Positive electrode active material for lithium secondary battery, preparation method thereof and lithium secondary battery comprising the same

By using a cathode active material with secondary particles with a specific crystal plane structure and doping element distribution, the problems of short life and limited capacity of lithium secondary batteries are solved, and lithium secondary batteries with high discharge capacity and long life are realized.

CN114365308BActive Publication Date: 2024-10-29辰星锂电
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202080064162.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-06-30
Publication Date
2024-10-29
Estimated Expiration
2040-06-30

AI Technical Summary

Technical Problem

The cathode active material of existing lithium secondary batteries has a short lifespan and limited capacity during the charge and discharge process, making it difficult to meet the needs of high energy density and high stability.

Method used

The cathode active material uses secondary particles formed by agglomeration of multiple primary particles. The primary particles have a specific crystal face structure and doping element distribution. By controlling the crystal face shape and the concentration of doping elements, the insertion and desorption of lithium ions is improved. stability in the process.

Benefits of technology

It achieves high discharge capacity and long life of lithium secondary batteries, reduces cracks between primary particles during charge and discharge, and improves the cycle stability and electrochemical efficiency of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114365308B_ABST
    Figure CN114365308B_ABST
Patent Text Reader

Abstract

The present invention relates to a positive electrode active material, which includes secondary particles composed of aggregates of multiple primary particles, including first primary particles arranged on the surface of the secondary particles, at least a part of which is in the form of thin sheets having a pair of first crystal faces facing each other, the first crystal faces of the first primary particles are arranged in a radial direction, one end of the pair of first crystal faces is provided with multiple crystal faces different from the first crystal faces to connect one end of the pair of first crystal faces, the longitudinal section of the first primary particle includes a pair of first crystal faces spaced apart from each other and a second crystal face and a third crystal face connecting one end of the pair of first crystal faces to each other, the second crystal face and the third crystal face are arranged at the outermost side of the secondary particles and are connected to form an angle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a positive electrode active material, a preparation method thereof and a lithium secondary battery including the same. More specifically, the present invention relates to a positive electrode active material having an improved lifespan and simultaneously exhibiting a high capacity, a preparation method thereof and a lithium secondary battery including the same. Background Art

[0002] With the development of portable mobile electronic devices such as smartphones, MP3 players, and tablet computers, the demand for secondary batteries that can store electrical energy has exploded. Specifically, with the emergence of electric vehicles, large and medium-sized energy storage systems, and portable devices that require high energy density, the demand for lithium secondary batteries is increasing.

[0003] As the demand for lithium secondary batteries increases, various research and development are being conducted to improve the characteristics of positive electrode active materials for lithium secondary batteries. For example, in Korean Patent Publication 10-2014-0119621 (Application No. 10-2013-0150315), a secondary battery with high voltage capacity and long life characteristics is disclosed, wherein a precursor for preparing a lithium excess positive electrode active material is used to adjust the type and composition of the metal substituted in the precursor, and the type and amount of the added metal are adjusted. Summary of the invention

[0004] Technical Purpose

[0005] One technical objective to be achieved by the present application is to provide a high-capacity positive electrode active material, a preparation method thereof, and a lithium secondary battery comprising the same.

[0006] Another technical objective of the present application is to provide a long-life positive electrode active material, a preparation method thereof, and a lithium secondary battery comprising the same.

[0007] Another technical objective to be achieved by the present disclosure is to provide a highly stable positive electrode active material, a preparation method thereof, and a lithium secondary battery comprising the same.

[0008] Still another technical object to be achieved by the present application is to provide a positive electrode active material having a high discharge capacity and at the same time having minimized lifespan degradation characteristics depending on the number of charge / discharge, a preparation method thereof, and a lithium secondary battery including the same.

[0009] The technical objectives to be achieved by this application are not limited to the above objectives.

[0010] Technical Solution

[0011] According to one aspect of the present invention, an embodiment of the present invention provides a positive electrode active material comprising secondary particles composed of aggregates of multiple primary particles, wherein at least a portion of the primary particles arranged on the surface of the secondary particles are first primary particles in the shape of flakes having a pair of first crystal faces facing each other, the first crystal faces of the first primary particles are arranged in a radial direction, one end of the pair of first crystal faces has multiple crystal faces different from the first crystal faces to connect one end of the pair of first crystal faces, the longitudinal section of the first primary particle includes a pair of first crystal faces separated from each other and a second crystal face and a third crystal face connecting one end of the pair of first crystal faces, the second crystal face and the third crystal face are arranged at the outermost side of the secondary particles and are connected to form an angle.

[0012] The first primary particle has a first length as a major axis of a first crystal plane, a second length as a minor axis of the first crystal plane perpendicular to the first length, and a third length as an interval between the pair of first crystal planes, wherein the third length may be in the range of 10 nm to 400 nm.

[0013] In one embodiment, a ratio of the first length to the third length is in the range of 2 to 100, and a ratio of the second length to the third length may be in the range of 1.5 to 80.

[0014] In one embodiment, the positive electrode active material is a layered rhombohedral system compound (Rhombohedral system), and the first crystal plane is ( Where h = 0, k = 0, and n is an integer), the configuration of the first crystal plane is different from the second crystal plane and the third crystal plane.

[0015] In one embodiment, the angle between the second crystal plane and the third crystal plane may be in the range of 30° to 170°.

[0016] In one embodiment, when a 2032 coin-type half-cell made using the positive active material as the positive electrode and lithium metal as the negative electrode is charged to 4.3V at a constant current of 0.5C and discharged to 2.7V at a constant current of 0.5C for 100 cycles, the intensity of the peak corresponding to the phase change from H2 to H3 in the dQ / dV curve can be more than 40% compared to 1 cycle.

[0017] In one embodiment, the primary particles include nickel (Ni), M1 and M2, wherein the M1 is composed of at least any one of manganese (Mn), cobalt (Co) and aluminum (Al), the nickel (Ni) is 65 mol% or greater, and the M2 is a doping element and can be composed of 0.05 mol% to 5 mol%.

[0018] In one embodiment, M2 can be composed of boron (B); or boron (B) and any one or more selected from tungsten (W), molybdenum (Mo), tantalum (Ta), niobium (Nb), hafnium (Hf), silicon (Si), tin (Sn), zirconium (Zr), calcium (Ca), germanium (Ge), gallium (Ga), indium (In), ruthenium (Ru), tellurium (Te), antimony (Sb), iron (Fe), chromium (Cr), vanadium (V) and titanium (Ti).

[0019] In one embodiment, a coating layer including boron (B) covering at least a portion of the second crystal plane and the third crystal plane may be formed on the second crystal plane and the third crystal plane.

[0020] In one embodiment, the concentration of the boron (B) is uniform in the secondary particles and has a concentration gradient in the coating layer, and the average concentration of the boron (B) in the coating layer may be higher than the average concentration of the boron (B) in the secondary particles.

[0021] In one embodiment, the coating layer may include LiBO2, LiB3O5, LiB5O8, α-LiBO2, Li2B2O4, Li2B2O7, Li2B4O7, Li2B6O7, Li2B6O 10 、Li2B8O 13 、Li3BO3、Li3B7O 12 , Li4B2O5, α-Li4B2O5, β-Li4B2O5, Li4B 10 O 17 and Li6B4O9.

[0022] In one embodiment, in the cross-section of the secondary particles when a half-cell made using the positive active material as the positive electrode and the lithium metal as the negative electrode is charged to 4.3V at a constant current of 0.5C, the area of ​​microcracks which are spaces formed between the boundaries of adjacent primary particles may be less than 15% of the cross-sectional area of ​​the secondary particles.

[0023] In one embodiment, when the secondary particles are measured using an X-ray diffraction analysis obtained using a device with an output of 45 kV and 40 mA with a Cu Ka beam source at a scanning rate of 1 degree per minute with a step spacing of 0.0131, the intensity ratio of the 003 peak to the 104 peak can be in the range of 1.6 to 2.3.

[0024] In one embodiment, as the content of the doping element increases, the intensity ratio of the 003 peak to the 104 peak may decrease.

[0025] In one embodiment, the secondary particle has a spherical shape including a central portion and a surface portion, wherein the first crystal plane of the first primary particle is disposed in a direction from the central portion toward the surface portion, and the second crystal plane and the third crystal plane of the first primary particle are disposed in the surface portion of the secondary particle, so that the outermost surface of the surface portion of the secondary particle can form an uneven structure through the second crystal plane and the third crystal plane.

[0026] In one embodiment, the secondary particle is represented by the following <Chemical Formula 1>, and the surface portion of the secondary particle may further include a coating layer covering at least a part of the second crystal plane and the third crystal plane.

[0027] <Chemical Formula 1>

[0028] Li a M x D y O2,

[0029] (M represents at least any one of Ni, Co, Mn, or Al; D represents a doping element composed of only B, or co-doped with any one of B and W, Mo, Nb, Ta, and Sb, where 0.9 < a < 1.1, and x + y = 1, and 0.95 < x < 1, 0 < y < 0.05.)

[0030] In one embodiment, the first primary particle has a first length as the major axis of the first crystal plane, a second length as the minor axis of the first crystal plane perpendicular to the first length, and a third length as the interval between the pair of first crystal planes. The content of the doping element is in the range of 0.05 mol% to 5 mol%. As the concentration of the doping element increases, the first length of the first primary particle increases, and at the same time, the third length may decrease.

[0031] According to another aspect of the present invention, an embodiment of the present invention provides a positive electrode for a secondary battery, which includes the above positive electrode active material.

[0032] According to an excellent aspect of the present invention, an embodiment of the present invention provides a lithium secondary battery including the positive electrode.

[0033] According to other aspects of the present invention, an embodiment of the present invention provides a battery module including the lithium secondary battery as a unit cell.

[0034] According to other aspects of the present invention, an embodiment of the present invention provides a battery pack including the above battery module, and the battery pack is used as a power source for large and medium-sized devices, and the large and medium-sized devices are selected from the group consisting of electric vehicles, hybrid vehicles, plug-in hybrid vehicles, and power storage systems.

[0035] Technical Effects

[0036] According to the present invention as described above, the positive electrode active material according to the present invention includes secondary particles formed as agglomerates of a plurality of primary particles, and the secondary particles may include a high content of nickel and a doping element.

[0037] The doping element may control the flake form of the first primary particle, thereby providing a positive electrode active material that can be stably used for a long time and has a high discharge capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1a is a SEM image showing secondary particles according to an embodiment of the present disclosure.

[0039] Figure 1b It is used to show Figure 1a Radial diagram of the secondary particles.

[0040] Figure 1c : is a schematic diagram schematically showing a cross section of a secondary particle according to an embodiment of the present invention.

[0041] Figure 2 is a flow chart showing a method for preparing a positive active material according to another embodiment of the present invention.

[0042] Figure 3 : are SEM images of the metal composite hydroxides according to Example 1 and Example 2.

[0043] Figure 4 are SEM images of the positive electrode active materials according to Example 1 and Example 2.

[0044] Figure 5 : are SEM images of the metal composite hydroxides according to Examples 4 to 7.

[0045] Figure 6 are SEM images of the positive electrode active materials according to Examples 4 to 7.

[0046] Figure 7 : are SEM images of the metal composite hydroxides according to Examples 9 to 12.

[0047] Figure 8 are SEM images of the positive electrode active materials according to Examples 9 to 12.

[0048] Fig. 9 : is a SEM image measuring the thickness of the primary particle located on the surface of the secondary particle according to the boron (B) doping amount in the NCO-based positive active material including 90 mol % of Ni.

[0049] Fig.10 yes Fig. 9 SEM image of the positive electrode active material not doped with boron (B).

[0050] Fig.11 yes Fig. 9 FIG. 5 is a SEM image of a positive electrode active material doped with 0.5 mol % of boron (B).

[0051] Fig.12 yes Fig. 9 FIG. 5 is an SEM image of a positive electrode active material doped with 1 mol % of boron (B).

[0052] Fig.13 yes Fig. 9 SEM image of the positive electrode active material doped with 1.5 mol % of boron (B).

[0053] Fig.14 yes Fig. 9 FIG. 5 is an SEM image of a positive electrode active material doped with 2 mol % of boron (B).

[0054] Fig.15a Graph showing the third length of primary particles located at the surface of secondary particles in the primary particles, that is, the interval between the (003) plane and the (003) plane, measured using SEM images in an NCO-based positive electrode active material using a metal composite hydroxide containing 90 mol % Ni.

[0055] Fig.15b This is a graph showing the length of the (003) plane depending on the amount of boron (B) doping.

[0056] Fig.16a is a graph showing a first length, a second length, and a third length based on a boron (B) doping amount.

[0057] Fig.16b is a graph showing a first length and a ratio of a second length to a third length based on a boron (B) doping amount.

[0058] Fig.17 are SEM images of the positive electrode active materials according to Example 24 and Comparative Example 7.

[0059] Fig.18 are FIB TEM images of the positive electrode active materials according to Example 24 and Comparative Example 7.

[0060] Fig.19 3 are FIB TEM images of the positive electrode active materials according to Example 24 and Comparative Example 7 before the initial cycle.

[0061] Fig. 20 yes Fig.19 FIB TEM image of Example 24 before initial cycling.

[0062] Fig.21 This is the FIB TEM image of Example 24 after 100 cycles.

[0063] Figure 22 to Figure 24 These are the analysis results of the coating layer formed on the primary particles located on the surfaces of the secondary particles in Example 24.

[0064] Fig.25 is a TEM image of the primary particles of Example 24.

[0065] Figure 26 to Figure 28 These are the XRD analysis results of boron oxide and lithium hydroxide before and after heat treatment.

[0066] Fig.29 3 is a cycle curve diagram of a full battery using the positive electrode active materials according to Example 24 and Comparative Example 7.

[0067] Fig.30 are SEM images showing cross sections of secondary particles when the positive electrode active materials according to Example 24 and Comparative Example 7 were charged at different charging voltages.

[0068] Fig.31 SEM images of half cells and full cells using the positive electrode active materials according to Example 24 and Comparative Example 7 after cycling are shown.

[0069] Fig.32 and Fig.33 These are the in-situ XRD data of Example 24 and Comparative Example 7. DETAILED DESCRIPTION

[0070] Specific details of other embodiments are included in the detailed description and accompanying drawings.

[0071] The advantages and features of the present invention and its implementation method can be clarified by the accompanying drawings and the embodiments described in detail below. However, the present invention is not limited to the embodiments disclosed below, but can be realized by different multiple ways. All numerals, values, and / or expressions of the content of the components, reaction conditions and components of the present invention under the gases clearly described below are approximate values ​​of the various uncertainties of the measurements that appear when these values ​​are obtained, which are different in the nature of these numerals. Therefore, it should be understood to be modified by "about" in all cases. In addition, when a numerical range is disclosed in this specification, the range is continuous and includes all values ​​of the minimum value of the range to the maximum value including the maximum value in the absence of other representations. In addition, when this range represents an integer, it includes all integers of the minimum value to the maximum value including the maximum value in the absence of other clear indications.

[0072] In addition, in the present invention, when a range is recorded for a variable, it should be understood that the variable includes all values ​​within the recorded range including the endpoints of the range. For example, it should be understood that the range of "5 to 10" includes not only 5, 6, 7, 8, 9 and 10, but also any lower ranges such as 6 to 10, 7 to 10, 6 to 9, 7 to 9, and any values ​​between appropriate integers of the ranges recorded such as 5.5, 6.5, 7.5, 5.5 to 8.5 and 6.5 to 9. For example, the range "10% to 30%" includes not only all integers such as 10%, 11%, 12%, 13% to 30%, but also any lower ranges such as 10% to 15%, 12% to 18% or 20% to 30%, and any values ​​between appropriate integers of the ranges recorded such as 10.5%, 15.5%, 25.5%.

[0073] In one embodiment, the size and particle diameter of various particles such as primary particles and secondary particles can be numerically expressed by a method of measuring the average size of the aggregate, but generally used are all diameters representing the maximum value of the distribution, the median diameter equivalent to the median of the integral distribution curve, and various average diameters (number average, length average, area average, mass average, volume average, etc.). In the present invention, unless otherwise specified, the average size and average particle diameter are number average size and diameter, indicating the measurement D50 (particle diameter at a distribution rate of 50%).

[0074] Figure 1a is a SEM image showing secondary particles according to an embodiment of the present invention, Figure 1b It is used to show Figure 1a The radial diagram of the secondary particles, Figure 1c : is a schematic diagram schematically showing a cross section of a secondary particle according to an embodiment of the present invention.

[0075] Reference Figure 1a to Figure 1c The positive active material according to the present embodiment is composed of secondary particles 200 including a plurality of primary particles. The positive active material can be used as a positive active material for a lithium secondary battery.

[0076] The first primary particles 100 may include a flake-shaped first particle 100 in which at least a portion of the primary particles disposed on the surface of the secondary particle 200 has a pair of first crystal planes 110 facing each other.

[0077] The secondary particle 200 may be formed by agglomeration of a plurality of primary particles. Among the primary particles, the first crystal faces 110 of the first primary particle 100 having the pair of first crystal faces 110 may be arranged in a radial direction from the central portion C of the secondary particle 200 toward the surface portion. For example, one end of the pair of first crystal faces 110 disposed at the outermost portion constituting the secondary particle 200 may be connected by a plurality of crystal faces. More specifically, the pair of first crystal faces 110 are disposed parallel to each other and spaced apart, and one end of the pair of first crystal faces 110 may be connected to each other via a plurality of crystal faces different from the first crystal faces 110.

[0078] The first primary particle 100 having a thin plate shape may be formed by a pair of first crystal planes 110 parallel to each other and one or more second crystal planes 120 and third crystal planes 130 connecting one ends of the pair of first crystal planes 110, in a longitudinal section perpendicular to the pair of crystal planes 110 toward the center of the secondary particle 200. In addition, the second crystal planes 120 and the third crystal planes 130 may be connected to form an angle θ at the outermost surface of the secondary particle 200.

[0079] The radial direction refers to Figure 1b As shown in , the first primary particles 100 are arranged along a direction R from a central portion C of the secondary particle 200 toward a surface portion of the secondary particle 200 .

[0080] In the positive electrode active material according to the present embodiment, the first primary particles 100 having a pair of first crystal faces 110 may be arranged in a radial direction on the surface of the secondary particle 200. The first primary particle 100 may have a flake shape extending from one end to the other end, wherein one end of the first primary particle 100 may face the surface of the secondary particle 200, and the other end of the first primary particle 100 may face the center C of the secondary particle 200.

[0081] For example, in the first primary particle 100, the direction of the first crystal plane 110 is oriented parallel to the radial direction. Therefore, the diffusion of lithium ions from the surface to the inside of the secondary particle 200 can be promoted. In addition, the first primary particle 100 can be arranged parallel to the moving direction of the lithium ions, and the spacing arrangement between a pair of first crystal planes 110 is controlled. Therefore, even during the expansion and contraction caused by repeated reversible charge and discharge, the volume change can be reduced, and the cracks that may occur between the primary particles, such as the separation interval between the primary particles caused by the change in the shape of the primary particles due to the volume change of the electrochemical reaction, can be reduced, thereby improving the life characteristics of the secondary battery.

[0082] like Figure 1cAs shown in , the thin plate shape of the first primary particle 100 means that a pair of first crystal planes 110 are arranged at the outermost surface, and the pair of first crystal planes 110 have a thickness. In addition, the longitudinal section of the first primary particle 100 may be composed of a pair of first crystal planes 110 and a second crystal plane 120 and a third crystal plane 130 connecting one ends of the pair of first crystal planes 110 to each other.

[0083] The first primary particle 100 may include a first length f1 as a major axis of the first crystal plane 110 , a second length f2 as a minor axis of the first crystal plane 110 perpendicular to the first length f1 , and a third length f3 as an interval between the pair of first crystal planes 110 .

[0084] The first length f1 may be the longest length of the first crystal plane 110 parallel to the radial direction, and the second length f2 is one end of a pair of first crystal planes 110, that is, the shortest length of the portion of the first crystal plane 110 facing the surface of the secondary particle 200, and thus may be the length of the minor axis. The third length f3 is the interval between the pair of first crystal planes 110, and may be the thickness. The first length f1 is greater than the second length f2 and the third length f3, and the second length f2 may be greater than the third length f3.

[0085] The third length f3 may be in the range of 10nm to 400nm. When the third length f3 is less than 10nm, the surface area of ​​the secondary particles 200 increases, thereby increasing the contact area with the electrolyte, so that the electrolyte may penetrate into the interior during the cycle of the secondary battery based on this, resulting in a sharp decrease in life. In addition, when the third length f3 is greater than 400nm, the volume change caused by the repeated contraction and expansion of the primary particles during the charge / discharge process of the secondary battery may cause cracks, which may lead to a decrease in life. Preferably, the average value of the third length f3 may be in the range of 30nm to 300nm, and more preferably in the range of 50nm to 150nm.

[0086] A ratio of the first length f1 to the third length f3 may be in the range of 2 to 100, and a ratio of the second length f2 to the third length f3 may be in the range of 1.5 to 80.

[0087] In the first primary particle 100, the first length f1, the second length f2, and the third length f3 may affect each other. When the first length f1, the second length f2, and the third length f3 are within the above range, the secondary particles including the first primary particle 100 can stably maintain a high discharge capacity due to the high capacity Ni, and can maintain a constant structure after a plurality of cycles, thereby improving life characteristics.

[0088] The positive electrode active material is a layered rhombohedral system compound, and the first crystal plane 110, the second crystal plane 120 and the third crystal plane 130 are determined by Miller index. The first crystal plane 110, the second crystal plane 120 and the third crystal plane 130 may be different crystal planes. For example, the first crystal plane has Where h = 0, k = 0, n may be an integer, and the second crystal plane and the third crystal plane may be crystal planes different from the first crystal plane.

[0089] The first crystal plane 110, the second crystal plane 120 and the third crystal plane 130 may be formed of crystal planes forming a layered rhombohedral compound. It can be at least one of (003), (006), (009), (0012) and (0015), and the second crystal plane 120 and the third crystal plane 130 can be formed by removing the layered rhombus system. The rest of the first crystal plane 110 The second crystal plane 120 and the third crystal plane 130 may be composed of crystal planes that connect one ends of a pair of first crystal planes 110 that are spaced apart from each other.

[0090] The first primary particle 100 according to the present embodiment may have a flake shape including at least four crystal faces, which are planes representing the outer shape of a crystal and are planes parallel to a lattice plane.

[0091] The pair of first crystal faces 110 constituting the first primary particle 100 are a pair of wide faces facing each other in the thin sheet shape. The second crystal face 120 and the third crystal face 130 are respectively connected to any one side and the other side of the pair of thin sheet shapes, and one end of the thin sheet shape can be configured to have a triangular cross-section through the second crystal face 120 and the third crystal face 130.

[0092] In the first primary particle 100, the first crystal plane 110 may be a (003) plane. One end of a pair of first crystal planes 110 in the first primary particle 100, that is, both ends of the portion disposed on the outer surface of the secondary particle 200, may be connected to each other so that the second crystal plane 120 and the third crystal plane 130 have an angle with each other.

[0093] For example, at the end of either side of the pair of first crystal planes 110, the second crystal plane 120 may be connected to form an angle of 90° or more. At the other end of the pair of first crystal planes 110, the third crystal plane 130 may be connected to form an angle of 90° or more. The second crystal plane 120 and the third crystal plane 130, which respectively connect the two ends of the pair of first crystal planes 110, are connected to form a predetermined angle. Therefore, the end of the first primary particle 100 may cause the outer surface of the secondary particle 200 to have sharp concave and convex. In addition, with respect to the cross section from the surface portion of the secondary particle 200 toward the center portion C and perpendicular to the pair of first crystal planes 110, the angle θ between the second crystal plane and the third crystal plane may be in the range of 30° to 170°. When the angle θ between the second crystal plane and the third crystal plane is less than 30°, the surface area of ​​the secondary particle increases, thereby increasing the contact area with the electrolyte. Therefore, during the charge and discharge process, the electrolyte flows into the center portion of the secondary particle 200, which may cause microcracks to form on the secondary particle. When the angle θ between the second crystal plane and the third crystal plane exceeds 170°, the efficiency of lithium ions moving into the secondary particle 200 is reduced. Specifically, the angle θ between the second crystal plane and the third crystal plane may be in the range of 90° to 170°, more specifically, in the range of 110° to 170°, and more specifically, in the range of 120° to 160°.

[0094] A 2032 coin-type half-cell using the positive active material as a positive electrode and lithium metal as a negative electrode was tested. After 100 cycles of discharging at 2.7V at a constant current of 0.5C and charging at 4.3V at a constant current of 0.5C, in a curve obtained by first-order differentiation of the charge and discharge curve, that is, a dQ / dV curve, the intensity of the peak corresponding to the phase change of H2-H3 can be 40% or more compared to one cycle, preferably, can be 60% to 98%, and more preferably, can be 70% to 90%.

[0095] The primary particles include Ni and M1 and M2, wherein M1 may be composed of at least one of Mn, Co and Al, the content of Ni is 65 mol% or more, and M2 is a doping element and may be composed of 0.05 mol% to 5 mol%.

[0096] The primary particles according to the present embodiment may include a high content of nickel (Ni) of more than 65 mol%, and may further include a doping element. The doping element may be made of a substance other than lithium (Li), nickel (Ni), manganese (Mn), cobalt (Co) and aluminum (Al). The content of the doping element may be 0.05 mol% to 5 mol%.

[0097] The doping element can improve the life characteristics of the secondary battery by controlling the shape of the first primary particle 100 among the primary particles and controlling the shape of the contraction and expansion that occurs during the insertion or desorption of lithium ions. When the content of the doping element is less than 0.05 mol%, it is difficult for the first primary particles to be arranged radially, thereby reducing the efficiency of lithium ion movement. When it exceeds 5 mol%, the interval between a pair of first crystal planes 110 in the first primary particle 100 is too small, so cracks may occur during the cycle.

[0098] Preferably, the doping element M2 may include boron (B).

[0099] In the present invention, a coating layer including boron (B) and covering at least a portion of the second crystal plane 120 and the third crystal plane 130 may be provided on the second crystal plane 120 and the third crystal plane 130 provided on the outer surface of the secondary particle 200. The boron (B) may be present in the secondary particle 200 in a doping manner. The boron (B) may be formed as a coating layer covering at least a portion of the outer surface of the secondary particle while controlling the shape of the first primary particle.

[0100] The first primary particles 100 according to the present embodiment include boron (B). A coating layer including the boron (B) may be provided on the outer surface of the secondary particles 200. The concentration of the boron (B) may be uniform in the secondary particles 200, and may have a concentration gradient in the coating layer. Preferably, the average concentration of the boron (B) in the coating layer may be higher than the average concentration of the boron (B) in the secondary particles 200.

[0101] The coating layer may include LiBO2, LiB3O5, LiB5O8, α-LiBO2, Li2B2O4, Li2B2O7, Li2B4O7, Li2B6O7, Li2B6O 10 、Li2B8O 13 、Li3BO3、Li3B7O 12 , Li4B2O5, α-Li4B2O5, β-Li4B2O5, Li4B 10 O 17 Lithium boron oxide composed of at least any one of Li6B4O9 and Li6B4O9.

[0102] The coating layer can be formed by reacting a lithium compound with boron oxide, for example, by the following reaction formula:

[0103] Li2CO3+B2O3→Li2B2O4+CO2

[0104] LiOH+B2O3→Li2B2O4+H2O

[0105] Li2CO3+2B2O3→Li2B4O7+CO2

[0106] 2LiOH+B2O3→Li2B4O7+H2O

[0107] For example, secondary particles composed of aggregates of primary particles can be prepared using at least one metal compound of manganese (Mn), cobalt (Co) and aluminum (Al) and boron (B) as a doping element while using nickel (Ni). Then, the secondary particles can be mixed with a lithium compound and sintered to prepare a positive electrode active material. The secondary particles can have a controlled concentration of boron oxide. The boron oxide can react with the lithium compound as shown in the above reaction formula to form a coating layer on the outer surface of the secondary particles. The above reaction formula for preparing the coating layer is an illustration. The lithium boron oxide constituting the coating layer can be formed in various reaction formulas.

[0108] In the secondary particle 200 according to the present embodiment, the secondary particle 200 is composed of an aggregate of a plurality of primary particles including a first primary particle 100. The first primary particle 100 may be disposed on the outer surface of the secondary particle 200, and the first crystal plane 110 of the first primary particle 100 is radially arranged in the secondary particle 200. In addition, the first primary particle 100 may be configured such that the second crystal plane 120 and the third crystal plane 130 of the first primary particle 100 are located on the outer surface of the secondary particle 200. The doping element may include boron (B), and the boron (B) may have a uniform concentration inside the first primary particle 100 to control the shape and position of the first primary particle 100. A coating layer may be formed to cover at least a portion of the second crystal plane 120 and the third crystal plane 130 of the first primary particle 100 to control the directional growth of the first crystal plane 110 of the first primary particle 100.

[0109] In addition, in another embodiment of the present invention, the M2 as the doping element may be composed of boron (B); and at least one of tungsten (W), molybdenum (Mo), tantalum (Ta), niobium (Nb), hafnium (Hf), silicon (Si), tin (Sn), zirconium (Zr), calcium (Ca), germanium (Ge), gallium (Ga), indium (In), ruthenium (Ru), tellurium (Te), antimony (Sb), iron (Fe), chromium (Cr), vanadium (V) and titanium (Ti). More preferably, the doping element M2 may be formed by co-doping of two doping elements, and may be composed of any one or more of boron (B) and tungsten (W), boron (B) and molybdenum (Mo), boron (B) and niobium (Nb), boron (B) and tantalum (Ta), and boron (B) and antimony (Sb).

[0110] In an embodiment of the present invention, a half-cell using the positive active material as the positive electrode and lithium metal as the negative electrode is charged to a cross-section of 4.3V at a constant current of 0.5C, and the area of ​​the microcracks as the space between the boundaries of adjacent primary particles can be less than 15% of the area of ​​the cross-section of the secondary particles.

[0111] When the spherical secondary particles are cut into cross sections, the microcracks can be formed in the form of spaces formed between primary particles and primary particles, and can be connected roughly from the center of the secondary particles toward the surface of the secondary particles. The microcracks start from the center of the secondary particles, can be formed due to a sharp change in volume in the case of charge and discharge, and can extend from the center to the surface during the charge and discharge cycle. The microcracks extending to the surface serve as a path for the electrolyte to flow in, and the electrolyte flows through the microcracks and forms a passivation layer inside the secondary particles, which acts as a resistor and can reduce electrical efficiency. In severe cases, the passivation layer increases the area of ​​the microcracks in the secondary particles, so that the secondary particles can be almost separated.

[0112] In contrast, in the secondary particles according to the present embodiment, microcracks are hardly formed in the case of multiple cycles. For example, in the cross-section of the secondary particle 200 charged to 4.3V at 0.5C using a 2032 coin-type half-cell, the area of ​​microcracks as the space between the boundaries of adjacent primary particles may be less than 15% of the area of ​​the cross-section of the secondary particle. Preferably, the area of ​​the microcracks may be less than 10%, and more preferably less than 7%.

[0113] In the X-ray diffraction analysis obtained by measuring the secondary particles 200 using a device with 45 kV and 40 mA output (Empyrean, Panalytical) using a Cu Ka beam source at a scanning rate of 1 degree per minute and a step spacing of 0.0131, the ratio of the intensity of the 003 peak excluding the background to the intensity of the 104 peak can be in the range of 1.6 to 2.15. In addition, as the content of the doping element increases, the ratio of the intensity of the 003 peak to the intensity of the 104 peak can decrease.

[0114] According to another aspect of the present invention, the secondary particle 200 is spherical with a central portion C and a surface portion, and the first primary particle 100 may be arranged such that the first crystal plane 110 faces the direction from the central portion C to the surface portion. In the first primary particle 100, the second crystal plane 120 and the third crystal plane 130 are provided on the surface portion of the secondary particle 200, so that the outermost surface of the surface portion of the secondary particle 200 can form an uneven structure through the second crystal plane 120 and the third crystal plane 130.

[0115] The secondary particle 200 is represented by the following <Chemical Formula 1>, and the surface portion of the secondary particle 200 may further include a coating layer covering at least a part of the second crystal plane 120 and the third crystal plane 130.

[0116] <Chemical Formula 1>

[0117] Li a M x D y O2

[0118] In the <Chemical Formula 1>, M represents at least one of Ni, Co, Mn, or Al; D represents a doping element composed only of B or a doping element composed of B and W, where 0.9 < a < 1.1, and x + y = 1, and 0.95 < x < 1, 0 < y < 0.05.

[0119] The first primary particle 100 may have a flake shape, and the flake shape has a first length f1 as the major axis of the first crystal plane 110, a second length f2 as the minor axis of the first crystal plane 110 perpendicular to the first length f1, and a third length f3 as the distance between the pair of first crystal planes 110. The first primary particle 100 having the flake shape may be arranged with the major axis facing the central portion C of the secondary particle 200.

[0120] The content of the doping element is from 0.05 mol% to 5 mol%. As the concentration of the doping element increases, the first length f1 of the first primary particle 100 may increase, and the third length f3 may decrease. Preferably, the content of the doping element is in the range of 0.05 mol% to 2 mol%, and more preferably, the content of the doping element may be in the range of 0.5 mol% to 2 mol%.

[0121] According to another aspect of the present invention, the present invention provides a positive electrode active material, comprising: spherical secondary particles, the spherical secondary particles are formed by a layered rhombohedral system compound including metal, lithium, a doping element and oxygen; a coating layer, arranged on the surface of the secondary particles, formed by a compound including lithium, the doping element and oxygen and having a crystal structure different from that of the secondary particles, wherein the metal can be nickel (Ni); and at least one of cobalt (Co), manganese (Mn) and aluminum (Al);

[0122] The average concentration of the doping element in the coating layer is higher than the average concentration of the doping element in the secondary particles. The coating layer may include LiBO2, LiB3O5, LiB5O8, α-LiBO2, Li2B2O4, Li2B2O7, Li2B4O7, Li2B6O7, Li2B6O 10 、Li2B8O 13 、Li3BO3、Li3B7O 12 , Li4B2O5, α-Li4B2O5, β-Li4B2O5, Li4B 10 O 17 Lithium boron oxide from the group consisting of at least one of Li6B4O9 and Li6B4O9.

[0123] The coating layer may have a thickness in the range of 1 nm to 10 nm. When the coating layer has a thickness less than 1 nm, it is difficult to effectively protect the surface of the secondary particles, resulting in degradation of the life characteristics of the secondary battery. When the coating layer has a thickness greater than 10 nm, the movement of lithium ions may be restricted, thereby reducing the capacity of the battery.

[0124] The first primary particle may have a crystal structure, wherein the a-axis of the crystal structure may be arranged parallel to the direction from the center portion of the secondary particle toward the surface portion. Therefore, the first primary particles having the flake shape may serve as a migration path for lithium ions and electrolytes, thereby improving the charge and discharge efficiency of the secondary battery including the present positive electrode active material.

[0125] According to one embodiment, the metal may have a concentration gradient in the secondary particles. For example, at least any one of nickel, cobalt, manganese and aluminum may have a continuous or discontinuous concentration gradient in at least one region of the secondary battery.

[0126] According to an embodiment of the present invention, the positive electrode active material may be prepared by sintering a lithium compound with a positive electrode active material precursor prepared using the metal and the doping element.

[0127] Optionally, according to another embodiment, the method for preparing the positive electrode active material may include the step of supplying the transition metal aqueous solution, the chelating agent and the doping source into a reactor to prepare the positive electrode active material precursor doped with the doping element, and the step of sintering the positive electrode active material precursor with a lithium salt.

[0128] According to another aspect of the present invention, an embodiment of the present invention includes a positive electrode for a secondary battery including the above-mentioned positive active material.

[0129] Furthermore, a lithium secondary battery including the positive electrode may be included.

[0130] Embodiments of the present invention may include a battery module including the lithium secondary battery as a unit battery.

[0131] Furthermore, a battery pack including the battery module is provided, wherein the battery pack is used as a power source for medium- to large-sized devices, wherein the medium- to large-sized devices are selected from the group consisting of electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, and power storage systems.

[0132] Figure 2 is a flow chart showing a method for preparing a positive active material according to another embodiment of the present invention.

[0133] Reference Figure 2 According to the present embodiment, the method for preparing a positive electrode active material includes: a step of preparing a metal solution (S210); a step of preparing a metal composite hydroxide through a coprecipitation reaction of the metal solution with an ammonia solution and a sodium hydroxide solution (S220); a step of preparing by crushing boron oxide into a first particle size (S230); a step of mixing the metal composite hydroxide, lithium hydroxide and the boron oxide of the first particle size, and pre-sintering the mixture for a first time in a first temperature range (S240); and a step of sintering the mixture for a second time in a second temperature range after the pre-sintering (S250), wherein the boron oxide is provided in the form of a powder, and the first particle size of the boron oxide powder can be in the range of 0.1 μm to 500 μm.

[0134] In the method for preparing a positive active material according to the present embodiment, in the step (S210) of preparing the metal solution, a metal solution including at least one of cobalt, manganese and aluminum and nickel may be prepared. In this regard, the metal solution may be provided to have one or more concentration ranges. For example, the metal solution may include a first metal solution composed of a metal combination using at least any one of the nickel, cobalt, manganese and aluminum and having a first concentration, and a second metal solution having a second concentration different from the first concentration. A metal composite hydroxide in which at least any one of nickel, cobalt, manganese and aluminum has a concentration gradient may be prepared using the first metal solution and the second metal solution.

[0135] In the step (S220) of preparing a metal composite hydroxide via a coprecipitation reaction, the metal solution can be used to prepare the metal composite hydroxide. The coprecipitation reaction can be carried out by continuously putting a metal solution, an ammonia solution and a sodium hydroxide solution into a coprecipitation reactor at different rates. In this regard, controlling the input rate and concentration of the metal solution, the ammonia solution and the sodium hydroxide solution can control the fine structure and shape of the primary particles and secondary particles constituting the metal composite hydroxide. The coprecipitation reaction can be carried out at 20°C to 60°C, preferably at 22°C to 47°C. In addition, the pH can be maintained at 10 to 12 during the coprecipitation reaction in the coprecipitation reactor.

[0136] Then, the prepared metal composite hydroxide can be filtered to remove liquid therefrom. After washing several times with distilled water, it can be made into a powder form by drying in a vacuum dryer. The temperature of the vacuum dryer can be in the range of 100°C to 160°C, preferably in the range of 100°C to 135°C.

[0137] In the step (S230) of preparing by crushing boron oxide into a first particle size, solid boron oxide (B2O3) can be used for preparation. The particle size can be controlled using a ball mill or the like. For example, the first particle size of boron oxide can be in the range of 0.1 μm to 500 μm. When the first particle size is less than 0.1 μm, the boron oxide particles may aggregate and be difficult to mix evenly with the metal composite hydroxide. When greater than 500 μm, there may be problems with not adhering to the metal composite hydroxide. Preferably, the first particle size can be in the range of 1 μm to 50 μm, more preferably in the range of 2 μm to 10 μm.

[0138] In the step (S240) of mixing and pre-sintering the metal composite hydroxide, lithium hydroxide and boron oxide, the metal composite hydroxide, lithium hydroxide and boron oxide may be first mixed for the first time. Thereafter, the pre-sintering may be performed by heating in a first temperature range and for a first time. The pre-sintering is preheated at a relatively low temperature before sintering with a high temperature, so that the electrochemical properties of the positive active material prepared by sintering can be further improved. The first temperature range may be 350°C to 500°C, and the first time may be 3 hours to 8 hours. Because the pre-sintering is performed in the first temperature range for the first time, the fine structure of the positive active material is controlled by subsequent sintering, so that the electrical characteristics can be further improved. In addition, boron controls the crystallinity of the primary particles on the surface of the positive active material, so that the movement path of the lithium ions can be more effectively formed. Preferably, the first temperature range may be 400°C to 500°C, and more preferably 410°C to 480°C. In addition, preferably, the first time may be 3 hours to 7 hours, and more preferably 4 hours to 6 hours.

[0139] Subsequently, a step (S250) of sintering for a second time in a second temperature range can be performed. The final positive active material doped with boron can be prepared by the sintering. The second temperature range is 700°C to 1000°C, and the second time can be 8 hours to 15 hours. When the second temperature range of the sintering step (S250) is lower than 700°C, the primary particles of the secondary particles constituting the positive active material are not arranged uniformly as a whole. When it exceeds 1000°C, part of the material evaporates, thereby reducing the process efficiency and causing problems. Preferably, the second temperature range can be 1.8 to 2.2 times the first temperature range.

[0140] Hereinafter, the present embodiment and comparative example of the present invention are described. However, the following embodiment is only a preferred embodiment of the present invention, and the right scope of the present invention is not limited to the following embodiment.

[0141] 1. Preparation of Examples and Comparative Examples

[0142] (1) Preparation of NCM-based positive electrode active materials

[0143] Example 1 (NCM65-B1)

[0144] 10 liters of distilled water were placed in a coprecipitation reactor (capacity 40L, output power of the rotary motor was 750W or more), and then N2 gas was supplied to the reactor at a rate of 6 liters / minute. Stirring was performed at 350rpm, while the temperature of the reactor was maintained at 45°C. Then, nickel sulfate aqueous solution (NiSO46H2O, Samchun Chemicals), cobalt sulfate aqueous solution (CoSO47H2O, Samchun Chemicals) and manganese sulfate aqueous solution (MnSO4H2O, Samchun Chemicals) were mixed in an amount of 65:15:20 molar ratio of nickel (Ni), cobalt (Co) and manganese (Mn) to prepare a metal solution with a concentration of 2M. The prepared metal solution was continuously added to the reactor at 0.561 liters / hour, ammonia solution (NH4OH, JUNSEI) with a concentration of 16M was continuously added to the reactor at 0.08 liters / hour, and sodium hydroxide solution (NaOH, Samchun Chemicals) with a concentration of 4M was continuously added to the reactor at 0.60 liters / hour for 24 hours. While the pH in the reactor is maintained in the range of 10 to 12, a coprecipitation reaction is performed to prepare Ni 0.65 Co 0.15 Mn 0.2 (OH)2 metal complex hydroxide.

[0145] The prepared Ni 0.65 Co 0.15 Mn 0.2 The (OH)2 metal composite hydroxide was filtered and washed several times with distilled water, and then dried in a vacuum dryer at 110°C for 12 hours to prepare a powder form. After preparing by grinding boron oxide (B2O3) into an average particle size of 50 μm using a ball mill, the powdered Ni 0.65 Co 0.15 Mn 0.2 (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed in a molar ratio of 0.99:0.005:1.01, heated at a heating rate of 2°C / min, and kept at 450°C for 5 hours for pre-sintering. Subsequently, it was sintered at 820°C for 10 hours to prepare a positive electrode active material powder (NCM65-B1) doped with 1 mol% boron (B). The content of each element of the prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer). Table 1 shows the B doping amount of the doping element, the molar ratio of metal (nickel (Ni), cobalt (Co) and manganese (Mn)) to ammonia in the process of preparing the metal composite hydroxide, and the sintering temperature.

[0146] Example 2 (NCM65-B1)

[0147] The positive active material powder (NCM65-B1) doped with 1 mol% boron (B) was prepared in the same manner as in Example 1, except for the following steps: During the preparation of the metal composite hydroxide, a 16M concentration of ammonia solution (NH4OH, JUNSEI) was continuously added to the coprecipitation reactor at 0.213 liters / hour to carry out the coprecipitation reaction. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 1.

[0148] Comparative Example 1 (NCM65)

[0149] The positive electrode active material powder (NCM65-B1) not doped with boron (B) was prepared in the same manner as in Example 1, except for the following steps: Ni 0.65 Co 0.15 Mn 0.2 The (OH)2 metal composite hydroxide and lithium hydroxide (LiOH) were mixed with each other at a molar ratio of 1:1.01 and pre-sintered. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 1.

[0150] Example 3 (NCM90-B0.4)

[0151] 10 liters of distilled water were placed in a coprecipitation reactor (capacity 40L, output power of the rotary motor was 750W or more), and then N2 gas was supplied to the reactor at a rate of 6 liters / minute. Stirring was performed at 350rpm, while the temperature of the reactor was maintained at 45°C. Then, nickel sulfate aqueous solution (NiSO46H2O, Samchun Chemicals), cobalt sulfate aqueous solution (CoSO47H2O, Samchun Chemicals) and manganese sulfate aqueous solution (MnSO4H2O, Samchun Chemicals) were mixed in an amount of nickel (Ni), cobalt (Co) and manganese (Mn) in a molar ratio of 90:5:5 to prepare a metal solution with a concentration of 2M. The prepared metal solution was continuously added to the reactor at 0.561 liters / hour, ammonia solution (NH4OH, JUNSEI) with a concentration of 16M was continuously added to the reactor at 0.08 liters / hour, and sodium hydroxide solution (NaOH, Samchun Chemicals) with a concentration of 4M was continuously added to the reactor at 0.60 liters / hour for 24 hours. While the pH in the reactor is maintained in the range of 10 to 12, a coprecipitation reaction is performed to prepare Ni 0.9 Co 0.05 Mn0.05 (OH)2 metal complex hydroxide.

[0152] The prepared Ni 0.9 Co 0.05 Mn 0.05 The (OH)2 metal composite hydroxide was filtered and washed several times with distilled water, and then dried in a vacuum dryer at 110°C for 12 hours to prepare a powder form. Boron oxide (B2O3) was crushed into an average particle size of 50 μm using a ball mill. The powdered Ni 0.9 Co 0.05 Mn 0.05 (OH)2 metal composite hydroxide, boron oxide (B2O3) particles and lithium hydroxide (LiOH) were mixed in a molar ratio of 0.996:0.002:1.01, heated at a heating rate of 2°C / min, and kept at 450°C for 5 hours. In this way, pre-sintering was carried out. Subsequently, it was sintered at 750°C for 10 hours to prepare a positive electrode active material powder (NCM65-B0.4) doped with 0.4 mol% boron (B). The prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer). Table 1 shows the B doping amount of the doping element, the molar ratio of metal (nickel (Ni), cobalt (Co) and manganese (Mn)) to ammonia in the process of preparing the metal composite hydroxide, and the sintering temperature.

[0153] Example 4 (NCM90-B1)

[0154] The positive electrode active material powder (NCM90-B1) doped with 1 mol% boron (B) was prepared in the same manner as in Example 3, except for the following steps: Ni 0.9 Co 0.05 Mn 0.05 (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed in a molar ratio of 0.99:0.005:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 1.

[0155] Example 5 (NCM90-B1)

[0156] The positive electrode active material powder (NCM90-B1) doped with 1 mol% boron (B) was prepared in the same manner as in Example 3, except that in the process of preparing the metal composite hydroxide, a 16M ammonia solution (NH4OH, JUNSEI) was continuously added to the coprecipitation reactor at 0.113 liters / hour to carry out a coprecipitation reaction, and the Ni prepared in powder form was0.9 Co 0.05 Mn 0.05 (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed in a molar ratio of 0.99:0.005:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 1.

[0157] Example 6 (NCM90-B1)

[0158] The positive electrode active material powder (NCM90-B1) doped with 1 mol% boron (B) was prepared in the same manner as in Example 3, except that in the following steps: during the preparation of the metal composite hydroxide, a 16 M ammonia solution (NH4OH, JUNSEI) was continuously added to the coprecipitation reactor at 0.146 L / h to perform a coprecipitation reaction, and the Ni prepared in powder form was 0.9 Co 0.05 Mn 0.05 (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed in a molar ratio of 0.99:0.005:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 1.

[0159] Example 7 (NCM90-B1)

[0160] The positive electrode active material powder (NCM90-B1) doped with 1 mol% boron (B) was prepared in the same manner as in Example 3, except that in the process of preparing the metal composite hydroxide, a 16M ammonia solution (NH4OH, JUNSEI) was continuously added to the coprecipitation reactor at 0.267 liters / hour to carry out a coprecipitation reaction, and the Ni prepared in powder form was 0.9 Co 0.05 Mn 0.05 (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed in a molar ratio of 0.99:0.005:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 1.

[0161] Comparative Example 2 (NCM90)

[0162] The positive electrode active material powder (NCM90) not doped with boron (B) was prepared in the same manner as in Example 3, except for the following steps: Ni 0.9 Co 0.05 Mn 0.05 The (OH)2 metal composite hydroxide and lithium hydroxide (LiOH) were mixed at a molar ratio of 1:1.01 and pre-sintered. The content of each element of the prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 1.

[0163] Example 8 (NCM92-B1)

[0164] 10 liters of distilled water were placed in a coprecipitation reactor (capacity 40L, output power of the rotary motor was 750W or more), and then N2 gas was supplied to the reactor at a rate of 6 liters / minute. Stirring was performed at 350rpm, while the temperature of the reactor was maintained at 45°C. Then, nickel sulfate aqueous solution (NiSO46H2O, Samchun Chemicals), cobalt sulfate aqueous solution (CoSO47H2O, Samchun Chemicals) and manganese sulfate aqueous solution (MnSO4H2O, Samchun Chemicals) were mixed in an amount of nickel (Ni), cobalt (Co) and manganese (Mn) in a molar ratio of 92:4:4 to prepare a metal solution with a concentration of 2M. The prepared metal solution was continuously added to the reactor at 0.561 liters / hour, ammonia solution (NH4OH, JUNSEI) with a concentration of 16M was continuously added to the reactor at 0.08 liters / hour, and sodium hydroxide solution (NaOH, Samchun Chemicals) with a concentration of 4M was continuously added to the reactor at 0.60 liters / hour for 24 hours. While the pH in the reactor is maintained in the range of 10 to 12, a coprecipitation reaction is performed to prepare Ni 0.92 Co 0.04 Mn 0.04 (OH)2 metal complex hydroxide.

[0165] The prepared Ni 0.92 Co 0.04 Mn 0.04 The (OH)2 metal composite hydroxide was filtered and washed several times with distilled water, and then dried in a vacuum dryer at 110°C for 12 hours to prepare a powder form. Boron oxide (B2O3) was crushed into an average particle size of 50 μm using a ball mill. The powdered Ni 0.92 Co 0.04 Mn 0.04After (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.99:0.005:1.01, they were heated at a heating rate of 2°C / min and pre-sintered at 450°C for 5 hours. Subsequently, it was sintered at 730°C for 10 hours to prepare a positive electrode active material powder (NCM92-B1) doped with 1 mol% boron (B). The content of each element of the prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer). Table 1 shows the B doping amount of the doping element, the molar ratio of metal (nickel (Ni), cobalt (Co) and manganese (Mn)) to ammonia in the process of preparing the metal composite hydroxide, and the sintering temperature.

[0166] Comparative Example 3 (NCM92)

[0167] The positive electrode active material powder (NCM92) not doped with boron (B) was prepared in the same manner as in Example 8, except for the following steps: Ni 0.92 Co 0.04 Mn 0.04 The (OH)2 metal composite hydroxide and lithium hydroxide (LiOH) were mixed at a molar ratio of 1:1.01 and pre-sintered. The content of each element of the prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 1.

[0168]

Table 1

[0169]

[0170]

[0171] (2) Preparation of LNO-based positive electrode active materials

[0172] Example 9 (LNO-B1)

[0173] 10 liters of distilled water are put into coprecipitation reactor (capacity 40L, the output power of rotary motor is 750W or greater), then N2 gas is supplied to reactor at a rate of 6 liters / minute. Stir with 350rpm, while the temperature of reactor is maintained at 45 ℃. Then, nickel sulfate aqueous solution (NiSO46H2O, Samchun Chemicals) is mixed with distilled water to prepare a metal solution with 2M concentration. The prepared metal solution is continuously added to reactor with 0.561 liters / hour, ammonia solution (NH4OH, JUNSEI) of 16M concentration is continuously added to reactor with 0.067 liters / hour, and sodium hydroxide solution (NaOH, Samchun Chemicals) of 4M concentration is continuously added to reactor with 0.60 liters / hour, continuing 24 hours. While the pH in the reactor is maintained at 10 to 12 range states, coprecipitation reaction is carried out to prepare Ni (OH)2 metal composite hydroxide.

[0174] The prepared Ni(OH)2 metal composite hydroxide was filtered and washed with distilled water several times, and then dried in a vacuum dryer at 110°C for 12 hours to prepare it in powder form. Boron oxide (B2O3) was crushed into an average particle size of 50μm using a ball mill for preparation. After the Ni(OH)2 metal composite hydroxide, boron oxide (B2O3) particles and lithium hydroxide (LiOH) prepared in powder form were mixed with each other in a molar ratio of 0.99:0.005:1.01, they were heated at a heating rate of 2°C / min and pre-sintered at 450°C for 5 hours. Subsequently, it was sintered at 650°C for 10 hours to prepare a positive active material powder (LNO-B1) doped with 1mol% boron (B). The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer). Table 1 shows the doping amount of B of the doping element, the molar ratio of metal (nickel (Ni)) to ammonia in the process of preparing the metal composite hydroxide, and the sintering temperature.

[0175] Example 10 (LNO-B1)

[0176] The positive active material powder (LNO-B1) doped with 1 mol% boron (B) was prepared in the same manner as in Example 9, except for the following steps: During the preparation of the metal composite hydroxide, a 16M concentration of ammonia solution (NH4OH, JUNSEI) was continuously added to the coprecipitation reactor at 0.13 liters / hour to carry out the coprecipitation reaction. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 2.

[0177] Example 11 (LNO-B1)

[0178] The positive active material powder (LNO-B1) doped with 1 mol% boron (B) was prepared in the same manner as in Example 9, except for the following steps: During the preparation of the metal composite hydroxide, a 16M concentration of ammonia solution (NH4OH, JUNSEI) was continuously added to the coprecipitation reactor at 0.2 liters / hour to carry out the coprecipitation reaction. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 2.

[0179] Example 12 (LNO-B1)

[0180] The positive active material powder (LNO-B1) doped with 1 mol% boron (B) was prepared in the same manner as in Example 9, except for the following steps: During the preparation of the metal composite hydroxide, a 16M concentration of ammonia solution (NH4OH, JUNSEI) was continuously added to the coprecipitation reactor at 0.26 liters / hour to carry out the coprecipitation reaction. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 2.

[0181] Comparative Example 4 (LNO)

[0182] The positive active material powder (LNO) not doped with boron (B) was prepared in the same manner as in Example 9, except for the following steps: During the preparation of the metal composite hydroxide, a 16M concentration of ammonia solution (NH4OH, JUNSEI) was continuously added to the reactor at 0.067 liters / hour to perform a coprecipitation reaction, and the Ni(OH)2 metal composite hydroxide prepared in powder form and lithium hydroxide (LiOH) were mixed with each other at a molar ratio of 1:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES and is shown in Table 2.

[0183]

Table 2

[0184]

[0185] (3) Preparation of NCO-based positive electrode active materials

[0186] Example 13 (NCO90-B0.05)

[0187] 10 liters of distilled water were placed in a coprecipitation reactor (capacity 40L, output power of the rotary motor was 750W or more), and then N2 gas was supplied to the reactor at a rate of 6 liters / minute. Stirring was performed at 350rpm, while the temperature of the reactor was maintained at 45°C. Then, an aqueous solution of nickel sulfate (NiSO46H2O, Samchun Chemicals) and an aqueous solution of cobalt sulfate (CoSO47H2O, Samchun Chemicals) were mixed in an amount of 9:1 molar ratio of nickel (Ni) and cobalt (Co) to prepare a metal solution with a concentration of 2M. The prepared metal solution was continuously added to the reactor at 0.561 liters / hour, an ammonia solution (NH4OH, JUNSEI) with a concentration of 16M was continuously added to the reactor at 0.11 liters / hour, and a sodium hydroxide solution (NaOH, Samchun Chemicals) with a concentration of 4M was continuously added to the reactor at 0.60 liters / hour for 24 hours. While the pH in the reactor was maintained in the range of 10 to 12, a coprecipitation reaction was performed to prepare Ni 0.9 Co 0.1 (OH)2 metal complex hydroxide.

[0188] The prepared Ni 0.9 Co 0.1 The (OH)2 metal composite hydroxide was filtered and washed with distilled water several times, and then dried in a vacuum dryer at 110°C for 12 hours to prepare a powder form. Boron oxide (B2O3) was crushed into an average particle size of 50 μm using a ball mill. The Ni prepared in powder form 0.9 Co 0.1 (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed in a molar ratio of 0.9995:0.00025:1.01, heated at a heating rate of 2°C / min, and kept at 450°C for 5 hours for pre-sintering. Subsequently, it was sintered at 730°C for 10 hours to prepare a positive electrode active material powder (NCO90-B0.05) doped with 0.05 mol% boron (B). ICP-OES (OPTIMA 8300, Perkin Elmer) was used to determine the content of each element in the prepared positive electrode active material powder. Table 3 shows the B doping amount of the doping element, the molar ratio of metal (nickel (Ni) and cobalt (Co)) to ammonia during the preparation of the metal composite hydroxide, and the sintering temperature.

[0189] Example 14 (NCO90-B0.1)

[0190] A positive electrode active material powder (NCO90-B0.1) doped with 0.1 mol% boron (B) was prepared in the same manner as in Example 13, except for the following steps: Ni0.9 Co 0.1 (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.999:0.0005:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 3.

[0191] Example 15 (NCO90-B0.5)

[0192] The positive electrode active material powder (NCO90-B0.5) doped with 0.5 mol% boron (B) was prepared in the same manner as in Example 13, except for the following steps: Ni 0.9 Co 0.1 (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.995:0.0025:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 3.

[0193] Example 16 (NCO90-B1)

[0194] A positive electrode active material powder (NCO90-B1) doped with 1 mol% boron (B) was prepared in the same manner as in Example 13, except for the following steps: Ni 0.9 Co 0.1 (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.99:0.005:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 3.

[0195] Example 17 (NCO90-B1.5)

[0196] A positive electrode active material powder (NCO90-B1.5) doped with 1.5 mol% boron (B) was prepared in the same manner as in Example 13, except for the following steps: Ni 0.9 Co 0.1(OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.985:0.0075:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 3.

[0197] Example 18 (NCO90-B2)

[0198] A positive electrode active material powder (NCO90-B2) doped with 2 mol% boron (B) was prepared in the same manner as in Example 13, except for the following steps: Ni 0.9 Co 0.1 (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.98:0.01:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA8300, Perkin Elmer) and is shown in Table 3.

[0199] Example 19 (NCO90-B3)

[0200] A positive electrode active material powder (NCO90-B3) doped with 3 mol% boron (B) was prepared in the same manner as in Example 13, except for the following steps: Ni 0.9 Co 0.1 (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.97:0.015:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA8300, Perkin Elmer) and is shown in Table 3.

[0201] Example 20 (NCO90-B4)

[0202] A positive electrode active material powder (NCO90-B4) doped with 4 mol% boron (B) was prepared in the same manner as in Example 13, except for the following steps: Ni 0.9 Co 0.1 (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.96:0.02:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 3.

[0203] Example 21 (NCO90-B5)

[0204] A positive electrode active material powder (NCO90-B5) doped with 5 mol% boron (B) was prepared in the same manner as in Example 13, except for the following steps: Ni 0.9 Co 0.1 (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.95:0.025:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA8300, Perkin Elmer) and is shown in Table 3.

[0205] Example 22 (NCO90-B0.5, Mo0.5)

[0206] A positive electrode active material powder (NCO90-B0.5, Mo0.5) doped with 0.5 mol% boron (B) and 0.5 mol% molybdenum (Mo) was prepared in the same manner as in Example 13, except for the following steps: Ni prepared in powder form was 0.9 Co 0.1 (OH)2 metal composite hydroxide, molybdenum trioxide (MoO3), boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.99: 0.005: 0.0025: 1.01. The content of each element of the prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 3.

[0207] Comparative Example 5 (NCO90)

[0208] The positive electrode active material powder (NCO90) not doped with boron (B) was prepared in the same manner as in Example 13, except for the following steps: Ni 0.9 Co 0.1 The (OH)2 metal composite hydroxide and lithium hydroxide (LiOH) were mixed with each other at a molar ratio of 1:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 3.

[0209] Comparative Example 6 (NCO90-B7)

[0210] A positive electrode active material powder (NCO90-B7) doped with 7 mol% boron (B) was prepared in the same manner as in Example 13, except for the following steps: Ni 0.9 Co 0.1(OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.93:0.035:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA8300, Perkin Elmer) and is shown in Table 3.

[0211]

Table 3

[0212]

[0213]

[0214] (4) Preparation of NCA-based positive electrode active materials

[0215] Example 23 (NCA88.5-B0.5)

[0216] 10 liters of distilled water were placed in a coprecipitation reactor (capacity 40L, output power of the rotary motor was 750W or more), and then N2 gas was supplied to the reactor at a rate of 6 liters / minute. Stirring was performed at 350rpm, while the temperature of the reactor was maintained at 45°C. Then, an aqueous solution of nickel sulfate (NiSO46H2O, Samchun Chemicals) and an aqueous solution of cobalt sulfate (CoSO47H2O, Samchun Chemicals) were mixed in an amount of nickel (Ni) and cobalt (Co) in a molar ratio of 9:1 to prepare a metal solution having a concentration of 2M. The prepared metal solution was continuously added to the reactor at 0.561 liters / hour, an ammonia solution (NH4OH, JUNSEI) with a concentration of 16M was continuously added to the reactor at 0.08 liters / hour, and a sodium hydroxide solution (NaOH, Samchun Chemicals) with a concentration of 4M was continuously added to the reactor at 0.60 liters / hour for 24 hours. While the pH in the reactor was maintained in the range of 10 to 12, a coprecipitation reaction was performed to prepare Ni 0.9 Co 0.1 (OH)2 metal complex hydroxide.

[0217] The prepared Ni 0.9 Co 0.1 The (OH)2 metal composite hydroxide was filtered and washed several times with distilled water, and then dried in a vacuum dryer at 110°C for 12 hours to prepare a powder form. Boron oxide (B2O3) was crushed into an average particle size of 50 μm using a ball mill. The Ni prepared in powder form 0.9 Co 0.1After (OH)2 metal composite hydroxide, aluminum hydroxide (Al(OH)3), boron oxide (B2O3) particles and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.98:0.015:0.0025:1.01, they were heated at a heating rate of 2°C / min and kept at 450°C for 5 hours for pre-sintering. Subsequently, it was sintered at 730°C for 10 hours to prepare a positive electrode active material powder (NCA88.5-B0.5) doped with 0.5 mol% boron (B). ICP-OES (OPTIMA 8300, Perkin Elmer) was used to determine the content of each element in the prepared positive electrode active material powder. Table 4 shows the B doping amount of the doping element, the molar ratio of metal (nickel (Ni) and cobalt (Co)) to ammonia during the preparation of the metal composite hydroxide, and the sintering temperature.

[0218] Example 24 (NCA88.5-B1)

[0219] A positive electrode active material powder (NCA88.5-B1) doped with 1 mol% boron (B) was prepared in the same manner as in Example 23, except that the following steps were performed: Ni 0.9 Co 0.1 (OH)2 metal composite hydroxide, aluminum hydroxide (Al(OH)3), boron oxide (B2O3) particles and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.975: 0.015: 0.005: 1.01. The content of each element of the prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 4.

[0220] Comparative Example 6 (NCA88.5)

[0221] The positive electrode active material powder (NCA88.5) not doped with boron (B) was prepared in the same manner as in Example 23, except for the following steps: Ni 0.9 Co 0.1 (OH)2 metal composite hydroxide, aluminum hydroxide (Al(OH)3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.985:0.015:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, PerkinElmer) and is shown in Table 4.

[0222] Example 25 (NCA80-B1)

[0223] 10 liters of distilled water were placed in a coprecipitation reactor (capacity 40L, output power of the rotary motor was 750W or more), and then N2 gas was supplied to the reactor at a rate of 6 liters / minute. Stirring was performed at 350rpm, while the temperature of the reactor was maintained at 45°C. Then, an aqueous solution of nickel sulfate (NiSO46H2O, Samchun Chemicals) and an aqueous solution of cobalt sulfate (CoSO47H2O, Samchun Chemicals) were mixed in an amount of 83:17 molar ratio of nickel (Ni) and cobalt (Co) to prepare a metal solution with a concentration of 2M. The prepared metal solution was continuously added to the reactor at 0.561 liters / hour, an ammonia solution (NH4OH, JUNSEI) with a concentration of 16M was continuously added to the reactor at 0.08 liters / hour, and a sodium hydroxide solution (NaOH, Samchun Chemicals) with a concentration of 4M was continuously added to the reactor at 0.60 liters / hour for 24 hours. While the pH in the reactor was maintained in the range of 10 to 12, a coprecipitation reaction was performed to prepare Ni 0.83 Co 0.17 (OH)2 metal complex hydroxide.

[0224] The prepared Ni 0.83 Co 0.17 The (OH)2 metal composite hydroxide was filtered and washed several times with distilled water, and then dried in a vacuum dryer at 110°C for 12 hours to prepare a powder form. Boron oxide (B2O3) was crushed into particles using a ball mill so that the average particle size was 50 μm. The Ni prepared in powder form 0.83 Co 0.17 (OH)2 metal composite hydroxide, aluminum hydroxide (Al(OH)3), boron oxide (B2O3) particles and lithium hydroxide (LiOH) are mixed with each other in a molar ratio of 0.95:0.04:0.005:1.01 to prepare a mixture. Then, the mixture is heated at a heating rate of 2°C / min and maintained at 450°C for 5 hours. In this way, preliminary sintering or pre-sintering is carried out. Subsequently, the pre-sintered mixture is sintered at 750°C for 10 hours to prepare a positive active material powder (NCA80-B1) doped with 1 mol% boron (B). ICP-OES (OPTIMA 8300, PerkinElmer) is used to determine the content of each element of the prepared positive active material powder. Table 4 shows the B doping amount of the doping element, the molar ratio of metal (nickel (Ni) and cobalt (Co)) to ammonia, and the sintering temperature during the preparation of the metal composite hydroxide.

[0225] Comparative Example 8 (NCA80)

[0226] The positive electrode active material powder (NCA80) not doped with boron (B) was prepared in the same manner as in Example 25, except for the following steps: Ni 0.83 Co 0.17 (OH)2 metal composite hydroxide, aluminum hydroxide (Al(OH)3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.96:0.04:1.01. The content of each element of the prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, PerkinElmer) and is shown in Table 4.

[0227]

Table 4

[0228]

[0229] (5) NMO-based positive electrode active material

[0230] Example 26 (NMO90-B0.5)

[0231] 10 liters of distilled water were placed in a coprecipitation reactor (capacity 40L, output power of the rotary motor was 750W or more), and then N2 gas was supplied to the reactor at a rate of 6 liters / minute. Stirring was performed at 350rpm, while the temperature of the reactor was maintained at 45°C. Then, an aqueous solution of nickel sulfate (NiSO46H2O, Samchun Chemicals) and an aqueous solution of manganese sulfate (MnSO4H2O, Samchun Chemicals) were mixed in an amount of nickel (Ni) and manganese (Mn) in a molar ratio of 9:1 to prepare a metal solution having a concentration of 2M. The prepared metal solution was continuously added to the reactor at 0.561 liters / hour, an ammonia solution (NH4OH, JUNSEI) with a concentration of 16wt% was continuously added to the reactor at 0.08 liters / hour, and a sodium hydroxide solution (NaOH, Samchun Chemicals) with a concentration of 4M was continuously added to the reactor at 0.60 liters / hour for 24 hours. While the pH in the reactor was maintained in the range of 10 to 12, a coprecipitation reaction was performed to prepare Ni 0.9 Mn 0.1 (OH)2 metal complex hydroxide.

[0232] The prepared Ni 0.9 Mn 0.1 The (OH)2 metal composite hydroxide was filtered and washed several times with distilled water, and then dried in a vacuum dryer at 110°C for 12 hours to prepare a powder form. Boron oxide (B2O3) was crushed into an average particle size of 50 μm using a ball mill. The Ni prepared in powder form 0.9 Mn 0.1After (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.995:0.0025:1.01, they were heated at a heating rate of 2°C / min and kept at 450°C for 5 hours for pre-sintering. Subsequently, it was sintered at 770°C for 10 hours to prepare a positive electrode active material powder (NMO90-B0.5) doped with 0.5 mol% boron (B). ICP-OES (OPTIMA 8300, PerkinElmer) was used to determine the content of each element in the prepared positive electrode active material powder. Table 5 shows the B doping amount of the doping element, the molar ratio of metal (nickel (Ni) and manganese (Mn)) to ammonia during the preparation of the metal composite hydroxide, and the sintering temperature.

[0233] Example 27 (NMO90-B1)

[0234] A positive electrode active material powder (NCM90-B1) doped with 1 mol% boron (B) was prepared in the same manner as in Example 26, except that the following steps were performed: Ni 0.9 Mn 0.1 (OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.99:0.005:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA8300, Perkin Elmer) and is shown in Table 5.

[0235] Comparative Example 9 (NMO90)

[0236] The positive electrode active material powder (NMO90) not doped with boron (B) was prepared in the same manner as in Example 26, except for the following steps: Ni 0.9 Mn 0.1 The (OH)2 metal composite hydroxide and lithium hydroxide (LiOH) were mixed with each other at a molar ratio of 1:1.01. The content of each element of the prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 5.

[0237]

Table 5

[0238]

[0239] (6) Preparation of concentration gradient positive electrode active materials

[0240] Example 28 (gradient NCM89-B1)

[0241] 10 liters of distilled water were placed in a coprecipitation reactor (capacity 40L, output power of the rotary motor was 750W or more), and then N2 gas was supplied to the reactor at a rate of 6 liters / minute. Stirring was performed at 350rpm, while the temperature of the reactor was maintained at 45°C. Then, a nickel sulfate aqueous solution (NiSO46H2O, Samchun Chemicals), a cobalt sulfate aqueous solution (CoSO47H2O, Samchun Chemicals) and a manganese sulfate aqueous solution (MnSO4H2O, Samchun Chemicals) were mixed with each other in an amount of 100:0:0 molar ratio of nickel (Ni), cobalt (Co) and manganese (Mn) to prepare a first metal solution having a concentration of 2M, and a second metal solution having a concentration of 2M was mixed with each other in an amount of 80:16:04 molar ratio of nickel (Ni), cobalt (Co) and manganese (Mn) to prepare a second metal solution having a concentration of 2M. The prepared first metal solution was continuously added to the reactor at 0.561 liters / hour, a 16M concentration ammonia solution (NH4OH, JUNSEI) was continuously added to the reactor at 0.08 liters / hour, and a 4M concentration sodium hydroxide solution (NaOH, Samchun Chemicals) was continuously added to the reactor at 0.60 liters / hour for 14 hours, thereby forming a first concentration holding portion. Thereafter, the second metal solution was added to the first metal solution water tank at 0.561 liters / hour to continuously add for 10 hours while constantly changing the concentration of the metal solution supplied to the reactor, forming a second concentration gradient portion on the outer contour of the first concentration holding portion. Thereafter, after stopping the addition of the second metal solution to the first metal solution, only the first metal solution with a changed concentration was added to the reactor at 0.561 liters / hour to form a third concentration gradient portion on the outer contour of the second concentration gradient portion. While the pH in the reactor was maintained in a state in the range of 10 to 12, a coprecipitation reaction was performed to prepare Ni 0.90 Co 0.08 Mn 0.02 A concentration gradient type metal composite hydroxide having an average composition of (OH)2.

[0242] The prepared Ni 0.90 Co 0.08 Mn 0.02 The (OH)2 concentration gradient metal composite hydroxide was filtered, washed several times with distilled water, and then dried in a vacuum dryer at 110°C for 12 hours to prepare a powder form. Boron oxide (B2O3) was crushed into an average particle size of 50 μm using a ball mill. The Ni prepared in powder form 0.90 Co 0.08 Mn 0.02(OH)2 metal composite hydroxide, boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.99:0.005:1.01, heated at a heating rate of 2°C / min, and pre-sintered at 450°C for 5 hours. Subsequently, it was sintered at 820°C for 10 hours to prepare a positive active material powder (NCM89-B1) doped with 1 mol% boron (B). The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA8300, Perkin Elmer). Table 6 shows the B doping amount of the doping element, the molar ratio of metal (nickel (Ni), cobalt (Co) and manganese (Mn)) to ammonia during the preparation of the metal composite hydroxide, and the sintering temperature.

[0243] Comparative Example 10 (NCM90)

[0244] 10 liters of distilled water were placed in a coprecipitation reactor (capacity 40L, output power of the rotary motor was 750W or more), and then N2 gas was supplied to the reactor at a rate of 6 liters / minute. Stirring was performed at 350rpm, while the temperature of the reactor was maintained at 45°C. Then, an aqueous solution of nickel sulfate (NiSO46H2O, Samchun Chemicals), an aqueous solution of cobalt sulfate (CoSO47H2O, Samchun Chemicals), and an aqueous solution of manganese sulfate (MnSO4H2O, Samchun Chemicals) were mixed with each other in an amount such that nickel (Ni), cobalt (Co), and manganese (Mn) became a 90:8:2 molar ratio, thereby preparing a metal solution having a concentration of 2M. The prepared metal solution was continuously added to the reactor at 0.561 liters / hour, an ammonia solution (NH4OH, JUNSEI) with a concentration of 16M was continuously added to the reactor at 0.08 liters / hour, and a sodium hydroxide solution (NaOH, Samchun Chemicals) with a concentration of 4M was continuously added to the reactor at 0.60 liters / hour for 24 hours. While the pH in the reactor is maintained in the range of 10 to 12, a coprecipitation reaction is performed to prepare Ni 0.90 Co 0.08 Mn 0.02 (OH)2 metal complex hydroxide.

[0245] The positive electrode active material powder (NCM90) not doped with boron (B) was prepared in the same manner as in Example 28, except for the following steps: Ni 0.90 Co 0.08 Mn 0.02The (OH)2 metal composite hydroxide and lithium hydroxide (LiOH) were mixed with each other at a molar ratio of 1:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 6.

[0246] Example 29 (Gradient NCA88.5-B1)

[0247] 10 liters of distilled water were placed in a coprecipitation reactor (capacity 40L, output power of the rotary motor was 750W or more), and then N2 gas was supplied to the reactor at a rate of 6 liters / minute. Stirring was performed at 350rpm, while the temperature of the reactor was maintained at 45°C. Then, a nickel sulfate aqueous solution (NiSO46H2O, Samchun Chemicals) and a cobalt sulfate aqueous solution (CoSO47H2O, Samchun Chemicals) were mixed with each other in an amount of 100:0 molar ratio of nickel (Ni) and cobalt (Co) to prepare a first metal solution with a concentration of 2M, and mixed with each other in an amount of 80:20 molar ratio to prepare a second metal solution with a concentration of 2M. The prepared first metal solution was continuously added to the reactor at 0.561 liters / hour, a 16M concentration ammonia solution (NH4OH, JUNSEI) was continuously added to the reactor at 0.08 liters / hour, and a 4M concentration sodium hydroxide solution (NaOH, Samchun Chemicals) was continuously added to the reactor at 0.60 liters / hour for 14 hours to prepare a first concentration holding portion. Thereafter, the second metal solution was added to the first metal solution tank at 0.561 liters / hour, and the addition was continued for 10 hours while the concentration of the metal solution supplied to the reactor was constantly changed, and a second concentration gradient portion was formed outside the first concentration maintenance portion. Thereafter, after the addition of the second metal solution to the first metal solution was stopped, only the first metal solution with a changed concentration was put into the reactor at 0.561 liters / hour to form a third concentration gradient portion outside the second concentration gradient portion. While the pH in the reactor was maintained in a range of 10 to 12, a coprecipitation reaction was performed to prepare Ni 0.90 Co 0.10 A concentration gradient type metal composite hydroxide having an average composition of (OH)2.

[0248] The prepared Ni 0.90 Co 0.10 The (OH)2 concentration gradient metal composite hydroxide was filtered, washed several times with distilled water, and then dried in a vacuum dryer at 110°C for 12 hours to prepare a powder form. After preparing by grinding boron oxide (B2O3) into an average particle size of 50 μm using a ball mill, the Ni0.90 Co 0.10 (OH)2 metal composite hydroxide, aluminum hydroxide (Al(OH)3), boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.975:0.015:0.005:1.01, heated at a heating rate of 2°C / min, and pre-sintered at 450°C for 5 hours. Subsequently, it was sintered at 700°C for 10 hours to prepare a positive electrode active material powder (NCA88.5-B1) doped with 1 mol% boron (B). The content of each element in the prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer). Table 6 shows the B doping amount of the doping element, the molar ratio of metal (nickel (Ni) and cobalt (Co)) to ammonia during the preparation of the metal composite hydroxide, and the sintering temperature.

[0249] Comparative Example 11 (NCA88.5)

[0250] 10 liters of distilled water were placed in a coprecipitation reactor (capacity 40L, output power of the rotary motor was 750W or more), and then N2 gas was supplied to the reactor at a rate of 6 liters / minute. Stirring was performed at 350rpm, while the temperature of the reactor was maintained at 45°C. Then, an aqueous solution of nickel sulfate (NiSO46H2O, Samchun Chemicals) and an aqueous solution of cobalt sulfate (CoSO47H2O, Samchun Chemicals) were mixed with each other in an amount such that nickel (Ni) and cobalt (Co) had a molar ratio of 90:10, thereby preparing a metal solution having a concentration of 2M. The prepared metal solution was continuously added to the reactor at 0.561 liters / hour, an ammonia solution (NH4OH, JUNSEI) having a concentration of 16M was continuously added to the reactor at 0.08 liters / hour, and a sodium hydroxide solution (NaOH, Samchun Chemicals) having a concentration of 4M was continuously added to the reactor at 0.60 liters / hour for 24 hours. While the pH in the reactor was maintained in the range of 10 to 12, a coprecipitation reaction was performed to prepare Ni 0.90 Co 0.10 (OH)2 metal complex hydroxide.

[0251] The positive electrode active material powder (NCA88.5) not doped with boron (B) was prepared in the same manner as in Example 29, except for the following steps: Ni 0.90 Co 0.10(OH)2 concentration gradient type metal composite hydroxide, aluminum hydroxide (Al(OH3)) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.985:0.015:1.01. The content of each element of the prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 6.

[0252] Comparative Example 12 (Gradient NCA88.5)

[0253] The positive electrode active material powder (gradient NCM89) not doped with boron (B) was prepared in the same manner as in Example 29, except for the following steps: Ni 0.90 Co 0.10 (OH)2 concentration gradient type metal composite hydroxide, aluminum hydroxide (Al(OH3)) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.985:0.015:1.01. The content of each element of the prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 6.

[0254]

Table 6

[0255]

[0256]

[0257] (7) Preparation of co-doping positive electrode active materials

[0258] Example 30 (NCO96-B0.5, Ta0.5)

[0259] 10 liters of distilled water were placed in a coprecipitation reactor (capacity 40L, output power of the rotary motor was 750W or more), and then N2 gas was supplied to the reactor at a rate of 6 liters / minute. Stirring was performed at 350rpm, while the temperature of the reactor was maintained at 45°C. Then, an aqueous solution of nickel sulfate (NiSO46H2O, Samchun Chemicals) and an aqueous solution of cobalt sulfate (CoSO47H2O, Samchun Chemicals) were mixed with each other in an amount such that nickel (Ni) and cobalt (Co) had a molar ratio of 96:4, thereby preparing a metal solution having a concentration of 2M. The prepared 2M concentration metal solution was continuously added to the reactor at 0.561 liters / hour, an ammonia solution (NH4OH, JUNSEI) with a concentration of 16M was continuously added to the reactor at 0.11 liters / hour, and a sodium hydroxide solution (NaOH, Samchun Chemicals) with a concentration of 4M was continuously added to the reactor at 0.60 liters / hour for 24 hours. While the pH in the reactor was maintained in the range of 10 to 12, a coprecipitation reaction was performed to prepare Ni 0.96 Co 0.04 (OH)2 metal complex hydroxide.

[0260] The prepared Ni 0.96 Co 0.04 The (OH)2 metal composite hydroxide was filtered, washed several times with distilled water, and then dried in a vacuum dryer at 110°C for 12 hours to prepare a powder form. 0.96 Co 0.04 (OH)2 metal composite hydroxide, tantalum pentoxide (Ta2O5), boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.99: 0.0025: 0.0025: 1.01, heated at a heating rate of 2°C / min, and kept at 450°C for 5 hours for pre-sintering. Subsequently, it was sintered at 730°C for 10 hours to prepare a positive active material powder (NCO96-B0.5, Ta0.5) doped with 0.5 mol% tantalum (Ta) and 0.5 mol% boron (B). ICP-OES (OPTIMA 8300, PerkinElmer) was used to determine the content of each element in the prepared positive active material powder. Table 7 shows the doping amount of the doping element, the molar ratio of the metal (nickel (Ni) and cobalt (Co)) to ammonia during the preparation of the metal composite hydroxide, and the sintering temperature.

[0261] Example 31 (NCO96-B0.5, Mo0.5)

[0262] A positive electrode active material powder (NCO96-B0.5, Mo0.5) doped with 0.5 mol% molybdenum (Mo) and 0.5 mol% boron (B) was prepared in the same manner as in Example 30, except that the following steps were performed: Ni 0.96 Co 0.04 (OH)2 metal composite hydroxide, molybdenum trioxide (MoO3), boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.99: 0.005: 0.0025: 1.01. The content of each element of the prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 7.

[0263] Example 32 (NCO96-B0.5, Nb0.5)

[0264] A positive electrode active material powder (NCO96-B0.5, Nb0.5) doped with 0.5 mol% niobium (Nb) and 0.5 mol% boron (B) was prepared in the same manner as in Example 30, except that the following steps were performed: Ni prepared in powder form was 0.96 Co 0.04 (OH)2 metal composite hydroxide, niobium pentoxide (Nb2O5), boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.99: 0.0025: 0.0025: 1.01. The content of each element of the prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 7.

[0265] Example 33 (NCO96-B0.5, Sb0.5)

[0266] A positive electrode active material powder (NCO96-B0.5, Sb0.5) doped with 0.5 mol% antimony (Sb) and 0.5 mol% boron (B) was prepared in the same manner as in Example 30, except that the following steps were performed: Ni 0.96 Co 0.04 (OH)2 metal composite hydroxide, antimony trioxide (Sb2O3), boron oxide (B2O3) and lithium hydroxide (LiOH) were mixed with each other in a molar ratio of 0.99: 0.0025: 0.0025: 1.01. The content of each element of the prepared positive electrode active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 7.

[0267] Comparative Example 13 (NCO96)

[0268] The positive electrode active material powder (NCO96) was prepared in the same manner as in Example 31, except for the following steps: Ni 0.96 Co 0.04 The (OH)2 metal composite hydroxide and lithium hydroxide (LiOH) were mixed with each other at a molar ratio of 1:1.01. The content of each element of the prepared positive active material powder was determined using ICP-OES (OPTIMA 8300, Perkin Elmer) and is shown in Table 7.

[0269] 2. Preparation of half-cells and full-cells using the examples and comparative examples

[0270] Half cells and full cells were prepared using Examples 1 to 33 and Comparative Examples 1 to 13, respectively.

[0271] In order to prepare half-cells and full cells, the positive active material in powder form (1 g basis) prepared according to Examples 1 to 33 and Comparative Examples 1 to 13, polyvinylidene fluoride (PVDF) and carbon black were added to 0.4 g of N-methyl pyrrolidone at a weight ratio of 90:4.5:5.5, respectively, and mixed uniformly to prepare positive electrode slurry. The prepared positive electrode slurry was coated on aluminum foil, the coating was roll-pressed, and then vacuum dried to prepare a positive electrode.

[0272] When a half-cell was prepared using the prepared positive active material, the positive electrode prepared as a slurry was coated on an aluminum foil to make a positive electrode so that the loading level of the positive active material was 5 mg / cm 2 (Indicates that when the aluminum foil coated with positive electrode active material is sampled into 1cm 2 square, the weight of only the positive electrode active material in the components of the positive electrode is 5 mg) ethylene carbonate and ethyl methyl carbonate (EC:EMC=3:7 v / v) are used as solvents, and 2 wt% vinylene carbonate (VC) as an additive and 1.2 mol / L LiPF6 as a lithium salt are uniformly dissolved therein as an electrolyte. o A 2032 coin-type half-cell (hereinafter, referred to as a coin cell) as a negative electrode.

[0273] When the prepared positive electrode active material is used to make a full battery, the positive electrode prepared as a slurry is coated on an aluminum foil to make a positive electrode, so that the loading level of the positive electrode active material is 8.5 mg / cm2 The graphite prepared as slurry was coated on copper foil so that its loading level was 6.5 mg / cm 2 , followed by rolling and then vacuum drying to make a negative electrode. Ethylene carbonate and ethyl methyl carbonate (EC:EMC=3:7v / v) were used as solvents, and 2wt% vinylene carbonate (VC) and lithium salt 1.2mol / LLiPF6 as additives were uniformly dissolved therein as electrolytes. The positive electrode, separator (Celgard, Model 2320) and negative electrode were stacked in a pouch-type battery case and sealed with the prepared electrolyte to make a pouch-type full battery.

[0274] 3. Evaluation of Examples, Comparative Examples and Preparation Examples

[0275] (1) Use half-cell to confirm capacity and cycle

[0276] The prepared half-cell was charged to 4.3 V and discharged to 2.7 V at a constant current of 0.5 C (100 mA / g) at 30° C., and 100 cycles were performed under the same conditions as the charge and discharge test to confirm the recovery capacity (hereinafter, 2.7 V-4.3 V) and shown in Table 7.

[0277]

Table 7

[0278]

[0279]

[0280]

[0281]

[0282] (2) Confirmation of the fine structure of the precursor and positive electrode active material using SEM

[0283] The fine structure of the metal composite hydroxide (precursor) before the positive electrode active material of the example and the comparative example was confirmed using SEM (Nova Nano SEM 450, FEI).

[0284] Figure 3 is the SEM image of the metal composite hydroxide according to Example 1 and Example 2, Figure 4 are SEM images of the positive electrode active materials according to Example 1 and Example 2.

[0285] exist Figure 3 and Figure 4When comparing (a) Example 1 and (b) Example 2, which are NCM-based positive electrode active materials with a Ni content of approximately 65 mol%, it can be confirmed that when the same content of metal (nickel, cobalt, manganese) is used, when the molar ratio of ammonia to metal increases from 1.2 to 3.2, the shape of the primary particles in the metal composite hydroxide before pre-sintering is different.

[0286] exist Figure 3 It can be confirmed that in the case of the metal composite hydroxide, in Example 1, the primary particles are separated from each other and have a flake shape, while in Example 2, a plurality of primary particles are combined to form an agglomerated form. Figure 4 It can be confirmed that in the top view of the primary particles of Example 1 and Example 2, the primary particles roughly have an angle on the corner side, as the positive electrode active material obtained by sintering with lithium hydroxide at a high temperature while doping with boron (B). In addition, it can be confirmed that the primary particles of Example 1 exist separately from each other, and in Example 2, the aggregation morphology of the primary particles observed in the metal composite hydroxide is also observed in the positive electrode active material after sintering.

[0287] In Table 7, when it is confirmed that the 0.1C discharge capacity of Example 1 and Example 2 is 200.7 mAh / g and 183.2 mAh / g, and the capacity retention after 100 cycles is 97.4% and 90%, in the case of Example 2 where the primary particles exist in an aggregated form, when the same content of nickel (Ni) is used and boron (B) is doped in the same manner, when the addition amount of ammonia relative to the metal is high, the discharge capacity and the capacity retention are lower than those of Example 1.

[0288] Figure 5 are SEM images of the metal composite hydroxides according to Examples 4 to 7, Figure 6 These are SEM images of the positive electrode active materials according to Examples 4 to 7.

[0289] exist Figure 5 It can be confirmed that when comparing the metal composite hydroxides of (a) Example 4, (b) Example 5, (c) Example 6 and (d) Example 7 which are NCM-based positive active materials with a Ni content of approximately 90 mol%, as the molar ratio of ammonia to metal (A / M) increases from 1.2 to 4, the primary particles exist in the metal composite hydroxide in an aggregated form and their size increases relatively.

[0290] Reference Figure 6, it can be confirmed that when (a) Example 4 and (b) Example 7 are compared with each other, the trend shown in the metal composite hydroxide is also reflected even after sintering after doping with 1 mol% of boron (B). Referring to Table 7, the 0.1C discharge capacity of Example 4, Example 5, Example 6 and Example 7 is 230.7mAh / g, 229.3mAh / g, 225.4mAh / g and 214.1mAh / g. The capacity retention rates after 100 cycles are 91.4%, 88.5%, 90.2% and 85.7%, respectively. It can be confirmed that in the case of 90mol% NCM-based positive electrode active material, only when the molar ratio of ammonia to metal is 4, the 0.1C discharge capacity decreases slightly, and the capacity retention rate after 100 cycles decreases slightly, and the molar ratio of ammonia to metal is less than 4, for example, it is almost the same when it is less than or equal to 2.2.

[0291] When the Comparative Example 1 and Example 1 including 65 mol% nickel (Ni) are compared with the Comparative Example 2 and Example 4 including 90 mol% nickel (Ni) in the case of preparing the NCM-based positive active material from the metal composite hydroxide, it can be confirmed that the discharge capacity of Comparative Example 2 and Example 4 is relatively high, which is summarized in the following Table 8. On the contrary, it can be confirmed that the 100 cycle capacity retention rate of Comparative Example 1 and Example 1 is relatively high. That is, it can be confirmed that the discharge capacity increases when the content of nickel (Ni) in the NCM-based positive active material increases, while the cycle characteristics decrease.

[0292] When Comparative Example 1 and Example 1 are compared with each other, and Comparative Example 2 and Example 4 are compared with each other, it can be confirmed that there is no significant difference in discharge capacity when boron (B) is doped at 1ml%, but the 100 cycle capacity retention rate is improved. In addition, it can be confirmed that it is more significant when the nickel content is 90mol%. In Example 1 and Example 4, the primary particles of the refined structure (Refined Structure) appearing in the positive electrode active material after sintering are clearly confirmed, while in Comparative Example 1 and Comparative Example 2, only spherical particles of irregular block agglomeration appear, and the primary particles with the same fine structure as the morphology observed in Example 1 and Example 4 cannot be clearly confirmed.

[0293] That is, due to the doped boron (B), the cycle characteristics of the NCM-based positive active material including nickel (Ni) are improved, and it can be confirmed that the effect is further increased as the content of nickel (Ni) increases. In addition, it is judged that this is because the doping of boron (B) improves the fine structure of the positive active material.

[0294]

Table 8

[0295]

[0296] Figure 7 are SEM images of the metal composite hydroxides according to Examples 9 to 12, Figure 8 are SEM images of the positive electrode active materials according to Examples 9 to 12.

[0297] Reference Figure 7 It can be confirmed that when the metal composite hydroxide is composed of 100 mol% Ni, as the molar ratio of ammonia to metal increases ((a) Example 9, (b) Example 10, (c) Example 11, (d) Example 12), the primary particles aggregate and shorten. On the other hand, Figure 8 As shown in the figure, it can be confirmed that (a) in Example 9, the thickness of the primary particles remains thin even after sintering, while in the case of (b) in Example 12, it can be confirmed that the primary particles melt to form a morphology in which multiple primary particles are aggregated with each other and microcracks are formed inside.

[0298] Referring to Table 7, it can be confirmed that the 0.1C discharge capacities of Examples 9 to 12 are 247.3 mAh / g, 248.2 mAh / g, 247.5 mAh / g, and 244.7 mAh / g, respectively, which remain similar. However, in terms of the capacity retention rate after 100 cycles, Example 12 in which the molar ratio of ammonia to metal is 4 is relatively poor.

[0299] That is, it can be confirmed that as the ratio of ammonia to metal in the LNO-based positive electrode active material increases, the primary particles of the metal composite hydroxide tend to aggregate with each other, and in the sintered positive electrode active material, when the molar ratio of ammonia to metal is 4, the primary particles melt, thereby increasing the thickness of the primary particles, so that the capacity retention characteristics after 100 cycles are also deteriorated. It is judged that in the case of Example 12, microcracks are generated in the center of the secondary particles during the sintering process, so the cycle characteristics are deteriorated.

[0300] Fig. 9 This is a SEM image measuring the thickness of primary particles located on the surface of secondary particles based on the boron (B) doping amount in the NCO-based positive electrode active material using a metal composite hydroxide containing 90 mol % of Ni. Fig.10 yes Fig. 9 SEM image of the positive electrode active material not doped with boron (B). Fig.11 yes Fig. 9 FIG. 5 is a SEM image of a positive electrode active material doped with 0.5 mol % of boron (B). Fig.12 yes Fig. 9 SEM image of the positive electrode active material doped with 1 mol% of boron (B), Fig.13 yes Fig. 9 SEM image of the positive electrode active material doped with 1.5 mol% of boron (B), Fig.14 yes Fig. 9FIG. 5 is an SEM image of a positive electrode active material doped with 2 mol % of boron (B).

[0301] Table 9 below shows Fig. 9 The thickness (third length) of the primary particles located on the surface of the secondary particles based on the amount of boron (B) doping in the NCO-based positive electrode active material using a metal composite hydroxide containing 90 mol% Ni ((003) plane average width [nm]), the value calculated based on the XRD data using the Scherrer equation using the (003) reflection, the presence or absence of a fine structure (Refined Structure), and the I(003) / I(104) ratio are shown in the figure.

[0302]

Table 9

[0303]

[0304] Reference Figures 9 to 14 As shown in Table 9, in the NCO-based positive electrode active material using a metal composite hydroxide containing 90 mol% Ni, as the boron (B) doping amount increases, the thickness gradually decreases. In Table 9, the third length of the interval between a pair of (003) planes and (003) planes of the primary particles located at the outermost surface of the primary particles constituting the secondary particles is measured, and its value ((003) plane average width [nm]) is shown.

[0305] Fig.15a is a graph showing the results of measuring the interval between the (003) plane and the (003) plane of the primary particle located at the surface of the secondary particle in the NCO-based positive electrode active material using a metal composite hydroxide containing 90 mol% Ni using a SEM image. Table 10 shows Fig.15a The mean, standard deviation, maximum, and minimum of the values ​​in . Fig.15b This is a graph showing the length of the (003) plane based on the amount of boron (B) doping. In the following, the unit of the length of the primary particle of the positive electrode active material is nm.

[0306]

Table 10

[0307]

[0308] Reference Fig.15aFrom Table 10, it can be confirmed that in the NCO-based positive electrode active material using a metal composite hydroxide containing 90 mol% Ni, as the doping amount of boron (B) increases, the average value of the third length decreases, and at the same time, the standard deviation of the third length decreases. In other words, it can be confirmed that by boron (B) doping, the third length of the primary particles located on the surface of the secondary particles in the primary particles is gradually reduced while being within the control range. In other words, it can be confirmed that doping with boron (B) reduces the third length and can control the third length within a predetermined range.

[0309] Referring to Table 10, it can be confirmed that Comparative Example 7, which is an NCA group not doped with boron (B), shows an average and standard deviation similar to those of Comparative Example 5, which is an NCO group. That is, it can be confirmed that the average and standard deviation of the third length of the primary particles located on the surface of the secondary particles in the primary particles are controlled according to the content of doped boron (B) regardless of the type of the positive electrode active material.

[0310] In addition, in Table 10, the grain size of the (003) plane ((003) plane grain size [nm]) is described, which is a value calculated by using the (003) reflection and applying the Scherrer's equation based on the XRD data. Fig.15b In FIG. 1 , the value measured using the SEM image (average width of the (003) plane [nm]) and the value calculated using the Scherrer equation (grain size of the (003) plane [nm]) are compared and shown as a graph.

[0311] Table 11 below shows the results of measuring the first length f1, the second length f2, and the third length f3 using SEM images. The first length f1 is the major axis of the (003) plane of the primary particle located at the surface of the secondary particle in the primary particle, the second length f2 is the minor axis of the (003) plane of the primary particle in the direction perpendicular to the first length f1, and the third length f3 is the distance between the (003) plane and the (003) plane. In Table 12, based on the average values ​​of the first length f1, the second length f2, and the third length f3, the ratio of the first length f1 to the third length f3 and the ratio of the second length f2 to the third length f3 are shown. Fig.16a is a graph showing a first length, a second length, and a third length based on boron (B) doping, and Fig.16b is a graph showing a first length and a ratio of a second length to a third length based on boron (B) doping.

[0312]

Table 11

[0313]

[0314]

Table 12

[0315] distinguish Comparative Example 5 Embodiment 15 Example 16 Embodiment 17 Embodiment 18 B doping B 0mol% B 0.5 mol% B 1mol% B 1.5 mol% B 2mol% f1 665.2 1230.3 1045.9 991.9 1102.4 f2 519.0 446.2 437.2 477.8 588.2 f3 351.3 145.8 55.5 40.6 30.0 f1 / f3 1.894 8.437 18.850 24.425 36.71 f2 / f3 1.478 3.060 7.881 11.764 19.583

[0316] Refer to Table 9 and Fig.15b , the value based on XDR data is equivalent to the overall average value of the primary particles constituting the secondary particles (dashed line, hereinafter, the value based on XRD). The value measured using the SEM image represents the measured value of the third length of the primary particles located on the surface of the secondary particles (solid line, hereinafter, the measured value). It can be confirmed that when 0 mol% of undoped boron (B) and 0.05 mol% of boron (B) are doped, the measured value is greater than the value based on XRD, and when boron (B) is doped at 0.5 mol%, 1 mol%, 1.5 mol% and 2 mol%, the measured value is less than the value based on XRD. Referring to the ratio of I(003) / I(104) obtained using XRD data in Table 9, it can be confirmed that the value decreases with the increase in the doping amount of boron (B). This is believed to be because the size of the primary particles is reduced due to the doping of boron (B), so the I(003) peak is relatively reduced.

[0317] Reference Figures 10 to 14 , it can be confirmed that as the doping amount of boron (B) increases, the third length of the primary particle gradually decreases. When viewed from the outside of the secondary particle, it can be confirmed that the cross-section of the primary particle has a roughly rectangular shape. That is, it can be confirmed that when the doping amount of boron (B) is 0mol%, the corners of the primary particle are unclear when confirmed from the top, and part of it exists in a curved surface form, and as the doping amount of boron (B) increases, the corners of the primary particle have an angular shape, and have a rectangular shape with a gradually decreasing third length.

[0318] Refer to Table 11 and Fig.16a It can be confirmed that in the NCO-based positive electrode active material, due to boron (B) doping, the second length f2 has no significant difference, and with respect to the first length f1, it increases until the boron (B) concentration reaches 0.5 mol%, but from then on it no longer changes and remains at a constant level. In addition, it can be confirmed that the third length decreases with the increase in the amount of boron (B) doping, but it no longer decreases from the addition of about 1.5 mol% of boron (B). In other words, it can be confirmed that the first length f1, the second length f2, and the third length f3 are all affected by boron (B) doping.

[0319] Refer to Table 12 and Fig.16b It can be confirmed that the ratio of the first length f1 to the third length f3 and the ratio of the second length f2 to the third length f3 are both increased. As for the increase degree, it can be confirmed that the slope of the ratio of the first length f1 to the third length f3 is larger.

[0320] In the following Table 13, the case where no boron (B) is doped in the NCO-based positive electrode active material (Comparative Example 5), the case where boron (B) is doped at 0.5 mol% (Example 15), the case where boron (B) is doped at 1 mol% (Example 16), and the case where boron (B) and molybdenum (Mo) are co-doped at 0.5 mol% respectively are confirmed.

[0321] It can be confirmed from the following Table 13 that Comparative Example 5, Example 15, Example 16, and Example 22 exhibit similar 0.1C discharge capacities. On the other hand, it can be confirmed that the capacity retention rate after 100 cycles of Comparative Example 5 not doped with boron (B) is 67.2%, which is lower than that of Examples 15, 16, and 22.

[0322] When comparing Example 15 doped with 0.5 mol% boron (B) and Example 22 doped with 0.5 mol% boron (B) and 0.5 mol% molybdenum (Mo), it can be confirmed that Example 22 has a greater capacity retention rate after 100 cycles than Example 15. In addition, when comparing Example 16 and Example 22 doped with 1 mol% boron (B), it can also be confirmed that when both are doped with 1 mol%, Example 22 has a greater capacity retention rate after 100 cycles than Example 16 with the same doping amount. In other words, it is believed that doping with molybdenum (Mo) while doping with boron (B) will enhance the effect of boron (B).

[0323]

Table 13

[0324]

[0325] Fig.17 are SEM images of the positive electrode active materials according to Example 24 and Comparative Example 7, Fig.18 are FIB TEM images of the positive electrode active materials according to Example 24 and Comparative Example 7. Fig.19 is a FIB TEM image of the positive electrode active materials according to Example 24 and Comparative Example 7 before the initial cycle, Fig. 20 yes Fig.19 FIBTEM image of Example 24 before initial cycling. Fig.21 This is the FIB TEM image of Example 24 after 100 cycles. Figure 22 to Figure 24 These are the results of analysis of the coating layer formed on the primary particles located on the surfaces of the secondary particles in Example 24. Fig.25 is a TEM image of the primary particles of Example 24. Figure 26 to Figure 28 These are the XRD analysis results of boron oxide and lithium hydroxide before and after heat treatment.

[0326] Referring to Table 9, in the case of preparing an NCA-based positive electrode active material using a metal composite hydroxide containing 88.5 mol% nickel (Ni), no refined structure was found in Comparative Example 7 without boron (B), but only in Examples 23 and 24 doped with 0.5 mol% and 1 mol% boron (B), respectively. The fine structure was found. In addition, the 0.1C discharge capacities of Comparative Example 7, Example 23, and Example 24 are similar to each other, that is, 225.1 mAh / h, 224 mAh / g, and 229.8 mAh / g, respectively. However, the capacity retention rates after 100 cycles are 83.7%, 92.2%, and 96.2%, respectively. It can be confirmed that the capacity increases with the increase in the amount of boron (B) doping.

[0327] Refer to Table 9. Fig.17 and Fig.18 It can be confirmed that in Comparative Example 7, the third length of the primary particle is relatively thick, while in Example 24, the third length of the primary particle is thin and the corners of the primary particle on the upper side have angles, and the cross section is rectangular. This is considered to be because, in the case of Example 24, due to boron (B) doping, the terminal parts of the primary particles located on the surface of the secondary particles in the primary particles are connected to each other via the crystal plane.

[0328] Fig.19 : is an enlarged FIB TEM image of the surface part of Comparative Example 7 and Example 24. In Comparative Example 7, the tip is rounded, while in Example 24, it has a morphology in which two crystal planes such as (012) plane and (014) plane are connected to each other.

[0329] Reference Fig. 20 and Fig.21 It can be confirmed that in Example 24, the (003) plane and the (003) plane of the primary particle located on the surface of the secondary particle face each other, and corresponding to the longitudinal section perpendicular to a pair of (003) planes and the two side crystal planes of the (003) plane, the (012) plane and the (014) plane are connected to form an angle with each other.

[0330] Reference Fig. 20 , it can be confirmed that in the case of Example 24, before the initial cycle, a pair of (003) faces of the primary particles located on the surface of the secondary particles in the primary particles are arranged parallel to each other, and the pair of (003) faces are connected via at least two crystal planes. Here, it can be confirmed that when the pair of (003) faces are cut vertically relative to the pair of (003) faces, the pair of (003) faces are connected via two different crystal planes. As above, Example 24 is composed of a pair of (003) faces and a plurality of crystal planes connecting the pair of (003) faces. As a result, the surface portion of the secondary particles forms a concave-convex.

[0331] Fig.21Secondary particles were confirmed after 100 cycles of Example 24. It was confirmed that Example 24 still had crystal planes after 100 cycles.

[0332] The positive electrode active material according to the present embodiment is doped with boron (B). Therefore, the third length of the thickness of the primary particle located at the surface portion of the secondary particle in the primary particle can be thin. In addition, it can be confirmed that in the positive electrode active material of the embodiment, in the top view of the secondary particle, the primary particle located at the surface portion of the secondary particle in the primary particle forms an angle in at least a part of the corner, and the primary particle arranged at the surface portion of the secondary particle is a different crystal plane and forms an angle along the surface cut from the surface portion of the secondary particle toward the center portion.

[0333] It can be confirmed that in the positive electrode active material according to the present embodiment, at the surface of the secondary particles, the ends are connected by two or more crystal planes, and the structure is maintained after multiple cycles. Therefore, in the positive electrode active material according to the embodiment, the crystal planes at the surface of the secondary particles are connected to each other, thereby preventing the electrolyte from easily immersing in the secondary particles. Therefore, the life characteristics of the battery can be improved. In addition, while the crystal planes are arranged, the primary particles are arranged in the direction toward the center of the secondary particles, so that lithium ions can easily move to the center of the secondary particles along the direction of the arrangement of the primary particles, and the formation of microcracks is suppressed during the charge and discharge process, thereby improving the electrochemical efficiency and improving the life characteristics.

[0334] Reference Figure 22 to Figure 25 and Fig.19 It was confirmed that, although it did not appear in Comparative Example 7, in Example 24, the outer surface of the surface portion also had a coating layer. When the coating layer formed in Example 24 was analyzed, it was confirmed that boron oxide was contained.

[0335] exist Fig. 22 In the embodiment of the present invention, it can be determined that the concentration of the boron (B) has a concentration gradient in the coating layer, but is uniform in the secondary particles. In addition, the average concentration of the boron (B) in the secondary particles can be within an error range of 0.05 mol% from the concentration of the boron (B) added to the composite metal hydroxide of 1 mol%.

[0336] For example, regarding the concentration of the boron (B), when the concentration of the boron (B) added to the composite metal hydroxide is Y1, the average concentration of the boron (B) in the secondary particles is Y2, and the average concentration of the boron (B) in the coating layer is Y3, it can be expressed by the following formulas 1 and 2.

[0337] (Formula 1) Y1-0.005≤Y2≤Y1+0.005

[0338] (Formula 2)Y2 <Y3

[0339] exist Figure 23 to Figure 25 In the embodiment, based on the result of confirming the surface portion of the secondary particles using TEM, it can be determined that the coating layer is provided to cover the second crystal plane and the third crystal plane of the first primary particle. Fig.23 and Fig.24 , it can be confirmed that the spacing between the crystal planes that do not occur in the secondary particles is 0.30nm, 0.28nm and 0.22nm to 0.24nm. It can be confirmed that this corresponds to the XRD results that appear when heat treatment is performed in the presence of a mixture of boron oxide and lithium hydroxide as follows (see Fig.26 and Fig.28 ).

[0340] That is, during the pre-sintering of the metal composite hydroxide, boron oxide and lithium hydroxide at 450°C, the boron oxide is uniformly contained in the secondary particles, and at the same time, a portion of the boron oxide chemically reacts with the lithium hydroxide on the surface of the secondary particles to form a coating layer. It is judged that the formation of the coating layer is comprehensively related to the second crystal plane and the third crystal plane formed on the surface of the secondary particles, the concentration of each substance constituting the positive electrode active material, the process of heat treatment thereof, and the pH controlled during the coprecipitation process.

[0341] Fig.29 3 is a cycle curve diagram of a full battery using the positive electrode active materials according to Example 24 and Comparative Example 7. Fig.30 are SEM images showing cross sections of secondary particles when the positive electrode active materials according to Example 24 and Comparative Example 7 were charged at different charging voltages. Fig.31 SEM images of half cells and full cells after cycling using the positive electrode active materials according to Example 24 and Comparative Example 7 are shown. Fig.32 and Fig.33 It is the in-situ XRD data of Example 24 and Comparative Example 7.

[0342] The full cells of Example 24 and Comparative Example 7 were cycled at 25°C with a constant current of 1C at 3.0V (discharge voltage) and 4.2V (charge voltage) (see Fig.29 ). The capacity of Example 24 did not change significantly until 1000 cycles, while the capacity of Comparative Example 7 decreased from 200 cycles. At 1000 cycles, Example 24 showed a capacity retention rate of 83.4%, while Comparative Example 7 showed a capacity retention rate of 49%. It can be confirmed that there is a difference in life characteristics.

[0343] Reference Fig.30, it can be confirmed that the result of charging while increasing the state of charge (SOC) at 3.9 V, 4.0 V, 4.1 V, 4.2 V and 4.2 V, Comparative Example 7 has weak wire drawing at 4.1 V, and micro cracks start to form from the center of the secondary particles at 4.2 V, and then at 4.3 V, the micro cracks extend to the surface of the secondary particles. On the contrary, it can be confirmed that Example 24 extends to the surface of the secondary particles at 4.3 V, but it is less than that of Comparative Example 7 at 4.1 V, and no micro cracks are formed.

[0344] For Comparative Example 7 and Example 24, the cross sections of the secondary particles charged to 4.3 V and then discharged to 4.1 V and the secondary particles charged to 4.3 V and discharged to 27 V were compared. It was confirmed that microcracks formed at 4.3 V also occurred only in the secondary particles of Comparative Example 7 charged to 4.3 V and then discharged to 4.1 V.

[0345] The positive electrode active material undergoes a continuous phase transition from H1 (hexagonal system 1) -> M (monoclinic system) -> H2 (hexagonal system 2) -> H3 (hexagonal system 3) during charging. The volume changes slowly until the voltage of 4.15V before the H2->H3 phase transition begins, but the volume of the 4.2V battery decreases sharply when the H2->H3 phase transition begins.

[0346] It was confirmed that after charging to 4.3V, which is the portion where the volume begins to change sharply, microcracks were formed in the fine structure of the secondary particles of Comparative Example 7 at 4.1V, but such a structure did not appear in Example 24. This is considered to be because in Example 24, even during the H2->H3 phase transition as described above, the primary particles were aligned in the secondary particles so that microcracks in the fine structure due to anisotropic volume change were not formed. In the case of Comparative Example 7, during the cycle, the volume change that occurred during the H2->H3 phase transition could not be fully recovered reversibly, and some of the residual irreversible parts accumulated, so cracks were formed in the secondary particles after the cycle (refer to Fig.32 and Fig.33 ).

[0347] Fig.31 SEM images of secondary particles after 100 cycles of a half cell and 1000 cycles of a full cell are shown, wherein the half cell and the full cell are prepared using Comparative Example 7 and Example 24. Fig.31 As shown in , it can be confirmed that microcracks are formed throughout the secondary particles in the case of Comparative Example 7, and in severe cases, the secondary particles are almost decomposed. However, it can be confirmed that the primary particle shape is almost maintained in both the half cell and the full cell of Example 24.

[0348] That is to say, in the case of Example 24, it is judged that the primary particles doped with boron (B) and formed during the preparation of the metal composite hydroxide are arranged to form secondary particles. For the primary particles located on the surface of the secondary particles among the primary particles, there is a coating layer on the surface and multiple crystal planes are formed. Therefore, its volume change is reversible during the charge and discharge process, so that microcracks do not occur, thereby improving the cycle characteristics.

[0349] The half-cell using the positive active material according to the embodiment and the comparative example as the positive electrode was cycled 100 times, wherein each cycle consisted of a 2.7V discharge at a constant current of 0.5C and a 4.3V charge at a constant current of 0.5C. Then, the peak intensity corresponding to the H2-H3 phase transition after 100 cycles relative to 1 cycle is shown. The intensity of the peak corresponding to the H2-H3 phase transition is confirmed using a curve obtained by first-order differentiation of the charge-discharge curve, that is, a dQ / dV curve.

[0350]

Table 14

[0351]

[0352] Referring to Table 14, it can be confirmed that the peak intensity corresponding to the H2-H3 phase transition after 100 cycles of Example 3 and Example 4 (H2 / H3 peak retention rate [%] after 100 cycles) is 73.4% and 82.7%, respectively, compared with that after 1 cycle. It can be confirmed that when Comparative Example 5, Comparative Example 6 and Examples 13 to 21 are compared with each other, Examples 13 to 21 are greater than or equal to 40%, while Comparative Example 5 has a low value of 38.1%. It can be confirmed that when Examples 13 to 19 are compared with each other, the value increases as the doping amount increases. That is, it can be confirmed that as the doping amount of boron increases, a structure similar to that after 1 cycle is maintained even after 100 cycles. In addition, it can be confirmed that a similar trend occurs when Comparative Example 7, Example 23 and Example 24 are compared with each other.

[0353] Table 15 below shows the codoping of adding boron and also adding other doping elements.

[0354]

Table 15

[0355]

[0356] Referring to Table 15, it can be confirmed that fine structures also appear in the case of co-doping of boron and molybdenum (Example 22), co-doping of boron and tantalum (Example 30, Example 32), co-doping of boron and niobium (Example 31), and co-doping of boron and antimony (Example 33). The capacity retention rate after 100 cycles is greater than or equal to 80%, which is better than the case of no boron doping.

[0357] It can be confirmed that when Comparative Example 5, Example 15, Example 16 and Example 22 are compared with each other, in the case of Ni 90mol%, the capacity retention rate is better as the boron content increases. Comparing Example 16 and Example 22, it can be confirmed that Example 22 co-doped with boron and molybdenum has a better capacity retention rate than Example 16 doped with only boron.

[0358] When Comparative Example 13 and Examples 30 to 33 are compared with each other, it can be confirmed that when co-doped with boron, a refined structure appears and an excellent capacity retention rate is exhibited even after 100 cycles, regardless of the type of the co-doped dopant.

[0359] Those skilled in the art will appreciate that the present invention may be implemented in other specific ways without changing its technical concept or essential features. Therefore, it should be understood that the embodiments described above are illustrative and non-restrictive in all respects. The scope of the present invention is indicated by the appended claims rather than the above detailed description, and the meaning and scope of the claims and all changes or deformations derived from their equivalent concepts are included in the scope of the present invention.

[0360] Reference numerals

[0361] 100: First primary particle

[0362] 110: First crystal plane

[0363] 120: Second crystal plane

[0364] 130: The third crystal plane

[0365] 200: Secondary particles

Claims

1. A positive electrode active material comprising secondary particles composed of aggregates of a plurality of primary particles, including first primary particles in which at least a portion of the primary particles disposed on the surface of the secondary particles are flake-shaped first primary particles having a pair of first crystal planes facing each other, The first crystal faces of the first primary particles are arranged in a radial direction, one end of the pair of first crystal faces has a plurality of crystal faces different from the first crystal faces to connect one end of the pair of first crystal faces, The longitudinal section of the first primary particle includes a pair of first crystal planes spaced apart from each other and a second crystal plane and a third crystal plane connecting one end of the pair of first crystal planes. The second crystal plane and the third crystal plane are arranged at the outermost surface of the secondary particle and are connected to form an angle; in, The angle between the second crystal plane and the third crystal plane is in the range of 30° to 170°; Wherein, the primary particles include nickel, M1 and M2, wherein said M1 is composed of at least any one of manganese, cobalt and aluminum, The nickel content is 65 mol% or more, The M2 is a doping element, and its content is 0.05mol% to 5mol%; wherein M2 is composed of boron and any one or more selected from tungsten, molybdenum, tantalum, niobium, hafnium, silicon, tin, zirconium, calcium, germanium, gallium, indium, ruthenium, tellurium, antimony, iron, chromium, vanadium and titanium; wherein the second crystal plane and the third crystal plane have a coating layer including boron covering at least a portion of the second crystal plane and the third crystal plane; wherein the boron concentration is uniform in the secondary particles and has a concentration gradient in the coating layer, wherein an average concentration of boron in the coating layer is higher than an average concentration of boron in the secondary particles; The coating layer includes LiBO2, LiB3O5, LiB5O8, Li2B2O4, Li2B2O7, Li2B4O7, Li2B6O7, Li2B6O 10 、Li2B8O 13 、Li3BO3、Li3B7O 12 、Li4B2O5、Li4B 10 O 17 and Li6B4O9.

2. The positive electrode active material according to claim 1, wherein the first primary particle has a first length as the major axis of the first crystal plane, a second length as the minor axis of the first crystal plane perpendicular to the first length, and a third length as the interval between the pair of first crystal planes, The third length is in the range of 10 nm to 400 nm. 3 . The positive active material according to claim 2 , wherein a ratio of the first length to the third length is in a range of 2 to 100, and a ratio of the second length to the third length is in a range of 1.5 to 80. 4 .

4. The positive electrode active material according to claim 2, wherein the positive electrode active material is a layered rhombohedral compound, The first crystal plane has Miller indices hkl, where h=0, k=0, l=3n, and n is an integer, The Miller index of the first crystal plane is different from those of the second crystal plane and the third crystal plane.

5. According to the positive electrode active material according to claim 1, after a 2032 coin-type half-cell made using the positive electrode active material as a positive electrode and lithium metal as a negative electrode is charged to 4.3V at a constant current of 0.5C and discharged to 2.7V at a constant current of 0.5C for 100 cycles, the intensity of the peak corresponding to the phase transition from H2 to H3 in the dQ / dV curve is 40% or more compared to 1 cycle.

6. The positive electrode active material according to claim 1, wherein in a cross-section of a secondary particle obtained by charging a half-cell using the positive electrode active material as a positive electrode and lithium metal as a negative electrode to 4.3 V at a constant current of 0.5 C, the area of microcracks as spaces formed between boundaries of adjacent primary particles is less than 15% of the cross-sectional area of the secondary particle.

7. The positive electrode active material according to claim 1, wherein in an X-ray diffraction analysis of the secondary particle measured at a scanning rate of 1 degree per minute with a step spacing of 0.0131 using a CuKa beam source of a device having an output of 45 kV and 40 mA, the intensity ratio of the 003 peak to the 104 peak is in the range of 1.6 to 2.

3.

8. The positive electrode active material according to claim 7, wherein as the content of the doping element increases, the intensity ratio of the 003 peak to the 104 peak decreases.

9. The positive electrode active material according to claim 1, wherein the secondary particle has a spherical shape including a central portion and a surface portion. The first crystal plane of the first primary particle is arranged in a direction from the central portion toward the surface portion. The second crystal plane and the third crystal plane in the first primary particle are arranged in the surface portion of the secondary particle, so that the outermost surface of the surface portion of the secondary particle forms an uneven structure through the second crystal plane and the third crystal plane.

10. The positive electrode active material according to claim 9, wherein the secondary particle is represented by the following <Chemical Formula 1>, and the surface portion of the secondary particle further includes a coating layer covering at least a part of the second crystal plane and the third crystal plane. <Chemical Formula 1> Li a M x D y O2 M is composed of Ni and at least any one selected from Co, Mn, and Al; D represents a doping element composed of co-doping of B and any one selected from W, Mo, Nb, Ta, and Sb, 0.9 < a < 1.1, and x + y = 1, and 0.95 < x < 1, 0 < y < 0.

05.

11. The positive electrode active material according to claim 10, wherein the first primary particle has a first length as the major axis of the first crystal plane, a second length as the minor axis of the first crystal plane perpendicular to the first length, and a third length as the interval between the pair of first crystal planes. The content of the doping element is in the range of 0.05 mol% to 5 mol%. As the concentration of the doping element increases, the first length of the first primary particle increases, and at the same time, the third length decreases.

12. A positive electrode for a secondary battery, comprising the positive electrode active material according to any one of claims 1 to 11.

13. A lithium secondary battery, comprising the positive electrode according to claim 12.

14. A battery module, comprising the lithium secondary battery according to claim 13 as a unit cell.

15. A battery pack, comprising the battery module according to claim 14. The battery pack is used as a power source for large and medium-sized devices. The large and medium-sized equipment is selected from any one of the following: an electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, and an electric power storage system.

Citation Information

Patent Citations

  • Precusor for lithium rich active material and lithium rich active material made by the same

    KR1020140119621A

  • Cathode active material for secondary battery, and secondary battery comprising same

    CN107925068A

  • Nickel-based active material for lithium secondary battery, preparing method thereof, and lithium secondary battery comprising positive electrode including nickel-based active material

    KR1020180010122A