A composite solid electrolyte membrane and preparation method thereof
By adopting a composite solid electrolyte membrane and a positive electrode/electrolyte integrated design in lithium-ion batteries, the safety hazards and mechanical performance problems of traditional lithium-ion batteries are solved, and the high energy density and cycling performance are improved, which is suitable for large-scale production.
Patent Information
- Application Number
- CN202210169455.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-02-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-02-23
AI Technical Summary
Traditional lithium-ion batteries have safety hazards and high-temperature operation requirements for organic liquid electrolytes. The mechanical properties and room temperature ionic conductivity of solid electrolytes are low, which limits the battery's energy density and application feasibility.
Using composite solid electrolyte membranes, a high mechanical strength, ultra-thin composite solid electrolyte membrane is prepared by adding inorganic oxides and lithium salts to the polymer, combined with high porosity porous support materials, and designed through the integrated design of positive electrode/electrolyte. Modify the liquid phase interface to improve interface compatibility.
It realizes a solid-state battery with wide electrochemical window, high energy density and low interface resistance, which improves the cycling performance and energy density of the battery and is suitable for large-scale production.
Smart Images

Figure CN114335701B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of lithium ion batteries, and in particular to a composite solid electrolyte membrane and a preparation method thereof. Background Art
[0002] With the development of science and technology, the requirements for the specific energy and safety of electric energy in aerospace, new energy and other fields are getting higher and higher. The organic liquid electrolyte of traditional lithium-ion batteries is flammable and explosive at high temperatures, causing thermal runaway of the battery, which poses a great safety hazard. At the same time, since the metal lithium negative electrode is very easy to produce dendrites in the electrolyte, it pierces the diaphragm and causes a short circuit in the battery. The application of high working voltage positive electrode materials is an important way to further improve the energy density of lithium-ion batteries, but traditional liquid electrolytes will undergo severe oxidative decomposition when the voltage is higher than >4.3V, resulting in large irreversible capacity and severe capacity decay. Therefore, traditional lithium-ion batteries based on organic electrolytes use non-lithium metal negative electrodes, which limits the further improvement of battery energy density. Solid-state lithium batteries using solid electrolytes can solve the above problems well.
[0003] Organic polymer solid electrolytes have the advantages of simple preparation method, better ductility, stronger flexibility, good film-forming performance, and good electrode electrolyte interface contact, but they have the disadvantages of poor mechanical properties and low ion conductivity at room temperature. For example, the ion conduction mechanism of the polyethylene oxide (PEO) system is to realize Li by the chain segment movement in the amorphous phase of PEO. + Migration, the proportion of amorphous phase region is small at room temperature, which leads to low ionic conductivity. The proportion of amorphous region is often increased by adding other inorganic substances. The electrochemical window of PEO solid polymer electrolyte is relatively narrow (<4V), which is difficult to match high-voltage positive electrode materials. The improvement of solid-state battery energy density is relatively limited, and PEO-based solid-state batteries need to operate at relatively high temperatures (60-80°C), which greatly increases the operating cost. In addition to PEO-based polymer systems, polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyacrylonitrile (PAN), etc. are also important polymer electrolyte systems. Among them, due to the strong polar group -CH2 - CF2 - The strong electronegativity of fluorine atoms is conducive to promoting the dissociation of lithium salts and increasing the concentration of lithium ions in the PVDF matrix, making PVDF a medium for conducting lithium ions. In addition, it also has excellent thermodynamic properties. However, almost all polymer electrolytes have relatively low room temperature ionic conductivity (10 -8 ~10 -5 S cm -1 ) and the low lithium ion migration number (<0.5) limit its application feasibility.
[0004] In order to take into account the high ionic conductivity of inorganic solid electrolytes and the flexibility of solid polymer electrolytes, the development of organic / inorganic composite solid electrolytes by adding inorganic fillers to polymer electrolytes has become a key breakthrough for solid-state lithium batteries; organic / inorganic composite solid electrolytes have simple preparation methods, good ductility, and stronger flexibility. At the same time, they have good film-forming properties and relatively good electrode electrolyte interface contact, but the mechanical strength and stability of the electrolyte still cannot meet the requirements of long-cycle stable operation of solid-state batteries.
[0005] Patent application number CN201611112927.X discloses "composite solid electrolyte membrane, preparation method and lithium-ion battery", which includes a porous support material; a first composite adhesive layer coated on both sides of the porous support material; a second composite adhesive layer coated on the first composite adhesive layer; the inorganic content of the second composite adhesive layer is lower than the inorganic content of the first composite adhesive layer. The present invention adds a porous support material to the electrolyte membrane, thereby ensuring the flexibility of the membrane and enhancing the mechanical strength of the membrane, and the sandwich structure electrolyte membrane can improve the interface compatibility and improve the cycle performance of the battery. However, the preparation process of the composite solid electrolyte membrane in this scheme is relatively cumbersome, and the battery data of the embodiment are all obtained under a high temperature of 60°C, and the electrochemical performance of the solid-state battery at room temperature is not provided. At the same time, the thickness of the composite electrolyte membrane is not clearly stated in this scheme.
[0006] Compared with traditional liquid lithium-ion batteries, solid-state batteries use solid electrolytes, which have the advantages of wider electrochemical window, higher energy density, more flexibility, better battery safety at high temperatures, etc. However, solid-state batteries still have a series of problems such as poor stability of the electrode / solid electrolyte membrane interface, large interface impedance, non-uniform deposition of lithium ions during long cycles leading to dendrite growth and poor electrochemical performance. Therefore, it is of great significance to design a thin-film solid electrolyte that is both rigid and flexible. Summary of the invention
[0007] In view of the deficiencies of the prior art, the present invention provides a composite solid electrolyte membrane and a preparation method thereof.
[0008] This is achieved specifically through the following technical solutions:
[0009] A composite solid electrolyte membrane is prepared by uniformly dispersing a polymer in an organic solvent, then adding an inorganic oxide to disperse the polymer evenly, and finally adding a lithium salt to stir the mixture to obtain a composite electrolyte slurry. The composite electrolyte slurry is coated on a porous support material with high porosity and dried to obtain a high mechanical strength and ultra-thin composite solid electrolyte membrane.
[0010] The mass ratio of polymer, inorganic oxide and lithium salt in the composite solid electrolyte membrane is 20-80:10-30:10-60.
[0011] The lithium salt in the composite electrolyte slurry accounts for 10-60% of the total weight of the solid solute; the solid solute is a polymer, an inorganic oxide and a lithium salt.
[0012] The polymer consists of component A and component B in a mass ratio of 1:5 to 2:1; the component A is polyethylene oxide (PEO), and the component B is one or more of polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polymethyl methacrylate (PMMA), and polypropylene carbonate (PPC).
[0013] The inorganic oxide is any one or more mixtures of lithium lanthanum zirconium oxide (LLZO), tantalum-doped lithium lanthanum zirconium oxide (LLZTO), lithium lanthanum titanate (LLTO), lithium aluminum titanium phosphide (LATP), and lithium aluminum germanium phosphide (LAGP).
[0014] The lithium salt is any one or more mixtures of lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(oxalatoborate) (LiBOB), lithium hexafluorophosphate (LiPF6), and lithium perchlorate (LiClO4).
[0015] The organic solvent is one or more of acetonitrile, N,N-dimethylformamide, N-methylpyrrolidone, isopropanol and acetone.
[0016] The invention is mainly based on PEO, and the addition of PPC, PMMA, PVDF, PVDF-HFP, etc. can effectively broaden the room temperature electrochemical window of PEO, especially PPC and PMMA can broaden the electrochemical window and enhance its mechanical strength; the addition of inorganic oxides can enhance the mechanical strength of organic polymers, among which LLZTO has high ion conductivity, LATP is stable to lithium at high voltage, and has high ion conductivity; lithium salt can provide lithium ions, LiFSI has high conductivity, low water sensitivity, good thermal stability, but is expensive; LiTFSI has high solubility and conductivity, high thermal decomposition temperature, is not easy to hydrolyze, and the delocalization of large anion TFSI in LiTFSI makes LiTFSI higher than LiPF6 and LiClO4 with high content are more easily dissolved and dissociated in the polymer matrix; lithium bis(oxalatoborate) (LiBOB) has high conductivity, wide electrochemical window, good thermal stability, but low solubility; lithium hexafluorophosphate (LiPF6) has high solubility, high ionic conductivity, easy film formation, but poor thermal stability and easy decomposition reaction. Therefore, LiTFSI and LiFSI are preferred lithium salts in the present invention; therefore, the present invention uses PEO as the main polymer, and adds other polymers to improve its electrochemical window and mechanical properties; the composite of inorganic oxides and polymers can improve their mechanical strength and room temperature ionic conductivity, and inorganic oxides with high ionic conductivity at room temperature such as LLZTO and LATP are preferred.
[0017] A method for preparing a composite solid electrolyte membrane comprises the following steps:
[0018] 1) dissolving the polymer in an organic solvent and dispersing it evenly by mechanical stirring or planetary stirring, then adding an inorganic oxide and dispersing it evenly, and finally adding a lithium salt and dispersing it evenly to obtain a composite electrolyte slurry;
[0019] 2) The composite electrolyte slurry is coated on a porous support material with high porosity and dried to obtain a high mechanical strength and ultra-thin composite solid electrolyte membrane.
[0020] The porous support material is any one of a high-porosity polyethylene (PE) based film with a thickness of ≤8 μm, a non-woven fabric membrane, a glass fiber mesh, or an electrospinning membrane.
[0021] The composite electrolyte slurry is coated on a porous support material with high porosity, and the thickness of the composite solid electrolyte membrane after drying is ≤15 μm.
[0022] A composite solid electrolyte membrane is used in the manufacture of a solid-state battery, and the specific application method includes:
[0023] S1 battery cell production: winding or stacking the integrated positive electrode sheet, composite solid electrolyte membrane and negative electrode sheet membrane into a battery cell;
[0024] S2 battery cell hot pressing: hot press the battery cell at 25-40℃ and pressure of 0.1-0.2MPa for 0.5-1h;
[0025] S3 liquid phase interface modification: Place the battery cell in the shell and add 0.3-1.0g / Ah electrolyte for interface modification.
[0026] The active material of the integrated positive electrode sheet is any one or more mixtures of high-voltage lithium cobalt oxide, high-nickel ternary materials, and lithium-rich manganese-based materials.
[0027] The integrated positive electrode sheet is prepared by coating the composite electrolyte slurry in the composite solid electrolyte membrane manufacturing process on the surface of the positive electrode sheet active material by surface spin coating or scraping. After drying, the composite solid electrolyte membrane layer thickness on the positive electrode sheet surface is ≤5 μm.
[0028] The negative electrode sheet is a lithium metal or lithium alloy negative electrode.
[0029] The electrolyte is an ester or ether electrolyte, and the lithium salt in the electrolyte is any one or more mixtures of lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(oxalatoborate) (LiBOB), lithium hexafluorophosphate (LiPF6), and lithium perchlorate (LiClO4), and the total concentration of lithium salt in the electrolyte is 1.0-1.5 mol / L.
[0030] Beneficial effects:
[0031] The present invention introduces a high-porosity support material into the composite electrolyte to prepare an ultra-thin composite solid electrolyte membrane having wide window, rigidity and flexibility, and low interface resistance characteristics. In addition, the positive electrode / electrolyte integrated design, liquid phase modification, battery hot pressing and other processes are adopted in the solid-state battery to further improve the interface compatibility, effectively solve the problem of large internal interface impedance and easy micro-short circuit of the all-solid-state battery, and the positive electrode of the solid-state battery can use a high-voltage positive electrode, which can further improve the energy density of the solid-state battery, and the battery has excellent electrochemical performance. The preparation method of the present invention is simple, the prepared solid-state battery has excellent performance, and is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a SEM image of the PE base film used in Example 1;
[0033] Figure 2 This is a SEM image of the composite solid electrolyte membrane prepared in Example 1;
[0034] Figure 3 is an electrochemical window of the composite solid electrolyte membrane prepared according to Example 1;
[0035] Figure 4This is a first charge and discharge curve diagram of the solid-state battery prepared according to Example 1;
[0036] Figure 5 This is a cycle performance diagram of the solid-state battery prepared according to Example 2. DETAILED DESCRIPTION
[0037] The specific embodiments of the present invention are further described in detail below, but the present invention is not limited to these embodiments, and any improvement or substitution based on the basic spirit of the present embodiment still falls within the scope of protection required by the claims of the present invention.
[0038] Example 1
[0039] A preparation method of a composite solid electrolyte membrane comprises the following steps:
[0040] 1) PEO, PPC, PMMA, LiTFSI and LLZTO powders are weighed in a mass ratio of 8:3:3:3:4, PEO, PPC and PMMA are dispersed in an acetonitrile solution by mechanical stirring and uniformly mixed, LLZTO is then added and uniformly dispersed, and finally LiTFSI is added and uniformly dispersed to prepare a composite electrolyte slurry;
[0041] 2) The composite electrolyte slurry was coated on a 5 μm PE base film, the acetonitrile solvent was dried in a forced air drying oven at 55°C, and then transferred to a vacuum drying oven at 60°C and vacuum dried for 24 hours to obtain a composite solid electrolyte membrane with a thickness of 11 μm;
[0042] The amount of the acetonitrile solution added is sufficient to dissolve the solid solute, and the total mass ratio of the acetonitrile solution to the solid solute is 6:1; the solid solute is a polymer, an inorganic oxide, or a lithium salt;
[0043] Figure 1 The SEM image of the PE base film used in this embodiment; Figure 2 This is a SEM image of the composite solid electrolyte membrane prepared in this example. It can be seen from the image that the composite solid electrolyte membrane is relatively dense and has no obvious pores.
[0044] Example 2
[0045] A preparation method of a composite solid electrolyte membrane comprises the following steps:
[0046] 1) PEO, PPC, PVDF-HFP, lithium salt LiFSI and LLZTO powders are weighed in a mass ratio of 4:3:5:5:3, PEO, PPC and PVDF-HFP are first dispersed in a DMF solution by planetary stirring and uniformly mixed, then LLZTO is added and uniformly dispersed, and finally LiFSI is added and uniformly dispersed to prepare a composite electrolyte slurry;
[0047] 2) The composite electrolyte slurry was coated on a 5 μm PE base film, the DMF solvent was dried in a blast drying oven at 60°C, and then transferred to a 60°C vacuum drying oven and vacuum dried for 24 hours to obtain a composite solid electrolyte membrane with a thickness of 12 μm;
[0048] The amount of DMF added is sufficient to dissolve the solid solute, and the total mass ratio of DMF to the solid solute is 5:1; the solid solute is a polymer, an inorganic oxide, or a lithium salt.
[0049] Example 3
[0050] A preparation method of a composite solid electrolyte membrane comprises the following steps:
[0051] 3) PEO, PPC, PVDF, lithium salt LiTFSI and LLZTO powders are weighed in a mass ratio of 3:3:4:6:4, PEO, PPC and PVDF are first dispersed in an NMP solution by planetary stirring and uniformly mixed, LLZTO is then added and uniformly dispersed, and finally LiTFSI is added and uniformly dispersed to prepare a composite electrolyte slurry;
[0052] 4) The composite electrolyte slurry was coated on a 5 μm PE base film, the NMP solvent was dried in a blast drying oven at 60°C, and then transferred to a 60°C vacuum drying oven and vacuum dried for 24 hours to obtain a composite solid electrolyte membrane with a thickness of 13 μm;
[0053] The amount of NMP added is sufficient to dissolve the solid solute, and the total mass ratio of NMP to the solid solute is 5:1; the solid solute is a polymer, an inorganic oxide, or a lithium salt.
[0054] Example 4
[0055] The application of the composite solid electrolyte membrane prepared in Example 1 in the manufacture of button batteries specifically includes the following steps:
[0056] 1) Preparation of integrated positive electrode sheet: high voltage lithium cobalt oxide LCO and conductive carbon black are mixed evenly, dissolved in an N-methylpyrrolidone solution containing polyvinylidene fluoride, wherein the mass ratio of high voltage lithium cobalt oxide LCO, conductive carbon black and polyvinylidene fluoride is 94:3:3, and dispersed evenly by planetary stirring, and the evenly dispersed slurry is evenly coated on an aluminum foil current collector, vacuum dried at 100° C. for 48 hours, and rolled and sliced to obtain a positive electrode sheet; then a layer of the composite electrolyte slurry prepared in Example 1 is spin-coated on the surface of the positive electrode sheet, the solvent is first dried in a blast drying oven at 55° C., and then transferred to a vacuum drying oven at 60° C. for vacuum drying for 24 hours to obtain an integrated positive electrode sheet, and the thickness of the solid electrolyte membrane of the electrode sheet after drying is ≤5 μm;
[0057] 2) Preparation of button cell: A lithium sheet is used as the negative electrode. In a dry room with air moisture content less than 3% or a glove box with argon atmosphere, a button cell is assembled with the negative electrode sheet / composite solid electrolyte membrane / stainless steel gasket to test the composite solid electrolyte ion conductivity EIS. The composite solid electrolyte ion conductivity at room temperature is about 4.4×10 -4 S / cm, the impedance value of the composite solid electrolyte membrane is about 1.8Ω; the negative electrode sheet / composite solid electrolyte membrane / stainless steel gasket are assembled into a button cell to test the electrochemical window of the composite solid electrolyte membrane; in addition, the integrated positive electrode sheet / composite solid electrolyte membrane / negative electrode sheet are assembled, and 20μL of electrolyte is dripped at the interface to assemble a 2016 button cell, and then an electrochemical test is performed; the lithium salt in the electrolyte is LITFSI, and its concentration is 1.0mol / L; the solvent in the electrolyte is a mixture of dimethyl ether (DME) and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) in a molar ratio of 1.3:3;
[0058] See Figure 3 and Figure 4 ;like Figure 3 As shown, its electrochemical window is as high as 4.5V, which can be adapted to high-voltage lithium cobalt oxide positive electrodes; Figure 4 The first charge and discharge curve of the solid-state battery shown in the figure shows that at room temperature, 3-4.4V, 0.1C charge / 0.1C discharge conditions, the first discharge capacity of the solid-state battery is 167.9mAh / g.
[0059] Example 5
[0060] The application of the composite solid electrolyte membrane prepared in Example 2 in the manufacture of a solid-state battery specifically comprises the following steps:
[0061] 1) Preparation of integrated positive electrode sheet: The preparation of the positive electrode sheet is the same as in Example 4, and the composite electrolyte slurry prepared in Example 2 is scraped on the surface of the positive electrode sheet. Other conditions are the same as those described in Example 1;
[0062] 2) Preparation of solid-state battery: A lithium sheet is used as the negative electrode, and the composite solid electrolyte membrane of Example 2 is assembled in a connection relationship between the integrated positive electrode sheet and the lithium sheet. The wound soft-pack battery is assembled in a drying room with an air moisture content of <3%. The battery capacity is 2.1Ah, and the battery core is hot-pressed for 0.5h at 40°C and a pressure of 0.15MPa, and then 0.84g of electrolyte is added for interface modification. The electrolyte is added at 0.4g / Ah, and the battery is left to stand for 0.5h. After vacuuming, the battery is packaged and then electrochemically tested at room temperature, 3-4.4V, 0.1C charge / 0.1C discharge conditions; the battery specific energy is as high as 350Wh / Kg, and the cycle performance diagram of the solid-state battery is shown in Figure 5The lithium salt in the electrolyte is LITFSI, and its concentration is 1.2 mol / L; the solvent in the electrolyte is a mixture of dimethyl ether (DME) and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) in a molar ratio of 1.5:3;
[0063] like Figure 5 As shown, after 80 cycles, the solid-state battery has a discharge capacity of 1.96Ah and a capacity retention rate of 93.4%, indicating good cyclability.
[0064] Example 6
[0065] The application of the composite solid electrolyte membrane prepared in Example 3 in the manufacture of a solid-state battery specifically comprises the following steps:
[0066] 1) Preparation of integrated positive electrode sheet: The preparation of the positive electrode sheet is the same as in Example 4, and the composite electrolyte slurry prepared in Example 3 is scraped on the surface of the positive electrode sheet. Other conditions are the same as those described in Example 1;
[0067] 2) Preparation of solid-state battery: A lithium sheet was used as the negative electrode, and the composite solid electrolyte membrane of Example 3 was placed between the integrated positive electrode sheet and the lithium sheet for assembly. The wound soft-pack battery was assembled in a drying room with an air moisture content of <3%. The battery capacity was 2.8Ah, and the battery core was hot-pressed at 35°C and a pressure of 0.1MPa for 0.5h, and then 1.40g of electrolyte was added for interface modification. The electrolyte was added at 0.5g / Ah, and it was left to stand for 0.5h. After vacuuming, the battery was packaged and then Cyclic tests were conducted at room temperature, 3-4.4V, 0.1C charge / 0.1C discharge conditions; the battery specific energy was as high as 360Wh / Kg; the lithium salts in the electrolyte were LiFSI and LiBOB, and the total lithium salt concentration was 1.2mol / L; the lithium salts LiFSI and LiBOB in the electrolyte were mixed in a molar ratio of 5:1, and the solvent was a mixture of dimethyl ether (DME) and 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether (TTE) in a molar ratio of 1.2:3;
[0068] The prepared solid-state battery was cycled for 70 cycles, with a discharge capacity of 2.63Ah and a capacity retention rate of 93.9%, indicating good cyclability.
[0069] In summary, the present invention prepares a composite solid electrolyte by organic / inorganic composite, and introduces a high-porosity rigid skeleton to prepare an ultra-thin, low-impedance rigid-flexible composite solid electrolyte, which has a higher voltage window, higher mechanical strength, higher ionic conductivity, and lower impedance compared to traditional PEO-based polymer electrolytes; in addition, through the design of positive electrode / electrolyte integration, interface modification of trace electrolyte, and battery core hot pressing process, a high-voltage solid-state metal lithium battery is prepared, which further improves the interface compatibility, and the battery has a higher output voltage, a high discharge capacity, is relatively stable to the metal lithium negative electrode, and has excellent cycle performance, and has a high application prospect. The method is simple, controllable, and suitable for large-scale production.
Claims
1. A composite solid electrolyte membrane, characterized in that: The composite solid electrolyte membrane is prepared by uniformly dispersing a polymer in an organic solvent, then adding an inorganic oxide to disperse the polymer, and finally adding a lithium salt to mix the mixture to obtain a composite electrolyte slurry. The composite electrolyte slurry is coated on a porous support material with a high porosity, and then dried to obtain a high mechanical strength and ultra-thin composite solid electrolyte membrane. The polymer is composed of component A and component B in a mass ratio of 1:5 to 2:1; the component A is polyethylene oxide, and the component B is one or more of polyvinylidene fluoride-hexafluoropropylene, polyvinylidene fluoride, polyacrylonitrile, polymethyl methacrylate, and polypropylene carbonate: The inorganic oxide is any one or more mixtures of LLZO, LLZTO, LLTO, LATP, and LAGP; The porous support material is any one of a high-porosity polyethylene-based film with a thickness of ≤8 μm, a non-woven fabric membrane, a glass fiber mesh, or an electrospun membrane; The composite electrolyte slurry is coated on a porous support material with high porosity, and the thickness of the composite solid electrolyte membrane after drying is ≤15 μm.
2. A composite solid electrolyte membrane as claimed in claim 1, characterized in that: The mass ratio of polymer, inorganic oxide and lithium salt in the composite solid electrolyte membrane is 20-80:10-30:10-60.
3. A composite solid electrolyte membrane as claimed in claim 1, characterized in that: The lithium salt in the composite electrolyte slurry accounts for 10-60% of the total weight of the solid solute.
4. A composite solid electrolyte membrane as claimed in claim 1 or 2, characterized in that: The lithium salt is any one or more mixtures of LiFSI, LiTFSI, LiBOB, LiPF 6 , and LiClO 4 .
5. A composite solid electrolyte membrane as claimed in claim 1, characterized in that: The organic solvent is one or more of acetonitrile, N,N-dimethylformamide, N-methylpyrrolidone, isopropanol and acetone.
6. A method for preparing a composite solid electrolyte membrane according to claim 1, characterized in that: Includes steps: 1) dissolving the polymer in an organic solvent and dispersing it evenly by mechanical stirring or planetary stirring, then adding an inorganic oxide and dispersing it evenly, and finally adding a lithium salt and dispersing it evenly to obtain a composite electrolyte slurry; 2) The composite electrolyte slurry is coated on a porous support material with high porosity and dried to obtain a high mechanical strength and ultra-thin composite solid electrolyte membrane.
Citation Information
Cited By
Coating material, preparation method of laminated electrolyte and solid-state battery
CN116053569A
Coating material, method for manufacturing laminated electrolyte, and solid-state battery
CN116053569B