A high-purity water-soluble silicon wafer cleaning agent and preparation method thereof

Through the formulation of high-purity water-soluble silicon wafer cleaning agent, combined with the synergistic effect of surfactant, polymer builder and enhancer, the problem of poor surface corrosion and oil stain cleaning effect of silicon wafers is solved, and efficient and safe silicon wafers are achieved Cleaning reduces wastewater discharge and the use of toxic substances, and meets the cleaning requirements of high-end chip manufacturing.

CN114317128BActive Publication Date: 2024-12-03SHANGHAI CHEM REAGENT RES INST
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202111620195.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-12-28
Publication Date
2024-12-03
Estimated Expiration
2041-12-28

AI Technical Summary

Technical Problem

The existing silicon wafer cleaning agents have problems such as strong corrosion on the surface of the silicon wafer, poor oil and stain cleaning effect, large usage, high COD content, difficult wastewater treatment and toxic and harmful substances, which affect the processing quality and environmental protection requirements of silicon wafers.

Method used

Using high-purity water-soluble silicon wafer cleaning agent formula, including surfactants, polymer builders, cosolvents and enhancers, the surface tension is reduced through surfactants adsorption at the interface, polymer builders adsorb metal ions, and cosolvent supplementary cleaning Effects and protects the surface of the silicon wafer, enhancers prevent corrosion, use high-purity water as solvent, combined with ion exchange and filtration treatment to ensure cleaning effect and safety.

Benefits of technology

实现了无毒、无害、无污染的高效硅片清洗,降低了使用量和废水排放量,确保了硅片表面的清洁度和安全性,提高了成品率,满足了高端芯片制造的清洗需求 .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003437689690000041
    Figure BDA0003437689690000041
  • Figure BDA0003437689690000051
    Figure BDA0003437689690000051
Patent Text Reader

Abstract

The present invention relates to a high-purity water-soluble silicon wafer cleaning agent and a preparation method thereof, comprising the following components in weight percentage: 5-10% surfactant, 5-15% polymer builder, 1-5% cosolvent, 25-40% enhancer and 35-50% high-purity water. Compared with the prior art, the primer of the present invention has a low VOC content, fast drying of the paint film, good toughness, good early water resistance and excellent anti-corrosion performance. In addition, the cleaning agent of the present invention is mainly used for cleaning and wiping silicon wafers after polishing, and mainly removes lubricants, dust and other dirt on the surface of the silicon wafers during processing. It is a non-toxic, harmless, safe and pollution-free cleaning agent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of chemical technology, and specifically relates to a high-purity water-soluble silicon wafer cleaning agent and a preparation method thereof, which is mainly used for cleaning and wiping silicon wafers after polishing, and mainly removes lubricants, dust and other dirt on the surface of silicon wafers during processing. It is a non-toxic, harmless, safe and pollution-free cleaning agent. Background Art

[0002] The substrates of solar panels and chips of various electronic products are all single-crystal silicon wafers. Single-crystal silicon wafers are made by cutting and processing single-crystal silicon. After cutting, they need to be polished. Lubricants and other substances are needed during the polishing process. Their components include organic and inorganic substances. In order to ensure that the cleanliness of the silicon wafers meets the requirements of subsequent processing, they need to be cleaned after polishing. During the cleaning process, strict requirements are imposed on the conductivity of the residual substances and the size of the residual particles after cleaning. In order to ensure that the standards are met, the cleaning agent formula needs to meet the conductivity and insoluble particle size within the silicon wafer processing quality indicators. At the same time, with increasingly stringent environmental protection requirements, traditional silicon wafer cleaning agents have the disadvantages of large usage, high COD content, large wastewater discharge, high difficulty in treatment, and even contain toxic and harmful substances.

[0003] Patent application CN201010566271.5 discloses a silicon wafer cleaning agent, which contains a surfactant, a cosolvent, a metal complex, a suspending agent, a silicon wafer corrosive agent and water, wherein the surfactant contains a water-soluble fluorinated nonionic surfactant and an alcohol ether surfactant, and the weight ratio of the water-soluble fluorinated nonionic surfactant and the alcohol ether surfactant is 1:10 to 1:40. The silicon wafer cleaning agent disclosed in the present invention neither causes severe corrosion to the surface of the silicon wafer nor has an excellent cleaning effect. The patented product has a low yield in the silicon wafer cleaning process used in high-end chip manufacturing. The main reason may be that the silicon wafer corrosive agent in its components causes severe corrosion to the silicon wafer surface. At the same time, it has a poor cleaning effect on the heavy oil stains on the silicon wafer surface.

[0004] Patent application CN202111008614.0 discloses a cleaning agent composition after silicon wafer processing, and the weight percentage of each component is as follows: surfactant 10-15%, penetrant 5-10%, organic polymer flocculant 0.01-0.3%, alkali 0.2-2%, deionized water balance. The cleaning liquid composition provided by the present invention is used to clean the processed silicon wafer. Because a large number of polar groups in the molecular chain of the high molecular weight organic flocculant can adsorb nano solid particles suspended on the surface of the workpiece or in the water, bridges between particles to form large floccules, promotes the agglomeration of nano particles into large particles, accelerates the stripping of nano particles on the surface of the workpiece and the sedimentation of particles in the suspension, and achieves the purpose of quickly and efficiently removing residual particle contaminants on the surface of the silicon wafer, achieving a good cleaning effect. The alkaline component of the patented product has a certain corrosiveness to the silicon wafer, causing pits on the surface of the silicon wafer, which is a fatal disadvantage for the quality of silicon wafers, especially high-end silicon wafers, and may cause a reduction in the yield rate during the later processing. Summary of the invention

[0005] The purpose of the present invention is to overcome the defects of the above-mentioned prior art and provide a non-toxic, harmless, pollution-free high-purity water-soluble silicon wafer cleaning agent and a preparation method thereof.

[0006] The purpose of the present invention can be achieved by the following technical scheme: a high-purity water-soluble silicon wafer cleaning agent, characterized in that it includes the following components in weight percentage: 5-10% surfactant, 5-15% polymer builder, 1-5% cosolvent, 25-40% enhancer and 35-50% high-purity water.

[0007] Furthermore, the surfactant is a mixture of one or more of linear alkylbenzene sulfonate (LAS), sodium alcohol polyoxyethylene ether sulfate (AES), ammonium alcohol polyoxyethylene ether sulfate (AESA), sodium lauryl sulfate (SDS), lauroyl glutamic acid, nonylphenol polyoxyethylene ether (TX-10), peregal O, stearic acid glycerol monoester, lignin sulfonate, heavy alkylbenzene sulfonate, alkyl sulfonate (petroleum sulfonate), diffuser NNO, diffuser MF, alkyl polyether (PO-EO copolymer), and fatty alcohol polyoxyethylene ether (AEO-3).

[0008] Furthermore, the surfactant is fatty alcohol polyoxyethylene ether ammonium sulfate (AESA).

[0009] Furthermore, the polymer builder is a mixture of one or more of acrylic acid copolymer, acrylamide polymer, carboxymethyl cellulose and vinyl alcohol polymer.

[0010] Furthermore, the polymer builder is an acrylic acid copolymer.

[0011] Furthermore, the enhancer is a formaldehyde aqueous solution with a mass concentration of 20-40%, preferably a formaldehyde aqueous solution with a mass concentration of 35%.

[0012] Furthermore, the high-purity water is high-purity water with a conductivity of ≥1M.

[0013] The present invention also provides a method for preparing a high-purity water-soluble silicon wafer cleaning agent, comprising the following steps: heating a surfactant, a polymer builder, and a cosolvent to 40-60°C to completely dissolve and mix, then adding high-purity water, stirring sufficiently, performing ion exchange, adding an enhancer, and filtering to obtain a finished product, wherein the finished product's density, pH, viscosity, metal impurities and other indicators are all within the control indicator range.

[0014] The ion exchange operation uses a cation exchange resin;

[0015] The pore size of the filter membrane used for filtration is 0.2 to 1.0 μm.

[0016] The quality indicators of the obtained product are density of 1.0-1.1 g / ml, pH of 2.5-6.5, and viscosity of 2.0-60 cm 2 / S, potassium ion content ≤1×10 -4 %, sodium ion content ≤1×10 -4 %, calcium ion content≤1×10 -4 %, copper ion content ≤1×10 -5 %, lead ion content≤1×10 -5 %, iron ion content ≤1×10 -5 %, magnesium ion content ≤1×10 -4 %.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] 1. The cleaning agent of the present invention is mainly used for cleaning and wiping silicon wafers after polishing, and is mainly used to remove lubricants, dust and other dirt on the surface of silicon wafers during processing. The substances used in the formula are all water-soluble substances and non-hazardous chemicals; the cleaning agent mentioned in the present invention is used to clean the polished silicon wafers, and its usage is about 40-50% of the existing cleaning agents, which reduces the discharge of three wastes; the ingredients used in the cleaning agent mentioned in the present invention are all commercially available non-toxic substances, and the safety is guaranteed. It is a non-toxic, harmless, safe and pollution-free cleaning agent.

[0019] 2. The surfactant in the formula of the present invention reduces the surface tension of water or the interfacial tension of oil and water by adsorption at the gas-liquid, liquid-liquid or solid-liquid interface, thereby achieving the effect of washing the oil on the surface of the silicon wafer. At the same time, the component also has a series of physical and chemical effects such as anti-sticking, demulsification, foaming, solubilization, dispersion, washing, anti-corrosion, and anti-static. The polymer builder adsorbs the excess metal ions in the silicon wafer cleaning process through the charged groups on the polymer structure, and at the same time, it plays a role in agglomeration, precipitation and removal of the washed substances. The main role of the cosolvent is to supplement the surfactant and polymer builder in the cleaning process, improve the silicon wafer cleaning effect and play a role in protecting the silicon wafer surface. The enhancer is mainly used for protecting the silicon wafer surface and preventing corrosion. High-purity water, as a solvent for the above components, plays the role of dissolving, diluting, washing, etc. In order to ensure the silicon wafer washing effect, the water quality conductivity has certain requirements, which is mainly guaranteed by high-purity water. DETAILED DESCRIPTION

[0020] The following is a detailed description of an embodiment of the present invention. This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and a specific operation process are given, but the protection scope of the present invention is not limited to the following embodiment.

[0021] Embodiment 1:

[0022] Start stirring, and use a vacuum pump to pump 140kg of fatty alcohol polyoxyethylene ether ammonium sulfate (AESA), 160kg of acrylic acid copolymer and 60kg of PEG-400 into a 2000L stainless steel reactor. Open the steam valve and heat to 40-60℃. After the pumped raw materials are completely melted, stop heating, and then add 700kg of conductive water with a resistivity of 1M. After stirring fully, ion exchange is carried out, and the liquid after ion exchange is stored in a 2000L plastic storage tank. Sampling analysis. The finished product density, PH, viscosity, metal impurities and other indicators are all within the control index range. After qualified analysis, add 500kg of 35% formaldehyde, and then filter with a 0.5μm filter membrane, sample the finished product again for analysis, and fill it with 25kg / barrel.

[0023] Embodiment 2:

[0024] Start stirring, and use a vacuum pump to pump 80kg of sodium sulfate of fatty alcohol polyoxyethylene ether, 120kg of acrylamide polymer and 30kg of PEG-600 into a 2000L stainless steel reactor, open the steam valve and heat to 40-60℃. After the pumped raw materials are completely melted, stop heating, and then add 470kg of conductive water with a resistivity of 1.5M. After stirring fully, ion exchange is carried out, and the liquid after ion exchange is stored in a 2000L plastic storage tank. Sampling analysis. The finished product density, PH, viscosity, metal impurities and other indicators are all within the control index range. After qualified analysis, add 300kg of 35% formaldehyde, and then filter with a 0.5μm filter membrane, sample the finished product again for analysis, and fill it with 25kg / barrel.

[0025] Embodiment 3:

[0026] Start stirring, and use a vacuum pump to pump 50kg of nonylphenol polyoxyethylene ether (TX-10), 150kg of vinyl alcohol polymer and 50kg of PEG-200 into a 2000L stainless steel reactor. Open the steam valve and heat to 40-60℃. After the pumped raw materials are completely melted, stop heating, and then add 450kg of conductive water with a resistivity of 1.5M. After stirring fully, ion exchange is carried out, and the liquid after ion exchange is stored in a 2000L plastic storage tank. Sampling analysis. The finished product density, PH, viscosity, metal impurities and other indicators are all within the control index range. After qualified analysis, add 300kg of 35% formaldehyde, and then filter with a 0.5μm filter membrane, sample the finished product again for analysis, and fill it with 25kg / barrel.

[0027] Embodiment 4:

[0028] Start stirring, and use a vacuum pump to pump 100kg fatty alcohol polyoxyethylene ether (AEO-3), 100kg carboxymethyl cellulose and 50kg PEG-400 into a 2000L stainless steel reactor, open the steam valve and heat to 40-60°C. After the pumped raw materials are completely melted, stop heating, and then add 350kg conductive water with a resistivity of 1.5M. After stirring fully, ion exchange is performed, and the liquid after ion exchange is stored in a 2000L plastic storage tank. Sampling analysis. The finished product density, PH, viscosity, metal impurities and other indicators are all within the control index range. After qualified analysis, add 400kg 30% formaldehyde, then filter with a 0.5μm filter membrane, sample the finished product again for analysis, and fill it with 25kg / barrel.

[0029] The products obtained in the above embodiments were analyzed and tested for performance, and the results are as follows:

[0030]

[0031]

[0032] It can be seen from the above table that after cleaning with the cleaning solution prepared by the present invention, the number of solid particle residues on the surface of the silicon wafer is 10 or less, which meets the needs of chip manufacturing such as solar energy and semiconductors.

[0033] For those skilled in the art, various corresponding changes made according to the technical solutions and concepts described above are all within the protection scope of the claims of the present invention.

Claims

1. A high-purity water-soluble silicon wafer cleaning agent, characterized in that: The invention is prepared from the following components in weight percentage: 5-10% surfactant, 5-15% polymer builder, 1-5% cosolvent, 25-40% enhancer and 35-50% high-purity water; The surfactant is one of fatty alcohol polyoxyethylene ether sodium sulfate AES, fatty alcohol polyoxyethylene ether ammonium sulfate AESA, nonylphenol polyoxyethylene ether TX-10, and fatty alcohol polyoxyethylene ether AEO-3; The polymer builder is one of acrylic acid copolymer, acrylamide polymer, carboxymethyl cellulose and vinyl alcohol polymer; the cosolvent is one of PEG200, PEG400 or PEG600; The enhancer is a formaldehyde aqueous solution with a mass concentration of 20-40%; The density of the cleaning agent is 1.0-1.1 g / ml, the pH is 2.5-6.5, and the viscosity is 2.0-60 cm 2 / S, potassium ion content ≤1×10 -4 %, sodium ion content ≤1×10 -4 %, calcium ion content ≤1×10 -4 %, copper ion content ≤1×10 -5 %, lead ion content ≤1×10 -5 %, iron ion content ≤1×10 -5 %, magnesium ion content ≤1×10 -4 %; The high-purity water-soluble silicon wafer cleaning agent is prepared by the following method: the surfactant, polymer builder and cosolvent are heated to 40-60°C to completely dissolve and mix, then high-purity water is added, after sufficient stirring and ion exchange, an enhancer is added, and the finished product is obtained by filtering.

2. The high-purity water-soluble silicon wafer cleaning agent according to claim 1, characterized in that: The surfactant is fatty alcohol polyoxyethylene ether ammonium sulfate AESA.

3. The high-purity water-soluble silicon wafer cleaning agent according to claim 1, characterized in that: The polymer builder is an acrylic acid copolymer.

4. The high-purity water-soluble silicon wafer cleaning agent according to claim 1, characterized in that: The enhancer is a formaldehyde aqueous solution with a mass concentration of 35%.

5. A method for preparing a high-purity water-soluble silicon wafer cleaning agent as claimed in any one of claims 1 to 4, characterized in that: The method comprises the following steps: heating a surfactant, a polymer builder and a cosolvent to 40-60°C to completely dissolve and mix them, then adding high-purity water, stirring them sufficiently, performing ion exchange, adding an enhancer, and filtering to obtain a finished product.

6. The method for preparing the high-purity water-soluble silicon wafer cleaning agent according to claim 5, characterized in that: The ion exchange operation uses a cation exchange resin; The pore size of the filter membrane used for filtration is 0.2 to 1.0 μm.

Citation Information

Patent Citations

  • Silicon wafer cleaning agent

    CN102477358B

  • Semiconductor industrial cleaning agent and application thereof

    CN103881837A

  • Cleaning agent composition used after silicon wafer processing

    CN113667546A