Bismuth-containing compound, preparation method and application

By preparing bismuth-containing compounds as light extraction layer materials, the problem of low light extraction efficiency in OLED devices was solved, the external light emission efficiency of top-emitting devices was improved, and the feasibility of large-area processing was realized.

CN114380865BActive Publication Date: 2024-11-15PEKING UNIV SHENZHEN GRADUATE SCHOOL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202011118628.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2020-10-19
Publication Date
2024-11-15
Estimated Expiration
2040-10-19

AI Technical Summary

Technical Problem

Existing OLED devices have low light extraction efficiency, especially top-emitting devices which suffer from severe light loss, limiting their applications. Furthermore, commonly used light extraction layer materials are not suitable for large-area processing.

Method used

We designed and prepared bismuth-containing compounds as optical extraction layer materials. By introducing different organic functional groups, we changed the electron distribution and molecular packing of the materials, controlled the refractive index, and achieved solution-processable processing.

Benefits of technology

It improves the external light emission efficiency of OLED top-emitting devices, realizes the multi-functional application of materials, and is suitable for large-area processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN114380865B_ABST
    Figure CN114380865B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of organic light-emitting materials, and specifically to a bismuth-containing compound, a preparation method and an application thereof. The bismuth-containing compound introduces different organic functional groups on bismuth to change the electronic distribution and molecular stacking of the material, regulate the refractive index and thermal stability of the material, and the introduction of different functional groups can change the solubility of the material to achieve a solution-processable organic light extraction layer material. At the same time, the bismuth-based organic compound has strong fluorescence and can be used not only as a light extraction layer, but also as a light-emitting layer of an OLED device, realizing multiple functional applications of a material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of organic luminescent materials, and in particular to a bismuth-containing compound, a preparation method and an application thereof. Background Art

[0002] Organic light-emitting diodes (OLEDs) have been widely used in new light-emitting and display fields due to their advantages such as small thickness, light weight, no viewing angle problems, simple manufacturing process, low cost, high luminous efficiency, and roll-to-roll processing. They have been successfully applied in smart phones, televisions, lighting, large-screen displays and other fields, and have received extensive attention and research from academia and industry.

[0003] Since the discovery of organic light-emitting diodes (OLEDs), organic small molecule luminescent materials and luminescent devices have continued to make progress, with great improvements in luminous efficiency and stability. According to the structure of OLED devices, we can divide the devices into bottom-emitting and top-emitting devices. For bottom-emitting devices, in practical applications, since their optical path passes through the TFT array, the outgoing light will be scattered and absorbed when passing through the TFT array, which reduces the light output rate of the device. For top-emitting OLED light-emitting devices, due to the influence of factors such as the waveguide effect, most of the light emitted by the OLED device is reflected layer by layer in the organic layer, and the light is lost layer by layer inside the device, and part of it is converted into heat, which affects the stability of the organic layer material, causing its efficiency roll-off to become serious and the life span to be greatly reduced. In top-emitting devices, only about 20% of the light can be exported from the device for use by us, which reduces the external luminous efficiency of OLED and limits its application. Therefore, improving the light extraction efficiency is also a key research focus of OLED that needs to be solved at present.

[0004] At present, the method to improve the light extraction efficiency is to plate a light extraction layer on the surface of the OLED device electrode to increase the light extraction efficiency. Usually, some high refractive index materials are selected as the light extraction layer to reduce the light loss inside the device and improve the luminous efficiency. However, there are not many types of commonly used light extraction layers, and most of them are metal oxides. They all need to be formed by evaporation, which is not conducive to large-area processing. Therefore, it is very important to design a new type of high refractive index light extraction layer material. Summary of the invention

[0005] In view of the above shortcomings of light extraction layer materials, the present invention provides a bismuth-containing compound, a preparation method and application.

[0006] The technical solution of the present invention is achieved by providing a bismuth-containing compound having the following molecular formula:

[0007]

[0008] Wherein, R1, R2, and R3 are aromatic groups, and the bismuth-containing compound is a semiconductor.

[0009] Preferably, in the bismuth-containing compound of the present invention, R1, R2, and R3 are the same or different functional groups.

[0010] Preferably, in the bismuth-containing compound of the present invention, R1, R2, and R3 are any one of the following functional groups:

[0011]

[0012]

[0013]

[0014] On the other hand, the present invention also provides an organic light extraction layer material, which is obtained by polymerizing the above-mentioned bismuth-containing compound as a monomer.

[0015] On the other hand, the present invention also provides a bismuth-containing polymer compound, which is a polymer with Bi as the main chain, obtained by polymerizing the bismuth-containing compound of any one of claims 1 to 3 as a monomer.

[0016] Preferably, the bismuth-containing polymer compound of the present invention is one of the following structural formulas:

[0017]

[0018] On the other hand, the present invention also provides a method for preparing a bismuth-containing polymer compound, and the preparation principle is as follows:

[0019]

[0020] Among them, R1, R2, and R3 are aromatic groups, the monomer used is a bismuth-containing compound, and the bismuth-containing compound is a semiconductor.

[0021] On the other hand, the present invention also provides a bismuth-containing polymer compound, wherein the aforementioned bismuth-containing compound is used as a donor / acceptor unit and copolymerized with other small molecule donors and acceptors to form a DA, DAD or ADA copolymer.

[0022] Preferably, in the bismuth-containing polymer compound of the present invention, the other small molecule donor and acceptor is any one of the following small molecule units:

[0023]

[0024] Preferably, the bismuth-containing polymer compound of the present invention is one of the following structural formulas:

[0025]

[0026] The beneficial effects are as follows:

[0027] In order to improve the external luminous efficiency in OLED top-emitting devices, based on the current material research system, we have designed a new type of organic light extraction layer material based on bismuth compounds with bismuth as the core. Different organic functional groups are introduced on bismuth to change the electronic distribution and molecular stacking of the material, regulate the refractive index and thermal stability of the material, and the introduction of different functional groups can change the solubility of the material to achieve solution-processable organic light extraction layer materials. At the same time, bismuth-based organic compounds have strong fluorescence and can be used not only as a light extraction layer, but also as a light-emitting layer of OLED devices, realizing multiple functional applications of one material. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The figure is a schematic diagram of the structure of a top emission device made by using the bismuth-containing compound of the present invention. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the specific embodiments of the present invention and the corresponding drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0030] The present invention is further described in detail below with reference to the accompanying drawings and embodiments.

[0031] The bismuth-containing compounds of the present invention include but are not limited to:

[0032]

[0033]

[0034]

[0035]

[0036]

[0037]

[0038]

[0039]

[0040]

[0041]

[0042]

[0043] The above structures are only partial representatives. Other molecules with the same idea are all within the scope of protection of this patent. At the same time, the introduction of some alkyl chains, alkoxy chains, CN, F, Cl and other groups on the aromatic group of the molecule is also included in the scope of this patent.

[0044] Example 1 (Synthesis of symmetrically substituted compounds):

[0045]

[0046] Under an inert gas atmosphere, 1.57 g of bromobenzene was dissolved in 60 ml of anhydrous THF, two iodine grains and 2.16 g of fresh magnesium chips were added, and the reaction was initiated by heating. 7.85 g of bromobenzene was slowly added thereto, and the mixture was heated under reflux for 2 h, cooled, 6.3 g of BiCl3 was dissolved in 20 ml of THF, added to the Grignard reagent, and stirred for overnight reaction. Water was added to quench the reaction, and the mixture was extracted and purified by concentration column chromatography to obtain 5.2 g of a white solid with a yield of 59%. The refractive index was 1.82.

[0047] For the synthesis of asymmetric bismuth compounds, the ratio of the Grignard reagent can be changed to synthesize the product.

[0048] Example 2 (Synthesis of asymmetrically substituted compounds):

[0049]

[0050] Under an inert gas atmosphere, 1.57 g of bromobenzene was dissolved in 60 ml of anhydrous THF, two iodine grains and 2.16 g of fresh magnesium chips were added, and the reaction was initiated by heating. 7.85 g of bromobenzene was slowly added thereto, and the mixture was heated under reflux for 2 h. After cooling, 9.45 g of BiCl3 was dissolved in 20 ml of THF and added to the Grignard reagent, and the reaction was stirred overnight. Water was added to quench the reaction, and the mixture was extracted and purified by concentration column chromatography to obtain 7.2 g of a white solid with a yield of 60.3%.

[0051] Under an inert gas atmosphere, 0.5 g of bromonaphthalene was dissolved in 30 ml of anhydrous THF, two iodine grains and 0.36 g of fresh magnesium chips were added, and the reaction was initiated by heating. 1.56 g of bromobenzene was slowly added thereto, and the mixture was heated under reflux for 2 h. After cooling, 3.98 g of diphenylbismuth chloride was dissolved in 10 ml of THF and added to the Grignard reagent, and the reaction was stirred overnight. Water was added to quench the reaction, and the mixture was extracted and purified by concentration column chromatography to obtain 2.8 g of a white solid with a yield of 57%. The refractive index was 1.88.

[0052] Embodiment 3 (Synthesis of condensed ring compounds):

[0053]

[0054] Under anhydrous and oxygen-free nitrogen atmosphere, 1.38g of the reaction raw material was dissolved in 100ml of tetrahydrofuran, cooled to -78°C, and n-BuLi 24ml (2.5M) was added dropwise. After the addition was complete, the reaction system was heated and refluxed for 3h, cooled to -78°C again, and 1.335g of bismuth tribromide was added. Warm to room temperature, stir for 1h, cool to 0°C, add 10.3g of diisopropylethylamine, and heat under reflux overnight. Cool, add water to quench, extract with chloroform, concentrate, and purify by column chromatography to obtain 0.52g of a yellow solid with a yield of 30.1%. The refractive index is 1.91.

[0055] The bismuth-containing compound we prepared was used to prepare a top-emitting device, and the device structure is as follows Figure 1 As shown, the device performance is shown in the following table:

[0056] Light extraction layer CE(cd / A) EQE(%) Compound 11 110.5 28.2 Compound 26 106.3 25.4 Compound 32 127.4 34.3 Compound 41 131.5 36.8 Compound 48 118.4 31.4 Compound 77 132.3 37.5

[0057] We also considered introducing the above small molecules into polymers as side chain modifications to design and synthesize Bi-based polymer compounds, such as:

[0058]

[0059] At the same time, we also consider using the bismuth-containing compound of the present invention as a monomer to polymerize to obtain a polymer with Bi as the main chain, and then spin-coating the polymer by a solution method to obtain the desired film. The polymer structure is shown below, that is, we can obtain a linear polymer and a cross-linked polymer:

[0060]

[0061] The following are some examples of polymer structures based on the bismuth-containing compound of the present invention as a monomer:

[0062]

[0063] In addition, the bismuth-containing compound of the present invention is used as a monomer, as a donor / acceptor unit, and copolymerized with other small molecule donors and acceptors to form copolymers such as DA, DAD, and ADA, for example, copolymerized with the following small molecule units, wherein R is F, Cl, Br, CN, nitro, alkyl chain, or alkoxy chain:

[0064]

[0065] Its possible structural formula is listed below:

[0066]

[0067] The polymer structures listed above are only partial representatives, and other Bi-containing polymer molecules with the same concept are all within the scope of protection of this patent.

[0068] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A bismuth-containing compound, characterized in that The molecular formula is as follows: Wherein, R1, R2, and R3 are the same aromatic groups, and the bismuth-containing compound is a semiconductor; R1, R2, and R3 are any one of the following functional groups: