Carbon nanotube-resin composite and method for producing the same
By applying tensile force and attaching resin during the growth process of carbon nanotubes, oriented carbon nanotube collection lines are formed, which solves the problem of insufficient length of carbon nanotubes and improves the fracture strength and conductivity of the carbon nanotube-resin composite. , suitable for complex-shaped material applications.
Patent Information
- Application Number
- CN202080061094.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-09-03
- Filing Date
- 2020-08-28
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-08-28
AI Technical Summary
Existing carbon nanotube production technology makes it difficult to extend the length of carbon nanotubes, resulting in their breaking strength being insufficient to meet the requirements for use as wires or high-strength materials.
By supplying carbon-containing gas to the floating catalyst particles, the carbon nanotubes are grown and tensile force is applied to form oriented carbon nanotube collection lines, and the resin is attached to the collection lines, and the carbon nanotube-resin is obtained by evaporating the resin. complex.
The fracture strength of the carbon nanotube-resin composite is improved, making it suitable for complex-shaped carbon fiber reinforced plastic products, and enhancing the material's endurance and conductivity.
Smart Images

Figure CN114341262B_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a carbon nanotube-resin composite and a method for producing the carbon nanotube-resin composite. This application claims priority based on Japanese Patent Application No. 2019-160767 filed on September 3, 2019. All the contents described in the Japanese patent application are incorporated herein by reference. Background Art
[0002] Carbon nanotubes (hereinafter also referred to as "CNTs"), which have a cylindrical structure of graphene sheets in which carbon atoms are connected in hexagons, are a material with excellent properties, such as being one-fifth the weight of copper, 20 times the strength of steel, and having the conductivity of metal. Therefore, electric wires using carbon nanotubes are expected to contribute to (especially) improving the weight reduction, miniaturization, and corrosion resistance of automobile engines.
[0003] For example, as shown in Patent Document 1 (Japanese Patent Application Laid-Open No. 2005-330175), carbon nanotubes are obtained by a vapor phase growth method in which a raw material gas containing carbon is supplied while a fine catalyst such as iron is heated, so that carbon nanotubes grow from the catalyst.
[0004] Prior art literature
[0005] Patent Literature
[0006] Patent Document 1: Japanese Patent Application Publication No. 2005-330175
[0007] Non-patent literature
[0008] Non-patent literature 1: Agnieszka Lekawa-Raus et al. "Electrical Properties of Carbon Nanotube Based Fibers and Their Future Use in Electrical Wiring", Advanced Functional Materials, Vo. 24, pp3661-3682 (2014). DOI: 10.1002 / adfm.201303716 Summary of the invention
[0009] A carbon nanotube-resin composite according to one embodiment of the present disclosure includes:
[0010] A carbon nanotube assembly wire including a plurality of carbon nanotubes, and a resin,
[0011] In the carbon nanotube aggregate wire, the carbon nanotubes are oriented at an orientation degree of 0.9 or more and 1 or less.
[0012] One embodiment of the present disclosure is a method for producing a carbon nanotube-resin composite, the method comprising:
[0013] a growing step of growing a plurality of carbon nanotubes by supplying a carbon-containing gas to a plurality of catalyst particles in a floating state so that one or more carbon nanotubes grow from each of the plurality of catalyst particles;
[0014] an elongation step of applying a tensile force to the plurality of carbon nanotubes in a floating state so as to elongate the plurality of carbon nanotubes;
[0015] A step of aligning and aggregating the plurality of carbon nanotubes in a floating state along a flow direction of the carbon-containing gas to obtain a plurality of carbon nanotube aggregate lines;
[0016] a step of attaching a volatile liquid containing a resin to the plurality of carbon nanotube assembly wires while aligning and bundling the plurality of carbon nanotube assembly wires in the longitudinal direction thereof; and
[0017] The evaporation step is to obtain a carbon nanotube-resin composite by evaporating the volatile liquid attached to the plurality of carbon nanotube aggregate wires. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] [ Figure 1 ] Figure 1 This is a diagram illustrating a typical configuration example of a carbon nanotube aggregate wire included in a carbon nanotube-resin composite according to one embodiment of the present disclosure.
[0019] [ Figure 2 ] Figure 2 This is a diagram showing an example of carbon nanotubes included in a carbon nanotube-resin composite according to an embodiment of the present disclosure.
[0020] [ Figure 3 ] Figure 3 This is a diagram illustrating a typical configuration example of a carbon nanotube-resin composite production apparatus according to one embodiment of the present disclosure.
[0021] [ Figure 4 ] Figure 4 It is a graph showing stress-strain curves of samples 1 to 3. DETAILED DESCRIPTION
[0022] [Problems to be Solved by the Present Disclosure]
[0023] The carbon nanotubes obtained by the current carbon nanotube production technology have a diameter of about 0.4nm to 20nm and a maximum length of 55cm. In order to use carbon nanotubes as electric wires or high-strength materials, longer carbon nanotubes are required, so research has been conducted on technologies that can extend carbon nanotubes.
[0024] As a method of extending the carbon nanotubes, a method of orienting a plurality of carbon nanotubes in the longitudinal direction and gathering them to form a gathering line is considered.
[0025] As one of such methods, a method of obtaining a CNT aggregate wire by mixing a plurality of randomly oriented CNTs with a dispersant (surfactant, polymer, etc.) and injection molding the mixture into a fiber shape has been studied (Non-Patent Document 1).
[0026] However, the breaking strength of the CNT aggregate wire obtained by the above method sometimes tends to be lower than the breaking strength originally possessed by CNTs.
[0027] Therefore, an object of the present disclosure is to provide a carbon nanotube-resin composite having excellent breaking strength.
[0028] [Effects of the present disclosure]
[0029] According to the above aspect, a carbon nanotube-resin composite having excellent breaking strength can be provided.
[0030] [Description of Embodiments of the Present Disclosure]
[0031] First, embodiments of the present disclosure will be listed and described.
[0032] (1) The carbon nanotube-resin composite disclosed herein comprises:
[0033] A carbon nanotube assembly wire including a plurality of carbon nanotubes, and a resin,
[0034] In the carbon nanotube aggregate wire, the carbon nanotubes are oriented at an orientation degree of 0.9 or more and 1 or less.
[0035] According to the above aspect, a carbon nanotube-resin composite having excellent breaking strength can be provided.
[0036] (2) The carbon nanotube-resin composite preferably contains 0.1 mass % or more and less than 100 mass % of the resin.
[0037] This further improves the fracture strength of the carbon nanotube-resin composite.
[0038] (3) The resin is preferably a thermosetting resin or a photocurable resin.
[0039] Since the diameter of the CNT monomers that constitute the carbon nanotube-resin composite is as small as nanometer level, it can be applied to CFRP (Carbon Fiber Reinforced Plastics) products with large curvature and complex shapes that are difficult to handle with existing carbon fibers (minimum filament diameter: about several μm).
[0040] (4) The thermosetting resin is preferably a novolac type epoxy resin.
[0041] This further improves the fracture strength of the carbon nanotube-resin composite.
[0042] (5) The resin is preferably a thermoplastic resin.
[0043] Since the diameter of the CNT monomer constituting the carbon nanotube-resin composite is as small as nanometer level, it can be applied to CFRP products with large curvature and complex shape, which are difficult to handle with conventional carbon fibers (minimum filament diameter: about several μm).
[0044] (6) The thermoplastic resin is preferably polymethyl methacrylate resin.
[0045] This further improves the fracture strength of the carbon nanotube-resin composite.
[0046] (7) In the Raman spectrum of the carbon nanotube-resin composite, the Raman shift is 1590±20cm -1 The peak intensity G at and Raman shift 1350±20cm -1 The ratio D / G of the peak intensity D at is preferably 0 or more and 0.1 or less.
[0047] This further improves the fracture strength of the carbon nanotube-resin composite.
[0048] (8) A method for producing a carbon nanotube-resin composite according to one embodiment of the present disclosure is the method for producing the carbon nanotube-resin composite described above, the method comprising:
[0049] a growing step of growing a plurality of carbon nanotubes by supplying a carbon-containing gas to a plurality of catalyst particles in a floating state so that one or more carbon nanotubes grow from each of the plurality of catalyst particles;
[0050] an elongation step of applying a tensile force to the plurality of carbon nanotubes in a floating state so as to elongate the plurality of carbon nanotubes;
[0051] A step of aligning and aggregating the plurality of carbon nanotubes in a floating state along a flow direction of the carbon-containing gas to obtain a plurality of carbon nanotube aggregate lines;
[0052] a step of attaching a volatile liquid containing a resin to the plurality of carbon nanotube assembly wires while aligning and bundling the plurality of carbon nanotube assembly wires in the longitudinal direction thereof; and
[0053] The evaporation step is to obtain a carbon nanotube-resin composite by evaporating the volatile liquid attached to the plurality of carbon nanotube aggregate wires.
[0054] Thereby, a carbon nanotube-resin composite having excellent breaking strength can be obtained.
[0055] [Detailed description of embodiments of the present invention]
[0056] Hereinafter, a specific example of a carbon nanotube-resin composite (hereinafter also referred to as “CNT-resin composite”) according to an embodiment of the present disclosure will be described with reference to the drawings.
[0057] In the drawings of the present disclosure, the same reference numerals represent the same parts or equivalent parts. In addition, in order to make the drawings clear and simple, the dimensional relationships such as length, width, thickness, depth, etc. are appropriately changed, and do not necessarily represent the actual dimensional relationships.
[0058] In this specification, the expression of "A to B" means the upper and lower limits of the range (i.e., A or more and B or less). When the unit is not described for A and only the unit is described for B, the unit of A is the same as the unit of B. In addition, if the upper limit value of the range is C, it means that the upper limit of the range is less than C, and if the lower limit value of the range is D, it means that the lower limit of the range is greater than D.
[0059] [Embodiment 1: Carbon Nanotube-Resin Composite]
[0060] A carbon nanotube-resin composite according to one embodiment of the present disclosure includes a carbon nanotube aggregate wire including a plurality of carbon nanotubes and a resin, wherein the carbon nanotubes in the carbon nanotube aggregate wire are oriented at an orientation degree of 0.9 or more and 1 or less.
[0061] <Carbon Nanotube Wire>
[0062] Figure 1 1 is a diagram illustrating a representative configuration example of a carbon nanotube aggregate wire (hereinafter also referred to as a "CNT aggregate wire") contained in a carbon nanotube-resin composite. Figure 1 As shown, the carbon nanotube aggregate wire 1 includes a plurality of carbon nanotubes 2. In the CNT aggregate wire, the plurality of carbon nanotubes 2 are oriented at an orientation degree of 0.9 or more and 1.0 or less.
[0063] (Shape of carbon nanotubes)
[0064] As the carbon nanotubes included in the CNT aggregate wire, CNTs of known structures can be used, for example, single-walled carbon nanotubes having only one carbon layer (graphene) and in a cylindrical shape, double-walled carbon nanotubes having multiple carbon layers stacked and in a cylindrical shape, or multi-walled carbon nanotubes.
[0065] The shape of the carbon nanotubes is not particularly limited, and any one having a closed front end or an open front end can be used. Figure 2 As shown, the catalyst P used in manufacturing the carbon nanotubes may be attached to one or both ends of the tube portion T of the carbon nanotube 2. In addition, a cone portion C made of conical graphene may be formed at one or both ends of the tube portion T of the carbon nanotube 2.
[0066] The length of the carbon nanotube can be appropriately selected according to the purpose. The length of the carbon nanotube is, for example, preferably 10 μm or more, more preferably 100 μm or more. In particular, when the length of the carbon nanotube is 100 μm or more, it is preferred from the viewpoint of making a CNT assembly line. There is no particular upper limit on the length of the carbon nanotube, but from the viewpoint of manufacturing, it is preferably 600 mm or less. The length of the CNT is preferably 10 μm or more and 600 mm or less, more preferably 100 μm or more and 600 mm or less. The length of the CNT can be measured by observation using a scanning electron microscope.
[0067] The diameter of the carbon nanotube is preferably 0.6 nm to 20 nm, more preferably 1 nm to 10 nm, and further preferably 1 nm to 2 nm. When the diameter of the carbon nanotube is 1 nm to 10 nm, it is preferred from the viewpoint of heat resistance under oxidative conditions. When the diameter of the carbon nanotube is 0.6 nm to 2 nm, it is preferred from the viewpoint of improving fracture strength.
[0068] In this specification, the diameter of a carbon nanotube refers to the average outer diameter of a CNT. The average outer diameter of a CNT can be obtained by directly observing the cross-section of any two locations of the CNT using a transmission electron microscope, measuring the distance between the two most distant points on the periphery of the CNT in the cross-section, i.e., the outer diameter, and calculating the average value of the obtained outer diameters. In the case where one or both ends of the CNT include a cone, the diameter is measured at a position other than the cone.
[0069] (Orientation of carbon nanotubes)
[0070] The method for calculating the degree of orientation of CNTs in a CNT aggregate line is described below. In this specification, the degree of orientation of CNTs refers to a value calculated according to the following steps (a1) to (a6).
[0071] (a1) Imaging of CNT-resin composite
[0072] The CNT-resin composite was imaged under the following conditions using the following equipment: The CNT-resin composite was sliced into nanometer-scale slices using a focused ion beam (FIB) method or a microtome method.
[0073] Transmission electron microscope (TEM): "JEM2100" manufactured by JEOL (product name)
[0074] Imaging conditions: magnification 50,000-1.2 million times, acceleration voltage 60 kV-200 kV.
[0075] It is to be noted that it has been confirmed that as long as the measurement is performed by the applicant and the measurement is performed on the same sample, there is almost no deviation in the measurement results even if the selected position of the measurement field is changed to calculate the measurement results of the orientation degree described later multiple times.
[0076] (a2) Binarization of the image obtained by the camera
[0077] The image captured in the above (a1) is subjected to binarization processing according to the following steps using the following image processing program.
[0078] Image processing program: Non-destructive paper surface fiber orientation analysis program "FiberOri8single03" (http: / / www.enomae.com / FiberOri / index.htm)
[0079] Processing steps:
[0080] 1. Histogram average brightness correction
[0081] 2. Background removal
[0082] 3. Single Threshold Binarization
[0083] 4. Brightness inversion.
[0084] (a3) Fourier transform of the image obtained by binarization
[0085] The image obtained in (a2) above was subjected to Fourier transformation using the same image processing program as described above (non-destructive paper surface fiber orientation analysis program "FiberOri8single03" (http: / / www.enomae.com / FiberOri / index.htm)).
[0086] (a4) Calculation of orientation angle and orientation strength
[0087] In the Fourier transform image, the positive direction of the X axis is set to 0°, and the average amplitude with respect to the counterclockwise rotation angle (θ°) is calculated.
[0088] A graph showing the relationship between the orientation angle and the orientation strength is prepared from the Fourier transformed image.
[0089] (a5) Determination of half peak width
[0090] Based on the above graph, the full width at half maximum (FWHM: full width at half maximum) was measured.
[0091] (a6) Calculation of orientation
[0092] Based on the above full width at half maximum, the degree of orientation was calculated according to the following formula (1).
[0093] Orientation degree = (180°-full width at half maximum) / 180°…(1)
[0094] The case where the orientation degree is 0 means that there is no orientation at all, and the case where the orientation degree is 1 means that there is complete orientation.
[0095] In addition to the above methods, the degree of orientation of CNTs in a CNT aggregate wire may be evaluated using polarized Raman analysis or small-angle X-ray scattering.
[0096] In the carbon nanotube assembly wire involved in this embodiment, the plurality of carbon nanotubes are oriented with an orientation degree of 0.9 or more and 1.0 or less. This means that in the CNT assembly wire of this embodiment, the orientation of the plurality of CNTs is high. Thus, the CNT assembly wire involved in this embodiment can be extended while maintaining the electrical conductivity and breaking strength characteristics of CNTs.
[0097] When the orientation degree of CNTs in the CNT assembly wire is less than 0.9, the conductivity and the breaking strength tend to decrease. The lower limit of the orientation degree is preferably 0.93, more preferably 0.94, and further preferably 0.95. The upper limit of the orientation degree is preferably 0.99, and more preferably 1. The orientation degree of CNTs in the CNT assembly wire can be set to 0.93 to 0.99, 0.94 to 0.99, 0.95 to 0.99, 0.93 to 1, 0.94 to 1, and 0.95 to 1.
[0098] (Shape of carbon nanotube aggregate line)
[0099] The shape of the carbon nanotube aggregate wire is a filament in which a plurality of carbon nanotubes are aligned and aggregated in their longitudinal direction.
[0100] There is no particular limitation on the length of the carbon nanotube assembly line, and it can be appropriately adjusted according to the application. The length of the CNT assembly line is, for example, preferably 100 μm or more, more preferably 1000 μm or more, and further preferably 10 cm or more. There is no particular limitation on the upper limit of the length of the CNT assembly line, but from the manufacturing point of view, it is preferably 1 m or less. The length of the CNT assembly line can be measured by using a scanning electron microscope, an optical microscope, or visual observation.
[0101] There is no particular limitation on the diameter of the carbon nanotube assembly wire, and it can be adjusted appropriately according to the application. The diameter of the CNT assembly wire is, for example, preferably 0.1 μm or more, and more preferably 1 μm or more. There is no particular limitation on the upper limit of the diameter of the CNT assembly wire, but from a manufacturing point of view, it is preferably 100 μm or less. In this embodiment, the diameter of the CNT assembly wire is smaller than the length of the CNT assembly wire. That is, the length direction of the CNT assembly wire is equivalent to the longitudinal direction.
[0102] In this specification, the diameter of a carbon nanotube assembly line refers to the average outer diameter of a CNT assembly line. The average outer diameter of a CNT assembly line can be obtained by observing a cross section of any two locations of a CNT assembly line using a transmission electron microscope or a scanning electron microscope, measuring the distance between the two most distant points on the outer circumference of the CNT assembly line in the cross section, i.e., the outer diameter, and calculating the average value of the obtained outer diameters.
[0103] (Elements from Catalyst)
[0104] The carbon nanotube assembly wire may contain at least one metal element selected from the group consisting of iron, nickel, cobalt, molybdenum, gold, silver, copper, yttrium, chromium, palladium, platinum and tungsten. The metal element is preferably dispersed in the longitudinal direction of the carbon nanotube assembly wire. Here, the metal element is dispersed in the longitudinal direction of the CNT assembly wire means that the metal element does not exist locally in the longitudinal direction of the CNT assembly wire.
[0105] These metal elements come from the catalyst (ferrocene (Fe (C 5 H 5 ) 2 ), Ni(C 5 H 5 ) 2 ), Cobaltocene (Co(C 5 H 5 ) 2 In the CNT assembly wire, when these metal elements are dispersed in the longitudinal direction of the CNT assembly wire, the metal elements will not affect the conductivity of the CNT, so that the CNT assembly wire can be extended while maintaining the original conductivity.
[0106] The types and contents of metal elements contained in the CNT wire can be confirmed and measured by energy dispersive X-ray spectrometry (EDX). Based on the number of atoms, the total content of metal elements in the CNT wire is preferably 0.1% to 50%, more preferably 1% to 40%, and even more preferably 5% to 20%.
[0107] The dispersion of the metal elements contained in the CNT aggregate wire in the longitudinal direction of the carbon nanotube aggregate wire can be confirmed by EDX or electron energy loss spectrometry (EELS) which can be measured simultaneously with an electron microscope such as SEM or TEM.
[0108] The carbon nanotube assembly wire may contain sulfur. The sulfur element is preferably dispersed in the longitudinal direction of the carbon nanotube assembly wire. Here, the sulfur element is dispersed in the longitudinal direction of the CNT assembly wire, which means that the sulfur element does not exist locally in the longitudinal direction of the CNT assembly wire.
[0109] The sulfur element comes from the auxiliary catalyst (CS 2 ). In the CNT assembly wire, when sulfur is dispersed in the longitudinal direction of the CNT assembly wire, the sulfur element will not affect the conductivity and fracture strength of the CNT, and the CNT assembly wire can be extended while maintaining these properties.
[0110] Whether the CNT assembly wire contains sulfur and the sulfur content in the CNT assembly wire can be confirmed and measured by EDX, thermogravimetric analysis, and X-ray photoelectron spectroscopy. Based on the atomic number, the sulfur content in the CNT assembly wire is preferably 0.1% to 20%, more preferably 1% to 15%, and even more preferably 2% to 10%.
[0111] The dispersion of sulfur contained in the CNT assembly wire in the longitudinal direction of the carbon nanotube assembly wire can be confirmed by using EDX or EELS which can be measured simultaneously with an electron microscope such as SEM or TEM.
[0112] <Resin>
[0113] In the CNT-resin composite, the resin exists between the plurality of CNT aggregate wires, thereby improving the fracture strength of the CNT-resin composite.
[0114] As the resin, any of a thermosetting resin, a photocurable resin, and a thermoplastic resin can be used.
[0115] Examples of thermosetting resins include novolac epoxy resins, phenolic resins, melamine resins, urea resins, polyimides, unsaturated polyester resins, silicone resins, and polyurethanes. Among them, novolac epoxy resins are preferred because they have a benzene skeleton with high affinity for the CNT surface and form a network structure with a high cross-linking density, thereby obtaining a strong composite material.
[0116] As the photocurable resin, for example, an ultraviolet curable resin such as urethane acrylate can be used.
[0117] Examples of thermoplastic resins include polymethyl methacrylate resins, polyethylene, polypropylene, polyvinyl chloride, polystyrene, polyurethane, polyamide, polyacetal, polycarbonate, and polyester. Among them, polymethyl methacrylate resins are preferred because they can be composited without introducing defects into CNTs and have excellent molding processability.
[0118] The type of resin in the CNT-resin composite can be determined by infrared spectroscopy, Raman spectroscopy, and differential scanning calorimetry.
[0119] The CNT-resin composite preferably contains 0.1% by mass or more and less than 100% by mass of the resin, thereby further improving the fracture strength of the carbon nanotube-resin composite.
[0120] The content of the resin in the CNT-resin composite is preferably 0.1% by mass or more and less than 100% by mass, and more preferably 1% by mass or more and 80% by mass or less.
[0121] The content of the resin in the CNT-resin composite can be measured by thermogravimetric analysis.
[0122] (D / G ratio of carbon nanotube-resin composite)
[0123] In the Raman spectrum of the CNT-resin composite, the Raman shift is 1590±20cm -1 The peak intensity G at and Raman shift 1350±20cm -1 The ratio D / G of the peak intensity D at is preferably 0 or more and 0.1 or less.
[0124] The G band refers to the Raman shift of 1590 cm in the Raman spectrum obtained by Raman spectroscopy. -1 The D band refers to the peak derived from CNT observed near the Raman shift of 1350cm in the Raman spectrum obtained by Raman spectroscopy. -1Peaks derived from amorphous carbon, graphite, and defects in CNTs are observed nearby. Therefore, the smaller the value of the D / G ratio, the higher the crystallinity of the carbon nanotubes, and the smaller the amount of amorphous carbon and graphite with defects contained in the carbon nanotubes.
[0125] When the D / G ratio of the CNT-resin composite is less than 0.1, the defects of amorphous carbon and graphite are less and the crystallinity is high. Therefore, the CNT-resin composite can have high tensile strength and high conductivity. When the D / G ratio of the CNT-resin composite exceeds 0.1, the CNT may not have sufficient tensile strength and high conductivity. The D / G ratio is preferably less than 0.1, more preferably less than 0.01. The lower limit of the D / G ratio is not particularly limited, for example, it can be set to more than 0. The D / G ratio of the CNT-resin composite can be set to more than 0 and less than 0.1, more than 0 and less than 0.01.
[0126] In this specification, the D / G ratio of the CNT-resin composite is a value measured by the following method.
[0127] Raman spectroscopic analysis of the CNT-resin composite was performed under the following conditions to obtain a Raman spectrum (hereinafter also referred to as the Raman spectrum of the CNT-resin composite). In the Raman spectrum of the CNT-resin composite, the D / G ratio was calculated from the peak intensity of the G band and the peak intensity of the D band.
[0128] Raman spectroscopy analysis conditions
[0129] Wavelength: 532nm
[0130] Laser power: 17mW
[0131] Exposure time: 1 second
[0132] Average number of times: 3 times
[0133] Objective lens magnification: 50 times
[0134] [Embodiment 2: Method for producing a carbon nanotube-resin composite]
[0135] The CNT-resin composite of the first embodiment can be obtained, for example, by Figure 3 The carbon nanotube-resin composite manufacturing apparatus (hereinafter also referred to as "CNT-resin composite manufacturing apparatus") 500 is shown. The carbon nanotube-resin composite manufacturing apparatus 500 may include: a tubular carbon nanotube growth section (hereinafter also referred to as "CNT growth section") 21, a carbon-containing gas is introduced from one end ( Figure 3The gas supply unit 22 supplies the catalyst particles P to the CNT growth unit 21, and the catalyst supply unit 23 is arranged on the other end side of the CNT growth unit 21 ( Figure 3 The carbon nanotube assembly section 24 (hereinafter also referred to as the CNT assembly section) is formed on the left side of the CNT growth section 21, and the plurality of carbon nanotubes obtained in the CNT growth section 21 are oriented and assembled along the direction of the flow of the carbon-containing gas, and the carbon nanotube-resin composite forming section 50 is formed on the downstream side of the carbon nanotube assembly section 24. The carbon nanotube-resin composite forming section 50 may include: a liquid attachment device 51 that causes a volatile liquid 53 to adhere to the CNT assembly line obtained in the CNT assembly section 24; and a winding device 52 that applies tension to the carbon nanotube assembly line and orients and bundles the plurality of carbon nanotube assembly lines along the longitudinal direction thereof after the plurality of carbon nanotube assembly lines pass through a shrinking device 55 (reel) and is wound up.
[0136] The method for manufacturing a CNT-resin composite may include: a growth process of growing a plurality of carbon nanotubes by supplying a carbon-containing gas to a plurality of catalyst particles in a floating state so that one or more carbon nanotubes grow from each of the plurality of catalyst particles; an elongation process of elongating the plurality of carbon nanotubes by applying a tensile force to the plurality of carbon nanotubes in a floating state; an aggregation process of orienting and aggregating a plurality of carbon nanotubes in a floating state along the flow direction of the carbon-containing gas to obtain a plurality of carbon nanotube aggregate lines; an attachment process of orienting and bundling a plurality of carbon nanotube aggregate lines along their longitudinal direction while attaching a volatile liquid containing resin to the carbon nanotube aggregate lines; and an evaporation process of evaporating the volatile liquid attached to the plurality of carbon nanotube aggregate lines to obtain a carbon nanotube-resin composite.
[0137] <Growth Process>
[0138] First, a carbon-containing gas is supplied to a plurality of catalyst particles in a floating state, so that one or a plurality of carbon nanotubes are grown from each of the plurality of catalyst particles.
[0139] The growth process is performed inside the CNT growth section 21. The growth process is preferably performed under a temperature condition of 800°C to 1200°C. When the temperature is less than 800°C, the growth rate of CNTs tends to slow down. On the other hand, when the temperature exceeds 1200°C, the content of impurity carbon tends to increase. The temperature condition of the growth process is more preferably 900°C to 1150°C, and further preferably 950°C to 1050°C.
[0140] The catalyst 27 disposed inside the catalyst supply unit 23 is disintegrated into catalyst particles P by the wind pressure of the carbon-containing gas supplied from the gas supply unit 22 to the catalyst supply unit 23 and the CNT growth unit 21 , and the catalyst particles P are supplied to the CNT growth unit 21 .
[0141] For example, iron, nickel, cobalt, molybdenum, gold, silver, copper, palladium, and platinum can be used as the catalyst particles P. Among them, iron is preferably used from the viewpoint of mass production of long CNTs.
[0142] The carbon-containing gas is supplied from the gas supply unit 22 to the CNT growth unit 21 via the catalyst supply unit 23. As the carbon-containing gas, a reducing gas such as a hydrocarbon gas can be used. As such a carbon-containing gas, for example, a mixed gas of methane and argon, a mixed gas of ethylene and argon, a mixed gas of ethanol and argon, etc. can be used. The carbon-containing gas preferably contains carbon disulfide (CS2) as an auxiliary catalyst. 2 ).
[0143] The lower limit of the average flow rate of the carbon-containing gas supplied from the gas supply section 22 in the CNT growth section may be 0.05 cm / sec, preferably 0.10 cm / sec, and more preferably 0.20 cm / sec. On the other hand, the upper limit of the average flow rate in the CNT growth section 21 is preferably 10.0 cm / sec, and more preferably 5.0 cm / sec. In the case where the average flow rate of the carbon-containing gas in the CNT growth section 21 is less than the above lower limit, the carbon raw material gas supplied to the catalyst particles P is insufficient, and the growth of the carbon nanotubes formed between the catalyst particles P tends to stagnate. On the contrary, in the case where the average flow rate of the carbon-containing gas in the CNT growth section 21 exceeds the above upper limit, the growth of the carbon nanotubes stops due to the peeling of the carbon nanotubes from the catalyst particles P, and the formation of the carbon nanotubes tends to be hindered.
[0144] The lower limit of the Reynolds number of the flow of the carbon-containing gas supplied from the gas supply unit 22 in the CNT growth unit 21 is preferably 0.01, and more preferably 0.05. On the other hand, the upper limit of the above-mentioned Reynolds number is 1000, preferably 100, and more preferably 10. When the above-mentioned Reynolds number is less than the above-mentioned lower limit, the design of the device is excessively restricted, so that the carbon nanotube-resin composite production device 20 may become unnecessarily expensive, or the production efficiency of carbon nanotubes tends to be unnecessarily reduced. In the case where the above-mentioned Reynolds number exceeds the above-mentioned upper limit, the flow of the carbon-containing gas becomes turbulent, and the generation of carbon nanotubes between the catalyst particles P tends to be hindered.
[0145] The length of the CNT obtained by the growth process is preferably 0.1 μm to 20 μm. When the length of the CNT obtained by the growth process is less than 0.1 μm, adjacent CNTs are not oriented in the longitudinal direction but are entangled together, tending to form secondary particles. On the other hand, when the length of the CNT exceeds 20 μm, the time until the elongation process is performed becomes longer, and the manufacturing efficiency of the carbon nanotubes tends to be unnecessarily reduced. The length of the CNT obtained by the growth process is more preferably 0.5 μm to 15 μm, and more preferably 1 μm to 10 μm. The length of the CNT can be measured by observation using a scanning electron microscope.
[0146] <Stretching process>
[0147] Next, a tensile force is applied to the plurality of carbon nanotubes in a floating state produced in the CNT growth section, thereby extending the plurality of carbon nanotubes.
[0148] The elongation step is performed inside the CNT growing section 21 and the CNT aggregate section 24, or inside the CNT aggregate section 24. When the elongation step is performed inside the CNT growing section 21, it is preferably performed downstream of the carbon-containing gas in the CNT growing section 21, i.e., on the CNT aggregate section side.
[0149] Preferably, the tensile force is applied to the plurality of carbon nanotubes by changing the flow rate of the carbon-containing gas. For example, by making the average flow rate of the downstream side of the carbon-containing gas greater than the average flow rate of the upstream side of the carbon-containing gas, a tensile force in the downstream direction can be applied to the CNTs. By applying the tensile force to the ends of the carbon nanotubes, the carbon nanotubes extending from the catalyst particles P are stretched, thereby being elongated in the longitudinal direction while being plastically deformed and reduced in diameter.
[0150] In the elongation process, it is preferred to orient the plurality of carbon nanotubes along the flow direction of the carbon-containing gas and elongate them. It is believed that the carbon nanotubes are less likely to bend, and a straight carbon nanotube whose tube portion T is composed only of carbon in a six-membered ring can be obtained. The carbon nanotube composed only of carbon in a six-membered ring is less likely to deteriorate, and thus the quality can be maintained.
[0151] The average flow velocity of the downstream side of the carbon-containing gas is preferably 0.051 cm / sec to 10.001 cm / sec, and more preferably 0.201 cm / sec to 5.001 cm / sec. When the average flow velocity of the downstream side of the carbon-containing gas is less than 0.051 cm / sec, the elongation rate of the carbon nanotubes tends not to be sufficiently fast compared to the growth rate. On the other hand, when the average flow velocity of the downstream side of the carbon-containing gas exceeds 10.001 cm / sec, the growth of the carbon nanotubes stops due to the peeling of the carbon nanotubes from the catalyst particles P, and the formation of the carbon nanotubes tends to be hindered.
[0152] The average flow velocity of the upstream side of the carbon-containing gas is preferably 0.050 cm / sec to 10.000 cm / sec, more preferably 0.200 cm / sec to 5.000 cm / sec. When the average flow velocity of the upstream side of the carbon-containing gas is less than 0.050 cm / sec, the growth of the carbon nanotubes formed between the catalyst particles P tends to stagnate due to insufficient wind pressure. On the other hand, when the average flow velocity of the upstream side of the carbon-containing gas exceeds 10.000 cm / sec, the carbon nanotubes are peeled off from the catalyst particles P, so that the growth of the carbon nanotubes stops, and the formation of the carbon nanotubes tends to be hindered.
[0153] As a method for making the average flow velocity of the downstream side of the carbon-containing gas greater than the average flow velocity of the upstream side of the carbon-containing gas, for example, the cross-sectional area of the hollow portion through which the carbon-containing gas passes on the downstream side of the carbon-containing gas is smaller than that on the upstream side of the carbon-containing gas. More specifically, the cross-sectional area of the hollow portion through which the carbon-containing gas passes in the CNT gathering part (equivalent to the downstream side) is smaller than that in the CNT growth part (equivalent to the upstream side). As a result, an acceleration field is generated near the region where the cross-sectional area of the hollow portion is reduced, thereby increasing the flow velocity of the carbon-containing gas.
[0154] During the period when the carbon nanotubes are stretched by the tensile force, carbon nanotubes with the original diameter will also grow on the catalyst particles P. Figure 2 As shown, the carbon nanotube produced through the elongation step may include a tubular tube portion T and a conical tapered portion C whose diameter is continuously expanded from the end of the tube portion.
[0155] That is, in the elongation process, the carbon nanotubes formed by the vapor phase growth method are stretched by the tensile force while they are formed, so that a part of the hexagonal units of the carbon nanotubes are replaced by pentagonal units, thereby forming a conical cone portion, and by replacing them with hexagonal units again, a carbon nanotube with a small diameter, i.e., a tube portion, is formed.
[0156] In the elongation step, the carbon nanotubes grown on the catalyst particles P are grown while being stretched by a tensile force, so that the tube portion can be formed at a much higher speed than the growth speed of the carbon nanotubes on the catalyst particles P. Thus, a longer carbon nanotube can be formed in a shorter time. Therefore, even if the time for which the conditions for continuously growing the carbon nanotubes on the catalyst particles P can be maintained is short, a sufficiently long carbon nanotube can be formed.
[0157] It is believed that in the elongation step, the tensile force applied to the carbon nanotubes on the catalyst particles P promotes the acquisition of carbon atoms at the growth points of the carbon nanotubes, thereby increasing the growth rate of the carbon nanotubes and the increase rate of the length of the obtained carbon nanotubes.
[0158] It is considered that in the elongation step, by applying a tensile force to the carbon nanotubes on the catalyst particles P, the carbon nanotubes are less likely to bend, and a straight carbon nanotube consisting of a cylindrical body composed of a sheet of carbon having a six-membered ring can be obtained. The carbon nanotubes composed of carbon having a six-membered ring are less likely to deteriorate, and thus the quality can be maintained.
[0159] The length of the CNT obtained by the elongation step is preferably 10 μm or more, more preferably 100 μm or more. In particular, when the length of the carbon nanotube is 100 μm or more, it is preferred from the viewpoint of making a CNT assembly line. There is no particular upper limit on the length of the carbon nanotube, but from the viewpoint of manufacturing, it is preferably 600 mm or less. The length of the CNT can be measured by observation using a scanning electron microscope.
[0160] <Assembly process>
[0161] Next, the floating carbon nanotubes are aligned and aggregated along the flow direction of the carbon-containing gas, thereby obtaining a carbon nanotube aggregate wire. The aggregation step is performed inside the CNT aggregate portion 24 .
[0162] As a method for orienting and gathering a plurality of floating CNTs along the direction of the flow of the carbon-containing gas, a method of bringing a plurality of carbon nanotubes close to each other in an oriented state can be cited. For example, a method can be cited in which the cross-sectional area of the hollow portion through which the carbon-containing gas of the CNT gathering portion passes is smaller than the cross-sectional area of the hollow portion through which the carbon-containing gas of the CNT growth portion and the CNT extension portion passes. More specifically, a method can be cited in which the CNT gathering portion is configured as a honeycomb structure so that the longitudinal direction of the through-holes of the honeycomb structure becomes along the direction of the flow of the carbon-containing gas.
[0163] In this manual, if Figure 3 As shown in the honeycomb structure 29, the honeycomb structure is a porous body having a plurality of thin cylindrical through holes.
[0164] When the CNT aggregate portion is composed of a honeycomb structure, the cross-sectional area of one through hole is preferably 0.05 mm 2 Above 100mm 2 Less than, more preferably 0.1 mm 2 Above 50mm 2 Below, more preferably 0.5 mm 2 Above 10mm 2 When the cross-sectional area of a through hole is less than 0.05mm 2 On the other hand, when the cross-sectional area of a through hole exceeds 100 mm 2When the CNTs are not close enough to each other, they tend not to aggregate.
[0165] In the case where the CNT collection portion is composed of a honeycomb structure, the length along the direction of the through-holes of the honeycomb structure (longitudinal direction) is preferably 1 mm to 1 m, more preferably 10 mm to 50 cm, and further preferably 15 mm to 10 cm. When the length along the direction of the through-holes of the honeycomb structure is less than 1 mm, the CNTs floating in the gas phase cannot be fully accelerated, tending to inhibit the growth-promoting effect. On the other hand, when the length along the direction of the through-holes of the honeycomb structure exceeds 1 m, the amount of CNT deposition at the inner wall of the through-hole increases, so it tends to be difficult to recover the CNTs.
[0166] The average flow rate of the carbon-containing gas in the CNT collection part is preferably 0.05 cm / second to 10 cm / second, and more preferably 0.2 cm / second to 5 cm / second. When the average flow rate of the carbon-containing gas is less than 0.05 cm / second, a film-like unoriented CNT tends to be obtained. On the other hand, when the average flow rate of the carbon-containing gas exceeds 10 cm / second, the carbon-containing gas that reaches the CNT collection part without reacting will undergo an incomplete decomposition reaction, and tar tends to adhere.
[0167] In the above description, the case where the collection process is performed after the elongation process is described, but the elongation process and the collection process may be performed simultaneously. In addition, the elongation process and the collection process may be performed simultaneously after the elongation process is performed. For example, when a honeycomb structure is used as a CNT collection part, the elongation and collection of CNTs may be performed simultaneously in the through-holes of the honeycomb structure.
[0168] According to the above manufacturing method, by continuously supplying the carbon-containing gas to the catalyst supply unit, the CNT growth unit and the CNT assembly unit, the CNT assembly wire can be continuously manufactured without length limitation. The length of the CNT assembly wire can be appropriately adjusted by adjusting the flow rate and supply time of the carbon-containing gas.
[0169] The length of the CNT assembly wire obtained by the assembly step is preferably 100 μm or more, more preferably 1000 μm or more, and further preferably 10000 μm or more. There is no particular upper limit on the length of the CNT assembly wire, but from a manufacturing point of view, it is preferably 1 m or less. The length of the CNT assembly wire can be measured by using an optical microscope or visual observation.
[0170] <Attachment process>
[0171] Next, while the plurality of carbon nanotube aggregate wires obtained in the aggregation step are oriented and bundled in the longitudinal direction thereof, a volatile liquid containing a resin is attached to the carbon nanotube aggregate wires.
[0172] As a method of orienting and bundling a plurality of CNT aggregated wires in the longitudinal direction thereof, there is a method in which, after passing through a shrinking device 55 , the plurality of CNT aggregated wires are wound up by a winding device 52 while applying tension.
[0173] As a method of attaching the volatile liquid containing the resin to the carbon nanotube assembly wire, for example, the volatile liquid is atomized to form vapor 55 and the vapor 55 is sprayed onto the carbon nanotube assembly wire.
[0174] As the volatile liquid, for example, methanol, ethanol, isopropanol, acetone, methyl ethyl ketone, xylene, anisole, toluene, cresol, pyrrolidone, carbitol, carbitol acetate, water, epoxy monomer, acrylic monomer can be used. Ethanol, acetone, toluene, xylene, anisole can be used.
[0175] exist Figure 3 In the embodiment, the attachment process is performed before the plurality of carbon nanotube wires are oriented and bundled along their longitudinal direction (i.e., on the upstream side of the shrinker 55), but is not limited thereto. The attachment process may also be performed after the plurality of carbon nanotube wires are oriented and bundled along their longitudinal direction (i.e., on the downstream side of the shrinker 55).
[0176] The volatile liquid contains a resin. As the resin, the resin described in Embodiment 1 can be used.
[0177] The content of the resin in the volatile liquid is preferably from 0.1% by mass to 20% by mass, and more preferably from 1% by mass to 10% by mass.
[0178] <Evaporation process>
[0179] Next, the volatile liquid attached to the plurality of carbon nanotube wire groups in the attachment step is evaporated, thereby obtaining the carbon nanotube-resin composite 3 .
[0180] The evaporation step can be performed by natural drying.
[0181] [Note 1]
[0182] In the carbon nanotube-resin composite of the present disclosure, the length of the carbon nanotube is preferably 10 μm to 600 mm.
[0183] The length of the carbon nanotubes is preferably not less than 100 μm and not more than 600 mm.
[0184] [Note 2]
[0185] In the carbon nanotube-resin composite disclosed herein, the diameter of the carbon nanotube is preferably 0.6 nm or more and 20 nm or less.
[0186] The carbon nanotube preferably has a diameter of 1 nm to 10 nm.
[0187] The carbon nanotube preferably has a diameter of 1 nm to 2 nm.
[0188] [Note 3]
[0189] In the CNT aggregate wire of the carbon nanotube-resin composite of the present disclosure, the carbon nanotubes are preferably oriented at an orientation degree of 0.93 or more and 0.99 or less.
[0190] The degree of orientation is preferably 0.94 or more and 0.99 or less.
[0191] The degree of orientation is preferably 0.95 or more and 0.99 or less.
[0192] The above-mentioned orientation degree is preferably 0.93 or more and 1 or less.
[0193] The above-mentioned orientation degree is preferably 0.94 or more and 1 or less.
[0194] The above-mentioned orientation degree is preferably 0.95 or more and 1 or less.
[0195] [Note 4]
[0196] In the CNT assembly wire of the carbon nanotube-resin composite disclosed herein, the carbon nanotube assembly wire contains sulfur, and the content of sulfur in the carbon nanotube assembly wire is preferably 0.1% to 20% based on the number of atoms.
[0197] The content of sulfur in the carbon nanotube assembly wire is preferably 1% to 15%.
[0198] The content of sulfur in the carbon nanotube assembly wire is preferably 2% to 10%.
[0199] [Note 5]
[0200] In the CNT aggregate wire of the carbon nanotube-resin composite of the present disclosure, the content of the resin is preferably 1% by mass or more and 80% by mass or less.
[0201] [Note 6]
[0202] In the Raman spectrum of the carbon nanotube-resin composite disclosed in the present invention, the Raman shift is 1590±20cm -1 The peak intensity G at and Raman shift 1350±20cm -1 The ratio D / G of the peak intensity D at is preferably 0 to 0.01.
[0203] Example
[0204] The present embodiment will be further specifically described based on examples, but the present embodiment is not limited to these examples.
[0205] [Sample 1 and Sample 2]
[0206] <Preparation of Carbon Nanotube-Resin Composite Manufacturing Apparatus>
[0207] Prepared with Figure 3 A carbon nanotube-resin composite manufacturing apparatus having the same structure as the carbon nanotube-resin composite manufacturing apparatus shown in the figure. Specifically, the carbon nanotube growth section 21 and the carbon nanotube collection section 24 are arranged in an electric furnace 28. The CNT growth section is composed of a quartz tube with an inner diameter of 20 mm and a length of 800 mm. As the carbon nanotube collection section 24, a honeycomb structure composed of ceramics is arranged in the quartz tube continuous with the CNT growth section. The honeycomb structure has about 200 through holes per inch, and the cross-sectional area of one through hole is 0.8 mm 2 .
[0208] The catalyst supply unit 23 is arranged on the opposite side of the CNT growth unit 21 to the side continuous with the CNT aggregation unit 24. The catalyst supply unit 23 is composed of a quartz tube with an inner diameter of 20 mm and a length of 200 mm, and is arranged continuously with the CNT growth unit. Ferrocene as a catalyst is arranged on a catalyst holder 26 in the catalyst supply unit 23. The catalyst supply unit 23 is heated by a heater 25.
[0209] The gas supply unit 22 is disposed on the opposite side of the catalyst supply unit 23 to the side connected to the CNT growing unit 21 .
[0210] On the downstream side of the CNT assembly section 24, there are arranged: a liquid attachment device 51 for attaching a volatile liquid 53 containing a resin to the CNT assembly line obtained in the CNT assembly section 24; and a winding device 52 for orienting and bundling a plurality of carbon nanotube assembly lines in the longitudinal direction while applying tension to the carbon nanotube assembly line. The liquid attachment device is arranged on the upstream side of the shrinking device 55.
[0211] <Production of Carbon Nanotube-Resin Composite>
[0212] In Sample 1, first, argon gas having an argon concentration of 100 volume % was supplied from the gas supply unit to the CNT growth unit at a flow rate of 1000 cc / min (flow rate of 3.4 cm / sec) for 50 minutes, and the temperature in the electric furnace was raised to 1000° C. Then, in addition to argon gas, methane gas was supplied at a flow rate of 50 cc / min (flow rate of 0.17 cm / sec) and carbon disulfide (CS 2) gas was supplied at a flow rate of 1 cc / min (flow velocity 0.003 cm / sec) for 120 minutes. The total flow rate of the mixed gas containing argon gas, methane gas, and carbon disulfide (carbon-containing gas) was 3.6 cm / sec.
[0213] By supplying the argon gas, methane gas, and carbon disulfide gas, the catalyst is disintegrated and catalyst particles are released into the CNT growth section, and then CNTs grow in the CNT growth section.
[0214] Then, the CNTs are assembled while being stretched in the CNT assembly part, thereby obtaining a CNT assembly wire. While the obtained plurality of CNT assembly wires are wound up by a winding device, a volatile liquid is attached to the CNT assembly wire, and then the volatile liquid is evaporated, thereby obtaining a CNT-resin composite of sample 1. It should be noted that the volatile liquid used in sample 1 contains 1% by mass of a novolac resin. Sample 1 is equivalent to an example.
[0215] In Sample 2, a CNT-resin composite was produced under the same conditions as Sample 1, except that the volatile liquid contained 4 mass % of polymethyl methacrylate resin instead of the novolac resin. Sample 2 corresponds to Example.
[0216] [Sample 3]
[0217] As Sample 3, a CNT aggregated wire bundle was prepared by winding and bundling a plurality of CNT aggregated wires obtained in the CNT aggregate section of the apparatus 1 using a winding device. This CNT aggregated wire bundle does not contain a resin. Sample 3 corresponds to a comparative example.
[0218] <Measurement of Carbon Nanotube Aggregate Line>
[0219] (Orientation)
[0220] The CNT orientation degree was measured for the CNT-resin composites of Samples 1 and 2 and the CNT aggregate line bundle of Sample 3. The method for calculating the orientation degree is the same as that described in Embodiment 1, and therefore the description thereof will not be repeated.
[0221] The orientation degrees of samples 1 to 3 are all 0.9 or more and 1 or less.
[0222] (D / G ratio)
[0223] The D / G ratio was measured for the CNT-resin composites of Samples 1 and 2 and the CNT aggregate wire bundle of Sample 3. The method for measuring the D / G ratio is the same as that described in Embodiment 1, and therefore the description thereof will not be repeated.
[0224] The D / G ratios of Samples 1 to 3 were all 0 or more and 0.1 or less.
[0225] (resin content)
[0226] The resin contents of the CNT-resin composites of Samples 1 and 2 and the CNT aggregate wire bundle of Sample 3 were measured.
[0227] The resin content of sample 1 was 10% by mass. The resin content of sample 2 was 20% by mass. The resin content of sample 3 was 0% by mass.
[0228] (Breaking Strength)
[0229] Stress-strain curves were measured for the CNT-resin composites of Samples 1 and 2 and the CNT wire bundle of Sample 3. The stress-strain curve measurement method is as follows.
[0230] Prepare a CNT assembly wire of about 3 cm in length and fix its two ends to the tensile fixture plate with adhesive. Use a load cell (measurement instrument: "ZTS-5N" manufactured by Imada Co., Ltd.) to measure the tensile stress of the CNT assembly wire of 1 cm in length not fixed by the adhesive until it breaks. The obtained stress-strain curve is as follows: Figure 4 In the stress-strain curve, the greater the stress (vertical axis), the greater the fracture strength, and the greater the strain (horizontal axis), the greater the elongation.
[0231] It was confirmed that the breaking strength of sample 1 was increased by more than 15 times compared with sample 3.
[0232] It was confirmed that the breaking strength of sample 2 was increased by about 10 times compared with sample 3.
[0233] As mentioned above, although the embodiment and the example of the present disclosure have been described, it is originally intended that the configurations of the above-mentioned embodiments and the examples be appropriately combined or variously modified.
[0234] The embodiments and examples disclosed herein are illustrative in all aspects and are not restrictive. The scope of the present invention is not limited to the embodiments and examples described above, but is indicated by the scope of the claims, and is intended to include all changes within the meaning and scope equivalent to the claims.
[0235] Explanation of symbols
[0236] 1, 1a, 1b, 1c, 1d carbon nanotube assembly line 2 carbon nanotube 3 carbon nanotube-resin composite 21 CNT growth unit 22 gas supply unit 23 catalyst supply unit 24, 24a carbon nanotube assembly unit 25 heater 26 catalyst holder 27 catalyst 28 electric furnace 29 honeycomb structure 50 carbon nanotube-resin composite forming unit 51 liquid attachment device 52 winding device 53 volatile liquid 54 steam 55 shrinker 500 carbon nanotube-resin composite manufacturing device T tube part C cone part P catalyst particle
Claims
1. A carbon nanotube-resin composite comprising: A carbon nanotube assembly wire including a plurality of carbon nanotubes, and a resin, In the carbon nanotube assembly wire, the carbon nanotubes are oriented with an orientation degree of 0.9 or more and 1 or less, The carbon nanotube-resin composite includes a plurality of carbon nanotube wire assemblies, and the plurality of carbon nanotube wire assemblies are oriented and bundled along a longitudinal direction thereof.
2. The carbon nanotube-resin composite according to claim 1, wherein The carbon nanotube-resin composite contains 0.1 mass % or more and less than 100 mass % of the resin.
3. The carbon nanotube-resin composite according to claim 1 or claim 2, wherein: The resin is a thermosetting resin or a light-curing resin.
4. The carbon nanotube-resin composite according to claim 3, wherein The thermosetting resin is a novolac type epoxy resin.
5. The carbon nanotube-resin composite according to claim 1 or claim 2, wherein: The resin is a thermoplastic resin.
6. The carbon nanotube-resin composite according to claim 5, wherein The thermoplastic resin is polymethyl methacrylate resin.
7. The carbon nanotube-resin composite according to claim 1 or claim 2, wherein: In the Raman spectrum of the carbon nanotube-resin composite, the Raman shift is 1590±20cm -1 The peak intensity G at and Raman shift 1350±20cm -1 The ratio D / G of the peak intensity D at is greater than or equal to 0 and less than or equal to 0.
1.
8. A method for producing a carbon nanotube-resin composite, which is the method for producing a carbon nanotube-resin composite according to any one of claims 1 to 7, comprising: a growing step of growing a plurality of carbon nanotubes by supplying a carbon-containing gas to a plurality of catalyst particles in a floating state so that one or more carbon nanotubes grow from each of the plurality of catalyst particles; an elongation step of applying a tensile force to the plurality of carbon nanotubes in a floating state so as to elongate the plurality of carbon nanotubes; A step of aligning and aggregating the plurality of carbon nanotubes in a floating state along a flow direction of the carbon-containing gas to obtain a plurality of carbon nanotube aggregate lines; a step of attaching a volatile liquid containing a resin to the plurality of carbon nanotube assembly wires while aligning and bundling the plurality of carbon nanotube assembly wires in the longitudinal direction thereof; and The evaporation step is to obtain a carbon nanotube-resin composite by evaporating the volatile liquid attached to the plurality of carbon nanotube aggregate wires.
Citation Information
Patent Citations
Method for manufacturing carbon nano-structure
JP2005330175A
Carbon materials comprising carbon nanotubes and methods of making carbon nanotubes
CN103298738A
Carbon nanotube composite material
CN103842290A
Aligned single-walled carbon nanotube assembly, bulk aligned single-walled carbon nanotube assembly, powder-like aligned single-walled carbon nanotube assembly, and method for producing same
CN104192818A
Conductive body, distortion sensor and conductive body manufacturing method