A wet process for preparing non-shrinking tungsten skeleton
Through the wet preparation process, tungsten, molybdenum salt solution and hydrogen reduction technology are used to form a non-shrinkable tungsten skeleton, which solves the problem of size control in the preparation of existing tungsten skeletons and improves the consistency and quality stability of the product's chemical composition.
Patent Information
- Application Number
- CN202111485741.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-07
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-12-07
AI Technical Summary
The existing tungsten skeleton preparation method causes dimensional shrinkage due to the formation of sintered neck, which is difficult to control, resulting in inconsistent chemical composition of the product and affects the stability of quality.
The wet preparation process is used to immerse the degummed and pre-fired tungsten pressure blank in a solution containing tungsten and molybdenum salt. After drying, it is heated in a hydrogen atmosphere. The temperature is between 800-1100℃ to form a non-shrinkable tungsten skeleton. .
The precise control of the size of the tungsten skeleton is achieved, ensuring the uniform distribution of subsequent infiltration of metal elements, and significantly improving the consistency and quality stability of the product's chemical composition.
Smart Images

Figure CN114367664B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electric contacts or sweating materials, and in particular to a process for preparing a non-shrinking tungsten skeleton by a wet method. Background Art
[0002] The traditional preparation method of high-voltage electrical contacts or sweating materials is to use the melt infiltration method, that is, first prepare the skeleton and then infiltrate the metal elements. Tungsten is a metal element with a high melting point of 3410℃, and has good electrical and thermal conductivity. The price of tungsten raw materials is relatively cheap, so high-voltage electrical contacts and some sweating materials often use tungsten elements for skeleton preparation.
[0003] The preparation process of tungsten skeleton generally uses tungsten powder of a certain particle size as raw material, adds some activating substances and forming agents, presses into a certain shape of blank, and then sintered in a furnace. The sintering temperature of tungsten skeleton is relatively high. During the sintering process, tungsten atoms diffuse between tungsten powders to form sintering necks, so that metallurgical bonding is formed between tungsten powders, and a tungsten skeleton with a certain strength is obtained.
[0004] Since the sintering neck is formed by the gradual diffusion of tungsten atoms in the tungsten powder to the neck, the center distance between the original tungsten powder is shortened, causing the size of the green block to shrink, that is, the final tungsten skeleton size is smaller than the original green block size. Since the formation of the sintering neck is related to many factors, such as green compact pressure, sintering temperature, and the amount of activated material added, the final size of the tungsten skeleton is difficult to control.
[0005] The size of the tungsten skeleton is difficult to control, which results in that even if the same mass of tungsten powder is used to press out blocks of the same external size, after sintering, tungsten skeletons of different external sizes will be obtained due to different shrinkage rates. Tungsten skeletons of different sizes mean that different amounts of metal can be infiltrated, which directly leads to different chemical compositions and inconsistent performances of the same batch of infiltration products, resulting in unstable product quality. Some other related patents, such as CN 102747239 B, a method for manufacturing a copper-tungsten alloy with a tungsten skeleton, and CN104362015 B, a method for preparing a copper-tungsten contact material, will have problems such as inconsistent chemical compositions due to the difficulty in controlling the size of the tungsten skeleton. CN103981389B, a method for preparing a tungsten-copper alloy by low-temperature sintering of a tungsten skeleton, the main purpose of this patent is to ensure the formation of the connecting aperture of the tungsten skeleton by reducing the water vapor produced by blue tungsten with hydrogen, and to increase the density of the alloy after infiltration. Moreover, this patent does not adopt a wet method to prepare the tungsten skeleton, and due to the addition of a large amount of blue tungsten (5wt%-20wt% by mass), it can be reasonably inferred that the tungsten skeleton obtained by this method will undergo obvious volume shrinkage, which is completely different from the purpose of this patent. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the above-mentioned existing tungsten skeleton preparation method and provide a new tungsten skeleton preparation method, that is, a non-shrinkage tungsten skeleton preparation method. Since the tungsten skeleton prepared by the patent of the present invention hardly shrinks during the sintering process, the size of the billet has almost the same external dimensions as the final tungsten skeleton, that is, after the same mass of tungsten powder is pressed into billets of the same external dimensions, the sintered tungsten skeleton has the same external dimensions. This will ensure that the same volume in the tungsten skeleton is used to infiltrate metal elements, such as copper, to form a tungsten-copper alloy with the same chemical composition, thereby significantly improving the consistency of the chemical composition and quality stability of the infiltration product.
[0007] In order to prepare a non-shrinking tungsten skeleton, the present invention adopts the following technical scheme:
[0008] The debonded and pre-sintered tungsten compact is immersed in a tungsten and molybdenum salt solution, taken out after a certain period of time and heated and dried, and then heated in a hydrogen atmosphere at a temperature between 800-1100°C to form a non-shrinking tungsten skeleton. The specific process flow is as follows: prepare tungsten and molybdenum salt solution → immersion → take out → drying → reduction.
[0009] A process for preparing a non-shrinking tungsten skeleton by a wet method, characterized in that: the process for preparing a non-shrinking tungsten skeleton by a wet method comprises the following steps: immersing the debonded and pre-sintered tungsten compact in a solution containing tungsten and molybdenum salts, taking it out and heating and drying it, and then heating it in a hydrogen atmosphere at a temperature between 800-1100° C., so as to form a non-shrinking tungsten skeleton;
[0010] The debonding and pre-sintering of tungsten compacts can be completed in the same furnace, either in nitrogen or vacuum, with the pre-sintering temperature being less than 800°C.
[0011] The salt solution of tungsten and molybdenum is prepared by dissolving sodium tungstate, ammonium metatungstate or ammonium molybdate, ammonium metamolybdate in distilled water. The concentration of the salt solution is determined according to the content of tungsten or molybdenum to be added. The content of tungsten or molybdenum salt is 0.5-5%.
[0012] The tungsten compact is immersed in the salt solution for 10-30 minutes, which varies according to the bulk density, size and shape complexity of the tungsten compact to ensure that the salt solution fully wets the tungsten compact.
[0013] A thickener can be added to the salt solution to ensure that when the tungsten compact is fished out, it contains a higher quality of tungsten and molybdenum salt solution.
[0014] The drying temperature is between 100-200°C, the salt solution is precipitated in the tungsten compact, and then dried in the air.
[0015] The hydrogen reduction temperature is between 800-1100°C.
[0016] In a hydrogen atmosphere, the dew point of hydrogen is -50 to -20 degrees.
[0017] The principle of the non-shrinkage of the tungsten skeleton is as follows: the tungsten compact immersed in tungsten or molybdenum salt solution will precipitate salt during drying. When heated in a hydrogen furnace, the tungsten salt or molybdenum salt undergoes a reduction reaction, and the reduced tungsten atoms or molybdenum atoms are deposited near the contact points between the tungsten particles. The radius of curvature at the contact points is small, which is conducive to the deposition of tungsten or molybdenum atoms. These deposited tungsten atoms or molybdenum atoms connect the tungsten particles to form a sintering neck, that is, a metallurgical bond is generated to form a tungsten skeleton. Since the sintering neck of the tungsten skeleton of the present invention is formed by tungsten or molybdenum atoms in the salt, and not by tungsten atoms in the tungsten particles through diffusion, and the reduction temperature is relatively low, the center distance between the tungsten powders does not change significantly, that is, no shrinkage occurs. This result has been confirmed by experiments, see attached. Figure 1-2 .
[0018] Advantages of the present invention:
[0019] The wet method for preparing a non-shrinking tungsten skeleton of the present invention can accurately control the amount of tungsten or molybdenum added to the tungsten compact by controlling the concentration of the tungsten or molybdenum salt solution in the solution and the immersion time, and the precipitate is evenly distributed at the connection of the tungsten particles, ensuring that the strength of the tungsten skeleton is uniform everywhere. The present invention reduces the formation temperature of the tungsten skeleton, has a simple process, and because the tungsten skeleton does not shrink, the subsequent infiltration metal content can be accurately controlled, greatly improving the chemical composition and performance consistency of the infiltration product. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments:
[0021] Figure 1 This is a scanning electron microscope photo of a tungsten skeleton prepared by a wet method, low magnification;
[0022] Figure 2 This is a scanning electron microscope photo of the wet-prepared tungsten skeleton, high magnification. Specific embodiments
[0023] A wet process for preparing a non-shrinking tungsten skeleton, the preparation process is as follows: prepare tungsten and molybdenum salt solutions → immerse → fish out → dry → reduce. Compared with the traditional tungsten skeleton, the patented feature of the present invention is that the tungsten compact is immersed in a tungsten and molybdenum salt solution, then fished out and produces tungsten and molybdenum salt precipitates during drying, and then reduced by hydrogen (the reduction temperature is between 800-1100°C), and tungsten atoms or molybdenum atoms are deposited near the contact points between the tungsten particles, and a tungsten skeleton is formed by gradual diffusion. Since the tungsten skeleton formation temperature is low, the skeleton hardly shrinks. The concentration of the salt solution prepared in the present invention has a certain relationship with the bulk density and the shape of the tungsten compact, and the amount of tungsten salt or molybdenum salt added is about 0.5-5% of the skeleton mass. This non-shrinking tungsten skeleton brings great convenience to the accurate control of the infiltration metal content in the subsequent infiltration stage.
[0024] The non-shrinkable tungsten skeleton of the present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0025] Embodiment 1: The rapid preparation method of the wet non-shrinking tungsten skeleton process of this embodiment is:
[0026] The mass of the tungsten compact is 100 g and the volume is about 10 cm3. 10 g of ammonium metatungstate powder is added to 100 ml of distilled water to prepare a salt solution.
[0027] The tungsten compact was immersed in the salt solution for 10 minutes.
[0028] After the tungsten compact is taken out, it is heated and dried in air at a temperature of 120°C for 1 hour.
[0029] The dried tungsten compact is reduced in a hydrogen atmosphere with a hydrogen dew point of -20°C and a reduction temperature of 800°C to obtain a non-shrinking tungsten skeleton. The morphology of the tungsten skeleton is shown in the attached Figure 1 In the scanning electron microscope photo, the size of the tungsten skeleton is almost the same as the size of the blank after molding.
[0030] Example 2: The rapid preparation method of the non-shrinking tungsten skeleton in this example is:
[0031] The mass of the tungsten pressed blank is 200 g and the volume is about 20 cm3. 10 g of ammonium metatungstate and ammonium molybdate powder are added to 100 ml of distilled water to prepare a salt solution.
[0032] The tungsten compact was immersed in the salt solution for 15 minutes.
[0033] After the tungsten compact is taken out, it is heated and dried in air at a temperature of 150°C for 1 hour.
[0034] The dried tungsten compact is reduced in a hydrogen atmosphere with a hydrogen dew point of -30°C and a reduction temperature of 900°C to obtain a non-shrinking tungsten skeleton.
[0035] Embodiment 3: The rapid preparation method of the non-shrinking tungsten skeleton of this embodiment is:
[0036] The mass of the tungsten compact is 300 g and the volume is about 30 cm3. 30 g of ammonium metatungstate powder is added to 100 ml of distilled water to prepare a salt solution.
[0037] The tungsten compact was immersed in the salt solution for 20 minutes.
[0038] After the tungsten compact is taken out, it is heated and dried in air at a temperature of 180°C for 1 hour.
[0039] The dried tungsten compact is reduced in a hydrogen atmosphere with a hydrogen dew point of -40°C and a reduction temperature of 1000°C to obtain a non-shrinking tungsten skeleton.
[0040] Embodiment 4: The rapid preparation method of the non-shrinking tungsten skeleton of this embodiment is:
[0041] The mass of the tungsten compact is 400 g and the volume is about 40 cm3. 40 g of ammonium molybdate powder is added to 100 ml of distilled water to prepare a salt solution.
[0042] The tungsten compact was immersed in the salt solution for 20 minutes.
[0043] After the tungsten compact is fished out, it is heated and dried in air at a temperature of 200° C. for 1 hour.
[0044] The dried tungsten compact is reduced in a hydrogen atmosphere with a hydrogen dew point of -40°C and a reduction temperature of 1100°C to obtain a non-shrinking tungsten skeleton.
[0045] The above content is a further detailed description of the present invention in combination with specific preferred embodiments. It cannot be determined that the specific embodiments of the present invention are limited to these. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as belonging to the scope of patent protection determined by the submitted claims of the present invention.
Claims
1. A wet process for preparing a non-shrinking tungsten skeleton, characterized in that: The wet method for preparing a non-shrinking tungsten skeleton comprises the following steps: immersing the debonded and pre-sintered tungsten compact into a tungsten or molybdenum salt solution, taking it out and heating and drying it, and then heating it in a hydrogen atmosphere at a temperature between 800-1100° C., thereby forming a non-shrinking tungsten skeleton; Tungsten compact debonding and pre-sintering can be completed in the same furnace, either in nitrogen or vacuum, with a pre-sintering temperature of less than 800°C; Tungsten or molybdenum salt solution is prepared by dissolving sodium tungstate, ammonium metatungstate or ammonium molybdate, ammonium metamolybdate in distilled water. The concentration of the salt solution is determined according to the content of tungsten or molybdenum to be added. The content of tungsten or molybdenum salt is 0.5-5%; The tungsten compact is immersed in the salt solution for 10-30 minutes, which varies according to the bulk density, size and shape complexity of the tungsten compact to ensure that the salt solution fully wets the tungsten compact; A thickener can be added to the salt solution; The drying temperature is between 100-200°C, the salt solution is precipitated in the tungsten compact, and then dried in the air; In a hydrogen atmosphere, the dew point of hydrogen is -50 to -20 degrees.