, characterized in that: The pore volume of the mesoporous δ-Al2O3 is 0.6-1.0 cm 3 •g -1 .
3. The use according to claim 1, characterized in that: The organic molecule is PEG.
4. The use according to claim 1, characterized in that: The preparation method of the carrier comprises the following steps: Step 1: Use AlCl3·6H2O as aluminum source, add organic template, and stir; Step 2: Slowly add NH3·H2O solution, stir for 12 h, and filter; Step 3: After washing, drying and high temperature calcination at 800-900 °C, mesoporous δ-Al2O3 is obtained.
5. The use according to claim 4, characterized in that: The stirring temperatures in step 1 and step 2 are independently 30 to 80°C.
6. The use according to claim 4, characterized in that: In step 2, the pH value of the solution system is maintained at 7-10 during the dropwise addition of the NH3·H2O solution.
7. The use according to claim 1, characterized in that: The catalyst has Group VIB metal and Group VIII metal as active components, and the content of the active components is 15-25 wt%.
8. The use according to claim 7, characterized in that: The Group VIB metal is Mo, the Group VIII metal is Ni, and the molar ratio of Ni to Mo is Ni / (Ni+Mo)=0.1-0.9:
1.
9. The use according to claim 8, characterized in that: The molar ratio of Ni to Mo is Ni / (Ni+Mo)=0.2-0.5:
1.
10. The use according to claim 1, characterized in that: The impregnation is a stepwise impregnation, wherein the Group VIB metal is impregnated first and then the Group VIII metal is impregnated.
11. The use according to claim 10, characterized in that: Ultrasonic dispersion was performed during the immersion.
12. The use according to claim 10, characterized in that: The impregnation solution contains a Ni source and a Mo source respectively, wherein the Ni source is selected from at least one of nickel nitrate, nickel sulfate, nickel acetate and nickel acetylacetonate; and the Mo source is selected from at least one of ammonium dimolybdate, ammonium tetramolybdate, ammonium heptamolybdate and ammonium octamolybdate.
13. The use according to claim 12, characterized in that: The Ni source is nickel nitrate.
14. The use according to claim 12, characterized in that: The Mo source is ammonium heptamolybdate.
15. The use according to claim 1, characterized in that: In step (1), the drying temperature is 80-120°C and the time is 4-24 h; the calcination temperature is 400-580°C and the time is 4-12 h.
16. The use according to claim 1, characterized in that: The method for preparing the catalyst further comprises the following steps: (2) introducing an organic complexing agent into the catalyst obtained in step (1), followed by drying and calcining.
17. The use according to claim 16, characterized in that The organic complexing agent is at least one of ethylenediaminetetraacetic acid, aminotriacetic acid, acetylacetone, oxalic acid and citric acid; the molar ratio of the complexing agent to the active component is 1-5:
1.
18. The use according to claim 17, characterized in that The organic complexing agent is ethylenediaminetetraacetic acid.
19. The use according to claim 17, characterized in that: The molar ratio of the complexing agent to the active component is 1-2:
1.
20. The use according to claim 16, characterized in that In step (2), the drying temperature is 80-120°C and the time is 4-24 h; the calcination temperature is 400-580°C and the time is 4-12 h.