Inorganic composition products and crystallized glass

By reasonably preparing the components in the α-quartzite-based inorganic composition and forming a compressive stress layer, the problem of insufficient surface compression stress value in the prior art in the harsh environment is solved, and high strength and crack resistance are achieved Improved, suitable for protective components for smart phones and other devices.

CN114349351BActive Publication Date: 2024-11-26OHARA INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202210065741.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2019-03-06
Filing Date
2020-03-05
Publication Date
2024-11-26
Estimated Expiration
2040-03-05

AI Technical Summary

Technical Problem

The prior art has failed to effectively explore the surface compression stress values ​​of crystallized glass used in harsh environments, especially in protective components for devices such as smart phones or desktop PCs, which are difficult to meet the demand for higher hardness.

Method used

By reasonably preparing SiO2, Li2O, Al2O3, ZrO2 and other components in α-cune stone inorganic composition products, a compression stress layer is formed to ensure that the compression stress value of the surface reaches more than 600MPa, and combining chemical strengthening and heat treatment technology to form high-strength crystals Glass.

Benefits of technology

It realizes high-strength inorganic materials used in harsh environments, and is suitable for protective components of smart phones, desktop PCs and other equipment, improving mechanical strength and crack resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003480018230000101
    Figure BDA0003480018230000101
  • Figure BDA0003480018230000111
    Figure BDA0003480018230000111
  • Figure BDA0003480018230000121
    Figure BDA0003480018230000121
Patent Text Reader

Abstract

An inorganic composition product, containing one or more selected from α-cristobalite and α-cristobalite solid solution as the main crystalline phase, in which, in terms of mass % converted to oxides, the content of SiO2 component is 50.0% to 75.0%, the content of Li2O component is 3.0% to 10.0%, the content of Al2O3 component is 5.0% or more and less than 15.0%, the total content of Al2O3 component and ZrO2 component is 10.0% or more, and the surface compressive stress value is 600MPa or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an inorganic composition product with a hard surface and crystallized glass. Background Art

[0002] Various inorganic materials are expected to be used as cover glass or frames to protect the displays of portable electronic devices such as smartphones or desktop PCs, or as protective parts to protect the lenses of vehicle-mounted optical devices, interior bezels or main control panels, touch panel raw materials, smart locks, etc. In addition, these devices are required to be used in harsher environments than those required for hard disk substrates, and there is a growing demand for inorganic materials with higher hardness.

[0003] As a product for improving the strength of glass, there is crystallized glass. Crystallized glass is a glass with crystals precipitated inside, and is known to have superior mechanical strength compared to amorphous glass.

[0004] On the other hand, chemical strengthening is known as a method for improving glass strength. The basic components present in the glass surface layer are exchanged with basic components with larger ion radius than the basic components to form a compressive stress layer on the surface, thereby suppressing the development of cracks and improving mechanical strength. To this end, a sufficiently high compressive stress value must be obtained.

[0005] Patent Document 1 discloses an inorganic composition product for information recording media that can be chemically strengthened. The α-cristobalite-based inorganic composition product disclosed in Patent Document 1 can be chemically strengthened and can be used as a high-strength material substrate. However, for crystallized glass for information recording media represented by hard disk substrates, it is not envisioned to be used in harsh environments, and the surface compressive stress value accompanying chemical strengthening has not yet been studied.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 2008-254984 Summary of the invention

[0009] The object of the present invention is to provide an inorganic composition product and crystallized glass with high surface hardness.

[0010] The present invention provides the following contents.

[0011] (Method 1)

[0012] An inorganic composition product, containing one or more selected from α-cristobalite and α-cristobalite solid solution as a main crystalline phase,

[0013] Calculated in mass % of oxide conversion:

[0014] The content of SiO2 component is 50.0% to 75.0%,

[0015] The content of Li2O component is 3.0% to 10.0%,

[0016] The content of Al2O3 component is 5.0% or more and less than 15.0%,

[0017] The total content of Al2O3 and ZrO2 is 10.0% or more.

[0018] The surface compressive stress value is 600 MPa or more.

[0019] (Method 2)

[0020] The inorganic composition product as described in embodiment 1,

[0021] Calculated in mass % of oxide conversion:

[0022] The content of ZrO2 is greater than 0% and less than 10.0%,

[0023] The content of K2O component is 0% to 10.0%,

[0024] The content of P2O5 component is 0% to 10.0%.

[0025] (Method 3)

[0026] The inorganic composition product as described in method 1 or method 2,

[0027] Calculated in mass % of oxide conversion:

[0028] The content of Na2O component is 0% to 10.0%,

[0029] The content of MgO component is 0% to 10.0%,

[0030] The content of CaO component is 0% to 10.0%,

[0031] The content of SrO component is 0% to 10.0%,

[0032] The content of BaO component is 0% to 10.0%,

[0033] The content of ZnO component is 0% to 10.0%,

[0034] The content of Sb2O3 component is 0% to 3.0%.

[0035] (Method 4)

[0036] The inorganic composition product as described in any one of the embodiments 1 to 3, wherein the content of Nb2O5 component is 0% to 10.0% in terms of mass % of oxide conversion,

[0037] The content of Ta2O5 component is 0% to 10.0%,

[0038] The content of the TiO2 component is 0% or more and less than 7.0%.

[0039] (Method 5)

[0040] A crystallized glass containing one or more selected from α-cristobalite and α-cristobalite solid solution as a main crystalline phase, in terms of mass % converted to oxides:

[0041] The content of SiO2 component is 50.0% to 75.0%,

[0042] The content of Li2O component is 3.0% to 10.0%,

[0043] The content of Al2O3 component is 5.0% or more and less than 15.0%,

[0044] The content of ZrO2 is greater than 0% and less than 10.0%,

[0045] The total content of Al2O3 and ZrO2 components is 10.0% or more.

[0046] (Method 6)

[0047] The crystallized glass according to embodiment 5,

[0048] Calculated in mass % of oxide conversion:

[0049] The content of K2O component is 0% to 5.0%,

[0050] The content of P2O5 component is 0% to 10.0%.

[0051] (Method 7)

[0052] The crystallized glass according to Embodiment 5 or Embodiment 6,

[0053] Calculated in mass % of oxide conversion:

[0054] The content of Na2O component is 0% to 4.0%,

[0055] The content of MgO component is 0% to 4.0%,

[0056] The content of CaO component is 0% to 4.0%,

[0057] The content of SrO component is 0% to 4.0%,

[0058] The content of BaO component is 0% to 5.0%,

[0059] The content of ZnO component is 0% to 10.0%,

[0060] The content of Sb2O3 component is 0% to 3.0%.

[0061] (Method 8)

[0062] The crystallized glass according to any one of Modes 5 to 7,

[0063] Calculated in mass % of oxide conversion:

[0064] The content of Nb2O5 component is 0% to 5.0%,

[0065] The content of Ta2O5 component is 0% to 6.0%,

[0066] The content of the TiO2 component is 0% or more and less than 1.0%.

[0067] According to the present invention, an inorganic composition product and a crystallized glass having high surface hardness can be provided.

[0068] The inorganic composition product and crystallized glass of the present invention can be used as a high-strength inorganic material for protective parts of equipment. It can be used as a cover glass or frame of a smart phone, a component of a portable electronic device such as a desktop PC or a wearable terminal, or as a protective guard or a head-up display substrate used in a conveying body such as a vehicle or an airplane. In addition, it can be used in other electronic devices or mechanical appliances, building components, solar panel components, projector components, glasses or clock cover glass (windproof), etc. DETAILED DESCRIPTION

[0069] Hereinafter, the embodiments and examples of the inorganic composition product of the present invention will be described in detail, but the present invention is not limited to the following embodiments and examples, and can be implemented with appropriate changes within the scope of the purpose of the present invention.

[0070] The inorganic composition product of the present invention contains one or more selected from α-cristobalite and α-cristobalite solid solution as the main crystalline phase.

[0071] Calculated in mass % of oxide conversion:

[0072] The content of SiO2 component is 50.0% to 75.0%,

[0073] The content of Li2O component is 3.0% to 10.0%,

[0074] The content of Al2O3 component is 5.0% or more and less than 15.0%,

[0075] The total content of Al2O3 and ZrO2 is 10.0% or more.

[0076] The surface compressive stress value is 600 MPa or more.

[0077] By having this main crystalline phase, composition and compressive stress value, a hard inorganic composition product can be obtained.

[0078] The so-called "inorganic composition product" in the present invention is composed of inorganic composition materials such as glass, crystallized glass, ceramics, or their composite materials. The product of the present invention, for example, is a product formed into a desired shape by processing these inorganic materials or synthesizing based on chemical reactions. In addition, it also includes a compressed powder obtained by crushing and pressurizing the inorganic material or a sintered body obtained by sintering the compressed powder. The shape, smoothness, curvature, size, etc. of the product obtained herein are not limited. For example, it can be a plate-like substrate, a molded body with curvature, a three-dimensional structure with a complex shape, etc.

[0079] The crystallized glass of the present invention contains one or more selected from α-cristobalite and α-cristobalite solid solution as a main crystal phase.

[0080] In terms of mass % converted to oxides,

[0081] The content of SiO2 component is 50.0% to 75.0%,

[0082] The content of Li2O component is 3.0% to 10.0%,

[0083] The content of Al2O3 component is 5.0% or more and less than 15.0%,

[0084] The content of ZrO2 component is more than 0% and less than 10.0%,

[0085] The total content of Al2O3 and ZrO2 components is 10.0% or more.

[0086] By having such a main crystal phase and composition, a hard crystallized glass having a high compressive stress value on the surface can be obtained.

[0087] Crystallized glass, also known as glass ceramics, is a material that is made by heat treating glass to precipitate crystals inside the glass. Crystallized glass is a material that has a crystalline phase and a glass phase, which is different from an amorphous solid. Usually, the crystalline phase of crystallized glass is determined by the angle of the peak that appears in the X-ray diffraction pattern of X-ray diffraction analysis.

[0088] The inorganic composition product and the crystallized glass (hereinafter also referred to as the inorganic composition product) of the present invention are described below. The inorganic composition product is preferably a strengthened crystallized glass.

[0089] The inorganic composition product contains one or more selected from α-cristobalite and α-cristobalite solid solution as the main crystal phase. The inorganic composition product precipitating these crystal phases has high mechanical strength.

[0090] The "main crystalline phase" mentioned in this specification refers to the crystalline phase that is contained in the largest amount in the inorganic composition product as determined by the peaks of the X-ray diffraction pattern.

[0091] The content of each component in this specification is expressed in mass % of oxide conversion unless otherwise specified. Here, the so-called "oxide conversion" means that the amount of oxide of each component contained in the inorganic composition product is expressed in mass % when the total mass of the oxide is 100 mass % assuming that all the components of the inorganic composition product are decomposed and changed into oxides. In this specification, A% to B% means more than A% and less than B%.

[0092] The SiO2 component is a necessary component for constituting one or more selected from α-cristobalite and α-cristobalite solid solution. Preferably, the upper limit is 75.0% or less, less than 74.0%, less than 73.7%, less than 72.5%, or less than 72.0%. In addition, preferably, the lower limit is 50.0% or more, 55.0% or more, 58.0% or more, 60.0% or more, 62.0% or more, or 64.0% or more.

[0093] The Li2O component is an important component for improving the solubility of the original inorganic composition. However, if the amount of the Li2O component is less than 3.0%, the above effect cannot be obtained and the melting of the original glass becomes difficult. In addition, if it exceeds 10.0%, the formation of lithium disilicate crystals will increase.

[0094] Preferably, the lower limit is 3.0% or more, 3.5% or more, 4.0% or more, 4.5% or more, 5.0% or more, or 5.5% or more, and preferably, the upper limit is 10.0% or less, 9.0% or less, 8.5% or less, or 8.0% or less.

[0095] The Al2O3 component is an appropriate component for improving the mechanical strength of the inorganic composition product. Preferably, the upper limit is less than 15.0%, less than 14.5%, less than 14.0%, less than 13.5%, or less than 13.0%. In addition, preferably, the lower limit is more than 5.0%, more than 5.5%, more than 5.8%, more than 6.0%, or more than 6.5%.

[0096] The ZrO2 component is an arbitrary component added to improve the mechanical strength. Preferably, the upper limit is 10.0% or less, 9.5% or less, 9.0% or less, 8.8% or less, or 8.5% or less. In addition, preferably, the lower limit is greater than 0%, 0.1% or more, 1.0% or more, 1.5% or more, 1.8% or more, or 2.0% or more.

[0097] If the sum of the contents of Al2O3 and ZrO2, i.e. [Al2O3+ZrO2], is high, the surface compressive stress will increase during chemical strengthening, heat treatment strengthening, and ion implantation strengthening. Preferably, the lower limit of [Al2O3+ZrO2] is 10.0% or more, 10.5% or more, 11.0% or more, 12.0% or more, 13.0% or more, or greater than 13.5%.

[0098] On the other hand, the upper limit of [Al2O3+ZrO2] is preferably 22.0% or less, 21.0% or less, 20.0% or less, or 19.0% or less.

[0099] The lower limit of the total content of the SiO2 component, the Li2O component, the Al2O3 component, and the ZrO2 component can be set to 75.0% or more, 80.0% or more, 83.0% or more, or 85.0% or more.

[0100] The P2O5 component is any component that can be added to play the role of a crystal nucleating agent of the inorganic composition. Preferably, the upper limit is 10.0% or less, 9.0% or less, 8.0% or less, or 7.5% or less. In addition, preferably, the lower limit is 0% or more, 0.5% or more, 1.0% or more, or 1.5% or more.

[0101] The K2O component is an arbitrary component that can be added to increase the surface compressive stress. Preferably, the lower limit is 0% or more, 0.1% or more, 0.3% or more, 0.5% or more, or 0.8% or more.

[0102] If the content is excessive, crystals may become difficult to precipitate. Therefore, the upper limit is preferably 10.0% or less, 6.0% or less, 5.0% or less, 4.0% or less, 3.5% or less, or 3.0% or less.

[0103] The Na2O component is an arbitrary component that can be added to increase the surface compressive stress. If it is contained excessively, it is sometimes difficult to obtain the desired crystalline phase. Preferably, the upper limit is 10.0% or less, 5.0% or less, 4.0% or less, 3.0% or less, or 2.5% or less.

[0104] MgO, CaO, SrO, BaO, and ZnO are optional components used to improve the solubility of the inorganic composition, but if they are contained in excess, the resulting crystals tend to coarsen. Therefore, the upper limit of the MgO component is preferably 10.0% or less, 7.0% or less, 5.0% or less, 4.0% or less, 3.0% or less, or 2.5% or less. The upper limit of the CaO component is preferably 10.0% or less, 7.0% or less, 5.0% or less, 4.0% or less, 3.0% or less, or 2.0% or less. The upper limit of the SrO component is preferably 10.0% or less, 7.0% or less, 4.0% or less, 3.0% or less, 2.5% or less, or 2.3% or less. The upper limit of the BaO component is preferably 10.0% or less, 8.0% or less, 7.0% or less, 6.0% or less, 5.0% or less, or 4.0% or less. The upper limit of the ZnO component is preferably 10.0% or less, 9.0% or less, 8.8% or less, 8.5% or less, 8.0% or less, or 7.5% or less.

[0105] The total amount of SrO and BaO components is preferably less than 12.0%, and more preferably the upper limit is less than 10.0%, less than 8.0%, less than 6.0%, or 4.5% or less.

[0106] The inorganic composition product may contain Nb2O5, Ta2O5, and TiO2 components, or may not contain these components, within the range that does not impair the effect of the present invention. The upper limit of the Nb2O5 component is preferably 10.0% or less, 6.0% or less, 5.0% or less, or 3.0%. The upper limit of the Ta2O5 component is preferably 10.0% or less, 8.0%, 6.0%, or less than 4.0%. The upper limit of the TiO2 component is preferably less than 7.0%, less than 5.0%, less than 3.0%, less than 2.0%, less than 1.0%, less than 0.5%, or less than 0.1%.

[0107] In addition, the inorganic composition product may contain B2O3, La2O3, Y2O3, WO3, TeO2, and Bi2O3, or may not contain these components, within the range that does not impair the effect of the present invention. The blending amount may be 0% to 2.0%, 0% or more to less than 2.0%, or 0% to 1.0%.

[0108] Furthermore, the inorganic composition product may contain other components other than the above-mentioned components or may not contain these components within the range that does not impair the characteristics of the inorganic composition product of the present invention, such as metal components such as Gd, Yb, Lu, V, Cr, Mn, Fe, Co, Ni, Cu, Ag and Mo (including their metal oxides).

[0109] Sb2O3 may be contained as a glass clarifier. Preferably, the upper limit is 3.0% or less, more preferably 1.0% or less, and even more preferably 0.6% or less.

[0110] In addition, as a clarifier of the glass, in addition to the Sb2O3 component, one or more selected from the group consisting of SnO2, CeO2, As2O3, and F, NOx, and Sox may be contained, or these components may not be contained. The content of the clarifier is preferably limited to 3.0% or less, more preferably 1.0% or less, and most preferably 0.6% or less.

[0111] On the other hand, since each of Pb, Th, Tl, Os, Be, Cl and Se has become a harmful chemical substance and its use has tended to be reduced in recent years, it is preferable that these components are not substantially contained.

[0112] The inorganic composition product of the present invention is formed with a compressive stress layer having a compressive stress value CS (MPa) of more than 600MPa on the surface. In addition, the crystallized glass of the present invention can form a compressive stress layer on the surface. The compressive stress value of the compressive stress layer is preferably more than 600MPa, more preferably more than 650MPa, more preferably more than 680MPa, and particularly preferably more than 700MPa. The upper limit is, for example, less than 1400MPa, less than 1300MPa, less than 1200MPa or less than 1100MPa. By having such a compressive stress value, the development of cracking can be suppressed and mechanical strength can be improved.

[0113] The thickness DOLzero (μm) of the compressive stress layer is not limited because it also depends on the thickness of the inorganic composition product. For example, in the case of a crystallized glass substrate with a thickness of 10 mm, the lower limit of the thickness of the compressive stress layer can be greater than 1 μm, greater than 30 μm, greater than 50 μm, greater than 70 μm, greater than 100 μm, greater than 130 μm, greater than 150 μm, greater than 180 μm, or greater than 200 μm.

[0114] For example, when the inorganic composition product is a crystallized glass substrate, the product can be produced by the following method. That is, the raw materials are uniformly mixed in such a way that the above-mentioned components are within the prescribed content range, and the raw glass is produced by melting and molding. Then, the raw glass is crystallized to produce crystallized glass.

[0115] The heat treatment for crystallization can be performed in one or two stages.

[0116] In the two-step heat treatment, heat treatment is first performed at a first temperature to perform a nucleation step, and after the nucleation step, heat treatment is performed at a second temperature higher than the nucleation step to perform a crystal growth step.

[0117] The first temperature of the two-step heat treatment is preferably 450 to 750° C., more preferably 500 to 720° C., and further preferably 550 to 680° C. The holding time at the first temperature is preferably 30 to 2000 minutes, and more preferably 180 to 1440 minutes.

[0118] The second temperature of the two-step heat treatment is preferably 600° C. to 800° C., more preferably 650° C. to 750° C. The holding time at the second temperature is preferably 30 minutes to 600 minutes, more preferably 60 minutes to 400 minutes.

[0119] In the one-stage heat treatment, the nucleation step and the crystal growth step are performed continuously at one stage of temperature. Usually, the temperature is raised to a predetermined heat treatment temperature, and after reaching the heat treatment temperature, the temperature is maintained for a certain period of time, and then the temperature is lowered.

[0120] When heat treatment is performed at one stage, the heat treatment temperature is preferably 600 to 800° C., more preferably 630 to 770° C. The holding time at the heat treatment temperature is preferably 30 to 500 minutes, more preferably 60 to 400 minutes.

[0121] Crystallized glass can be processed into a glass molded body by grinding and polishing, etc. A crystallized glass substrate can be produced by processing the glass molded body into a thin plate shape.

[0122] The method for forming a compressive stress layer as an inorganic composition product and the method for forming a compressive stress layer in a crystallized glass without a compressive stress layer include: for example, a chemical strengthening method in which an alkaline component existing in the surface layer of a crystallized glass substrate is exchanged with an alkaline component having an ion radius larger than that of the alkaline component to form a compressive stress layer on the surface layer. In addition, there are also thermal strengthening methods in which a crystallized glass substrate is heated and then rapidly cooled, and ion implantation methods in which ions are implanted into the surface layer of a crystallized glass substrate.

[0123] The chemical strengthening method can be implemented, for example, by the following steps. The crystallized glass matrix is ​​contacted with or immersed in a salt containing potassium or sodium, such as potassium nitrate (KNO3), sodium nitrate (NaNO3) or a molten salt of a mixed salt or a composite salt thereof. The treatment of contacting or immersing in the molten salt (chemical strengthening treatment) can be performed in one stage or two stages.

[0124] For example, in the case of a two-stage chemical strengthening treatment, the first stage is contacted or immersed in a sodium salt or a mixed salt of potassium and sodium heated to 350°C to 550°C for 1 minute to 1440 minutes, preferably 90 minutes to 500 minutes. Then, the second stage is contacted or immersed in a potassium salt or a mixed salt of potassium and sodium heated to 350°C to 550°C for 1 minute to 1440 minutes, preferably 60 minutes to 600 minutes.

[0125] In the case of the one-step chemical strengthening treatment, the material is contacted with or immersed in a salt containing potassium or sodium, or a mixed salt thereof, heated to 350° C. to 550° C. for 1 minute to 1440 minutes.

[0126] The chemical strengthening of inorganic composition products can be carried out in one stage or in multiple stages, but in order to efficiently increase the surface compressive stress and increase the thickness of the compressive stress layer, it is preferred to carry out a two-stage strengthening treatment, that is, strengthening using a molten salt of sodium in the first stage and then strengthening using a molten salt of potassium in the second stage.

[0127] There is no particular limitation on the thermal strengthening method. For example, the inorganic composition product matrix can be heated to 300°C to 600°C, and then rapidly cooled by water cooling and / or air cooling. The compressive stress layer can be formed by the temperature difference between the surface and the interior of the glass substrate. In addition, the compressive stress layer can be formed more effectively by combining the thermal strengthening method with the above-mentioned chemical treatment method.

[0128] There is no particular limitation on the ion implantation method. For example, for the surface of the inorganic composition product matrix, any ions are implanted by causing them to collide with the matrix surface at an acceleration energy and an acceleration voltage that do not damage the matrix surface. Afterwards, heat treatment is performed as required, thereby forming a compressive stress layer on the surface in the same manner as other methods.

[0129] Example

[0130] Examples 1 to 28, Comparative Examples 1 and 2

[0131] As raw materials for the various components of crystallized glass, corresponding oxides, hydroxides, carbonates, nitrates, fluorides, chlorides, metaphosphate compounds and the like are selected, and these raw materials are weighed and uniformly mixed in such a manner as to have the compositions described in Tables 1 to 3.

[0132] Secondly, the mixed raw materials are put into a platinum crucible, and the melting difficulty of the glass composition is matched to use an electric furnace at 1300°C to 1600°C for 2 hours to 24 hours. Afterwards, the molten glass is stirred and homogenized, and then the temperature is lowered to 1000°C to 1450°C and then cast into a mold, and slowly cooled to make the original glass. In Examples 1 to 24 and Comparative Examples 1 and 2, the obtained original glass is crystallized by a two-stage heat treatment to make crystallized glass. The first stage is to nucleate at the temperature and time shown in the "nucleation conditions" of Tables 1 to 3, and the second stage is to crystallize at the temperature and time shown in the "crystallization conditions" of Tables 1 to 3. Example 25 to Example 28 is to crystallize the original glass by a one-stage heat treatment to make crystallized glass. Nucleation and crystallization are carried out simultaneously at the temperature and time shown in the "crystallization conditions" of Table 3.

[0133] The crystalline phase of the crystallized glass of Examples 1 to 28 and Comparative Examples 1 and 2 was determined by the angle of the peak that appeared in the X-ray diffraction pattern using an X-ray diffraction analysis device (manufactured by BRUKER, D8Dsicover). By observing the X-ray diffraction patterns of the crystallized glasses of Examples 1 to 28 and Comparative Examples 1 and 2, it can be seen that the main peak (the peak with the highest intensity and large peak area) appeared at the position corresponding to the peak pattern of α-cristobalite and / or α-cristobalite solid solution, and it can be determined that α-cristobalite and α-cristobalite solid solution were all precipitated as the main crystalline phase.

[0134] The produced crystallized glass is cut and polished, and further parallel grinding is performed on the opposite side in a manner that the thickness becomes 10mm to obtain a crystallized glass substrate. Secondly, in Example 1 to Example 23, Example 25, and Example 26, a chemically strengthened crystallized glass substrate is obtained by using a crystallized glass substrate as a mother material to carry out 2-stage strengthening. Specifically, after being immersed in NaNO at the temperature and time shown in Table 1 to Table 3, KNO is immersed in the temperature and time shown in Table 1 to Table 3. Molten salt (the second stage). The substrate obtained by Example 24, Comparative Example 1, and Comparative Example 2 is immersed in KNO at the temperature and time shown in Table 3. Molten salt has been strengthened in 1 stage. The strengthened substrate of Comparative Example 1 and Comparative Example 2 is a chemically strengthened crystallized glass substrate corresponding to Example 25 and Example 27 recorded in Patent Document 1. The substrate obtained by Example 27 and Example 28 is immersed in NaNO at the temperature and time shown in Table 3. Molten salt has been strengthened in 1 stage.

[0135] The compressive stress value (CS) of the surface of the tempered crystallized glass obtained in the above manner was measured. Examples 1 to 26, Comparative Examples 1 and 2 were measured using the glass surface stress gauge FSM-6000LE series manufactured by Orihara Manufacturing Co., Ltd.; Examples 27 and 28 were measured using the scattered light photoelastic stress gauge SLP-1000. As shown in Tables 1 to 3, in the case of the FSM-6000LE series, the light source of the measuring machine selected a light source with a wavelength of 596nm or 365nm for measurement according to the strengthening depth. In the case of the SLP-1000, a light source with a wavelength of 640nm was used for measurement.

[0136] The values ​​of the refractive index used as the CS measurement conditions are shown in Tables 1 to 3. The refractive index used in the CS measurement is the refractive index value of the wavelength (640nm, 596nm or 365nm) of the light source used in the measurement. In addition, the refractive index value of the specified wavelength is calculated by the quadratic approximation based on the measured values ​​of the refractive index of the wavelength of the C line, d line, F line, and g line according to the V block method specified in JIS B 7071-2:2018.

[0137] The values ​​of the photoelastic constants used as the CS measurement conditions were the values ​​shown in Tables 1 to 3. The photoelastic constants used in the CS measurement were the values ​​of the photoelastic constants of the wavelength (640 nm, 596 nm, or 365 nm) of the light source used in the measurement. The photoelastic constants of the wavelengths 640 nm, 596 nm, or 365 nm were calculated by a quadratic approximation based on the measured values ​​of the photoelastic constants of the wavelengths 435.8 nm, 546.1 nm, and 643.9 nm.

[0138] The photoelastic constant (β) is measured by grinding the sample surface to a disk shape of 25 mm in diameter and 8 mm in thickness, applying a compressive load in a specified direction, measuring the optical path difference at the center of the glass, and calculating it using the relationship δ = β·d·F. In the above formula, the optical path difference is δ (nm), the thickness of the glass is d (cm), and the stress is F (MPa).

[0139] In measuring the depth DOLzero (μm) (also referred to as stress depth) when the compressive stress of the compressive stress layer is 0 MPa, since the sensitivity of the device varies depending on the depth of DOLzero (μm), the measurement device is selected according to the depth.

[0140] In the depth measurement of Examples 1 to 23 and Examples 25 to 28, the scattered light photoelastic stress meter SLP-1000 was used, and in Example 24, Comparative Example 1, and Comparative Example 2, the glass surface stress meter FSM-6000LE series manufactured by Orihara Seisakusho was used for measurement. The wavelength of the light source, the refractive index of the sample, and the photoelastic constant were measured, and the values ​​shown in the table were used for calculation. In particular, when DOLzero (μm) exceeded 500 μm, it could not be measured with the above-mentioned measuring machine, so it was recorded as ">500".

[0141] The results are shown in Tables 1 to 3. As can be seen from Tables 1 to 3, the inorganic composition product (crystallized glass) of the present invention has a compressive stress layer with high CS on the surface and is hard.

[0142]

Table 1

[0143]

[0144]

Table 2

[0145]

[0146]

Table 3

[0147]

[0148] Several embodiments and / or examples of the present invention are described in detail above, but a person with ordinary knowledge in the technical field to which the invention belongs can easily add many changes to these exemplified embodiments and / or examples without substantially departing from the novel teachings and effects of the present invention. Therefore, these many changes are also included in the scope of the present invention. The contents of the documents described in this specification are all cited for use.

Claims

1. An inorganic composition product containing one or more selected from α-cristobalite and α-cristobalite solid solution as a main crystalline phase, In terms of mass % converted to oxides, The content of SiO2 is 50.0% to 75.0%. The content of Li2O is 3.0% to 10.0%. The content of Al2O3 component is 10.0% or more and less than 15.0%, The total content of Al2O3 and ZrO2 is 10.0% or more. The surface compressive stress value is more than 600MPa. The thickness of the compressive stress layer is 4 μm or more.

2. The inorganic composition product according to claim 1, wherein: In terms of mass % converted to oxides, The content of ZrO2 is greater than 0% and less than 10.0%. The content of K2O component is 0% to 10.0%, The content of P2O5 component is 0% to 10.0%.

3. The inorganic composition product according to claim 1 or 2, wherein: In terms of mass % converted to oxides, The content of Na2O is 0% to 10.0%. The content of MgO component is 0% to 10.0%, The content of CaO component is 0% to 10.0%, The content of SrO component is 0% to 10.0%, The content of BaO component is 0% to 10.0%, The content of ZnO component is 0% to 10.0%, The content of Sb2O3 component is 0% to 3.0%.

4. The inorganic composition product according to claim 1 or 2, wherein: In terms of mass % converted to oxides, The content of Nb2O5 is 0% to 10.0%. The content of Ta2O5 is 0% to 10.0%, The content of TiO2 component is greater than 0% and less than 7.0%.

5. A crystallized glass comprising one or more selected from α-cristobalite and α-cristobalite solid solution as a main crystalline phase, In terms of mass % converted to oxides, The content of SiO2 is 50.0% to 75.0%. The content of Li2O is 3.0% to 10.0%. The content of Al2O3 component is 10.0% or more and less than 15.0%, The content of ZrO2 is greater than 0% and less than 10.0%. The total content of Al2O3 and ZrO2 components is 12.0% or more.

6. The crystallized glass according to claim 5, wherein: In terms of mass % converted to oxides, The content of K2O component is 0% to 5.0%, The content of P2O5 component is 0% to 10.0%.

7. The crystallized glass according to claim 5 or 6, wherein: In terms of mass % converted to oxides, The content of Na2O is 0% to 4.0%. The content of MgO component is 0% to 4.0%, The content of CaO component is 0% to 4.0%, The content of SrO is 0% to 4.0%. The content of BaO component is 0% to 5.0%, The content of ZnO component is 0% to 10.0%, The content of Sb2O3 component is 0% to 3.0%.

8. The crystallized glass according to claim 5 or 6, wherein: In terms of mass % converted to oxides, The content of Nb2O5 is 0% to 5.0%, The content of Ta2O5 is 0% to 6.0%, The content of TiO2 component is greater than 0% and less than 1.0%.