A method for synthesizing linear alpha-olefins from synthesis gas

By using a composite catalyst of iron-based and nickel-based or cobalt-based catalysts in syngas, the problem of low selectivity of high-carbon linear α-olefins in the traditional syngas conversion process is solved, and high selectivity and efficient linear α-olefins are achieved. Production, especially products with carbon numbers of 6-15.

CN114369002BActive Publication Date: 2024-10-29PETROCHINA CO LTD +1
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202011098273.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-14
Publication Date
2024-10-29
Estimated Expiration
2040-10-14

Smart Images

  • Figure CN114369002B_ABST
    Figure CN114369002B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for synthesizing linear alpha-olefins from synthesis gas, and its purpose is to solve the problem of low selectivity of high-carbon linear alpha-olefins in the traditional synthesis gas conversion process. The method for synthesizing linear alpha-olefins from synthesis gas provided by the present invention comprises the following steps: under the conditions of 200-380°C and 0.5-5.0MPa, the synthesis gas is passed through a pretreated composite catalyst to synthesize linear alpha-olefins with a carbon number of 6 to 15; wherein the composite catalyst comprises a two-stage catalyst, the first-stage catalyst is an iron-based catalyst, and the iron-based catalyst uses iron oxide and / or iron-containing carbide as an active component; the second-stage catalyst is a nickel-based catalyst or a cobalt-based catalyst, the nickel-based catalyst uses nickel oxide as an active component, and the cobalt-based catalyst uses cobalt oxide as an active component.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for synthesizing olefins from synthesis gas, in particular to a method for synthesizing linear alpha-olefins from synthesis gas. Background Art

[0002] Olefins refer to hydrocarbons containing C=C bonds, alpha-olefins refer to monoolefins with C=C bonds at the ends of the molecular chains, and linear alpha-olefins (LAO) refer to alpha-olefins with linear alkyl groups connecting the C=C bonds. LAO has a wide range of uses in many fields, such as comonomers, surfactants, additives, etc. Among them, linear alpha-olefins with carbon numbers of 6-15 are the most widely used. At present, alpha-olefins are mainly produced by petroleum routes, mainly by using Ni-based catalysts to polymerize ethylene. The production of alpha-olefins from non-petroleum resources has become a research direction that has attracted much attention.

[0003] As a process for producing olefins from non-petroleum resources, syngas to olefins has been widely studied. There are two main routes. One is the synthesis of olefins from syngas via methanol. Currently, this technology has been industrialized, but the olefins synthesized by this technology are mostly low-carbon olefins such as ethylene and propylene. The other route is the direct synthesis of olefins from syngas via Fischer-Tropsch synthesis. Compared with the route of synthesizing olefins from syngas via methanol, the product selectivity of this route follows the ASF distribution, and the carbon number distribution of olefin products is relatively wide, and the selectivity of both low-carbon olefins and high-carbon olefins is relatively low. At present, there are few reports in the literature on the direct production of high-value-added LAOs from syngas, especially the synthesis of LAOs with carbon numbers between 6 and 15.

[0004] On this basis, the present invention proposes a method for converting syngas into high-carbon linear α-olefins on a composite catalyst composed of two-stage catalysts. The method can realize the direct and highly selective synthesis of LAO from syngas, especially LAO with a carbon number of 6-15, and provides a new idea for the effective synthesis of non-petroleum resources. Summary of the invention

[0005] The purpose of the present invention is to solve the problem of low selectivity of high-carbon linear α-olefins in the traditional synthesis gas conversion process and provide a method for directly and effectively synthesizing high-carbon linear α-olefins from synthesis gas.

[0006] To this end, the present invention provides a method for synthesizing linear α-olefins from synthesis gas, characterized in that it comprises the following steps:

[0007] Under the conditions of 200-380°C and 0.5-5.0MPa, the synthesis gas is passed through the pretreated composite catalyst to synthesize linear α-olefins with a carbon number of 6 to 15;

[0008] The composite catalyst comprises two-stage catalysts, wherein the first-stage catalyst is an iron-based catalyst, and the iron-based catalyst has iron oxide and / or iron-containing carbide as active components; the second-stage catalyst is a nickel-based catalyst or a cobalt-based catalyst, and the nickel-based catalyst has nickel oxide as an active component, and the cobalt-based catalyst has cobalt oxide as an active component.

[0009] As can be seen from the above, the present invention uses synthesis gas at a specific temperature and pressure to synthesize high-carbon linear α-olefins with high selectivity through a two-stage catalyst.

[0010] In the method for synthesizing linear α-olefins from synthesis gas of the present invention, it is preferred that the iron-containing oxide is ferrosoferric oxide and / or ferrous oxide, more preferably ferrosoferric oxide; and the iron-containing carbide is iron carbide.

[0011] In the method for synthesizing linear α-olefins from synthesis gas of the present invention, it is preferred that the iron-containing oxide is generated by reducing a precursor, and the molar ratio of Fe(III) to Fe(II) in the precursor is 1 / 5 to 8 / 1, more preferably 1 / 3 to 5 / 1.

[0012] In the method for synthesizing linear α-olefins from synthesis gas of the present invention, it is preferred that the iron-based catalyst further comprises an additive and a carrier, wherein the content of iron is 30%-90% based on the total mass of oxides and carbides, the content of the additive is 0.8%-15%, and the content of the carrier is the balance.

[0013] In the method for synthesizing linear α-olefins from synthesis gas of the present invention, it is preferred that the carrier is an inorganic oxide and its content does not exceed 30% of the total mass of the iron-based catalyst, and the carrier includes at least one of alumina and molecular sieve.

[0014] In the method for synthesizing linear α-olefins from synthesis gas of the present invention, preferably, the auxiliary agent comprises 0.3%-7% of alkali metal auxiliary agent and 0.5%-8% of transition metal auxiliary agent.

[0015] In the method for synthesizing linear α-olefins from synthesis gas of the present invention, it is preferred that the nickel oxide is partially reduced nickel oxide, and more preferably nickelous oxide.

[0016] In the method for synthesizing linear α-olefins from synthesis gas of the present invention, preferably, the nickel-based catalyst also includes an additive and a carrier, wherein the nickel content is 0.1%-15% by mass of the oxide, the additive content is 0-10%, and the carrier content is above 70%, more preferably above 75%.

[0017] In the method for synthesizing linear α-olefins from synthesis gas of the present invention, it is preferred that the auxiliary agent is selected from at least one of Co, Zn and Mo; and the carrier comprises at least one of alumina and molecular sieve.

[0018] In the method for synthesizing linear α-olefins from synthesis gas of the present invention, it is preferred that the cobalt oxide is partially reduced cobalt oxide, and more preferably cobaltous oxide.

[0019] In the method for synthesizing linear α-olefins from synthesis gas of the present invention, it is preferred that the cobalt-based catalyst also includes an additive and a carrier, wherein the content of cobalt is 0.1%-15% by mass of the oxide, the content of the additive is 0-10%, and the content of the carrier is above 70%, and more preferably above 75%.

[0020] In the method for synthesizing linear α-olefins from synthesis gas of the present invention, it is preferred that the auxiliary agent is selected from at least one of Ni, Zn and Mo; and the carrier comprises at least one of alumina and molecular sieve.

[0021] In the method for synthesizing linear α-olefins from synthesis gas of the present invention, preferably, the filling mass ratio of the first-stage catalyst to the second-stage catalyst is 1:5-5:1, more preferably 1:1-3:1, and the filling method of the first-stage catalyst and the second-stage catalyst is mixed particle filling or layered filling.

[0022] In the method for synthesizing linear α-olefins from synthesis gas of the present invention, it is preferred that the first-stage catalyst and the second-stage catalyst are filled in layers without contact with each other.

[0023] In the method for synthesizing linear α-olefins from synthesis gas of the present invention, preferably, the pretreatment is a reducing gas treatment, the treatment temperature of the first stage catalyst is 250-380°C, and the treatment temperature of the second stage catalyst is 180-250°C.

[0024] In the method for synthesizing linear α-olefins from synthesis gas described in the present invention, it is preferred that the reducing gas used for the reducing gas treatment of the first-stage catalyst is H2 or CO, the hydrogen treatment temperature of the first-stage catalyst is 280-380°C, and the CO treatment temperature is 250-350°C; the reducing gas used for the reducing gas treatment of the second-stage catalyst is H2, and the hydrogen treatment temperature of the second-stage catalyst is 180-250°C.

[0025] The method for synthesizing linear α-olefins from synthesis gas of the present invention is preferably that the composition of the synthesis gas is H2 / CO=1-5:1, CO2:1-10%; at this time, the reaction conditions of the synthesis are: the reaction temperature of the first stage catalyst is 250-380°C, the reaction temperature of the second stage catalyst is 200-300°C, the pressure is 0.1-5.0MPa, and the space velocity of the first stage catalyst raw gas is 1000-20000mL·h -1 gFeCat -1 .

[0026] In the method for synthesizing linear α-olefins from synthesis gas described in the present invention, it is preferred that the synthesis gas contains 0-10% of inert gas, and the inert gas comprises at least one of Ar, He, N2, and CH4.

[0027] The method for synthesizing linear α-olefins from synthesis gas provided by the present invention, specifically, each catalyst can be prepared by the following method:

[0028] (1) Preparation of a first-stage iron-based catalyst:

[0029] Mix Fe(III) salt and Fe(II) salt with water in a mass ratio of 1:8 to 8:1 to form an iron salt solution, and add a quantitative 3-13mol / L HCl solution. At 60°C, add 1-10% NH3·H2O solution at a uniform rate, and adjust the acidic pH value of the solution to about pH 10. After the addition is completed, stir at a constant temperature for 1-8h and cool to room temperature. After the reaction is completed, separate the deposited product by magnetic field adsorption, wash it with deionized water to neutrality, and dry it for use, referred to as Fe-Cat.

[0030] Weigh 5 g of the Fe-Cat sample prepared by the above method, and prepare the corresponding K and Mn salt solutions according to the required auxiliary agent content. Immerse an equal volume of 5 g of the iron catalyst Fe-Cat sample in the above-prepared salt solution and stir, then let it stand for 3-20 hours, dry at 60-100°C, and roast at 500-850°C for 3-10 hours. Finally, grind, tablet and sieve (20-40 mesh) before use to obtain.

[0031] The iron component of the iron-based catalyst prepared by this method is mainly iron oxide, mainly Fe3O4 and Fe2O3, and the Fe-Cat containing additives finally obtained is K-Mn-Fe2O3.

[0032] (2) Preparation of second-stage Ni-based catalyst:

[0033] Weigh the γ-Al2O3 sample, prepare the corresponding Ni salt solution according to the required Ni content, immerse an equal volume of γ-Al2O3 in the prepared Ni salt solution, stir and stand for 3-20 hours, dry at 60-100°C, calcine at 500-850°C for 3-10 hours, and finally grind, tablet and sieve (20-40 mesh) to obtain.

[0034] The method for synthesizing linear α-olefins from synthesis gas provided by the present invention, specifically, each catalyst can be evaluated by the following method:

[0035] The catalyst performance evaluation is carried out in a stainless steel fixed bed reactor (with an inner diameter of 14 mm). The iron-based catalyst is a first-stage catalyst, and the nickel-based catalyst or the cobalt-based catalyst is a second-stage catalyst. The two-stage catalysts are loaded at a certain mass ratio, and the catalyst particle size is 20-40 mesh. The catalyst bed is located in the constant temperature section of the heating furnace. Before the reaction, the catalyst is reduced and pretreated at 250-350°C under pure hydrogen conditions for 8-10 hours. After the reduction is completed, the reaction temperature is adjusted at a rate of 1°C / min, and the reaction raw gas (a mixture of H2 / CO / N2, N2 as an internal standard, and a H2 / CO volume ratio of 0.5:1-4:1) is switched, and the back pressure is set to the reaction pressure (1.0-3.0MPa). The reaction product is analyzed online by gas chromatography, and the reaction tail gas is directly heated and enters the first gas chromatograph for online analysis of all organic products. Then the product is cooled by a cold trap and enters the second gas chromatograph for analysis of N2, CO2, CO, and CH4. The reaction data are all obtained after the reaction is stable. The CO conversion rate was calculated by the N2 internal standard method, and the selectivity of hydrocarbon products was calculated by the area normalization method using the chromatographic peak areas after correction. The specific calculation method is as follows:

[0036] The CO conversion rate is calculated as follows:

[0037]

[0038] The CO2 selectivity calculation formula is as follows:

[0039]

[0040] The product hydrocarbon selectivity is calculated as follows:

[0041]

[0042] In the above formula, CO in and CO out represent the molar fractions of CO at the reactor inlet and outlet, CO 2out Represents the mole fraction of CO2 at the reactor outlet.

[0043] Beneficial effects of the present invention:

[0044] The reaction effects of synthesizing LAO from synthesis gas of the present invention are as follows: CO conversion rate>60%, CO conversion rate>70% can be obtained under optimized conditions, and CO conversion rate>80% can be obtained under further optimized conditions; olefin mass content in hydrocarbon products>65%, and olefin mass content in hydrocarbon products>70% can be obtained under optimized conditions; alpha-olefin linearity>60%, alpha-olefin linearity>65% can be obtained under optimized conditions, and alpha-olefin linearity>75% can be obtained under further optimized conditions. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 This is the full fraction distribution diagram of the hydrocarbon products after reacting for 75 hours in Example 8. DETAILED DESCRIPTION

[0046] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.

[0047] In the method for synthesizing linear α-olefins from synthesis gas provided by the present invention, in some embodiments, a first-stage iron-based catalyst can be prepared by the following method:

[0048] Mix Fe(III) salt and Fe(II) salt with water in a mass ratio of 1:8 to 8:1 to form an iron salt solution, and add 1-15mL of 3-13mol / L HCl solution. At 60°C and under stirring conditions, add NH3·H2O solution with a mass percentage concentration of 1-10wt% at a uniform rate, and adjust the acidic pH value of the solution to a pH value of about 10. After the addition is completed, stir at a constant temperature for 1-8h and cool to room temperature. After the reaction is completed, separate the deposited product by magnetic field adsorption, wash it with deionized water to neutrality, and dry it for use, referred to as Fe-Cat.

[0049] Weigh 5 g of the Fe-Cat sample prepared by the above method, prepare the corresponding K and Mn salt solutions according to the required additive content, immerse an equal volume of 5 g of the iron catalyst sample in the above-prepared salt solution, stir, let stand for 3-20 hours, dry at 60-100 ° C, calcine at 500-850 ° C for 3-10 hours, and finally grind, tablet and sieve (20-40 mesh) before use to obtain.

[0050] Example 1-1

[0051] (I) Preparation of one-stage catalyst-iron-based catalyst:

[0052] (1) 47.43 g FeCl3·6H2O and 18.81 g FeCl2·4H2O were mixed with 150 mL water to form an iron salt solution, and 7.65 mL of 12.1 mol / L HCl solution was added. About 550 mL of 5% NH3·H2O solution was added at a constant speed at 60°C with stirring. Within about 2 h, the acidic pH value of the solution was adjusted to a pH value of about 10. After the addition was completed, the solution was stirred at a constant temperature for 1 h and cooled to room temperature. After the reaction was completed, the deposited product was separated by magnetic field adsorption, washed with deionized water until neutral, and dried for use, referred to as Fe-Cat.

[0053] (2) Potassium chloride and manganese sulfate were used to prepare an impregnation solution of 5 mL, wherein the concentrations of potassium and manganese in the impregnation solution were 30 mg / mL and 15 mg / mL, respectively. 5 g of Fe-Cat sample was impregnated in the above-prepared 5 mL impregnation solution, stirred and then allowed to stand for 15 h, dried at 60° C., calcined at 500° C. for 3 h, and finally ground, tableted and sieved (20-40 mesh) before use to obtain an iron-based catalyst. The iron-based catalyst contained 1.5 wt% Mn and 3.0 wt% K.

[0054] (II) Preparation of second-stage catalyst-nickel-based catalyst:

[0055] 5 mL of impregnation solution was prepared with nickel nitrate, the concentration of nickel in the impregnation solution was 5 mg / mL, 5 g of γ-Al2O3 was impregnated in the prepared Ni salt solution, stirred and allowed to stand for 15 h, dried at 60 ° C, calcined at 500 ° C for 3 h, and finally ground, tableted and sieved (20-40 mesh) to obtain Ni-Cat. The nickel-based catalyst contains 0.5 wt% of Ni in terms of its oxide mass.

[0056] (III) Synthesis reaction

[0057] The first stage catalyst and the second stage catalyst were loaded in layers at a ratio of 1:1 (not in contact with each other), with a catalyst loading of 1g, and pre-treated at 250℃ for 8h under pure hydrogen conditions. After the reduction was completed, the temperature was adjusted to 300℃ at a rate of 1℃ / min, and the reaction raw gas (mixed gas of H2 / CO / N2, N2 as internal standard, H2 / CO volume ratio of 2 / 1, N2: 4%) was switched, and the back pressure was set to a reaction pressure of 2.0MPa. The catalyst was heated at 300℃, 2.0MPa, 4000ml·gCat -1 ·h -1 The reaction performance test was carried out under the following conditions, and the measured reaction performance of direct synthesis of linear α-olefins from synthesis gas is listed in Table 1.

[0058] Example 1-2

[0059] The difference from Example 1-1 is that the first-stage catalyst and the second-stage catalyst are filled in a ratio of 3:1.

[0060] Examples 1-3

[0061] The difference from Example 1-1 is that the first-stage catalyst and the second-stage catalyst are filled in a ratio of 5:1.

[0062] Table 1

[0063]

[0064]

[0065] It can be seen from the results in Table 1 that as the mass ratio of the first-stage catalyst to the second-stage catalyst in the composite catalyst decreases, the CO conversion of the catalytic reaction first increases and then decreases, and reaches a maximum value when the mass ratio is 3. The selectivity of hydrocarbon products does not change significantly and is basically controlled at 57-59%. The olefin content increases with the decrease of the mass ratio within the investigated ratio range, and basically maintains at 65% after the mass ratio drops to 3.

[0066] Therefore, when the mass ratio of the first-stage catalyst to the second-stage catalyst in the multi-stage catalyst of the present invention is 1:1 to 5:1, the composite catalyst exhibits excellent performance in converting synthesis gas to linear α-olefins.

[0067] Example 2

[0068] The catalyst preparation steps are the same as those in Example 1-1, except that the Ni in the second-stage catalyst preparation process is replaced by Co to obtain a Co-Al2O3 catalyst, which is used as the second-stage catalyst for the reaction. After the catalyst is pre-reduced with hydrogen at 350°C, the performance of synthesizing LAO is evaluated at 310°C, 3.0 MPa, and 2000 ml / (gCat·h). The performance is compared with that of the Ni-Al2O3 prepared in Example 1 under the same reaction conditions after reduction at 350°C. The reaction results are listed in Table 2.

[0069] Table 2

[0070] catalyst <![CDATA[K-Mn-Fe-Cat / Co-Al2O3]]> <![CDATA[K-Mn-Fe-Cat / Ni-Al2O3]]> CO conversion rate (mol%) 97.3 97.9 Hydrocarbon product selectivity (C%) 62.5 63.7 Olefin / Hydrocarbon Products (C%) 59.7 45.7 Olefin products (C%) <![CDATA[C 2-3 = ]]> 40.7 28.3 <![CDATA[C 4-5 = ]]> 24.9 37.1 <![CDATA[C 6-15 = ]]> 28.3 20.0 <![CDATA[C 16-18 = ]]> 0.9 2.5 <![CDATA[C 18+ = ]]> 5.2 12.1 <![CDATA[LAO in C 4-18 = ]]> 76.0 70.1 <![CDATA[LAO in C 6-15 = ]]> 70.0 62.1

[0071] As can be seen from Table 2, the CO conversion rate of the two catalysts can reach more than 97%, but the olefin selectivity is reduced. The distribution of high carbon olefins in Ni-Al2O3 tends to form more C 4-5 olefins, while Co-Al2O3 tends to form more C 6-15 Olefins. As for the linearity of high carbon olefins, Co-Al2O3 is dominant.

[0072] It can be seen from this that when the second-stage catalyst of the composite catalyst of the present invention adopts Co-Al2O3, the composite catalyst can also show excellent performance of converting synthesis gas to linear d-olefins.

[0073] Example 3-1

[0074] The catalyst used was the K-Mn-Fe-Cat / Ni-Al2O3 catalyst prepared in Example 1-1, except that the filling method in the two-stage catalyst evaluation was changed to powder mixed filling, and the reaction performance was compared with the layered filling method. -1 ·h -1 The reaction performances are listed in Table 3.

[0075] Example 3-2

[0076] The catalyst used was the K-Mn-Fe-Cat / Ni-Al2O3 catalyst prepared in Example 1-1, except that the filling method during the two-stage catalyst evaluation was changed to mixed particle filling (particle size 20-40 mesh), and the reaction performance was compared with the layered filling method. -1 ·h -1 The reaction performances are listed in Table 3.

[0077] Table 3

[0078] Example 3-1 3-2 1-1 Filling method Powder Mixing Particle mixing Layered filling CO conversion rate (mol%) 97.9 95.1 92.2 Hydrocarbon product selectivity (C%) 58.7 54.4 53.7 Olefin / Hydrocarbon Products (C%) 50.7 69.8 70.8 Olefin products (C%) <![CDATA[C 2-3 = ]]> 28.3 29.5 31.3 <![CDATA[C 4-5 = ]]> 37.1 29.9 31.8 <![CDATA[C 6-15 = ]]> 20.0 26.5 26.1 <![CDATA[C 16-18 = ]]> 2.5 7.7 4.0 <![CDATA[C 18+ = ]]> 12.1 6.3 6.8 <![CDATA[LAO in C 4-18 = ]]> 70.1 87.1 84.4 <![CDATA[LAO in C 6-15 = ]]> 62.1 84.0 77.1

[0079] Combined with the results in Table 3, it can be seen that as the filling method changes from powder mixing to particle mixing and then to layered filling, the contact tightness of the active components of the two-stage catalyst gradually decreases, the CO conversion rate and hydrocarbon product selectivity of the catalytic reaction gradually decrease, but the content of olefins in the hydrocarbon products gradually increases. In the distribution of olefin products, the target product olefin C 6-15 The olefin content and linear α-olefin content of the catalyst with mixed particle filling are the highest. This is related to the close contact between the two active components of the powder mixed filling catalyst, the generated low-carbon olefin intermediate active species are easy to hydrogenate to alkanes, thereby reducing the olefin product content, and the layered filling of the two active components is difficult to achieve the ideal synergistic catalytic effect.

[0080] From the above results, it can be seen that the two-stage catalyst can be filled in three ways, with particle mixing and layered filling being preferred, and layered filling being the best.

[0081] Example 4-1: The difference from Example 1-1 is that the reduction temperature in the synthesis reaction of step (iii) is 300°C.

[0082] Example 4-2: The difference from Example 1-1 is that the reduction temperature in the synthesis reaction of step (iii) is 350°C.

[0083] The reaction results of Example 1-1 and Examples 4-1 and 4-2 are listed in Table 4 respectively, and the influence of the catalyst reduction temperature is investigated.

[0084] Table 4 Effect of reduction temperature on the catalytic performance of K-Mn-Fe-Cat / Ni-Al2O3 catalyst

[0085] Example 1-1 Example 4-1 Example 1-2 Reduction temperature(℃) 250 300 350 CO conversion rate (mol%) 61.4 83.0 92.2 Hydrocarbon product selectivity (C%) 58.2 59.9 58.7 Olefin / Hydrocarbon Products (C%) 64.7 68.7 65.8 Olefin products (C%) <![CDATA[C 2-3 = ]]> 16.9 28.2 31.3 <![CDATA[C 4-5 = ]]> 15.8 30.1 31.8 <![CDATA[C 6-15 = ]]> 17.8 26.4 26.1 <![CDATA[C 16-18 = ]]> 33.6 7.2 4.0 <![CDATA[C 18+ = ]]> 16.0 9.1 6.8 <![CDATA[LAO in C 4-18 = ]]> 77.2 88.4 84.4 <![CDATA[LAO in C 6-15 = ]]> 79.3 84.1 77.1

[0086] From the results in Table 4, it can be seen that within the temperature range investigated, as the reduction temperature increases, the CO conversion rate gradually increases, and the hydrocarbon product selectivity and the olefin content in the hydrocarbon product reach the optimal value at a reduction temperature of 300°C. From the carbon number distribution of the olefin product, it can be seen that as the reduction temperature increases, the low-carbon olefin content gradually increases, the high-carbon olefin content gradually decreases, and the target product olefin C 6-15 Olefins are basically stable in the range of 300-350℃, while C 6-15 The linear α-olefin content in olefins reaches a maximum at a reduction temperature of 300°C.

[0087] It can be seen from the above that within the selected reduction temperature range, the composite catalyst exhibits excellent reaction performance.

[0088] Example 5

[0089] The catalyst used was the K-Mn-Fe-Cat / Ni-Al2O3 catalyst prepared in Example 1-1. The catalyst evaluation conditions were: raw gas: H2 / CO=2, CO2: 5% (volume percentage concentration), 2.5MPa, 3000ml·gCat -1 ·h -1 Under the conditions, the reaction performance is listed in Table 5.

[0090] Table 5

[0091]

[0092]

[0093] As shown in Table 5, when the reaction temperature of K-Mn-Fe-Cat component is changed from 280℃ to 300℃, the CO conversion rate, hydrocarbon product selectivity, olefin content in hydrocarbon product and C 6-15 = The contents of olefins increased, but the content of linear α-olefins decreased; similarly, the reaction temperature of Ni-Al2O3 component was within the range of 200-275℃. With the increase of temperature, CO conversion rate, hydrocarbon product selectivity, olefin content in hydrocarbon products and C 6-15 =The contents of olefins all tend to increase, but the content of linear α-olefins in olefins reaches the optimum value at 225°C and then begins to decrease.

[0094] From the above results, it can be seen that the composite catalyst of the present invention exhibits excellent reaction performance for converting synthesis gas to linear alpha olefins when the reaction temperature is 280-300°C for the first stage iron-based catalyst and 200-275°C for the second stage nickel-based catalyst.

[0095] Example 6

[0096] The catalyst preparation steps were the same as in Example 1-1, except that the K-Mn-Fe-Cat component was changed to Co-K-Mn-Fe-Cat, the pre-reduction temperature of the first stage catalyst was 350°C, and under the same reaction conditions (first stage catalyst 290°C, second stage catalyst 250°C, 2.0 MPa, 4000 ml·gCat -1 ·h -1 ) compared the reaction results of the multi-stage catalyst before and after Co modification, and the comparison results are listed in Table 6.

[0097] The difference from Example 1-1 is that: "Mix 47.43g FeCl3·6H2O and 18.81g FeCl2·4H2O with 150mL water to form an iron salt solution" is replaced by "add 18.52g Co(NO3)·6H2O, 47.43g FeCl3·6H2O and 18.81g FeCl2·4H2O to 150mL water and dissolve them to form a cobalt-iron salt solution".

[0098] Table 6 Performance of Co-modified iron composite catalyst for synthesis gas to linear α-olefins

[0099]

[0100] From the results in Table 6, it can be seen that the iron-based catalyst with the addition of Co significantly increased the selectivity of light olefins while keeping the CO conversion rate and hydrocarbon product selectivity basically unchanged. 6-15 However, the olefin selectivity decreased significantly, and the linearity of high-carbon olefins increased.

[0101] The above results show that adding Co as a promoter to the first-stage iron-based catalyst in the composite catalyst of the present invention is beneficial to improving the linearity of the catalytic conversion of synthesis gas to hydrocarbon products.

[0102] Example 7-1

[0103] The catalyst preparation steps were the same as in Example 1-1, except that the hydrogen reduction temperature of the first stage catalyst was changed to 350°C. K-Mn-Fe-Cat with a Mn content of 0.5%wt Mn was prepared and reacted under the following reaction conditions (first stage catalyst 290°C, second stage catalyst 250°C, 2.0 MPa, 4000 ml·gCat -1 ·h -1 )The synthesis gas conversion reaction performance of the composite catalyst was tested, and the results are listed in Table 7.

[0104] Example 7-2

[0105] The catalyst preparation steps were the same as in Example 1-1, except that the hydrogen reduction temperature of the first stage catalyst was changed to 350°C. K-Mn-Fe-Cat with a Mn content of 3.0%wt Mn was prepared and heated under the following reaction conditions (first stage catalyst 290°C, second stage catalyst 250°C, 2.0 MPa, 4000 ml·gCat -1 ·h -1 )The synthesis gas conversion reaction performance of the composite catalyst was tested, and the results are listed in Table 7.

[0106] Table 7: Effect of Mn content on the performance of iron-based catalysts for synthesis gas to linear α-olefins

[0107] Example 7-1 1-1 7-2 Mn / Fe-Mn-K (wt%) 0.5 1.5 3.0 CO conversion rate (mol%) 96.8 97.4 96.8 Hydrocarbon product selectivity (C%) 60.0 60.1 58.7 Olefin / Hydrocarbon Products (C%) 72.7 71.9 54.7 Olefin products (C%) <![CDATA[C 2-3 = ]]> 26.4 31.2 30.8 <![CDATA[C 4-5 = ]]> 26.3 31.7 36.3 <![CDATA[C 6-15 = ]]> 46.0 36.7 32.2 <![CDATA[C 16-18 = ]]> 1.3 0.4 0.7 <![CDATA[C 18+ = ]]> --- --- --- <![CDATA[LAO in C 4-18 = ]]> 72.1 74.9 60.9 <![CDATA[LAO in C 6-15 = ]]> 62.4 65.4 44.2

[0108] As shown in Table 7, when the Mn content of the iron-based catalyst changes from 0.5% to 1.5%, the performance of the catalyst remains basically stable, except for the high carbon olefins (C 6+ ) gradually decreases, and low-carbon olefins (C 2-5 ) gradually increases; however, as the Mn content further increases, the performance of the reaction changes significantly, the olefin product content decreases, the high-carbon olefin content and its linearity decrease significantly; at the same time, the hydrocarbon product content gradually decreases. This is related to the fact that the increase in Mn content is beneficial to the water-gas shift reaction and the hydrogenation performance of the intermediate olefins.

[0109] When the content of manganese promoter in the first-stage iron-based catalyst of the composite catalyst of the present invention is 0.5-1.5wt%, the composite catalyst exhibits excellent catalytic performance.

[0110] Example 8

[0111] The catalyst preparation and evaluation steps are the same as in Example 1, except that the pre-reduction temperature of the catalyst is changed to 350°C. The reaction conditions are: Ni-Al2O3 temperature 250°C, H2 / CO=2, 2.0MPa. The stability results of the catalyst reaction are shown in Table 8.

[0112] Table 8: Stability test results of direct synthesis of LAO from syngas using multi-stage catalysts

[0113]

[0114] As shown in Table 8, during the initial 5 to 10 hours of reaction, the CO conversion rate dropped rapidly from 90.5% to 52.4%. However, during the subsequent 32 hours of reaction, the performance of the catalyst remained basically stable, with the CO conversion rate being stable at 52%, the hydrocarbon product selectivity being 56%, the olefin content in the hydrocarbon product being about 65%, and the C 6-15 The olefin is stable at ~39%, and its linearity can reach 76%. The reaction temperature and reaction space velocity are adjusted to 300℃, 4000ml·gFe-Cat -1 ·h -1 The catalyst with a reaction time of 75 h can achieve the following reaction performances: 75.8% CO conversion rate and 56.5% hydrocarbon product selectivity, 66.2% olefin content in hydrocarbon products, and 1.3% C in olefins. 6-15 Olefins account for 40.5%, and its linearity can reach 71.7%. The composition distribution of the hydrocarbon products of the reaction is shown in Figure 1 .

[0115] The multi-stage composite catalyst of the present invention not only exhibits excellent performance in converting synthesis gas to produce linear alpha-olefins, but also exhibits good catalytic stability.

[0116] Example 9

[0117] The steps of catalyst preparation and evaluation were the same as those of Example 1-1, except that in the preparation step (2) of the one-stage catalyst-iron-based catalyst, "5 g Fe-Cat sample" was changed to "4 g Fe-Cat + 1 g carrier SiO2", thereby obtaining a two-stage composite catalyst consisting of an iron-based catalyst containing a SiO2 carrier and a supported Ni-based catalyst. The reaction performance of the composite catalyst for converting syngas into linear α-olefins was as follows: CO conversion rate was 62.8%, hydrocarbon selectivity was 65.0%, olefins accounted for about 64% of the hydrocarbon products, and C 4-18 The fraction accounts for 66.4%, of which linear α-olefins account for C 4-18 78.8% of olefins.

[0118] The above reaction results indicate that the iron-based catalyst containing a carrier also exhibits high reaction performance and good stability in the conversion of synthesis gas to linear α-olefins.

[0119] Comparative Example 1

[0120] Mix 23.72g FeCl3·6H2O and 9.41g FeCl2·4H2O with 75mL water to form an iron salt solution, and add 3.83mL of 12.1mol / L HCl solution. At 60℃, add about 275mL of 5% NH3·H2O solution at a uniform rate under stirring conditions. In about 2h, adjust the acidic pH value of the solution to a pH value of about 10. After the addition is completed, stir at a constant temperature for 1h and cool to room temperature. After the reaction is completed, separate the deposited product by magnetic field adsorption, wash it with deionized water to neutrality, and dry it for use, referred to as Fe-Cat-1.

[0121] The reaction performance evaluation conditions were the same as those in Example 2. The reaction performance results showed that the CO conversion rate was 78.5%, the hydrocarbon product selectivity was 60%, the main hydrocarbon product of the reaction was alkane, and the selectivity of olefins in the hydrocarbon product was only 38%, among which the high carbon olefins C 4-18 It accounts for 76% of total olefins, while LAO accounts for only 51%.

[0122] By comparing with Examples 1-9 of the present invention, it can be seen that the selectivity of olefins in hydrocarbon products in Comparative Example 1 is significantly reduced, accounting for only 38%. It can be seen that in the synthesis gas to LAO reaction of the present invention, not only a higher CO conversion rate is achieved, but also the selectivity of olefin products is significantly increased, and the proportion of LAO in high-carbon olefins is significantly increased.

[0123] Comparative Example 2

[0124] The preparation steps of the catalyst were the same as those in Example 2, but only one stage of the catalyst was loaded during the reaction evaluation. The reaction results were as follows: CO conversion rate: 97.9%, hydrocarbon product selectivity: 64.2%, olefin selectivity in hydrocarbon products: 73.7%, of which high carbon olefins C 4-18 Accounting for 67% of total olefins, LAO accounts for 86% of high carbon olefins. 6-15 It only accounts for 27% of the olefin products.

[0125] Compared with the one-stage catalyst of Comparative Example 2, the multi-stage catalyst of the present invention significantly improves the C 6-15 The production of olefins, whose proportion (mass ratio) in the olefin products can be increased from 27% to 40-50%. This shows that the two-stage catalyst production method of the present invention is conducive to the more widely used C 6-15 Olefins are formed.

[0126] In summary, the reaction effects of synthesizing LAO from synthesis gas of the present invention are as follows: CO conversion rate>60%, the optimized conditions can obtain a CO conversion rate>70%, and the further optimized conditions can obtain a CO conversion rate>80%; the mass content of olefins in the hydrocarbon products>65%, and the optimized conditions can obtain a mass content of olefins in the hydrocarbon products>70%; the α-olefin linearity>60%, the optimized conditions can obtain an α-olefin linearity>65%, and the further optimized conditions can obtain an α-olefin linearity>75%.

[0127] Of course, the present invention may have many other embodiments. Without departing from the spirit and essence of the present invention, technicians familiar with the field may make various corresponding changes and deformations based on the present invention, but these corresponding changes and deformations should all fall within the scope of protection of the present invention.

Claims

1. A method for synthesizing linear α-olefins from synthesis gas, characterized in that: The following steps are involved: Under the conditions of 200-380°C and 0.5-5.0MPa, the synthesis gas is passed through the pretreated composite catalyst to synthesize linear α-olefins with a carbon number of 6 to 15; The composite catalyst comprises two-stage catalysts, wherein the first-stage catalyst is an iron-based catalyst, wherein the iron-based catalyst has iron-containing oxide as an active component; the second-stage catalyst is a nickel-based catalyst or a cobalt-based catalyst, wherein the nickel-based catalyst has nickel oxide as an active component, and the cobalt-based catalyst has cobalt oxide as an active component; The iron-based catalyst further comprises a promoter and a carrier, wherein the content of iron is 30%-90% by weight of the oxide, the content of the promoter is 0.8%-15%, and the content of the carrier is the remainder; the carrier is silicon dioxide; the promoter comprises 0.3%-7% of an alkali metal promoter and 0.5%-8% of a transition metal promoter, the alkali metal is K, and the transition metal is Mn; The nickel-based catalyst further comprises a carrier, wherein the nickel content is 0.1%-15% by mass of the oxide, and the carrier content is above 70%; the carrier comprises at least one of alumina and molecular sieve; The cobalt-based catalyst further comprises a carrier, wherein the content of cobalt is 0.1%-15% by weight of the oxide, and the content of the carrier is above 70%; the carrier comprises at least one of alumina and molecular sieve; The filling mass ratio of the first stage catalyst to the second stage catalyst is 1:5-5:1, and the filling method of the first stage catalyst and the second stage catalyst is layered filling without contact with each other; The pretreatment is a reducing gas treatment, the reducing gas used is hydrogen, the reduction temperature of the first stage catalyst is 250-350°C, and the reduction temperature of the second stage catalyst is 180-250°C.

2. The method for synthesizing linear α-olefins from synthesis gas according to claim 1, characterized in that: The iron-containing oxide is ferroferric oxide and / or ferrous oxide.

3. The method for synthesizing linear α-olefins from synthesis gas according to claim 2, characterized in that: The iron-containing oxide is ferroferric oxide.

4. The method for synthesizing linear α-olefins from synthesis gas according to claim 1, characterized in that: The iron-containing oxide is generated by reducing a precursor, and the molar ratio of Fe(III) to Fe(II) in the precursor is 1 / 5 to 8 / 1.

5. The method for synthesizing linear α-olefins from synthesis gas according to claim 4, characterized in that: The iron-containing oxide is generated by reducing a precursor, and the molar ratio of Fe(III) to Fe(II) in the precursor is 1 / 3-5 / 1.

6. The method for synthesizing linear α-olefins from synthesis gas according to claim 1, characterized in that: The nickel oxide is partially reduced nickel oxide.

7. The method for synthesizing linear α-olefins from synthesis gas according to claim 1, characterized in that: The carrier content in the nickel-based catalyst is above 75%.

8. The method for synthesizing linear α-olefins from synthesis gas according to claim 1, characterized in that: The cobalt oxide is partially reduced cobalt oxide.

9. The method for synthesizing linear α-olefins from synthesis gas according to claim 1, characterized in that: The carrier content in the cobalt-based catalyst is above 75%.

10. The method for synthesizing linear α-olefins from synthesis gas according to claim 1, characterized in that: The filling mass ratio of the first stage catalyst to the second stage catalyst is 1:1-3:

1.

11. The method for synthesizing linear α-olefins from synthesis gas according to claim 1, characterized in that: The composition of the synthesis gas is H2 / CO = 1-5:1, CO2: 1~10%; at this time, the reaction conditions of the synthesis are: the reaction temperature of the first stage catalyst is 250-380°C, the reaction temperature of the second stage catalyst is 200-300°C, the pressure is 0.1-5.0MPa, and the space velocity of the first stage catalyst raw gas is 1000-20000 mL·h -1 gFeCat -1 .

12. The method for synthesizing linear α-olefins from synthesis gas according to claim 11, characterized in that: The synthesis gas contains 0-10% of inert gas, which is not 0, and the inert gas includes at least one of Ar, He, N2, and CH4.

Citation Information

Patent Citations

  • Method for deoxidizing and synthesizing hydrocarbon of molten iron, cobalt catalyst in use for Fischer - Tropsch synthesis